Conductive adhesive liquid, electrode sheet and its preparation method and battery
By forming a conductive adhesive layer on the electrode, the problem of powder shedding during lithium battery electrode cutting is solved, improving the production qualification rate and the safety and lifespan of the battery.
Patent Information
- Application Number
- CN202611182583.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-10
AI Technical Summary
Lithium-ion battery electrodes are prone to powder shedding during cutting, which leads to waste of active materials and short circuits inside the cell, affecting safety and cycle life.
A conductive adhesive liquid is used, which includes conductive filler, thermoplastic resin, heat-triggered crosslinking agent and solvent. The conductive adhesive layer is formed through heat treatment, which enhances the bonding strength and electrolyte resistance of the electrode and reduces the powder shedding rate.
Effectively controlling the powder loss rate of electrode sheets during cutting to less than 0.1% improves the production qualification rate, reduces material loss, and enhances the safety and cycle life of lithium batteries.
Smart Images

Figure CN123063102A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, specifically to a conductive adhesive liquid, an electrode sheet, a method for preparing the same, and a battery. Background Technology
[0002] Lithium-ion batteries are widely used in new energy vehicles, energy storage devices, and consumer electronics due to their high energy density, long cycle life, and environmental friendliness. As a core component of lithium-ion batteries, the quality of their fabrication directly affects the battery's performance and safety. Currently, during the fabrication of lithium-ion battery electrodes (especially negative electrodes), after coating, drying, and rolling (cold pressing) processes, powder shedding easily occurs at the electrode edges during die-cutting. This powder shedding not only wastes active materials and reduces the production yield, but can also lead to internal short circuits within the cell, affecting the safety and cycle life of the lithium-ion battery. Summary of the Invention
[0003] This application provides a conductive adhesive liquid, an electrode sheet, a method for preparing the same, and a battery, aiming to solve the problem of powder shedding during electrode sheet cutting.
[0004] This application provides a conductive adhesive liquid, which, by mass percentage, comprises 10%~30% conductive filler, 40%~60% thermoplastic resin, 5%~15% heat-triggered crosslinking agent, and 10%~20% solvent.
[0005] After the conductive adhesive liquid of the above formula is applied to the active material layer of the electrode and cross-linked and cured by heat treatment to form a conductive adhesive layer, the powder loss rate of the electrode during cutting can be controlled to less than or equal to 0.1%, thereby improving the production qualification rate and reducing material loss.
[0006] Optionally, in some embodiments of this application, the conductive filler includes at least one of carbon nanotubes, conductive carbon black, and graphene.
[0007] The aforementioned conductive filler has excellent conductivity and dispersibility, which can effectively reduce the volume resistivity of the conductive adhesive layer.
[0008] Optionally, in some embodiments of this application, the thermoplastic resin includes at least one of polyvinylidene fluoride and polyimide.
[0009] The polymer formed by cross-linking the above-mentioned thermoplastic resin has good thermal stability, electrolyte resistance and adhesive properties. It is solid at room temperature and can melt at high temperature to achieve bonding. It is also suitable for room temperature roller pressing and will not deform or stick due to roller pressing.
[0010] Optionally, in some embodiments of this application, the thermally triggered crosslinking agent includes at least one of dicumyl peroxide and benzoyl peroxide.
[0011] The aforementioned heat-triggered crosslinking agent enhances the bonding strength and electrolyte resistance of the resulting conductive adhesive layer by triggering crosslinking of the thermoplastic resin at high temperatures.
[0012] Optionally, in some embodiments of this application, the solvent includes at least one of N-methylpyrrolidone and dimethyl sulfoxide.
[0013] The solvents described above can fully dissolve the components to form a uniform adhesive solution. Furthermore, the solvents are volatile and can be completely removed during heat treatment, leaving no residue in the conductive adhesive layer.
[0014] Accordingly, this application also provides an electrode sheet, comprising: current collector; An active material layer is disposed on the current collector; and A conductive adhesive layer is disposed on the active material layer, wherein the conductive adhesive layer is formed by cross-linking and curing of the above-mentioned conductive adhesive liquid after heat treatment.
[0015] The electrode provided in this application includes a current collector, an active material layer, and a conductive adhesive layer stacked sequentially. The conductive adhesive layer is formed by cross-linking and curing a conductive adhesive liquid, which is formulated with conductive filler, thermoplastic resin, thermally triggered cross-linking agent, and solvent, after heat treatment. Thus, the conductive adhesive layer has four major characteristics: conductivity, room temperature inertness, high temperature adhesion, and resistance to electrolyte swelling. The conductive adhesive layer can not only improve the problem of powder shedding during electrode cutting, but also reduce the cell interface resistance and improve the adhesion between the electrode and the separator when the electrode is used in the battery, thereby improving the overall stability of the cell structure and enhancing the safety, economy, and cycle life of the lithium battery.
[0016] Optionally, in some embodiments of this application, the electrode is a negative electrode and the active material layer is a graphite-based active material layer.
[0017] The active material of the graphite-based active material layer is graphite. The adhesion of graphite in the negative electrode sheet is relatively weak, making it more prone to powder shedding during cutting. The conductive adhesive layer attached to the graphite-based active material layer can effectively improve the powder shedding problem.
[0018] Optionally, in some embodiments of this application, the adhesion of the conductive adhesive layer to the active material layer is ≥2.0N / 25mm.
[0019] In this case, it can be ensured that the conductive adhesive layer does not fall off during rolling, cutting and subsequent processes, effectively playing the role of preventing powdering and bonding.
[0020] Accordingly, this application also provides a method for preparing an electrode, comprising: A first initial electrode is provided, the first initial electrode comprising a current collector and an active material layer located on the current collector; A conductive adhesive layer is prepared on the surface of the active material layer, the conductive adhesive layer comprising the above-mentioned conductive adhesive; The conductive adhesive liquid layer is heat-treated to cross-link and solidify the conductive adhesive liquid to form a conductive adhesive layer, thereby obtaining a second initial electrode sheet; The second initial electrode is cut to obtain an electrode sheet.
[0021] The electrode prepared by the method provided in this application has a conductive adhesive layer. The conductive adhesive layer can effectively control the powder loss rate of the electrode during cutting to ≤0.1%, thereby improving the production qualification rate and reducing material loss.
[0022] Optionally, in some embodiments of this application, providing the first initial electrode includes: Electrode paste is deposited on a current collector to form an active material layer; The active material layer is subjected to a first rolling process to obtain a first initial electrode sheet, and the temperature of the first rolling process is a first temperature.
[0023] After densifying the active material layer through the first roll pressing process, a conductive adhesive layer is then prepared on the active material layer. This improves the bonding strength of the materials inside the active material layer and strengthens the bonding force between the active material layer and the conductive adhesive layer, thus improving the problem of powder shedding during electrode cutting.
[0024] Optionally, in some embodiments of this application, the temperature of the heat treatment is a second temperature, which is greater than the first temperature.
[0025] Optionally, in some embodiments of this application, the conductive adhesive liquid layer is prepared by spraying.
[0026] Spraying produces a uniform, high-quality conductive adhesive layer, ensuring full coverage and reducing the problem of missed areas.
[0027] Optionally, in some embodiments of this application, the spraying is atomized spraying.
[0028] Atomized spraying allows the conductive adhesive to be evenly covered to the edge of the first initial electrode, reducing the possibility of adhesive accumulation or missed spraying.
[0029] Optionally, in some embodiments of this application, the first rolling process is a cold pressing process.
[0030] Cold pressing is a physical compression method that can reduce the gaps between particles in the active material layer, thereby increasing the density of the active material layer.
[0031] Optionally, in some embodiments of this application, the thickness of the conductive adhesive liquid layer is 1μm to 10μm.
[0032] By controlling the thickness of the conductive adhesive layer, powder shedding can be prevented and the separator can be bonded while ensuring the electrochemical performance of the battery.
[0033] Optionally, in some embodiments of this application, the heat treatment is infrared shortwave drying treatment.
[0034] Infrared short-wave drying not only allows the solvent in the conductive adhesive layer to evaporate quickly, but also enables the heat-triggered crosslinking agent to promote the rapid crosslinking and curing of the thermoplastic resin, thus accelerating the formation of the conductive adhesive layer.
[0035] Optionally, in some embodiments of this application, the second temperature is 60°C to 120°C.
[0036] Optionally, in some embodiments of this application, the heat treatment time is 10 min to 30 min.
[0037] Optionally, in some embodiments of this application, the cutting process is a die-cutting process, wherein the die-cutting speed is 5m / min to 20m / min and the die-cutting accuracy is ±0.1mm.
[0038] The second initial electrode sheet is die-cut into strips to obtain the finished electrode sheet. The die-cutting speed and accuracy are further controlled to ensure that the electrode sheet edges are neat and reduce the risk of damage to the conductive adhesive layer due to die-cutting deviation. Since the rolling process has completed the tight bonding between the conductive adhesive layer and the active material layer, the electrode sheet edges are less likely to shed powder during die-cutting.
[0039] Optionally, in some embodiments of this application, the method for preparing the electrode sheet further includes: performing a second rolling process on the second initial electrode sheet, wherein the temperature of the second rolling process is a third temperature, and the third temperature is lower than the second temperature.
[0040] The second rolling process allows the conductive adhesive layer to bond tightly with the active material layer, further improving the adhesion and anti-powdering effect of the conductive adhesive layer. At the same time, controlling the third temperature to be lower than the second temperature can prevent high temperature from damaging the room temperature inert properties of the conductive adhesive layer.
[0041] In addition, this application also provides a battery comprising the above-described electrode or an electrode prepared by the above-described electrode preparation method.
[0042] Optionally, in some embodiments of this application, the battery has an electrolyte, which is a carbonate-based electrolyte. Attached Figure Description
[0043] Figure 1 This is a cross-sectional structural diagram of the electrode provided in an exemplary embodiment of this application. Detailed Implementation
[0044] The technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0045] This application provides a conductive adhesive liquid, an electrode sheet, a method for preparing the same, and a battery. These are described in detail below. It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc., are used merely as illustrative and do not impose numerical requirements or establish an order. Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Additionally, whenever a numerical range is indicated herein, it means including any referenced number (fraction or integer) within the indicated range.
[0046] This application provides a battery, which refers to a device that can convert chemical energy into electrical energy. The battery can have different forms, such as, but not limited to, a battery cell, a battery module, and a battery pack. Typically, a battery module and a battery pack each independently include multiple battery cells connected in series or parallel. Optionally, a battery module includes battery cells, and a battery pack includes battery modules.
[0047] In some embodiments of this application, the battery is a single battery cell. A single battery cell (also called a battery unit) is the basic unit for converting chemical energy into electrical energy. Optionally, the single battery cell is a secondary battery, such as a lithium-ion battery, in which case the single battery cell can realize the mutual conversion of chemical energy and electrical energy. Specifically, the single battery cell includes electrodes, which include a positive electrode and a negative electrode, and the positive electrode and the negative electrode are arranged opposite to each other.
[0048] In some embodiments of this application, the battery cell further includes a separator disposed between the positive and negative electrode plates to prevent short circuits caused by contact between the positive and negative electrode plates. The separator can be selected from one or more of polyolefin separators, non-woven fabric separators, ceramic-coated separators, and composite separators. As an example, a polyolefin separator includes at least one of polyethylene (PE) film and polypropylene (PP) film. The separator can be a dry-process separator or a wet-process separator, and is not limited thereto.
[0049] In some embodiments of this application, the positive electrode sheet includes a positive electrode active material layer, which contains a positive electrode active material. As an example, the positive electrode sheet also includes a positive electrode current collector, with the positive electrode active material layer disposed on the current collector; in another example, the positive electrode sheet is a self-supporting structure, comprising only the positive electrode active material layer without a current collector. Further, the positive electrode active material layer also contains a conductive agent and a binder. In the positive electrode sheet, the conductive agent includes at least one of carbon black, graphite, carbon nanotubes (CNTs), graphene, and carbon fiber; the binder includes polyvinylidene fluoride (PVDF); the current collector includes aluminum foil; and the positive electrode active material includes at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium nickel manganese oxide, lithium cobalt oxide, lithium-rich manganese-based oxide, and lithium manganese oxide.
[0050] In some embodiments of this application, the negative electrode sheet includes a negative electrode active material layer, which contains a negative electrode active material. The negative electrode active material can be selected from at least one of carbon-based and silicon-based negative electrode materials. Carbon-based negative electrode materials not only have good structural stability, effectively buffering volume changes and thus extending the cycle life of individual battery cells, but also have high conductivity, improving the charge and discharge efficiency of the battery. Common carbon-based negative electrode materials include graphite-based materials, such as natural graphite, artificial graphite, and mesophase carbon microspheres (MCI); hard carbon materials, such as amorphous carbon; soft carbon materials, such as graphene and carbon nanotubes; and nanocarbon materials, such as graphene, carbon nanotubes, and carbon fibers. Silicon-based negative electrode materials are another type of negative electrode material different from carbon-based negative electrode materials. Silicon-based negative electrode materials use silicon as the main active material and achieve energy storage through a chemical reaction with lithium ions. Silicon-based anode materials have a theoretical specific capacity far exceeding that of carbon-based anode materials, allowing the anode sheet to provide greater energy storage capacity and significantly improve battery life. Furthermore, silicon-based anode materials have a lower delithiation potential, which helps to inhibit lithium deposition, thus reducing the risk of lithium plating. Common silicon-based anode materials include silicon-oxygen composites, silicon-carbon composites, and silicon-based alloys. However, silicon-based anode materials have low conductivity and experience significant volume expansion during charge and discharge, which can easily lead to pulverization of the anode active material layer and instability of the SEI film, thereby affecting the cycle performance and safety of the battery cell. Optionally, the anode active material layer also includes a conductive agent and a binder. As an example, in the anode sheet, the conductive agent includes at least one of carbon black, graphite, carbon nanotubes (CNTs), graphene, and carbon fiber, and the binder includes at least one of styrene-butadiene rubber (SBR) and polyacrylic acid (PAA). In some examples, the anode sheet is a self-supporting structure, consisting only of the anode active material layer without a current collector. In other examples, the negative electrode sheet also includes a negative current collector, on which a layer of negative active material is disposed. As an example, the negative current collector includes copper foil.
[0051] In some embodiments of this application, the battery cell further includes an electrolyte used to wet the positive and negative electrode plates. The electrolyte provides ion channels during the charging and discharging process of the battery cell, enabling charge transfer between the positive and negative electrode plates, thereby completing energy storage and release. The electrolyte mainly includes a non-aqueous organic solvent and an electrolyte salt. Taking a lithium-ion battery cell as an example, the electrolyte salt includes lithium salts, which may include at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate, lithium bis(oxalato)borate (LiBOB), lithium difluorooxalato)borate (LiODFB), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI); the non-aqueous organic solvent includes at least one of carbonate solvents, carboxylic acid ester solvents, and ether solvents. Optionally, the electrolyte also includes functional additives. Functional additives are generally diverse and have different functions. As examples, functional additives include film additives, overcharge protection additives, flame retardant additives, high and low temperature additives, conductive additives, and additives for controlling water and HF content, etc. The film additive includes at least one of vinylene carbonate (VC) and fluoroethylene carbonate (FEC). The flame retardant additive includes at least one of organophosphorus compounds, organofluorine compounds, and haloalkyl phosphates.
[0052] In some embodiments of this application, the battery cell further includes a solid electrolyte membrane disposed between the positive and negative electrode plates. The solid electrolyte membrane can also prevent the positive and negative electrode plates from conducting. Optionally, the solid electrolyte membrane includes at least one of oxide solid electrolyte, sulfide solid electrolyte, and polymer solid electrolyte. If the solid electrolyte membrane can be used to completely replace the electrolyte and separator in the battery cell, then the battery cell is an all-solid-state battery.
[0053] Of course, in other embodiments, the battery cell may also be a semi-solid-state battery or a liquid battery.
[0054] In view of the fact that powder is easily shed from the edges of the electrode sheet during the die-cutting process in the preparation of battery electrode sheets, this application also provides an electrode sheet.
[0055] Please see Figure 1 The electrode 10 includes a current collector 1, an active material layer 2, and a conductive adhesive layer 3. The active material layer 2 is disposed on the current collector 1; the conductive adhesive layer 3 is disposed on the active material layer 2, and the conductive adhesive layer 3 is formed by cross-linking and curing a conductive adhesive liquid after heat treatment. By mass percentage, the conductive adhesive liquid includes 10%~30% conductive filler, 40%~60% thermoplastic resin, 5%~15% heat-triggered cross-linking agent, and 10%~20% solvent.
[0056] The electrode 10 can be either a positive electrode or a negative electrode. When the electrode 10 is a positive electrode, the current collector 1 is a positive current collector and the active material layer 2 is a positive active material layer; when the electrode 10 is a negative electrode, the current collector 1 is a negative current collector and the active material layer 2 is a negative active material layer.
[0057] The conductive adhesive layer 3 is formed by cross-linking and curing a conductive adhesive liquid after heat treatment. The conductive adhesive liquid includes conductive fillers, thermoplastic resin, a heat-triggered cross-linking agent, and a solvent. During heat treatment, the heat-triggered cross-linking agent triggers a further cross-linking reaction between the polymer chains of the thermoplastic resin to form a polymer, while the solvent evaporates upon heating, thus curing and forming the conductive adhesive layer 3. The conductive fillers do not react during heat treatment; the conductive fillers dispersed in the conductive adhesive liquid remain dispersed within the polymer formed by the cross-linking and curing of the thermoplastic resin.
[0058] The electrode 10 comprises a current collector 1, an active material layer 2, and a conductive adhesive layer 3, which are sequentially stacked. When the electrode 10 is used in a battery, the conductive adhesive layer 3 is used to contact the separator. It can be understood that the conductive adhesive layer 3 includes conductive fillers and a polymer formed by cross-linking thermoplastic resin. The conductive fillers are dispersed in the polymer formed by cross-linking thermoplastic resin, thereby constructing a highly efficient conductive network. This gives the conductive adhesive layer 3 good conductivity. When the electrode 10 is used in a battery, its own good electronic conductivity can reduce the risk of cell performance degradation due to the insulation of the polymer in the conductive adhesive layer 3.
[0059] Thermoplastic resin is a polymeric resin material that softens when heated, hardens when cooled, and maintains its properties unchanged during repeated heating and cooling. However, after cross-linking, thermoplastic resin transforms into a thermosetting polymer. This type of polymer is inert at room temperature (25±5℃) and does not react with the active material layer 2 or the separator. However, at high temperatures (80℃~160℃), it can effectively bond with the separator, achieving a strong bond between the electrode 10 and the separator during the hot pressing process of the battery cell, thus improving the overall structural integrity of the battery cell.
[0060] The high molecular polymer formed after cross-linking of thermoplastic resin imparts its room-temperature inertness and high-temperature adhesion to the conductive adhesive layer 3. Compared with room-temperature adhesive conductive adhesive layers, the room-temperature inertness of the conductive adhesive layer 3 makes it less likely to stick to equipment in subsequent battery manufacturing processes, while the high-temperature adhesion of the conductive adhesive layer 3 allows it to be firmly bonded to the separator through the adhesive layer during high-temperature hot pressing. In this way, the conductive adhesive layer 3 can be adapted to low-cost separators (such as PP base film and PE base film). Compared with composite separators with ceramic coatings and PVDF adhesive layers, this bare base film that does not require additional coating is expected to reduce separator costs by 30% to 50%, thereby reducing the overall cost of the battery cell and demonstrating significant industrialization value.
[0061] Furthermore, thanks to the high molecular polymer formed after crosslinking of thermoplastic resins, it is well compatible with non-aqueous solvents, especially carbonate solvents. It is insoluble in carbonate solvents (such as EC, DMC, EMC, etc.) and does not easily swell in carbonate solvents.
[0062] Electrode 10 typically requires cutting during manufacturing to achieve the desired size or shape. However, the electrode 10 in this application utilizes a conductive adhesive layer 3 on the active material layer 2. By bonding the active material layer 2 with the conductive adhesive layer 3, the probability of edge powder shedding from the electrode 10 (specifically, the active material layer 2) can be reduced during cutting. In particular, when the conductive adhesive liquid used to prepare the conductive adhesive layer 3 is formulated as follows: 10wt%~30wt% conductive filler, 40wt%~60wt% thermoplastic resin, 5wt%~15wt% thermally triggered crosslinking agent, and 10wt%~20wt% solvent, the powder shedding rate of the electrode 10 is ≤0.1%, improving production yield and reducing material waste.
[0063] As an example, in the conductive adhesive liquid, the mass percentage of conductive filler is 10wt%, 15wt%, 20wt%, 25wt%, or 30wt%, the mass percentage of thermoplastic resin is 40wt%, 45wt%, 50wt%, 55wt%, or 60wt%, the mass percentage of thermally triggered crosslinking agent is 5wt%, 7wt%, 9wt%, 11wt%, 13wt%, or 15wt%, and the mass percentage of solvent is 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, or 20wt%.
[0064] In summary, the electrode 10 provided in this application embodiment includes a current collector 1, an active material layer 2, and a conductive adhesive layer 3 stacked sequentially. The conductive adhesive layer 3 is formed by cross-linking and curing a conductive adhesive liquid containing conductive filler, thermoplastic resin, thermally triggered cross-linking agent, and solvent after heat treatment. Thus, the conductive adhesive layer 3 simultaneously possesses four major characteristics: conductivity, room temperature inertness, high-temperature adhesion, and resistance to electrolyte swelling. The conductive adhesive layer 3 not only improves the problem of powder shedding during electrode 10 cutting, but also reduces the cell interface resistance and improves the adhesion between the electrode 10 and the separator when the electrode 10 is applied to the battery, thereby improving the overall stability of the cell structure and enhancing the safety, economy, and cycle life of the lithium battery.
[0065] In some embodiments of this application, the conductive filler includes at least one of carbon nanotubes, conductive carbon black, and graphene. The aforementioned conductive filler exhibits excellent conductivity and dispersibility, effectively reducing the volume resistivity of the conductive adhesive layer 3.
[0066] In some embodiments of this application, the thermoplastic resin includes at least one of polyvinylidene fluoride (PVDF) and polyimide (PI). The polymer formed by crosslinking the above-mentioned thermoplastic resin has good thermal stability, electrolyte resistance, and adhesive properties. It is solid at room temperature and can melt at high temperature to achieve bonding. It is also suitable for room temperature roller pressing and will not deform or stick due to roller pressing.
[0067] In some embodiments of this application, the heat-triggered crosslinking agent includes at least one of dicumyl peroxide and benzoyl peroxide. Both dicumyl peroxide (DCP) and benzoyl peroxide (BPO) belong to the organic peroxide type crosslinking agent category. Organic peroxide crosslinking agents can decompose under heating conditions to generate free radicals. These free radicals attack the polymer molecular chains, causing linear or slightly branched polymer chains to crosslink and form a three-dimensional network structure, thus achieving crosslinking. The aforementioned heat-triggered crosslinking agent, by triggering the crosslinking of thermoplastic resin at high temperatures, improves the adhesive strength and electrolyte resistance of the resulting conductive adhesive layer 3.
[0068] In some embodiments of this application, the solvent includes at least one of N-methylpyrrolidone and dimethyl sulfoxide. The solvent allows for complete dissolution of the components, forming a homogeneous adhesive solution. Furthermore, the solvent is volatile and can be completely removed during heat treatment, leaving no residue in the conductive adhesive layer 3.
[0069] In some embodiments of this application, electrode 10 is a negative electrode, and active material layer 2 is a graphite-based active material layer. The active material of the graphite-based active material layer is graphite. The adhesion of graphite in the negative electrode is relatively weak, making it more prone to powder shedding during cutting. The conductive adhesive layer 3, attached to the graphite-based active material layer, can effectively improve the powder shedding problem.
[0070] In some embodiments of this application, the adhesion of the conductive adhesive layer 3 to the active material layer 2 is ≥2.0N / 25mm. In this case, it can be ensured that the conductive adhesive layer 3 does not fall off during rolling, cutting and subsequent processes, effectively playing a role in preventing powder shedding and bonding.
[0071] This application embodiment also provides a method for preparing electrode 10, including: A first initial electrode is provided, the first initial electrode comprising a current collector 1 and an active material layer 2 disposed on the current collector 1; A conductive adhesive layer is prepared on the surface of the active material layer 2, the conductive adhesive layer containing the aforementioned conductive adhesive; The conductive adhesive liquid layer is heat-treated to cross-link and solidify the conductive adhesive liquid layer to form conductive adhesive layer 3, thus obtaining the second initial electrode sheet; The second initial electrode is cut to obtain electrode 10.
[0072] The electrode 10 prepared by the method provided in this application embodiment has a conductive adhesive layer 3. The conductive adhesive layer 3 can effectively control the powder loss rate to ≤0.1% when the electrode 10 is cut, thereby improving the production qualification rate and reducing material loss.
[0073] The conductive adhesive layer 3 of the electrode 10 is inert at room temperature, can adhere to the separator at high temperature, and is compatible with carbonate electrolytes without affecting the cell performance. The conductive adhesive layer 3 has excellent conductivity and is suitable for room temperature rolling without adhesion, ensuring smooth production and stable cell performance. The conductive adhesive layer 3 of the electrode 10 is compatible with low-cost bare base films (such as polyolefin separators), eliminating the need for additional coatings. This is expected to reduce separator costs by 30% to 50%, thereby reducing the overall cell cost and demonstrating significant industrialization value.
[0074] The electrode 10 preparation method provided in this application embodiment is simple and can be modified on existing production lines without adding complex equipment. The film formation process has a reasonable timing sequence that does not interfere with production, making it easy to scale up mass production and improving the adhesion of the adhesive layer. High-temperature hot pressing can firmly bond the electrode 10 and the separator through the conductive adhesive layer 3, improving the overall stability of the cell structure and enhancing the safety and cycle life of the lithium battery.
[0075] In summary, by preparing a conductive adhesive layer with specific properties during the rolling process, three core pain points in the industry—powder shedding during electrode cutting, insufficient bonding strength between the electrode and the separator, and high separator procurement costs—can be solved in one go, thereby improving the safety and economy of the battery cell.
[0076] In some embodiments of this application, providing a first initial electrode includes: The electrode paste is subjected to film formation treatment on the current collector 1 to form an active material layer 2; The active material layer 2 is subjected to a first rolling process to obtain a first initial electrode sheet. The temperature of the first rolling process is a first temperature.
[0077] After densifying the active material layer 2 by first rolling, a conductive adhesive layer 3 is then prepared on the active material layer 2. This improves the bonding strength of the materials inside the active material layer 2 and strengthens the bonding force of the conductive adhesive layer 3, thus improving the problem of powder shedding during the cutting of the electrode sheet 10.
[0078] In some embodiments of this application, the preparation process of the first initial electrode includes: coating an electrode paste onto the surface of the current collector 1 to obtain a wet film layer; and subjecting the wet film layer to a baking and drying process to remove the solvent, thereby obtaining a dried electrode. The baking and drying process is performed at a temperature of 50°C to 120°C and a drying time of 15 min to 30 min. As an example, the drying temperature is 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, or 120°C; and the drying time is 15 min, 20 min, 25 min, or 30 min.
[0079] In some embodiments of this application, the first rolling process is a cold pressing process. Cold pressing is a physical compression method that can reduce the interparticle gaps in the active material layer 2, thereby increasing the density of the active material layer 2. As an example, the temperature of the cold pressing process is less than or equal to 23°C, i.e., the first temperature is ≤23°C.
[0080] In some embodiments of this application, a conductive adhesive layer is prepared by spraying. Spraying produces a uniform, high-quality conductive adhesive layer, ensuring complete coverage and reducing the problem of missed coating. Specifically, after the first initial electrode sheet is dried and subjected to one roll pressing (cold pressing), a layer of conductive adhesive is sprayed onto the first initial electrode sheet. Immediately after spraying, the conductive adhesive layer is heat-treated to remove the solvent from the conductive adhesive layer, allowing the conductive adhesive layer 3 to completely cure and form, ensuring the adhesion and performance stability of the conductive adhesive layer 3.
[0081] In some embodiments of this application, the coating is atomized spraying. Atomized spraying allows the conductive adhesive to be uniformly covered to the edge of the first initial electrode, reducing the possibility of adhesive accumulation or missed areas. Atomized spraying ensures that the conductive adhesive is accurately sprayed to the edge of the first initial electrode without affecting the performance of the central active region of the first initial electrode.
[0082] In some embodiments of this application, the thickness of the conductive adhesive liquid layer is 1 μm to 10 μm. The thickness of the conductive adhesive liquid layer directly determines the thickness of the conductive adhesive layer 3. If the thickness of the conductive adhesive layer 3 is too thin, it cannot effectively prevent powder shedding and achieve separator adhesion, while if the thickness of the conductive adhesive layer 3 is too large, it will increase the internal resistance of the battery. As an example, the thickness of the conductive adhesive liquid layer is 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm. By controlling the thickness of the conductive adhesive liquid layer, powder shedding and separator adhesion can be prevented while ensuring the electrochemical performance of the battery.
[0083] In some embodiments of this application, the heat treatment is infrared short-wave drying. Infrared short-wave drying is a technique that uses infrared rays to rapidly heat the surface of an object to achieve drying. Infrared short-wave drying not only allows the solvent in the conductive adhesive layer to evaporate quickly, but also enables the heat-triggered crosslinking agent to promote the rapid crosslinking and curing of the thermoplastic resin, thus accelerating the formation of the conductive adhesive layer 3.
[0084] In some embodiments of this application, the heat treatment temperature is a second temperature, which is greater than the first temperature.
[0085] In some embodiments of this application, the second temperature is 60°C to 120°C. As an example, the second temperature is 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, or 120°C.
[0086] In some embodiments of this application, the heat treatment time is 10 min to 30 min. As examples, the heat treatment time is 15 min, 20 min, 25 min, or 30 min.
[0087] In some embodiments of this application, the preparation method of the electrode 10 further includes: performing a second rolling process on the second initial electrode, wherein the temperature of the second rolling process is a third temperature, which is lower than the second temperature. If the second rolling process and the first rolling process are considered as a complete rolling process, then the preparation method of the electrode 10 provided in this application integrates the forming process of the conductive adhesive layer 3 into the rolling process. The second rolling process allows the conductive adhesive layer 3 to be tightly bonded to the active material layer 2, further improving the adhesion and anti-powdering effect of the conductive adhesive layer 3; at the same time, controlling the third temperature to be lower than the second temperature can prevent high temperature from damaging the room temperature inert properties of the conductive adhesive layer 3. As an example, the second rolling process is a room temperature rolling process.
[0088] In some embodiments of this application, the cutting process is a die-cutting process, the die-cutting speed is 5m / min to 20m / min, and the die-cutting accuracy is ±0.1mm.
[0089] The second initial electrode sheet is die-cut into strips to obtain the finished electrode sheet. The die-cutting speed and accuracy are further controlled to ensure that the electrode sheet edges are neat and reduce the risk of damage to the conductive adhesive layer due to die-cutting deviation. Since the rolling process has completed the tight bonding between the conductive adhesive layer 3 and the active material layer 2, the electrode sheet edges are less likely to shed powder during die-cutting.
[0090] As an example, the die-cutting speed is 5m / min, 10m / min, 15m / min or 20m / min, and the die-cutting accuracy is ±0.1mm.
[0091] In some embodiments of this application, the battery includes the aforementioned electrode 10 or the electrode 10 prepared by the aforementioned electrode 10 preparation method.
[0092] In some embodiments of this application, the electrolyte of the battery is a carbonate-based electrolyte. A carbonate-based electrolyte refers to an electrolyte in which the solvent is a carbonate solvent. The conductive adhesive layer 3 in the electrode 10 is well compatible with the carbonate-based electrolyte, and the swelling rate of the conductive adhesive layer 3 in the carbonate-based electrolyte is low.
[0093] The following description is based on specific embodiments.
[0094] Example 1 This embodiment provides a negative electrode sheet, the preparation process of which is as follows: S1. Preparation of negative electrode sheet: The negative electrode active material graphite, conductive agent SP and binder SBR are weighed in a mass ratio of 97:2:1 and added to NMP (N-methylpyrrolidone) solvent. After stirring, a negative electrode slurry with a solid content of 49% is prepared. The negative electrode slurry is coated on the surface of copper foil current collector, and then baked and dried (drying temperature 80℃, drying time 20min) to remove NMP solvent, so as to obtain a dry negative electrode sheet with a stable active material layer. The negative electrode sheet is then subjected to cold pressing once.
[0095] S2. Adhesive Spraying and Rolling: Conductive adhesive is sprayed onto the negative electrode sheet using an atomized spraying method to ensure that the conductive adhesive evenly covers the edges of the negative electrode sheet without accumulation or missed spraying; the spraying thickness is 5μm; immediately after spraying, infrared short-wave drying (drying temperature 80℃, drying time 20min) is performed to remove the solvent in the conductive adhesive and allow the conductive adhesive layer to fully cure and form; after drying, a second room temperature rolling is performed to avoid high temperature damaging the room temperature inert properties of the conductive adhesive layer, so that the conductive adhesive layer is tightly bonded to the active material layer, improving the adhesion and anti-powdering effect of the conductive adhesive layer.
[0096] The conductive adhesive liquid contains the following components (by mass percentage): 20% conductive filler (conductive carbon black), 50% thermoplastic resin (PVDF), 8% thermally triggered crosslinking agent (diisopropylbenzene peroxide), and 12% solvent (N-methylpyrrolidone), which ensures that the performance of the conductive adhesive liquid meets the standards.
[0097] S3. Die-cutting and slitting: The electrode sheets after room temperature roller pressing are die-cut and slitting. The die-cutting speed is 10m / min, and the die-cutting accuracy is controlled within ±0.1mm to ensure that the edges of the electrode sheets are neat and to avoid damage to the adhesive layer due to die-cutting deviation. Since the secondary roller pressing has achieved a tight bond between the adhesive layer and the active material layer, there is no powder shedding during die-cutting.
[0098] Example 2 This embodiment provides a negative electrode sheet, the preparation process of which is as follows: S1. Preparation of negative electrode sheet: The negative electrode active material graphite, conductive agent SP and binder PVDF are weighed in a mass ratio of 97.5:1:1.5 and added to NMP (N-methylpyrrolidone) solvent. After stirring, a negative electrode slurry with a solid content of 68% is prepared. The negative electrode slurry is coated on the surface of copper foil current collector and baked and dried (drying temperature 50℃, drying time 30min) to remove NMP solvent, so as to obtain a dry negative electrode sheet with a stable active material layer. Then, the negative electrode sheet is subjected to cold pressing once.
[0099] S2. Adhesive spraying and rolling: Conductive adhesive is sprayed onto the negative electrode sheet using an atomized spraying method, with a spraying thickness of 1μm. Immediately after spraying, infrared short-wave drying (drying temperature 60℃, drying time 30min) is used to remove the solvent in the conductive adhesive and allow the conductive adhesive layer to solidify. After drying, a second room temperature rolling is performed to achieve a tight bond between the conductive adhesive layer and the active material layer.
[0100] The conductive adhesive liquid has the following components (by mass percentage): 10% conductive filler (carbon nanotubes), 60% thermoplastic resin (PI), 5% thermally triggered crosslinking agent (benzoyl peroxide), and solvent (5% dimethyl sulfoxide + 5% N-methylpyrrolidone), which meet the core requirements of conductivity and room temperature inertness of the adhesive liquid.
[0101] S3. Die-cutting and slitting: Die-cutting speed 5m / min, die-cutting accuracy ±0.1mm, meeting the die-cutting accuracy requirements, ensuring that the electrode edges are neat, and that there is no damage to the adhesive layer or powder falling off during the die-cutting process.
[0102] Example 3 This embodiment provides a negative electrode sheet, the preparation process of which is as follows: S1. Preparation of negative electrode sheet: The negative electrode active material graphite, conductive agent SP and binder SBR are weighed in a mass ratio of 97:2:1 and added to NMP (N-methylpyrrolidone) solvent. After stirring, a negative electrode slurry with a solid content of 49% is prepared. The negative electrode slurry is coated on the surface of copper foil current collector, baked and dried (drying temperature 120℃, drying time 15min) to remove NMP solvent, and a dry negative electrode sheet with stable active material layer is obtained. Then, the negative electrode sheet is subjected to cold pressing once.
[0103] S2. Adhesive spraying and rolling: Conductive adhesive is sprayed onto the negative electrode sheet using an atomized spraying method, with a spraying thickness of 10μm. Immediately after spraying, infrared short-wave drying (drying temperature 120℃, drying time 10min) is performed to ensure that the conductive adhesive layer is completely cured and formed. After drying, a second room temperature rolling is performed to strengthen the bonding force between the conductive adhesive layer and the active material layer, achieving the effects of preventing powder shedding and high-temperature bonding.
[0104] The conductive adhesive liquid is composed (by mass percentage) of the following components: 30% conductive filler (graphene + conductive carbon black, mass ratio 1:1), 40% thermoplastic resin (PI), 15% thermally triggered crosslinking agent (dicumyl peroxide), and 15% solvent (dimethyl sulfoxide). This composition ensures excellent conductivity and good high-temperature bonding performance of the adhesive liquid. S3. Die-cutting and slitting: Die-cutting speed 20m / min, die-cutting accuracy ±0.1mm, meeting the die-cutting requirements, ensuring that the electrode edges are neat, and that there is no powder shedding or damage to the adhesive layer during the die-cutting process.
[0105] Example 4 This embodiment provides a negative electrode sheet, the preparation process of which is as follows: S1. Preparation of negative electrode sheet: The negative electrode active material graphite, conductive agent SP and binder SBR are weighed in a mass ratio of 97:2:1 and added to NMP (N-methylpyrrolidone) solvent. After stirring, a negative electrode slurry with a solid content of 49% is prepared. The negative electrode slurry is coated on the surface of copper foil current collector and baked and dried (drying temperature 70℃, drying time 25min) to remove NMP solvent, and a dry negative electrode sheet with stable active material layer is obtained.
[0106] S2. Adhesive Spraying and Rolling: Conductive adhesive is sprayed onto the negative electrode sheet using an atomized spraying method, with a spray thickness of 3μm. Immediately after spraying, infrared short-wave drying (drying temperature 70℃, drying time 25min) is performed to remove the solvent in the conductive adhesive and allow the conductive adhesive layer to fully cure and form. After drying, a second room temperature rolling process is performed to meet process requirements and improve the adhesion and anti-powdering effect of the conductive adhesive layer.
[0107] The conductive adhesive liquid is composed (by mass percentage) of the following components: 15% conductive filler (carbon nanotubes + graphene, mass ratio 2:1), 55% thermoplastic resin (PVDF + PI, mass ratio 1:1), 7% thermally triggered crosslinking agent (benzoyl peroxide), and 23% solvent (N-methylpyrrolidone). S3. Die-cutting and slitting: Die-cutting speed 12m / min, die-cutting accuracy ±0.1mm, meeting the patented die-cutting accuracy requirements, with no adhesive layer damage or powder shedding during the die-cutting process.
[0108] Example 5 This embodiment provides a negative electrode sheet, the preparation process of which is as follows: S1. Preparation of negative electrode sheet: The negative electrode active material graphite, conductive agent SP and binder SBR are weighed in a mass ratio of 97:2:1 and added to NMP (N-methylpyrrolidone) solvent. After stirring, a negative electrode slurry with a solid content of 49% is prepared. The negative electrode slurry is coated on the surface of copper foil current collector and baked and dried (drying temperature 90℃, drying time 18min) to remove NMP solvent, and a dry negative electrode sheet with stable active material layer is obtained.
[0109] S2. Adhesive spraying and rolling: Conductive adhesive is sprayed onto the negative electrode sheet using an atomized spraying method, with a spraying thickness of 7μm. Immediately after spraying, infrared short-wave drying (drying temperature 90℃, drying time 18min) is performed to remove the solvent in the conductive adhesive and allow the conductive adhesive layer to fully cure and form. After drying, a second room temperature rolling process is performed to ensure that the conductive adhesive layer and the active material layer are tightly bonded.
[0110] The components (by mass percentage) of the conductive adhesive are as follows: 25% conductive filler (conductive carbon black + graphene, mass ratio 3:1), 45% thermoplastic resin (PI + PVDF, mass ratio 1:2), 10% thermally triggered crosslinking agent (diisopropylbenzene peroxide), and 20% solvent (dimethyl sulfoxide + N-methylpyrrolidone, mass ratio 1:1).
[0111] S3. Die-cutting and slitting: Die-cutting speed 15m / min, die-cutting accuracy ±0.1mm, meeting die-cutting requirements, ensuring neat electrode edges, and no powder shedding during the die-cutting process.
[0112] Example 6 This embodiment provides a negative electrode sheet, the preparation process of which is as follows: S1. Preparation of negative electrode sheet: The negative electrode active material graphite, conductive agent SP and binder SBR are taken at a mass ratio of 97:2:1 and added to NMP (N-methylpyrrolidone) solvent. After stirring, a negative electrode slurry with a solid content of 49% is prepared. The negative electrode slurry is coated on the surface of copper foil current collector and baked and dried (drying temperature 100℃, drying time 22min) to remove NMP solvent, and a dry negative electrode sheet with stable active material layer is obtained.
[0113] S2. Adhesive spraying and rolling: Conductive adhesive is sprayed onto the negative electrode sheet using an atomized spraying method, with a spraying thickness of 6μm. Immediately after spraying, infrared short-wave drying (drying temperature 100℃, drying time 15min) is used to remove the solvent in the conductive adhesive and allow the conductive adhesive layer to fully cure and form. After drying, a second room temperature rolling is performed to achieve a tight bond between the conductive adhesive layer and the active material layer, playing a role in preventing powder shedding and high-temperature bonding.
[0114] The conductive adhesive liquid has the following components (by mass percentage): 22% conductive filler (carbon nanotubes), 48% thermoplastic resin (PI), 8% thermally triggered crosslinking agent (benzoyl peroxide), and 22% solvent (N-methylpyrrolidone), which meet the requirements for conductivity, room temperature inertness, high temperature adhesion, and electrolyte compatibility.
[0115] S3. Die-cutting and slitting: Die-cutting speed 18m / min, die-cutting accuracy ±0.1mm, meeting the die-cutting accuracy requirements, with no adhesive layer damage or powder shedding during the die-cutting process.
[0116] Comparative Example 1 This comparative example provides a negative electrode sheet. The preparation process of this negative electrode sheet can be found in Example 1. The difference is that the conductive adhesive liquid is omitted in S2, so that the negative electrode sheet obtained has no conductive adhesive layer.
[0117] Comparative Example 2 This comparative example provides a negative electrode sheet. The preparation process of this negative electrode sheet can be found in Example 1, except that the thermally triggered crosslinking agent of the conductive adhesive liquid in S2 is omitted.
[0118] Performance testing: The following performance tests were performed on the negative electrode sheets provided in Examples 1-6 and Comparative Examples 1-2: 1. Adhesion of the conductive adhesive layer: Test standard: Refer to GB / T 2792-2014 "Test method for peel strength of adhesive tape".
[0119] Test steps: 1) Cut the negative electrode sheet to be tested into a 25 mm × 100 mm sample; 2) Apply a 25 mm wide strip of 3M strong adhesive tape to the surface of the conductive adhesive layer and press it firmly to remove air bubbles; 3) An electronic universal tensile testing machine was used to perform a 180° peel test at a rate of 300 mm / min; 4) Record the average peeling force during the peeling process, in N / 25mm. Each group of samples was tested 5 times and the average value was taken.
[0120] 2. Volume resistivity of the conductive adhesive layer: Test standard: Refer to GB / T 1410-2006 "Test methods for volume resistivity and surface resistivity of solid insulating materials", four-probe method.
[0121] Test steps: 1) Remove the current collector from the electrode sheet, leaving the cured conductive adhesive layer; 2) The sheet resistance of the adhesive layer was tested using a four-probe resistance tester at room temperature (25°C). 3) Calculate the volume resistivity based on the adhesive layer thickness (μm); 4) Test 5 different locations in each group and take the average value.
[0122] 3. High-temperature adhesive strength (peel force) of the conductive adhesive layer: Test steps: 1) Align and bond the electrode to be tested with the bare PP diaphragm, and hot press at 120℃ and 0.8 MPa for 3 min; 2) Cut the sample into 25 mm × 100 mm pieces; 3) The electronic universal testing machine performs 180° peeling at a rate of 300 mm / min; 4) Record the peel force at the electrode-diaphragm interface, unit: N / 25mm, averaged after 5 times.
[0123] 4. Powder shedding rate of the electrode: Test method: Die-cutting and weighing method.
[0124] Test steps: 1) Take electrodes from the same batch and weigh the total mass m0 of the electrodes before die-cutting; 2) Complete die-cutting according to the set die-cutting speed and precision; 3) Collect the powder that falls off the edges during die cutting and weigh the powder mass m1; 4) Powder shedding rate = (m1 / m0) × 100%; 5) Test 10 pieces in each group in parallel and take the average value.
[0125] 5. Electrolyte compatibility (swelling rate): Test steps: 1) Peel off the conductive adhesive layer, dry it to constant weight, and weigh the initial mass W0; 2) Soak in carbonate electrolyte (1 mol / L LiPF6, EC:DMC:EMC=1:1:1) at 60℃ for 72 hours; 3) After removing it, use filter paper to absorb the surface electrolyte and weigh the wet weight W1; 4) Swelling rate = [(W1-W0) / W0] × 100%, take the average of 3 parallel tests.
[0126] 6. Cycle capacity retention (2000 cycles): Test steps: 1) Assemble the negative electrode sheet and positive electrode sheet (active material is lithium iron phosphate, conductive agent SP and binder PVDF in a mass ratio of 97.5:1.5:1) and PP separator of the example / comparative example into a soft-pack battery cell; 2) At room temperature (25℃), 1C constant current and constant voltage charging and 1C constant current discharging, with a voltage range of 2.5V~3.65V; 3) Repeat the cycle 2000 times, recording the discharge capacity C1 of the first cycle and the discharge capacity C2 of the 2000th cycle. 2000 ; 4) Capacity retention rate = (C 2000 / C1)×100%.
[0127] 7. Compatibility with PP base film: Test steps: 1) Hot-press the electrode sheet to the bare PP diaphragm (120℃, 0.8 MPa, 3 min); 2) Observe whether the interface shows delamination, curling edges, or bubbles; 3) Perform bending and peeling tests. If there is no delamination or obvious interface separation, it is considered a fit.
[0128] The test results for the above test items are recorded in Table 1.
[0129] Table 1
[0130] Results analysis: Compared to Comparative Example 1, Example 1 showed a sharp increase in electrode powder shedding rate and a significant decrease in battery capacity retention due to the lack of a conductive adhesive layer. Compared to Comparative Example 2, Example 2 omitted the thermally triggered crosslinking agent, resulting in insufficient cohesion of the conductive adhesive layer. This led to decreased adhesion and bonding strength of the conductive adhesive layer, consequently increasing electrode powder shedding rate and swelling rate of the conductive adhesive layer. In Comparative Example 2, insufficient cohesion of the conductive adhesive layer hindered the construction of a continuous conductive network, increasing the volume resistivity of the conductive adhesive layer, leading to increased internal resistance and decreased battery cycle performance.
[0131] Examples 1-6 show adhesion ≥2.0 N / 25 mm, electrode powder shedding rate ≤0.05%, and low volume resistivity (≤2.5 × 10⁻⁶). -3 The electrode exhibits high strength (Ω·cm), high-temperature bonding strength ≥3.1N / 25mm, swelling rate ≤0.9%, and capacity retention rate ≥87% after 2000 cycles. All are compatible with inexpensive PP base films, effectively preventing electrode powder shedding and ensuring stable adhesion to the inexpensive base film. Example 3, with the highest conductive filler content and largest coating thickness, exhibits the best performance across all aspects. Example 2, with the lowest conductive filler content and thinnest coating thickness, has slightly lower performance than other examples, but still meets basic requirements. The appropriate parameters can be selected based on actual production costs and performance needs.
[0132] The conductive adhesive liquid, electrode sheet, preparation method, and battery provided in the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are only for the purpose of helping to understand the methods and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.
Claims
1. A conductive adhesive liquid, characterized in that, The conductive adhesive comprises, by weight percentage, 10% to 30% conductive filler, 40% to 60% thermoplastic resin, 5% to 15% thermally triggered crosslinking agent, and 10% to 20% solvent.
2. The conductive adhesive liquid according to claim 1, characterized in that, The conductive filler includes at least one of carbon nanotubes, conductive carbon black, and graphene; and / or, The thermoplastic resin includes at least one of polyvinylidene fluoride and polyimide; and / or, The thermally triggered crosslinking agent includes at least one of dicumyl peroxide and benzoyl peroxide; and / or, The solvent includes at least one of N-methylpyrrolidone and dimethyl sulfoxide.
3. An electrode sheet, characterized in that, include: current collector; An active material layer is disposed on the current collector; as well as A conductive adhesive layer is disposed on the active material layer, wherein the conductive adhesive layer is formed by cross-linking and curing of the conductive adhesive liquid as described in claim 1 or 2 after heat treatment.
4. The electrode sheet according to claim 3, characterized in that, The electrode is a negative electrode, and the active material layer is a graphite-based active material layer; and / or, The adhesion of the conductive adhesive layer to the active material layer is ≥2.0N / 25mm.
5. A method for preparing an electrode sheet, characterized in that, include: A first initial electrode is provided, the first initial electrode comprising a current collector and an active material layer located on the current collector; A conductive adhesive layer is prepared on the surface of the active material layer, the conductive adhesive layer comprising the conductive adhesive as described in claim 1 or 2; The conductive adhesive liquid layer is heat-treated to cross-link and solidify the conductive adhesive liquid to form a conductive adhesive layer, thereby obtaining a second initial electrode sheet; The second initial electrode is cut to obtain an electrode sheet.
6. The method for preparing the electrode according to claim 5, characterized in that, The provision of the first initial electrode includes: Electrode paste is deposited on a current collector to form an active material layer; The active material layer is subjected to a first rolling process to obtain a first initial electrode sheet, and the temperature of the first rolling process is a first temperature.
7. The method for preparing the electrode according to claim 6, characterized in that, The heat treatment temperature is a second temperature, which is greater than the first temperature.
8. The method for preparing the electrode according to claim 7, characterized in that, The first rolling process is a cold pressing process; and / or, The second temperature is 60℃~120℃; and / or, The method for preparing the electrode sheet further includes: performing a second rolling process on the second initial electrode sheet, wherein the temperature of the second rolling process is a third temperature, and the third temperature is lower than the second temperature.
9. The method for preparing the electrode sheet according to any one of claims 5 to 8, characterized in that, The conductive adhesive liquid layer is prepared by spraying.
10. The method for preparing the electrode according to claim 9, characterized in that, The spraying is atomized spraying.
11. The method for preparing the electrode sheet according to any one of claims 5 to 10, characterized in that, The thickness of the conductive adhesive liquid layer is 1μm~10μm; and / or, The heat treatment is infrared short-wave drying; and / or, the heat treatment time is 10 min to 30 min; and / or The cutting process is a die-cutting process, and the die-cutting speed is 5m / min to 20m / min, with a die-cutting accuracy of ±0.1mm.
12. A battery, characterized in that, The electrode includes the electrode prepared by the method described in claim 3 or 4, or the electrode prepared by any one of claims 5 to 11.
13. The battery according to claim 12, characterized in that, The battery includes an electrolyte, which is a carbonate-based electrolyte.