Compositions for preparing crosslinked polymer systems, crosslinked polymer systems, their preparation methods and applications
By using calcium ion crosslinking agents and organophosphonic acid additives to transform intramolecular crosslinking into intermolecular crosslinking, the problem of polymer viscosity decreasing instead of increasing was solved, forming a high-viscosity gel and improving oilfield recovery.
Patent Information
- Application Number
- CN202510597123.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-10
Smart Images

Figure CN123063167A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of oilfield development technology, specifically relating to a composition for preparing a crosslinked polymer system, the crosslinked polymer system, its preparation method, and its application. Background Technology
[0002] Crosslinking polymers have been used for profile control, water shut-off, and displacement control for decades. The polymers mainly include natural and synthetic polymers. However, due to issues such as cost and stability, natural polymers have not been widely adopted. Currently, the main application is with polymers synthesized primarily from acrylamide monomers. One company attempted to synthesize polymer gels by partially hydrolyzing polyacrylamide (HPAM) and aluminum citrate, becoming the first company to apply this profile control technology.
[0003] The core of cross-linked polymers is the cross-linking agent, which can be classified into metal ion cross-linking systems and organic cross-linking agents. Metal ion cross-linking agents are mostly multivalent metal ions, such as Al. 3+ Cr 3+ Fe 3+ Zr 4+ These polyvalent cations exist either as inorganic ions or dissolved in solution as compounds. These ions form coordination bonds with negatively charged carboxyl functional groups. The crosslinking rate is related to the charge density on the polymer molecular chain and the number of inorganic ions in the solution; temperature, mineralization, and pH affect the gelation process.
[0004] Initially, aluminum sulfate was used as a crosslinking agent for HPAM, but due to its rapid gelation time, it was quickly replaced by other crosslinking agents. To control the gelation time, Cr... 6+ As a crosslinking agent, Cr 6+ It does not participate in cross-linking reactions; when it encounters a reducing agent, it is converted into Cr. 3+ Crosslinked HPAM. Cr 6+ Crosslinking agents have obvious disadvantages: (1) short gelation time in high-temperature reservoirs; (2) high sensitivity to H2S in reservoirs; (3) Cr 6+ Toxic and carcinogenic.
[0005] Sydansk R DA new conformance-improvement-treatment chromium(III) gel technology [R]. SPE 17329-MS, 1988. The literature discloses that in 1984, Marathon Petroleum Company developed a chromium acetate crosslinking agent and achieved great success in oilfield applications. It also exhibits some resistance to environmental factors such as ions, H2S, and CO2 in formation water.
[0006] Southwell GP, Posey S M. Applications and results of acrylamide-polymer / chromium(III)carboxylate gels [R]. SPE27779-MS, 1994. The literature discloses that from 1989 to 1992, crude oil production in the Big Horn Basin, Wyoming, increased by 19 × 10⁻⁶ due to the injection of the HPAM / chromium acetate gel system. 4 m 3 This crosslinked polymer system is suitable for relatively low temperatures. When the reservoir temperature exceeds 90°C, the crosslinking rate increases significantly, and the system also experiences severe dehydration under high-temperature conditions. To improve the temperature resistance of the chromium crosslinked system, researchers used chromium malonate instead of chromium acetate, extending the gelation time by several orders of magnitude. A problem with the chromium crosslinked system is that gel prepolymer microparticles form before the gel network is established, and the reservoir rocks have a certain filtering and retention effect on these microparticles. Furthermore, current environmental regulations are also restricting the use of chromium. 3+ Heavy metal ions of this type.
[0007] Mack JC, Smith J E. In-depth colloidal dispersion gels improve oil recovery efficiency [R]. SPE 27780-MS, 1994. The literature discloses that in the 1990s, BP Exploration and ARCO developed colloidal dispersion gels (CDGs) by introducing an HPAM / aluminum citrate crosslinking system.
[0008] Al-Assi AA, Willhite PG, Don GW, et al. Formation and propagation of gel aggregates using partially hydrolyzed polyacrylamide and aluminum citrate[R]. SPE 100049-MS, 2006.
[0009] Ranganathan R, Lewis R, McCool CS, et al. Experimental study of the gelation behavior of a polyacrylamide / aluminum citrate colloidal-dispersiongel system[J]. SPE Journal, 1998, 3(4): 337-343. The literature discloses that Tirco has reported some successful application examples, but the technology is still controversial because many experimental results show that CDG can only achieve effective migration in formations with permeability of several Darcy or higher.
[0010] To control crosslinking time, Hutchins RD, Dovan HT, Sandiford BB. Field applications of high temperature organic gels for water control [R]. SPE 35444-MS, 1996. The literature discloses that Pfizer invented a crosslinking system composed of phenolic compounds (such as phenol and resorcinol) and aldehyde (formaldehyde) compounds. Due to the carcinogenicity of formaldehyde, many scholars are researching formaldehyde substitutes. The most successful is hexamethylenetetramine, which can produce formaldehyde and ammonia through thermal decomposition, thereby extending the gelation time and reducing the pungent odor of formaldehyde in ground applications. Some researchers have also found that glyoxal or 1,3,5-trioxane can be used to replace formaldehyde, but their application is less common. Phenol is also highly toxic; it can be replaced by catechol, resorcinol, hydroquinone, etc. Some researchers have also proposed using aspirin, anthranilic acid, phenyl salicylate, etc., to replace phenol. Aspirin hydrolyzes slowly, gradually forming acetic acid and salicylic acid in the reservoir, which prolongs the cross-linking time. The cross-linking sites of anthranilic acid are located at the ortho and para positions of the amino functional groups, thus its cross-linking rate is much lower than that of phenol. The subsequently developed sulfonylmethylphenolic resin (SMRF) system has higher salt and alkali resistance, a longer gelation time, and a wider applicable pH range. Because phenolic cross-linking agents have certain toxicity, their application requires caution.
[0011] Hardy M, Bothmans W, Smith P. New organically cross-linked polymer system provides competent propagation at high temperature in conformance treatments [R]. SPE 39690, 1998. The literature discloses that in 1997, Morgan et al. first proposed a special organically cross-linked PAM gel system. The cross-linking delay of this system is not determined by the chemical composition of the cross-linking agent, but by the composition of the polymer. It forms a gel based on the cross-linking of acrylamide / tert-butyl copolymer (PAtBA) and polyethyleneimine (PEI). Polyethyleneimine has only very weak toxicity compared to phenolic compounds, and its cross-linking reaction generally occurs through amide group reactions or transamide group reactions of functional groups on the polymer side chains. Moreover, under the same environmental conditions, the transport distance of this PAM system is 8 times that of chromium-based systems. The disadvantages are that it is more expensive, and the formed cross-linked polymer is prone to dehydration under high temperature conditions. To improve the gel strength of this system under high temperature conditions, researchers added solid powders such as cement and silica to the system. To enhance the long-term stability of the system, researchers used chelating agents such as citrate, salicylate, oxalate, tartrate, lactate, and disodium EDTA to inhibit the dehydration of the crosslinked polymer gel at high temperatures. The crosslinking time can be extended by using chemical agents, such as polyamino acids, sodium carbonate, and ammonium chloride, which can alter the chemical properties of the crosslinking agent and thus prolong the gelation time between the polymer and the crosslinking agent.
[0012] While cross-linked polymer systems are an effective means of enhancing oil recovery and have advantages such as strong adaptability, they also have some drawbacks. The main drawbacks are that phenolic and organochromium cross-linking agents are toxic to humans and can pollute the environment. In recent years, research on polyethyleneimine and polypropyleneimine as cross-linking agents has received increasing attention, but their current costs are still relatively high, and their stability at high temperatures needs improvement. Ca is commonly found in oil reservoirs. 2+ It can interact with the carboxyl groups on acrylamide polymer molecules, but due to steric hindrance and other reasons, this crosslinking is mainly intramolecular crosslinking, which causes the viscosity of the polymer to decrease rather than increase.
[0013] Therefore, researching and developing a new cross-linked polymer system is of great significance. Summary of the Invention
[0014] The purpose of this invention is to overcome the defect in existing cross-linked polymer systems where cross-linking is mainly intramolecular, leading to a decrease in polymer viscosity instead of an increase. This invention provides a composition for preparing a cross-linked polymer system, the cross-linked polymer system itself, its preparation method, and its applications. This invention utilizes an additive to transform the intramolecular cross-linking of calcium ions with the polymer into intermolecular cross-linking, forming a new cross-linked polymer system. Furthermore, by injecting the cross-linked polymer system into the reservoir, a high-viscosity gel is formed in the reservoir using the reservoir temperature, thereby improving the subsequent waterflooding effect and increasing oil recovery.
[0015] To achieve the above objectives, a first aspect of the present invention provides a composition for preparing a crosslinked polymer system, wherein the composition comprises one or more of a hydrophobic associating polymer, water, a crosslinking agent, and an auxiliary agent;
[0016] The hydrophobic associative polymer is obtained by copolymerization of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid and monomers containing hydrophobic chains;
[0017] The crosslinking agent is a water-soluble salt containing calcium ions;
[0018] The adjuvants are organophosphonic acids and pH adjusters.
[0019] A second aspect of the present invention provides a method for preparing a crosslinked polymer system using the aforementioned composition, wherein the method comprises:
[0020] (1) An aqueous solution of organophosphonic acid is mixed with a pH adjuster to obtain an auxiliary agent solution A;
[0021] (2) Prepare a hydrophobic associative polymer solution using water or reservoir water to obtain solution P;
[0022] (3) Mix the crosslinking agent with water to obtain solution C;
[0023] (4) Under stirring conditions, add auxiliary agent solution A dropwise to solution P, then add solution C dropwise, and stir until the mixture is uniform to carry out the reaction and obtain the cross-linked polymer system.
[0024] A third aspect of the present invention provides a crosslinked polymer system prepared by the method described above.
[0025] A fourth aspect of the present invention provides an application of the aforementioned crosslinked polymer system in oil reservoirs.
[0026] The beneficial effects of the present invention through the above technical solution include:
[0027] (1) The viscosity of the cross-linked polymer system prepared by the present invention can reach 5-80 times the initial viscosity after gelation. After gelation, it has a certain fluidity, which can effectively reduce the flow rate of subsequent injected water, expand the coverage area, and improve the recovery rate.
[0028] (2) The present invention uses an additive to transform the intramolecular crosslinking of calcium ions and polymers into intermolecular crosslinking, forming a new crosslinked polymer system; further, by injecting the crosslinked polymer system into the reservoir, a high-viscosity gel is formed in the reservoir using the reservoir temperature, thereby improving the subsequent water drive effect and increasing the crude oil recovery rate. Attached Figure Description
[0029] Figure 1 This is a schematic diagram of the transaction time curve of the crosslinked polymer system prepared in Example 1;
[0030] Figure 2 This is a schematic diagram of the transaction time curve of the crosslinked polymer system prepared in Example 2;
[0031] Figure 3 This is a schematic diagram of the transaction time curve of the cross-linked polymer system prepared in Example 3. Detailed Implementation
[0032] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0033] As previously stated, the first aspect of the present invention provides a composition for preparing a crosslinked polymer system, wherein the composition comprises one or more of a hydrophobic associating polymer, water, a crosslinking agent, and an auxiliary agent;
[0034] The hydrophobic associative polymer is obtained by copolymerization of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid and monomers containing hydrophobic chains;
[0035] The crosslinking agent is a water-soluble salt containing calcium ions;
[0036] The adjuvants are organophosphonic acids and pH adjusters.
[0037] In this invention, it should be noted that: "intramolecular crosslinking" refers to the reaction of calcium ions with two groups on the same polymer molecular chain, causing the polymer molecular chain to curl; "intermolecular crosslinking" refers to the reaction of calcium ions with groups on two polymer molecular chain segments in water with the help of an auxiliary agent, linking the two polymer molecules together. When multiple calcium ions act, the polymer molecules interpenetrate to form a network structure, thereby increasing the viscosity of the aqueous phase.
[0038] The inventors of this invention discovered that by utilizing an additive, the intramolecular crosslinking of calcium ions with the polymer is transformed into intermolecular crosslinking, forming a new crosslinked polymer system. In other words, intermolecular and intramolecular crosslinking theoretically coexist. Without the additive, intramolecular crosslinking is absolutely dominant; with the additive, calcium ions first bind to the additive and then react with the functional groups on the polymer, resulting in intermolecular crosslinking being absolutely dominant. In this invention, the viscosity of the aqueous solution indirectly reflects which crosslinking mode is dominant. Intramolecular crosslinking reduces viscosity, while intermolecular crosslinking significantly increases viscosity.
[0039] Furthermore, by injecting a cross-linked polymer system into the reservoir, a high-viscosity gel is formed in the reservoir using the reservoir temperature, thereby improving the subsequent waterflooding effect and increasing the crude oil recovery rate.
[0040] According to the present invention, the organophosphonic acid is selected from one or more of aminotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, hydroxyethylenephosphonic acid, diethylenetriaminepentamethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, and 2-phosphonobutyl-1,2,4-tricarboxylic acid, preferably one or more of diethylenetriaminepentamethylenephosphonic acid, hydroxyethylenephosphonic acid, aminotrimethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, and 2-phosphonobutyl-1,2,4-tricarboxylic acid.
[0041] In this invention, when the organophosphonic acid is selected from two of aminotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, hydroxyethylenephosphonic acid, diethylenetriaminepentamethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, and 2-phosphonobutyl-1,2,4-tricarboxylic acid, the ratio of their contents can be 1:(1-3), preferably 1:(1-2; for example, when the organophosphonic acid is selected from diethylenetriaminepentamethylenephosphonic acid and hydroxyethylenephosphonic acid, the ratio of the contents of diethylenetriaminepentamethylenephosphonic acid and hydroxyethylenephosphonic acid can be 1:(1-3), preferably 1:(1-2).
[0042] According to the present invention, the content of the organophosphonic acid is 0.02-0.5 wt% of the total weight of the crosslinked polymer system, preferably 0.05-0.2 wt%.
[0043] According to the present invention, the pH adjuster is selected from one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, and ammonia water, preferably sodium carbonate.
[0044] According to the present invention, the pH of the crosslinked polymer system is 7-8.
[0045] According to the present invention, the crosslinking agent is calcium chloride and / or calcium bromide, preferably calcium chloride.
[0046] According to the present invention, the content of the crosslinking agent, based on the calcium ion content, is 0.05-0.2 wt% of the total weight of the crosslinked polymer system, preferably 0.08-0.15 wt%.
[0047] According to the present invention, the monomer containing the hydrophobic chain is selected from one or more of the following: dodecyl methacrylate, octadecyl methacrylate, tetradecyl methacrylate, linoleic acid acrylate, hexadecyl acrylate, cyclohexyl methacrylate, isodecanyl methacrylate, nonyl methacrylate, tridecyl methacrylate, pentadecyl methacrylate, 3-methylbutenyl methacrylate, 3,7-dimethyloctyl-2,6-dienyl methacrylate, and diallylmethylhexadecylammonium bromide, preferably hexadecyl acrylate. It should be noted that in the present invention, the hydrophobic chain refers to a long-chain alkyl group, such as dodecyl, octadecyl, or tetradecyl.
[0048] According to the present invention, the molar content of acrylamide monomer in the hydrophobic associative polymer is 70-95%; the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5-25%; and the molar content of monomers containing hydrophobic chains is 0.05-1%, preferably 0.1-0.5%.
[0049] In this invention, the preparation method of the hydrophobic associating polymer includes copolymerizing acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and a monomer containing a hydrophobic chain. In this invention, the hydrophobic associating polymer is purchased from Zhengzhou Zhengli Polymer Technology Co., Ltd.; wherein the molar content of the acrylamide monomer in the hydrophobic associating polymer is 94.5%; the molar content of the 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%; and the molar content of the monomer containing the hydrophobic chain is 0.5%.
[0050] According to the present invention, the content of the hydrophobic associative polymer is 0.05-0.5 wt% of the total weight of the crosslinked polymer system, preferably 0.1-0.25 wt%.
[0051] A second aspect of the present invention provides a method for preparing a crosslinked polymer system using the aforementioned composition, wherein the method comprises:
[0052] (1) An aqueous solution of organophosphonic acid is mixed with a pH adjuster to obtain an auxiliary agent solution A;
[0053] (2) Prepare a hydrophobic associative polymer solution using water or reservoir water to obtain solution P;
[0054] (3) Mix the crosslinking agent with water to obtain solution C;
[0055] (4) Under stirring conditions, add auxiliary agent solution A dropwise to solution P, then add solution C dropwise, and stir until the mixture is uniform to carry out the reaction and obtain the cross-linked polymer system.
[0056] According to the present invention, the pH of the auxiliary agent solution A is 7-8, preferably 7.2-7.8.
[0057] According to the present invention, in step (1), the concentration of the aqueous solution of the organophosphonic acid is 20-30%, preferably 20-25%.
[0058] According to the present invention, in step (2), the concentration of solution P is 0.05-0.5%, preferably 0.15-0.2%.
[0059] According to the present invention, in step (2), the reservoir water can be oilfield production reinjection water, fresh water, etc. According to the present invention, in step (3), the concentration of the solution C is 15-25%, preferably 20-25%.
[0060] According to the present invention, in step (4), the reaction conditions include: a temperature of 60-90°C and a time of 10-120 days.
[0061] According to the present invention, in step (4), the amount of the organophosphonic acid is 0.02-0.5 wt%, preferably 0.05-0.2 wt%, based on the total weight of the solution; the amount of the hydrophobic associating polymer is 0.05-0.5 wt%, preferably 0.1-0.25 wt%; and the amount of the crosslinking agent, based on the calcium ion content, is 0.05-0.2 wt%, preferably 0.08-0.15 wt%.
[0062] A third aspect of the present invention provides a crosslinked polymer system prepared by the method described above.
[0063] According to the present invention, the viscosity of the crosslinked polymer system after gelation is 100-1000 mPa·s, preferably 200-500 mPa·s.
[0064] A fourth aspect of the present invention provides an application of the aforementioned crosslinked polymer system in oil reservoirs.
[0065] The present invention will be described in detail below through embodiments.
[0066] In the following examples and comparative examples:
[0067] The crosslinked polymer system solution was placed in ampoules for deoxygenation and sealed, then placed in an oven. The gelation time and the strength after gelation were evaluated by measuring the viscosity change. Viscosity was measured using a rheometer or viscometer, in accordance with the oil and gas industry standard SY_T 6576-2016, "Polymer Evaluation Methods for Enhanced Oil Recovery".
[0068] In this example, the viscosity was measured using a HAAKE MARSⅢ rheometer. The drum was Z41, the rotor was Z43, the shear rate was 7.341 / s, and the temperature was 62°C.
[0069] The polymer used was a commercially available product manufactured by Zhengzhou Zhengli Polymer Technology Co., Ltd., and all other reagents were commercially available products.
[0070] Example 1
[0071] (1) Prepare a 25% aqueous solution by mixing diethylenetriaminepentimethylenephosphonic acid and hydroxyethylenephosphonic acid in a mass ratio of 1:2. Slowly add sodium carbonate as a pH adjuster to the solution, measure the pH value of the solution in real time, and adjust the pH value of the solution to 7.5 to obtain auxiliary solution A.
[0072] (2) Prepare a hydrophobic associating polymer solution with a mass percentage of 0.15% using 1% sodium chloride brine to simulate formation water. The selected hydrophobic associating polymer contains 0.4% of monomers with hydrophobic chains (specifically hexadecyl acrylate). In the hydrophobic associating polymer, the molar content of acrylamide monomer is 94.5%, the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%, and the molar content of monomers containing hydrophobic chains is 0.5%. Continue until the polymer is completely dissolved to obtain solution P.
[0073] (3) Dissolve calcium chloride in water to prepare a 20% calcium chloride aqueous solution C;
[0074] (4) Add auxiliary agent solution A to solution P under stirring at a stirring speed of 500 rpm. The amount of hydrophobic associating polymer is 0.15% of the solution and the amount of organophosphonic acid is 0.1% of the solution. After the mixture is completely homogeneous, add calcium chloride aqueous solution C to make the calcium ion content in the solution 0.1%. Stir until the mixture is homogeneous to obtain the cross-linked polymer system.
[0075] The initial viscosity of the crosslinked polymer system was 18.1 mPa·s. The crosslinked polymer system was placed in multiple ampoules for deoxygenation and sealing, then placed in a 62°C oven. The viscosity of each ampoule was measured at regular intervals to evaluate the gelation time. After 150 days, the viscosity was 375 mPa·s. (See attached image) Figure 1 , Figure 1 This is a schematic diagram of the transaction time curve of the crosslinked polymer system prepared in Example 1. Figure 1 It can be seen that the cross-linking time is slow under these conditions, which is conducive to migration to deeper parts of the reservoir.
[0076] Example 2
[0077] (1) Prepare a 25% aqueous solution by mixing diethylenetriaminepentimethylenephosphonic acid and hydroxyethylenephosphonic acid in a mass ratio of 1:2. Slowly add sodium carbonate to the solution, measure the pH value of the solution in real time, and adjust the pH value of the solution to 7.5 to obtain auxiliary agent solution A.
[0078] (2) Prepare a hydrophobic associating polymer solution with a mass percentage of 0.18% using 1% sodium chloride brine to simulate formation water. The selected hydrophobic polymer contains 0.4% of monomers with hydrophobic chains (specifically hexadecyl acrylate). In the hydrophobic associating polymer, the molar content of acrylamide monomer is 94.5%, the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%, and the molar content of monomers containing hydrophobic chains is 0.5%. Continue until the polymer is completely dissolved to obtain solution P.
[0079] (3) Dissolve calcium chloride in water to prepare a 20% aqueous solution C;
[0080] (4) Add auxiliary agent A to solution P while stirring at a stirring speed of 500 rpm. The amount of hydrophobic associating polymer is 0.18% of the solution and the amount of organophosphonic acid is 0.15% of the solution. After the mixture is completely homogeneous, add solution C to make the calcium ion content in the solution 0.1%. Stir until the mixture is homogeneous to obtain the cross-linked polymer system.
[0081] The initial viscosity of the crosslinked polymer system was 24.3 mPa·s. The crosslinked polymer solution was placed in multiple ampoules for deoxygenation and sealing, then placed in a 62°C oven. The viscosity of each ampoule was measured at regular intervals to evaluate the gelation time. After 150 days, the viscosity was 460.4 mPa·s. (See attached image) Figure 2 , Figure 2 This is a schematic diagram of the transaction time curve of the crosslinked polymer system prepared in Example 2. Figure 2 It can be seen that the cross-linking time is slow under these conditions, which is conducive to migration to deeper parts of the reservoir.
[0082] Example 3
[0083] (1) Prepare a 25% aqueous solution by mixing diethylenetriaminepentimethylenephosphonic acid and hydroxyethylenephosphonic acid in a mass ratio of 1:2. Slowly add sodium carbonate to the solution, measure the pH value of the solution in real time, and adjust the pH value of the solution to 7.5 to obtain auxiliary agent solution A.
[0084] (2) Prepare a hydrophobic associating polymer solution with a mass percentage of 0.12% using 1% sodium chloride brine to simulate formation water. The selected hydrophobic associating polymer contains 0.4% of monomers with hydrophobic chains (specifically hexadecyl acrylate). In the hydrophobic associating polymer, the molar content of acrylamide monomer is 94.5%, the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%, and the molar content of monomers containing hydrophobic chains is 0.5%. Continue until the polymer is completely dissolved to obtain solution P.
[0085] (3) Dissolve calcium chloride in water to prepare a 20% aqueous solution C;
[0086] (4) Add auxiliary agent A to solution P while stirring at a stirring speed of 500 rpm. The amount of hydrophobic associating polymer is 0.12% of the solution and the amount of organophosphonic acid is 0.09% of the solution. After the mixture is completely homogeneous, add solution C to make the calcium ion content in the solution 0.1%. Stir until the mixture is homogeneous to obtain the cross-linked polymer system.
[0087] The initial viscosity of the crosslinked polymer system was 11.8 mPa·s. The crosslinked polymer solution was placed in multiple ampoules for deoxygenation and sealing, then placed in a 62°C oven. The viscosity of each ampoule was measured at regular intervals to evaluate the gelation time. After 150 days, the viscosity was 352 mPa·s. (See attached image) Figure 3 , Figure 3 This is a schematic diagram of the transaction time curve of the crosslinked polymer system prepared in Example 3. Figure 3 It can be seen that the cross-linking time is slow under these conditions, which is conducive to migration to deeper parts of the reservoir.
[0088] Example 4
[0089] (1) Prepare a 25% aqueous solution of aminotrimethylenephosphonic acid, slowly add sodium carbonate to the solution, measure the pH value of the solution in real time, adjust the pH value of the solution to 7.0, and obtain auxiliary solution A;
[0090] (2) Prepare a hydrophobic associating polymer solution with a mass percentage of 0.15% using 1% sodium chloride brine to simulate formation water. The selected hydrophobic polymer contains a hydrophobic monomer (specifically, hexadecyl acrylate) with a molar ratio of 0.4%. In the hydrophobic associating polymer, the molar content of acrylamide monomer is 94.5%, the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%, and the molar content of monomers containing hydrophobic chains is 0.5%. Continue until the polymer is completely dissolved to obtain solution P.
[0091] (3) Dissolve calcium chloride in water to prepare a 20% aqueous solution C;
[0092] (4) Add auxiliary agent A to solution P while stirring at a stirring speed of 500 rpm. The amount of hydrophobic associating polymer is 0.15% of the solution and the amount of organophosphonic acid is 0.12% of the solution. After the mixture is completely homogeneous, add solution C to make the calcium ion content in the solution 0.12%. Stir until the mixture is homogeneous to obtain the cross-linked polymer system.
[0093] The initial viscosity of the crosslinked polymer system was 35.2 mPa·s. The crosslinked polymer system solution was placed in multiple ampoules for deoxygenation and sealing, and then placed in a 90°C oven. At regular intervals, one ampoule was taken out to measure the viscosity. After 15 days, the viscosity was measured to be 857 mPa·s.
[0094] Example 5
[0095] (1) Prepare a 25% aqueous solution of aminotrimethylenephosphonic acid, slowly add sodium carbonate to the solution, measure the pH value of the solution in real time, adjust the pH value of the solution to 7.8, and obtain auxiliary solution A;
[0096] (2) Prepare a hydrophobic associating polymer solution with a mass percentage of 0.16% using 1.5% sodium chloride brine to simulate formation water. The selected hydrophobic polymer contains 0.4% of monomers with hydrophobic chains (specifically hexadecyl acrylate). In the hydrophobic associating polymer, the molar content of acrylamide monomer is 94.5%, the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%, and the molar content of monomers containing hydrophobic chains is 0.5%. Continue until the polymer is completely dissolved to obtain solution P.
[0097] (3) Dissolve calcium chloride in water to prepare a 20% aqueous solution C;
[0098] (4) Add additive A to solution P while stirring at a speed of 500 rpm. The amount of hydrophobic associating polymer is 0.16% of the solution and the amount of organophosphonic acid is 0.06% of the solution. After the mixture is completely homogeneous, add solution C to make the calcium ion content in the solution 0.12%. Stir until the mixture is homogeneous to obtain the cross-linked polymer system.
[0099] The initial viscosity of the crosslinked polymer system was 18.3 mPa·s. The crosslinked polymer system solution was placed in multiple ampoules for deoxygenation and sealing, and then placed in an 80°C oven. The viscosity of one ampoule was measured at intervals. After 31 days, the viscosity was measured to be 433 mPa·s.
[0100] Example 6
[0101] (1) Prepare a 25% aqueous solution by mixing aminotrimethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, and 2-phosphonobutyl-1,2,4-tricarboxylic acid in a mass ratio of 1:2:1. Slowly add sodium carbonate to the solution, measure the pH value of the solution in real time, and adjust the pH value of the solution to 7.5 to obtain auxiliary agent solution A.
[0102] (2) Prepare a hydrophobic associating polymer solution with a mass percentage of 0.18% using 1.5% sodium chloride brine to simulate formation water. The selected hydrophobic polymer contains a hydrophobic monomer (specifically hexadecyl acrylate) with a molar ratio of 0.4%. In the hydrophobic associating polymer, the molar content of acrylamide monomer is 94.5%, the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%, and the molar content of monomers containing hydrophobic chains is 0.5%. Continue until the polymer is completely dissolved to obtain solution P.
[0103] (3) Dissolve calcium chloride in water to prepare a 20% aqueous solution C;
[0104] (4) Add auxiliary agent A to solution P while stirring at a stirring speed of 500 rpm. The amount of hydrophobic associating polymer is 0.18% of the solution and the amount of organophosphonic acid is 0.15% of the solution. After the mixture is completely homogeneous, add solution C to make the calcium ion content in the solution 0.12%. Stir until the mixture is homogeneous to obtain the cross-linked polymer system.
[0105] The initial viscosity of the crosslinked polymer system was 32.8 mPa·s. The crosslinked polymer system solution was placed in multiple ampoules for deoxygenation and sealing, and then placed in an 80°C oven. At regular intervals, one ampoule was taken out to measure the viscosity. The viscosity was 145 mPa·s after 15 days and 1217 mPa·s after 50 days.
[0106] Example 7
[0107] (1) Prepare a 25% aqueous solution of diethylenetriaminepentimethylenephosphonic acid, slowly add sodium carbonate to the solution, measure the pH value of the solution in real time, adjust the pH value of the solution to 7.5, and obtain auxiliary agent solution A;
[0108] (2) Prepare a hydrophobic associating polymer solution with a mass percentage of 0.12% using 1% sodium chloride brine to simulate formation water. The selected hydrophobic associating polymer contains 0.4% of monomers with hydrophobic chains (specifically hexadecyl acrylate). In the hydrophobic associating polymer, the molar content of acrylamide monomer is 94.5%, the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%, and the molar content of monomers containing hydrophobic chains is 0.5%. Continue until the polymer is completely dissolved to obtain solution P.
[0109] (3) Dissolve calcium chloride in water to prepare a 20% aqueous solution C;
[0110] (4) Add auxiliary agent A to solution P while stirring at a stirring speed of 500 rpm. The amount of hydrophobic associating polymer is 0.12% of the solution and the amount of organophosphonic acid is 0.18% of the solution. After the mixture is completely homogeneous, add solution C to make the calcium ion content in the solution 0.1%. Stir until the mixture is homogeneous to obtain the cross-linked polymer system.
[0111] The initial viscosity of the crosslinked polymer system was 18.9 mPa·s. The crosslinked polymer solution was placed in multiple ampoules for deoxygenation and sealing, and then placed in an 80°C oven. At regular intervals, one ampoule was removed to measure the viscosity and evaluate the gelation time. The viscosity was measured to be 83.5 mPa·s after 17 days and 811.3 mPa·s after 50 days.
[0112] Example 8
[0113] (1) Prepare a 25% aqueous solution of diethylenetriaminepentimethylenephosphonic acid, slowly add sodium carbonate to the solution, measure the pH value of the solution in real time, adjust the pH value of the solution to 7.5, and obtain auxiliary agent solution A;
[0114] (2) Prepare a hydrophobic associating polymer solution with a mass percentage of 0.12% using 1% sodium chloride brine to simulate formation water. The selected hydrophobic polymer contains 0.6% of monomers with hydrophobic chains (specifically hexadecyl acrylate). In the hydrophobic associating polymer, the molar content of acrylamide monomer is 94.5%, the molar content of 2-acrylamido-2-methylpropanesulfonic acid monomer is 5%, and the molar content of monomers containing hydrophobic chains is 0.5%. Continue until the polymer is completely dissolved to obtain solution P.
[0115] (3) Dissolve calcium chloride in water to prepare a 20% aqueous solution C;
[0116] (4) Add auxiliary agent A to solution P while stirring at a stirring speed of 500 rpm. The amount of hydrophobic associating polymer is 0.12% of the solution and the amount of organophosphonic acid is 0.12% of the solution. After the mixture is completely homogeneous, add solution C to make the calcium ion content in the solution 0.1%. Stir until the mixture is homogeneous to obtain the cross-linked polymer system.
[0117] The initial viscosity of the crosslinked polymer system was 26.8 mPa·s. The crosslinked polymer solution was placed in multiple ampoules for deoxygenation and sealing, then placed in an 80°C oven. The viscosity of each ampoule was measured at regular intervals to evaluate the gelation time. The viscosity was 156.2 mPa·s after 17 days and 1025.4 mPa·s after 50 days.
[0118] Example 9
[0119] The crosslinked polymer system was prepared using the same method as in Example 1, except that "diethylenetriaminepentamethylenephosphonic acid and hydroxyethylenephosphonic acid in a mass ratio of 1:2" in Example 1 was replaced with "ethylenediaminetetramethylenephosphonic acid".
[0120] The initial viscosity of the prepared crosslinked polymer system was 18.1 mPa·s. The crosslinked polymer system was placed in multiple ampoules for deoxygenation and sealing, and then placed in an oven at 62°C. At regular intervals, one ampoule was taken out to measure the viscosity and evaluate the gelation time. After 150 days, the viscosity was 126 mPa·s.
[0121] Comparative Example 1
[0122] The crosslinked polymer system was prepared using the same method as in Example 1, except that "diethylenetriaminepentamethylenephosphonic acid and hydroxyethylenephosphonic acid" were not used in Example 1.
[0123] The initial viscosity of the prepared crosslinked polymer system was 18.1 mPa·s. The crosslinked polymer system was placed in multiple ampoules for deoxygenation and sealing, then placed in a 62°C oven. The viscosity of each ampoule was measured periodically to evaluate the gelation time; after 30 days, the viscosity was 8.6 mPa·s. This demonstrates that intramolecular crosslinking occurs without additives.
[0124] Comparative Example 2
[0125] The crosslinked polymer system was prepared using the same method as in Example 1, except that the phrase “a 25% aqueous solution of diethylenetriaminepentimethylenephosphonic acid and hydroxyethylenephosphonic acid in a 1:2 ratio” in Example 1 was replaced with “25% phosphoric acid”.
[0126] The initial viscosity of the prepared crosslinked polymer system was 18.5 mPa·s. The crosslinked polymer system was placed in multiple ampoules for deoxygenation and sealing, and then placed in an oven at 62°C. At regular intervals, one ampoule was taken out to measure the viscosity and evaluate the gelation time. After 30 days, the viscosity was 8.4 mPa·s.
[0127] Comparative Example 3
[0128] The crosslinked polymer system was prepared using the same method as in Example 1, except that in step (4) of Example 1, "the amount of organophosphonic acid is 0.1% of the solution" was replaced with "the amount of organophosphonic acid is 0.6% of the solution".
[0129] The initial viscosity of the prepared crosslinked polymer system was 18.3 mPa·s. The crosslinked polymer system was placed in multiple ampoules for deoxygenation and sealing, and then placed in an oven at 62°C. At each time interval, one ampoule was taken out to measure the viscosity and evaluate the gelation time. The viscosity after 150 days was 21.3 mPa·s.
[0130] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A composition for preparing a crosslinked polymer system, characterized in that, The composition comprises one or more of a hydrophobic associative polymer, water, a crosslinking agent, and an additive. The hydrophobic associative polymer is obtained by copolymerization of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid and monomers containing hydrophobic chains; The crosslinking agent is a water-soluble salt containing calcium ions; The adjuvants are organophosphonic acids and pH adjusters.
2. The composition according to claim 1, wherein, The organophosphonic acid is selected from one or more of aminotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, hydroxyethylenephosphonic acid, diethylenetriaminepentamethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, and 2-phosphonobutyl-1,2,4-tricarboxylic acid; And / or, the content of the organophosphonic acid is 0.02-0.5 wt% of the total weight of the crosslinked polymer system, preferably 0.05-0.2 wt%.
3. The composition according to claim 1, wherein, The crosslinking agent is calcium chloride and / or calcium bromide, preferably calcium chloride; And / or, the content of the crosslinking agent, based on the calcium ion content, is 0.05-0.2 wt% of the total weight of the crosslinked polymer system, preferably 0.08-0.15 wt%.
4. The composition according to claim 1, wherein, The monomer containing the hydrophobic chain is selected from one or more of the following: dodecyl methacrylate, octadecyl methacrylate, tetradecyl methacrylate, linoleic methacrylate, hexadecyl methacrylate, cyclohexyl methacrylate, isodecanyl methacrylate, nonyl methacrylate, tridecyl methacrylate, pentadecyl methacrylate, 3-methylbutenyl methacrylate, 3,7-dimethyloctyl methacrylate, and diallylmethylhexadecylammonium bromide.
5. The composition according to claim 1, wherein, The hydrophobic associative polymer contains 70-95% acrylamide monomer, 5-25% 2-acrylamido-2-methylpropanesulfonic acid monomer, and 0.05-1% monomers containing hydrophobic chains. And / or, the content of the hydrophobic associating polymer is 0.05-0.5 wt% of the total weight of the crosslinked polymer system, preferably 0.1-0.25 wt%.
6. The composition according to claim 1, wherein, The pH adjuster is selected from one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, and ammonia water, preferably sodium carbonate; And / or, the pH of the crosslinked polymer system is 7-8.
7. A method for preparing a crosslinked polymer system using the composition according to any one of claims 1-6, characterized in that, The method includes: (1) An aqueous solution of organophosphonic acid is mixed with a pH adjuster to obtain an auxiliary agent solution A; (2) Prepare a hydrophobic associative polymer solution using water or reservoir water to obtain solution P; (3) Mix the crosslinking agent with water to obtain solution C; (4) Under stirring conditions, add auxiliary agent solution A dropwise to solution P, then add solution C dropwise, and stir until the mixture is uniform to carry out the reaction and obtain the cross-linked polymer system.
8. The method according to claim 7, wherein, The pH of the auxiliary agent solution A is 7-8; And / or, in step (1), the concentration of the aqueous solution of the organophosphonic acid is 20-30%; And / or, in step (2), the concentration of solution P is 0.05-0.5%; And / or, in step (3), the concentration of solution C is 15-25%; And / or, in step (4), the reaction conditions include: a temperature of 60-90°C and a time of 10-120 days; And / or, in step (4), based on the total weight of the solution, the amount of the organophosphonic acid is 0.02-0.5 wt%, preferably 0.05-0.2 wt%; the amount of the hydrophobic associating polymer is 0.05-0.5 wt%, preferably 0.1-0.25 wt%; and the amount of the crosslinking agent, based on the calcium ion content, is 0.05-0.2 wt%, preferably 0.08-0.15 wt%.
9. A crosslinked polymer system prepared by the method of claim 7 or 8.
10. The crosslinked polymer system according to claim 9, wherein, The viscosity of the crosslinked polymer system after gelation is 100-1000 mPa·s.
11. The application of the crosslinked polymer system according to claim 9 or 10 in an oil reservoir.