A high-temperature hot delivery production method of an alloy structural steel plate 30MnB
By optimizing the parameter control of continuous casting, heating and rolling processes and eliminating the billet stacking process, high-temperature hot delivery production of 30MnB steel plates was achieved, solving the problems of thermal stress sensitivity and production rhythm, reducing energy consumption and improving steel plate quality.
Patent Information
- Application Number
- CN202611353068.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-10
AI Technical Summary
In the current production of 30MnB steel plates, the high carbon equivalent leads to a high tendency to harden, poor thermal conductivity, and sensitivity to thermal stress, making it prone to cracking during heating. Furthermore, the long billet stacking time affects the production rhythm, increases energy consumption, and extends the processing cycle.
By controlling the superheat, casting speed, and secondary cooling water ratio in the continuous casting process, the billet is rapidly conveyed and fed into the furnace at high temperature. Combined with the stepped temperature control of the heating process and the rolling cooling process, the billet stacking process is eliminated. ACC cooling and tempering heat treatment are adopted to achieve high-temperature hot delivery of the billet.
It reduced production energy consumption, increased production speed, avoided heating cracks in the cast billet, met the quality requirements of alloy structural steel, and achieved a balance between high strength and toughness.
Smart Images

Figure CN123063582A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical rolling technology, specifically relating to a production method of 30MnB alloy structural steel plate. Background Technology
[0002] 30MnB steel plate is a high-strength boron alloy steel widely used in the field of engineering machinery. Its high carbon content and the addition of trace amounts of boron (B) significantly improve hardenability. Combined with subsequent heat treatment, it achieves an excellent balance of strength and toughness. It is mainly used to manufacture excavator buckets, pins, and gears, as well as agricultural harvester blades and plowshares—components that need to withstand high loads and wear.
[0003] This steel grade also faces some challenges in production. Due to its high carbon equivalent, it has a strong tendency to harden, poor thermal conductivity, and is extremely sensitive to thermal and structural stress. To avoid excessive thermal stress caused by the low temperature of the billet entering the furnace, which could lead to billet breakage or surface / internal cracking, the process clearly requires that the billet charging temperature be maintained above 150℃ to ensure that the billet retains a certain degree of plasticity, thus ensuring that it can smoothly complete the microstructure transformation and stress release during reheating. In addition, the stacking time is limited, and it is often required that the billet be stacked and slowly cooled for more than 24 hours to ensure that the billet temperature drops below 600℃, avoiding post-rolling hot-pressing cracks and achieving hydrogen evolution in the billet.
[0004] Patent application CN109852882A discloses a 30MnB steel plate for alloy structures and its production method. By designing a medium carbon composition and adding B element, the density and hot rolling performance of the steel are improved, and the strength of the steel plate is increased. However, this invention requires the billet to be stacked for 24-30 hours, which seriously restricts the production line rhythm.
[0005] In actual production, due to factors such as fluctuations in the rhythm of the steelmaking-rolling process, billet turnover, extended stacking time, or equipment maintenance, the temperature of some billets drops below 150℃ before entering the furnace. At this time, the temperature difference between the billet and the furnace is too large, which can easily cause thermal stress cracks. Therefore, they cannot be directly loaded into the furnace and must undergo secondary heating treatment to raise their temperature back to above 150℃ before they can be loaded into the furnace. The process of cooling and then heating the billet not only increases the additional heating energy consumption and processing cycle, but also disrupts the original production rhythm.
[0006] Therefore, there is an urgent need for a production method for high carbon equivalent steel grades such as 30MnB that can achieve high-temperature hot charging to reduce energy consumption and heating cycle, while avoiding heating cracking of 30MnB billets. Summary of the Invention
[0007] The technical problem to be solved by the present invention is to provide a high-temperature hot conveying production method for 30MnB alloy structural steel, which can significantly reduce energy consumption costs and reduce the difficulty of production organization, while the overall quality of the alloy structural steel plate meets customer requirements.
[0008] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: A high-temperature hot-feeding production method for 30MnB alloy structural steel includes continuous casting, billet heating, rolling, controlled cooling, and quenching and tempering heat treatment processes.
[0009] Furthermore, in the continuous casting process described in this invention, the superheating temperature during casting is controlled at 15–25°C, the water content in the secondary cooling zone is controlled at 0.48–0.52 L / kg, and the casting speed is controlled at 0.85–0.90 m / min. After the continuously cast billet exits the fan-shaped section, it is cut to the target size by a flame cutter and then conveyed to the furnace inlet via a roller conveyor. During the conveying process, the roller conveyor is covered with an insulation cover throughout to prevent the hot billet from remaining in the air. It enters the furnace within 60 minutes, ensuring that the billet temperature upon entering the furnace is 730–850°C. The higher furnace temperature can reduce the temperature difference between the billet and the furnace temperature after entering the furnace, thereby reducing thermal stress.
[0010] By controlling the superheat and appropriately reducing the casting speed, the solidification quality of the continuously cast billet can be improved. Reducing the specific water content in the secondary cooling zone lowers the surface stress of the billet after exiting the fan-shaped section, thus reducing the risk of hot-carrying cracks after the billet enters the furnace. Controlling the superheat at 15-25℃ ensures that the columnar / equiaxed crystal ratio at the solidification front of the billet is within a reasonable range. The specific water content in the secondary cooling zone is 0.48-0.52 L / kg, providing low-intensity cooling that matches the superheat, preventing excessive solidification shrinkage stress on the billet surface. Controlling the casting speed at 0.85-0.90 m / min, corresponding to the aforementioned superheat and cooling intensity, ensures that the billet's exit temperature in the fan-shaped section is within a reasonable range, keeping the residual stress after the superposition of surface structural stress and thermal stress below the critical crack propagation stress threshold. These three factors together determine the initial stress level of the billet exiting the fan-shaped section, providing the stress conditions for subsequent high-temperature hot-carrying.
[0011] Furthermore, in the continuous casting process of the present invention, after the continuously cast billet exits the fan-shaped section, it is cut to the target size by a flame cutting machine and then conveyed to the inlet of the heating furnace via a roller conveyor. During the conveying process, the roller conveyor is covered with a heat insulation cover throughout to prevent the hot billet from staying in the air. It enters the furnace within 60 minutes to ensure that the billet temperature in the furnace is 730-850°C. The higher furnace temperature can reduce the temperature difference between the billet and the furnace temperature after entering the heating furnace, thereby reducing thermal stress.
[0012] Furthermore, in the billet heating process described in this invention, the temperature of the first heating section is controlled at 950±30℃, the temperature of the second heating section at 1100±20℃, the temperature of the third heating section at 1200±20℃, and the temperature of the soaking section at 1240±20℃, with the soaking time controlled at 180~250min. This segmented heating section temperature control within the furnace, based on the relatively high initial furnace temperature of 30MnB, achieves gradual heating of the billet under a lower temperature difference, reducing the risk of billet cracking due to excessive thermal stress.
[0013] Furthermore, the rolling process described in this invention is a two-stage rolling process, with an initial rolling temperature of 1050-1100℃, a waiting-to-heat thickness ≥1.8a, where a is the finished thickness of the steel plate, a final waiting-to-heat temperature ≤830℃, and a final rolling temperature controlled at 800-830℃.
[0014] Furthermore, the controlled cooling process described in this invention employs ACC controlled cooling. The ACC section adopts a weak cooling mode, with the cooling rate controlled at 3-5℃ / s and the final cooling temperature controlled at 640-670℃. After cooling, the 30MnB steel plate is hot-straightened and then directly conveyed to the stacking area via roller conveyor for slow cooling without passing through a cooling bed. This avoids warping of the 30MnB due to uneven cooling on the cooling bed. At the same time, the temperature of the steel plate during stacking is above 400℃. In this temperature range, the hydrogen diffusion coefficient is tens of times higher than at room temperature. High-temperature stacking allows hydrogen in the core to begin escaping to the surface while the steel plate as a whole is still at a relatively high temperature. Thus, hydrogen evolution through steel plate stacking replaces hydrogen evolution through billet stacking.
[0015] Furthermore, the weak cooling mode described in this invention refers to setting the ACC water volume to a relatively small volume, that is, controlling the water supply volume at 150-180 L / (min*m2), and the water volume ratio of the upper and lower manifolds of the ACC section to 1.7-1.9.
[0016] Furthermore, in the quenching and tempering heat treatment process of the present invention, the quenching heating temperature is 860-870℃, and the holding time is 120-150min; the tempering temperature is 195-205℃, and the tempering holding time is 180-220min.
[0017] Furthermore, the chemical composition and mass percentage of the alloy structural steel 30MnB described in this invention are as follows: C: 0.28–0.31%, Si: 0.20–0.30%, Mn: 1.20–1.30%, Cr: 0.45–0.55%, Ti: 0.015–0.025%, B: 0.0012–0.0025%, Als: 0.015–0.025%, P≤0.018%, S≤0.005%, with the balance being Fe and unavoidable residual elements and impurities from the production process. The Als content is intentionally controlled to prevent AlN precipitation at the grain boundaries of the cast billet, which weakens the grain boundary bonding and reduces the risk of red-heat cracking during the billet heating process.
[0018] Al is an important deoxidizer in steelmaking, and maintaining a certain amount of Al ensures the purity of molten steel deoxidation. According to the precipitation kinetics of Al, reducing the Al content will reduce the supersaturation of Al in local areas, significantly increasing the critical nucleation work and reducing the possibility of AlN nucleation and growth. By controlling the Al content below 0.025% and keeping the billet holding time within 60 minutes, Al carbonitrides in the billet have not yet begun to precipitate in large quantities, further reducing the crack sensitivity of the billet during hot delivery. In addition, it also ensures that the billet temperature entering the furnace is between 730℃ and 850℃, which, combined with the process setting of the first heating section temperature (950±30℃) in the heating process, can greatly reduce the thermal stress of the billet caused by temperature difference in the heating furnace.
[0019] Furthermore, the thickness of the alloy structural steel 30MnB described in this invention is 60-90 mm.
[0020] The alloy structural steel 30MnB produced by the method described in this invention has a tensile strength of 1433-1542 MPa, an elongation of 8.2-14.5%, an impact energy of 35-58 J at -20℃, and a Brinell hardness of 492-520 HBW.
[0021] The inventive principle and beneficial technical effects of this invention are as follows: This invention suppresses the continuous precipitation of AlN at grain boundaries by controlling the Al content at a low level of 0.015~0.025%, thereby improving grain boundary bonding from a metallurgical perspective. Simultaneously, through the coordinated matching of three parameters in the continuous casting process—superheat, secondary cooling water ratio, and casting speed—the residual stress in the fan-shaped section of the billet is controlled below the critical extended stress threshold. Based on this, the 30MnB billet stacking step is eliminated, and the original production path of "continuous casting → stacking and slow cooling → furnace loading" is restructured into a new path of "continuous casting → rapid conveying under a heat insulation hood → stepped heating," achieving a process transformation. By eliminating the billet stacking step and combining it with subsequent rolling, controlled cooling, and heat treatment processes, alloy structural steel 30MnB that meets the mechanical performance requirements is obtained. In this invention, the slow cooling method of the steel plate stacking after rolling is a natural cooling method after the steel plate's ACC (Advanced Crude Oil) has cooled to 640-670°C. It is naturally integrated with the rolling line and does not constitute an independent time-consuming process. Stacking is transformed from a bottleneck process restricting the production line rhythm into an auxiliary method for the natural cooling of the steel plate, achieving a fundamental change in the process logic. This invention solves the problem in the actual production of this type of alloy steel billet where the slow cooling time of stacking is too long due to fluctuations in the steelmaking-rolling process rhythm, billet turnover, or equipment maintenance, resulting in the billet temperature dropping below 150°C before entering the furnace and requiring secondary heating. It eliminates the fuel consumption of heating from low temperature to high temperature, and allows for continuous flow of the billet from continuous casting to the heating furnace. The production line rhythm is no longer constrained by fluctuations in stacking time, reducing additional heating energy consumption and processing cycles, and improving the production line's production rhythm. Attached Figure Description
[0022] Figure 1 This is a 500× microstructure image of 30MnB from Example 1; Figure 2 This is a 500× microstructure image of 30MnB from Example 2; Figure 3 This is a 500× microstructure image of 30MnB in Example 3; Figure 4 This is a 500× microstructure image of 30MnB from Example 4; Figure 5 This is a 500× microstructure image of 30MnB in Example 5; Figure 6 This is a 500× microstructure image of 30MnB in Example 6. Detailed Implementation
[0023] The specific embodiments of the present invention will be further described below with reference to examples, but the present invention is not limited to the scope of the embodiments described herein.
[0024] Examples 1-6 The chemical composition and mass percentage of the alloy structural steel 30MnB in each embodiment are shown in Table 1.
[0025] Table 1 Chemical composition and mass percentage (wt%) of high-strength steels in Examples 1-6
[0026] The high-temperature hot-feeding production method of alloy structural steel 30MnB in each embodiment includes continuous casting, billet heating, rolling, controlled cooling, and quenching and tempering heat treatment processes; the details are as follows: (1) Continuous casting process: The superheat of the casting is controlled at 15-25℃, the water content in the secondary cooling zone is controlled at 0.48-0.52L / kg, and the casting speed is controlled at 0.85-0.90m / min. After the continuous casting billet exits the fan-shaped section, it is cut to the target size by a flame cutting machine and then conveyed to the inlet of the heating furnace via roller conveyor. During the conveying process, the roller conveyor is covered with a heat insulation cover to prevent the hot billet from staying in the air. The billet conveying time is controlled within 60 minutes to ensure that the billet temperature entering the furnace is 730-850℃.
[0027] (2) Heating process: The temperature of the first heating section is controlled at 950±30℃, the temperature of the second heating section is controlled at 1100±20℃, the temperature of the third heating section is controlled at 1200±20℃, the temperature of the heat soaking section is controlled at 1240±20℃, and the heat soaking time is controlled at 180~250min.
[0028] (3) Rolling process: It is a two-stage rolling process. The initial rolling temperature is 1050~1100℃, the thickness after heating is ≥1.8a, where a is the thickness of the finished steel plate, the final heating temperature is ≤830℃, and the final rolling temperature is controlled at 800~830℃.
[0029] (4) Controlled cooling process: ACC controlled cooling is adopted. The ACC section adopts a weak cooling mode, the cooling rate is controlled at 3-5℃ / s, and the final cooling temperature is controlled at 640-670℃. After cooling, the 30MnB steel plate is hot straightened and then sent directly to the stacking area for slow cooling via roller conveyor without passing through the cooling bed. The temperature of the steel plate is above 400℃ during stacking.
[0030] (5) Tempering heat treatment process: Quenching heating temperature is 860~870℃, quenching holding time is 120~150min; tempering temperature is 195~205℃, tempering holding time is 180~220min.
[0031] The parameters for the continuous casting process, billet heating process, rolling and cooling process, and quenching and tempering heat treatment process of the alloy structural steel 30MnB in each embodiment are shown in Tables 2 to 5. Table 2 Parameters of continuous casting process in each embodiment
[0032] Table 3 Heating process parameters for each embodiment
[0033] Table 4 Rolling and cooling process parameters for each embodiment
[0034] Table 5. Parameters of the quenching and tempering heat treatment process in each embodiment.
[0035] The microstructures of alloy structural steel 30MnB in Examples 1-6 are shown in the figures below. Figures 1-6 .Depend on Figures 1-6 It is known that the 30MnB steel plate produced by the method of the present invention has a fine tempered martensite structure. The fine and uniform tempered martensite structure can ensure that the strength and low-temperature impact toughness of the steel plate meet the requirements under the alloy system of the present invention.
[0036] The thickness specifications and mechanical properties of the alloy structural steel 30MnB in each embodiment are shown in Table 6.
[0037] Table 3. Thickness specifications and mechanical properties of 30MnB steel in each example
[0038] Note: Charpy (V-notch) impact absorption energy is tested using a set of 3 individual samples. The impact test temperature for 30MnB is -20℃. The three values in Table 3 for the impact energy at -20℃ are the individual values of the 3 samples tested in a set of Charpy impact absorption energy tests.
[0039] As shown in Table 6, the 30MnB steel plate produced by the method of the present invention has a tensile strength of 1433-1542MPa, an elongation of 8.2-14.5%, an impact energy of 35-58J at -20℃, and a Brinell hardness of 492-520HBW.
Claims
1. A high-temperature hot conveying production method for 30MnB alloy structural steel, characterized in that, It includes continuous casting, billet heating, rolling, controlled cooling and tempering heat treatment processes; the continuous casting process: the casting superheat is controlled at 15-25℃, the water content in the secondary cooling zone is controlled at 0.48-0.52L / kg, and the casting speed is controlled at 0.85-0.90m / min.
2. The high-temperature hot conveying production method of alloy structural steel 30MnB according to claim 1, characterized in that, In the continuous casting process, after the continuous casting billet is cut, it is conveyed to the entrance of the heating furnace via roller conveyor. During the conveying process, the roller conveyor is covered with a heat insulation cover throughout, and the billet conveying time is controlled within 60 minutes to ensure that the billet temperature entering the furnace is 730-850℃.
3. The high-temperature hot conveying production method of alloy structural steel 30MnB according to claim 1, characterized in that, The billet heating process is as follows: the temperature of the first heating section is controlled at 950±30℃, the temperature of the second heating section is controlled at 1100±20℃, the temperature of the third heating section is controlled at 1200±20℃, the temperature of the soaking section is controlled at 1240±20℃, and the soaking time is controlled at 180~250min.
4. The high-temperature hot conveying production method of alloy structural steel 30MnB according to claim 1, characterized in that, The rolling process consists of two stages: an initial rolling temperature of 1050–1100℃, a waiting-to-heat thickness of ≥1.8a (where a is the finished steel plate thickness), a final waiting-to-heat temperature of ≤830℃, and a final rolling temperature controlled between 800 and 830℃.
5. The high-temperature hot conveying production method of alloy structural steel 30MnB according to claim 1, characterized in that, The controlled cooling process is as follows: ACC controlled cooling is adopted. The ACC section adopts a weak cooling mode, the cooling rate is controlled at 3-5℃ / s, and the final cooling temperature is controlled at 640-670℃. After cooling, the 30MnB steel plate is hot straightened and then directly sent to the stacking area for slow cooling via roller conveyor without passing through the cooling bed. The temperature of the steel plate is above 400℃ during stacking.
6. The high-temperature hot conveying production method of alloy structural steel 30MnB according to claim 1, characterized in that, The quenching and tempering heat treatment process includes: quenching heating temperature of 860-870℃ and quenching holding time of 120-150min; tempering temperature of 195-205℃ and tempering holding time of 180-220min.
7. The high-temperature hot conveying production method of alloy structural steel 30MnB according to claim 1, characterized in that, The chemical composition and mass percentage of the alloy structural steel 30MnB are as follows: C: 0.28-0.31%, Si: 0.20-0.30%, Mn: 1.20-1.30%, Cr: 0.45-0.55%, Ti: 0.015-0.025%, B: 0.0012-0.0025%, Als: 0.015-0.025%, P≤0.018%, S≤0.005%, with the balance being Fe and unavoidable residual elements and impurities from the production process.
8. The high-temperature hot conveying production method of alloy structural steel 30MnB according to claim 1, characterized in that, The alloy structural steel 30MnB produced by the method has a tensile strength of 1433-1542 MPa, an elongation of 8.2-14.5%, an impact energy of 35-58 J at -20℃, and a Brinell hardness of 492-520 HBW.
Citation Information
Patent Citations
30MnB steel plate for alloy structure and production method thereof
CN109852882A