Seamless pipeline pipes with yield strength of 360~485MPa for use in oil and gas fields containing CO2 and microbial corrosion, and their preparation methods
By using a low Cu + medium Cr alloying design and a tempering heat treatment process, a tempered bainite + ferrite microstructure is formed, which solves the problems of strength, toughness and resistance to HIC/SSC in CO2 and microbial corrosion environments, and realizes the preparation of high-performance seamless pipelines.
Patent Information
- Application Number
- CN202611427780.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies for manufacturing seamless pipelines for oil and gas fields containing CO2 and microbial corrosion have problems such as high Cu design leading to deterioration of hot working performance, high hardness of weld heat-affected zone, and lack of integrated solution for seamless pipeline composition design and process. In particular, it is difficult to balance resistance to microbial corrosion and resistance to HIC/SSC at steel grades of 360~485MPa.
A low-Cu + medium-Cr synergistic alloying design, combined with a tempering heat treatment process, forms a tempered bainite + ferrite dual-phase microstructure. A composite protective film is formed on the surface of the steel pipe by Cu, Ni, Mo, and As. Mo and Cr are synergistically enriched in the corrosion product film. C, V, and Nb are precipitated and strengthened during the tempering process, achieving a comprehensive match of strength, toughness, and resistance to HIC/SSC.
In CO2- and microbial corrosive environments, seamless pipeline pipes achieve high strength, toughness, and corrosion resistance, as well as unified HIC/SSC resistance, meeting high-pressure transmission requirements while ensuring dimensional accuracy and weldability.
Smart Images

Figure CN123063683A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of green and low-carbon product and seamless pipe preparation technology, and particularly relates to a seamless pipeline pipe with a yield strength of 360~485MPa for use in oil and gas fields containing CO2 and microbial corrosion, and its preparation method. Background Technology
[0002] Microbial corrosion is one of the main failure modes of oil and gas pipelines. A typical microbial group is sulfate-reducing bacteria (SRB), whose metabolic activity produces hydrogen sulfide (H2S), which can trigger hydrogen-induced cracking (HIC) and stress corrosion cracking (SSC). The main failure characteristic is perforation caused by localized pitting corrosion. Statistics show that approximately 15%–30% of pipeline steel corrosion is related to microbial corrosion. With the continuous development of shale gas and high-CO2 oil and gas fields, the corrosive environment where CO2 and SRB coexist is increasing, and there is a synergistic effect between the two. Furthermore, high Cl... - The presence of this substance makes the corrosion mechanism more complex, and the conventional carbon steel plus bactericide protection mode is no longer effective in preventing puncture accidents.
[0003] For the development of pipeline steel resistant to microbial corrosion, existing technologies mainly focus on optimizing chemical composition. Chinese patent CN106337104B, among others, employs a high Cu (≥1.0%) alloying route, utilizing Cu's contact sterilization mechanism to inhibit SRB biofilm growth. However, increasing Cu content significantly reduces the hot working performance of seamless pipes, leading to rolling defects such as cracks, scale, and outward folds, increasing production difficulty and cost. Chinese patent CN115558856B uses a high Cr (3.5%~5.5%) alloying route, improving corrosion resistance through the synergistic effect of low C, low Mn, Cr, and Cu. However, this scheme has a high Cr content (up to 5.5%), and studies have shown that 5% Cr steel has a high hardness in the weld heat-affected zone, which is detrimental to the long-term safe service of pipeline ring welded joints. Furthermore, this patent is used for preparing steel plate / welded pipe products and does not involve the production process of seamless pipeline pipes. For medium-to-high grade pipeline steels with yield strengths of 360-485 MPa, tempering is required to obtain a tempered bainitic microstructure to meet high-pressure transportation requirements. However, the high Cr and high Mo design leads to increased brittleness of quenched martensite, and H2S generated by SRB metabolism further exacerbates the risk of hydrogen-induced cracking (HIC). Existing technologies have not yet proposed an effective solution for achieving a comprehensive balance of strength, toughness, corrosion resistance, and HIC sensitivity for this type of steel in CO2- and microbial corrosive environments.
[0004] In summary, the existing technology has at least the following technical problems: (1) Although the high Cu design can improve the resistance to microbial corrosion, it seriously deteriorates the hot working performance of seamless tubes, resulting in a high rolling defect rate and increased production costs; (2) Although a high Cr design (≥3.5%) is beneficial to the formation of a protective corrosion product film, the hardness of the weld heat-affected zone is too high, which affects the safety and service life of the ring weld joint; (3) Existing microbial corrosion resistant pipeline steels are mostly produced by “controlled rolling + controlled cooling + coiling” process to prepare steel plates / welded pipes. There is a lack of integrated solution for composition design and process for seamless pipeline pipes. In particular, there are no reports on technical solutions that take into account both microbial corrosion resistance and HIC / SSC resistance under the quenching and tempering process of 360~485MPa steel grade. Summary of the Invention
[0005] To address the problems existing in the above-mentioned technologies, this invention provides a seamless pipeline pipe with a yield strength of 360~485MPa suitable for use in oil and gas fields containing CO2 and microbial corrosion, and its preparation method. Through a low-Cu + medium-Cr synergistic alloying design, excellent resistance to SRB and CO2 corrosion is achieved while ensuring the hot working performance of the seamless pipe. Simultaneously, through a tempering heat treatment process, a tempered bainite + ferrite dual-phase microstructure is obtained, enabling medium-to-high grade pipeline pipes to withstand corrosion in environments containing SRB, CO2, H2S, and high Cl2. - A comprehensive match of strength, toughness, corrosion resistance and HIC / SSC resistance in complex corrosive environments.
[0006] The technical problem solved by this invention is achieved through the following technical solution: This invention discloses a seamless pipeline pipe with a yield strength of 360-485 MPa suitable for use in oil and gas fields containing CO2 and microbial corrosion. The chemical composition and weight percentage content of the seamless pipeline pipe are as follows: C: 0.02-0.09%, Si: 0.12-0.35%, Mn: 0.12-0.45%, Nb: 0.005-0.035%, V: 0.005-0.05%, Mo: 0.13-0.55%, Ni: 0.14%. ~0.95%, Cr: 1.50~2.80%, Cu: 0.25~0.95%, Ti: 0.005~0.020%, O≤0.0040%, N≤0.0100%, H≤0.0002%, As: 0.0030~0.0300%, Al≤0.035%; B≤0.0005%, P≤0.015%, S≤0.003%, CEpcm≤0.25%, the remainder being Fe and unavoidable inclusions.
[0007] Preferably, the chemical composition and weight percentage content of the seamless pipeline tube are as follows: C: 0.03~0.05%, Si: 0.22~0.35%, Mn: 0.24~0.45%, Nb: 0.01~0.02%, V: 0.02~0.03%, Mo: 0.23~0.50%, Ni: 0.31~0.63%, Cr: 1.57~2.11%, Cu: 0.4~0.7%, Ti: 0.005~0.020%, O≤0.0040%, N≤0.0100%, H≤0.0002%, As: 0.0039~0.0072%, Al≤0.035%; B≤0.0005%, P≤0.015%, S≤0.003%, CEpcm≤0.25%, with the remainder being Fe and unavoidable inclusions.
[0008] Preferably, the seamless pipeline has the following properties: tensile strength 460~650MPa, elongation ≥30%, transverse full-size impact energy greater than 200J at -20℃, hardness ≤250HV10, yield strength ratio ≤0.92, and ductile-brittle transition temperature ≤-60℃.
[0009] Preferably, the metallographic structure of the seamless pipeline is a bidirectional structure of tempered bainite and ferrite.
[0010] Preferably, the seamless pipeline tube undergoes a HIC test in a hydrogen sulfide saturated solution and a SSC (four-point bending) test with a load of 80% of its actual yield strength. It exhibits no cracking after 96 hours of HIC resistance and no cracking after 720 hours of SSC resistance. This is achieved when the SRB concentration is >10%. 5 The test was conducted for 720 hours in an environment with SRB concentration > 10 μL and total pressure > 6 MPa. The average corrosion rate was < 0.015 mm / a, and the maximum pitting depth was < 25 μm. 5 With a maximum CO2 partial pressure environment of 1 MPa, the average corrosion rate is <0.076 mm / a, and the maximum pitting depth is <25 μm.
[0011] The specific optimized chemical composition is explained below: C: Its content is limited to 0.02-0.09% due to considerations of weldability and corrosion resistance.
[0012] Si: Considering toughness and corrosion resistance, its content is controlled within the range of 0.12% to 0.35%.
[0013] Mn: a strength element. Considering low-temperature toughness and corrosion resistance, its content is controlled within the range of 0.12% to 0.45%.
[0014] Nitrogen (Nb): A microalloying element that refines grain size and improves corrosion resistance. Its content should be controlled within the range of 0.005% to 0.035%.
[0015] V: A microalloying element that uses precipitation strengthening to improve the strength of steel. The V content should be controlled within the range of 0.005% to 0.05%.
[0016] Ti: A microalloying element that refines grains and improves strength and surface quality. Its content is controlled between 0.005% and 0.020%. Micro-Ti treatment improves the thermoplasticity of steel pipes and ensures their surface quality by adding a small amount.
[0017] Cr: A fundamental element that enhances corrosion resistance. It is a basic alloying element that can combine with microbial biofilms to form a protective film on the surface of steel pipes, preventing further corrosion and pitting. Excessive Cr content can worsen the weldability of steel; therefore, the Cr content is controlled within the range of 1.6% to 2.80%.
[0018] Mo: An alloying element that improves strength and corrosion resistance. It should be added appropriately according to the wall thickness of the steel pipe, and its content should be controlled within the range of 0.13% to 0.55%.
[0019] Ni: An alloying element that improves strength, resistance to microbial corrosion, and low-temperature toughness. Its content should be controlled within the range of 0.14% to 0.95%.
[0020] Cu: an alloying element that improves resistance to microorganisms and affects carbon equivalent and weldability. Its content should be controlled within the range of 0.25% to 0.95%.
[0021] O: Gaseous element. Considering corrosion performance, surface quality, etc., the content should be controlled as low as possible, O≤0.0040%.
[0022] As: It belongs to the residual elements in steel. Taking advantage of its ability to inhibit bacteria, its content is controlled to a certain extent without affecting the surface quality of the billet and the rolled product. Its content is controlled within the range of 0.0030-0.0300%.
[0023] CE Pcm =C+Si / 30+(Mn+Cu+Cr) / 20+Ni / 60+Mo / 15+V / 10+5B, with overall elemental control CEpcm≤0.25%.
[0024] Al ≤ 0.035%; B ≤ 0.0005%, P ≤ 0.015%, S ≤ 0.003%. B is a residual element; considering the surface quality and weldability of the steel, its content is controlled within the range of ≤ 0.0005%. P and S are impurity elements; their content is minimized during steelmaking, and the impurity element content is controlled at P ≤ 0.015% and S ≤ 0.003%.
[0025] Another aspect of the present invention discloses a method for preparing a seamless pipeline tube with a yield strength of 360~485MPa, the steps of which are as follows: (1) The ingredients are prepared according to the chemical composition and weight percentage content, and then smelted using a short process, followed by die casting and forging to obtain a round billet; (2) The round billet is rolled by MPM continuous rolling mill, PQF continuous rolling mill or 720REM skew rolling mill, including: cold centering, walking beam ring furnace heating, billet descaling, hot centering, piercing-continuous rolling, tube removal, high pressure water descaling, hot sizing, cold straightening and flaw detection processes to obtain rolled tube; (3) The rolled tube is heat-treated by quenching and high-temperature tempering to obtain seamless pipeline tube. First, the rolled tube is heated, then quenched at high temperature. The quenched seamless pipeline tube is sent to a tempering furnace for high-temperature tempering. After tempering, the steel tube is hot-straightened at high temperature, and then air-cooled to room temperature on a cooling bed. High-pressure water descaling devices are installed at the outlet of the quenching furnace and the high-temperature tempering furnace.
[0026] Preferably, the outer diameter tolerance of the round blank is ±1.2%D, the curvature per meter should be ≤3mm / m, the total curvature should be ≤25mm, and there should be no white spots, shrinkage cavities, delamination, cracks, bubbles, or peeling defects.
[0027] Preferably, the outer diameter tolerance of the rolled tube is ≤ ±1.6mm, the wall thickness tolerance is ±11.5%t, and the out-of-roundness of the outer diameter of the tube end is ≤3mm. High dimensional accuracy ensures the dimensional stability of the steel tube during subsequent heat treatment and on-site welding.
[0028] Preferably, the heating temperature is 910~980℃, the holding time is 15~60min, the quenching temperature is 890~980℃, the cooling rate is controlled at 8~20℃ / s, the tempering temperature is 670~720℃, and the holding time is 15~60min.
[0029] Preferably, a high-pressure water descaling device is installed at the outlet of the quenching furnace and the high-temperature tempering furnace. The descaling water pressure is 14~25MPa, which effectively removes the iron oxide scale on the outer surface and improves the surface quality. During the heat treatment process, the pressure inside the furnace is controlled in a slightly positive pressure state, with a pressure of 3~5Pa.
[0030] The advantages and positive effects of this invention are: (1) In terms of composition design, the present invention takes the combination of steel pipe surface and microbial corrosion biofilm to form a composite protective film as the core, and constructs a synergistic corrosion resistant system containing Cu (0.25~0.95%), Ni (0.14~0.95%), and Mo (0.13~0.55%). At the same time, through the systematic synergistic regulation of C (0.02~0.09%), Cr (1.60~2.80%), V (0.005~0.05%), Nb (0.005~0.035%), and As (0.0030~0.0300%), the comprehensive improvement of corrosion resistance, weldability and anti-HIC / SSC performance is achieved. Among them, Cu, Ni, Mo, and As combine with the SRB biofilm on the surface of the steel pipe to form a composite protective film that inhibits biofilm growth. Mo and Cr are synergistically enriched in the corrosion product film to form a more stable composite protective film. At the same time, Mo improves hardenability and tempering stability. C provides carbon source for the dispersed precipitation of carbides during the tempering process. V(C,N) and Nb(C,N) are dispersedly precipitated during the tempering process, and the strength is supplemented by precipitation strengthening and grain refinement strengthening.
[0031] (2) The present invention adopts a tempering process of quenching + high temperature tempering, which works synergistically with the above composition design: quenching + high temperature tempering fully enhances the hardenability of Mo and the precipitation strengthening effect of C, V and Nb, resulting in tempered bainite + ferrite structure, which ensures the unity of strength, toughness and resistance to HIC / SSC.
[0032] (3) The pipeline pipe provided by this invention, with a yield strength of 360~485MPa for oil and gas fields containing CO2 and microbial corrosion, can meet the requirements of a transmission pressure range of up to 10MPa, tensile strength of 460~720MPa, elongation ≥30%, transverse full-size impact energy greater than 200J at -20℃, and hardness ≤250HV10. When the SRB concentration is >10... 5 The test was conducted for 720 hours in an environment with SRB concentration > 10 μL and total pressure > 6 MPa. The average corrosion rate was < 0.015 mm / a, and the maximum pitting depth was < 25 μm. 5 The product has a per-L capacity, increases the CO2 partial pressure environment to a maximum of 1MPa, has an average corrosion rate of <0.076mm / a, a maximum pitting depth of <25μm, and achieves high dimensional accuracy (outer diameter tolerance ≤±1.6mm, wall thickness tolerance ±11.5%t, pipe end outer diameter out-of-roundness ≤3mm), high performance stability (strength fluctuation range ≤100MPa), high toughness (ductile-brittle transition temperature ≤-60℃), high ductility (elongation ≥30% (plate)), and high resistance to SSC corrosion (80%AYS four-point bending for 720 hours without cracking). Attached Figure Description
[0033] Figure 1This is a 100X micrograph of the seamless pipeline tube of Embodiment 1 of the present invention; Figure 2 The morphology and depth of pitting corrosion on the surface of the seamless pipeline pipe of Embodiment 1 of the present invention after 100X simulation of environmental corrosion are shown.
[0034] Figure 3 This is the ductile-brittle transition curve of the seamless pipeline pipe of Embodiment 1 of the present invention. Detailed Implementation
[0035] The present invention will be further described in detail below through specific embodiments. The following embodiments are merely descriptive and not limiting, and should not be used to limit the scope of protection of the present invention.
[0036] This embodiment provides a seamless pipeline pipe with a yield strength of 360~485MPa suitable for use in oil and gas fields containing CO2 and microbial corrosion. The chemical composition and weight percentage of the seamless pipeline pipe are as follows: C: 0.02~0.09%, Si: 0.12~0.35%, Mn: 0.12~0.45%, Nb: 0.005~0.035%, V: 0.005~0.05%, Mo: 0.13~0.55%, Ni: 0.14~0. 0.95%, Cr: 1.50~2.80%, Cu: 0.25~0.95%, Ti: 0.005~0.020%, O≤0.0040%, N≤0.0100%, H≤0.0002%, As: 0.0030~0.0300%, Al≤0.035%; B≤0.0005%, P≤0.015%, S≤0.003%, CEpcm≤0.25%, the remainder being Fe and unavoidable inclusions.
[0037] Preferably, the chemical composition and weight percentage content of the seamless pipeline tube are as follows: C: 0.03~0.05%, Si: 0.22~0.35%, Mn: 0.24~0.45%, Nb: 0.01~0.02%, V: 0.02~0.03%, Mo: 0.23~0.50%, Ni: 0.31~0.63%, Cr: 1.57~2.11%, Cu: 0.4~0.7%, Ti: 0.005~0.020%, O≤0.0040%, N≤0.0100%, H≤0.0002%, As: 0.0039~0.0072%, Al≤0.035%; B≤0.0005%, P≤0.015%, S≤0.003%, CEpcm≤0.25%, with the remainder being Fe and unavoidable inclusions.
[0038] The above-mentioned method for preparing seamless pipeline tubes includes the following steps: (1) Smelting process 1) Prepare the ingredients according to the above chemical composition and weight percentage content, using high-quality scrap steel, pig iron and molten iron as raw materials, and use hot charging molten iron process; 2) The raw materials are smelted using a short-process technology, including an ultra-high power electric arc furnace (UHP-EAF), a single-cover double-station ladle refining furnace, and an AOD vacuum degassing process. Then, the raw materials are die-cast and forged to obtain round billets. The outer diameter tolerance of the round billets is guaranteed to be ±1.2%D, the curvature per meter should be ≤3mm / m, the total curvature should be ≤25mm, and there should be no defects such as white spots, shrinkage cavities, delamination, cracks, bubbles, or peeling.
[0039] (2) Rolling of qualified round billets. The rolling process includes cold centering, heating in a walking beam ring furnace, hot centering, piercing-continuous rolling (two-roll 250MPM or three-roll 258PQF, 460PQF, 508PQF continuous rolling mill), tube removal, high-pressure water descaling, hot sizing, cold straightening, and flaw detection, so as to obtain rolled tubes with outer diameter tolerance ≤ ±1.6mm, wall thickness tolerance ±11.5%t, and tube end outer diameter out-of-roundness ≤ 3mm.
[0040] (3) Rolled tubes with qualified dimensions are subjected to heat treatment. The heat treatment process adopts quenching and high-temperature tempering process, including high-temperature walking beam furnace heating, high-temperature quenching, high-pressure water descaling, high-temperature tempering, high-pressure water descaling, high-temperature hot straightening process, and air cooling of the whole tube on the cooling bed.
[0041] Heating temperature: 910~980℃, holding time: 15~60min; quenching temperature: 890~980℃, cooling rate: 8~20℃ / s. Tempering temperature: 670~720℃, holding time: 15~60min; furnace pressure: controlled at a slightly positive pressure of 3~5Pa to prevent outside air from entering the furnace. High-pressure water descaling devices are installed at the outlet of the quenching furnace and high-temperature tempering furnace, with the descaling water pressure adjusted to 14~25MPa to remove iron oxide scale from the outer surface and improve surface quality.
[0042] Examples 1-4 High-strength seamless pipeline pipes with L415QS-CM steel grade and specifications of 219.1mm×7.0mm, resistant to microbial corrosion in oil and gas fields, were manufactured according to the above method. The chemical composition is shown in Tables 1 and 2 below. The smelting process yielded a 251mm round billet, which was rolled into a specification of 219.1mm x 7.0mm using 258PQF rolling. After high-temperature quenching at 950℃ and tempering at 690℃ for 45min, the pipe was then held at that temperature.
[0043] Comparative Example 1 The only difference from Example 1 is the chemical composition and weight percentage content.
[0044] Comparative Example 2 The only difference from Example 1 is that the Cu content is 0.50%, but there is no matching Ni content. The performance is not optimized in a high carbon dioxide environment, and the surface quality of the steel pipe is defective, requiring local grinding.
[0045] Comparative Example 3 The only difference from Example 1 is that the Cr content is 1.5%. Under the formulation and process of this invention, if the Cr content is too low, the biofilm formed will have insufficient corrosion resistance and its performance will decline.
[0046] Comparative Example 4 The only difference from Example 1 is that the Cr content is 3.5%. Under the formulation and process of this invention, the Cr content is too high, the performance has not been further optimized, and the increase in Cr content increases the manufacturing cost.
[0047] Comparative Example 5 The only difference from Example 1 is the heat treatment method. Quenching at 880℃ is used, while the tempering temperature and holding time are the same. The quenching temperature is too low, resulting in a coarse microstructure, which fails to achieve grain refinement and microstructure optimization, and reduces the resistance to hydrogen embrittlement.
[0048] The dimensional accuracy of the pipes is shown in Table 3, and the mechanical properties and resistance to hydrogen sulfide corrosion are shown in Table 4. The series of impact energy curves for the seamless pipeline pipe in Example 1 are shown below. Figure 3 The ductile-brittle transition temperature is ≤-60℃. This applies when the SRB concentration is >10%. 7 The test was conducted for 720 hours in a pure bacterial environment with a density of bacteria per L and a total pressure of 6.5 MPa. The average corrosion rate and maximum pitting depth are shown in Table 5. The average corrosion rate and maximum pitting depth were also observed in a pure bacterial environment with a CO2 partial pressure of 0.8 MPa.
[0049] Table 1. Chemical composition of seamless pipeline pipes in Examples 1-4 and comparative examples.
[0050] It should be noted that the pipeline's chemical composition contains other impurity elements, as shown in Table 2: Table 2 Other elemental composition of the pipeline in this embodiment
[0051] Table 3. Dimensional tolerances of the seamless pipeline in Example 1.
[0052] Note: The measurement is taken at the end of the steel pipe.
[0053] Table 4 Mechanical properties and hydrogen sulfide corrosion resistance of seamless pipeline pipes
[0054] Note: The specimen type is a plate-shaped specimen with a width of 38.1 mm and a gauge length of 50 mm; Rt0.5: specified total elongation strength, MPa; Rm: tensile strength, MPa; A: elongation after fracture; Y / T: yield strength ratio.
[0055] Table 5. Average corrosion rate and maximum pitting depth under different environments
[0056] Note: Simulated environment (25℃; CO2 partial pressure: 0.8MPa; total pressure: 6.5MPa (N2 supplement), solution pH=7.2, SRB quantity 1.4x10 7 The test solution contained 1.662 g / L CaCl2, 0.418 g / L MgCl2·6H2O, 1.377 g / L NaHCO3, 0.044 g / L Na2SO4, and 30.966 g / L NaCl.
[0057] Figure 1 This is a 100X photograph of the microstructure of Example 1. After heat treatment, a metallographic sample was taken and the microstructure was analyzed. The photograph was taken at a magnification of 100X. As can be seen from the image, the microstructure is uniform and the grains are fine, indicating that the microstructure is relatively uniform.
[0058] Figure 2 The surface condition of the seamless pipeline in Example 1 after simulated environmental corrosion is mainly observed. The pitting pits are relatively shallow, and no large-area pitting corrosion has occurred, indicating good resistance to microbial corrosion.
[0059] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several modifications and improvements can be made without departing from the inventive concept, and these all fall within the protection scope of the present invention.
Claims
1. A seamless pipeline pipe with a yield strength of 360~485MPa suitable for use in oil and gas fields containing CO2 and microbial corrosion, characterized in that, The chemical composition and weight percentage of the seamless pipeline are as follows: C: 0.02~0.09%, Si: 0.12~0.35%, Mn: 0.12~0.45%, Nb: 0.005~0.035%, V: 0.005~0.05%, Mo: 0.13~0.55%, Ni: 0.14~0.95%, Cr: 1.50~2.80%, Cu: 0.25~0.95%, Ti: 0.005~0.020%, O≤0.0040%, N≤0.0100%, H≤0.0002%, As: 0.0030~0.0300%, Al≤0.035%; B≤0.0005%, P≤0.015%, S≤0.003%, CEpcm≤0.25%, with the remainder being Fe and unavoidable inclusions.
2. The seamless pipeline pipe according to claim 1, characterized in that, The chemical composition and weight percentage of the seamless pipeline are as follows: C: 0.03~0.05%, Si: 0.22~0.35%, Mn: 0.24~0.45%, Nb: 0.01~0.02%, V: 0.02~0.03%, Mo: 0.23~0.50%, Ni: 0.31~0.63%, Cr: 1.57~2.11%, Cu: 0.4~0.7%, Ti: 0.005~0.020%, O≤0.0040%, N≤0.0100%, H≤0.0002%, As: 0.0039~0.0072%, Al≤0.035%; B≤0.0005%, P≤0.015%, S≤0.003%, CEpcm≤0.25%, with the remainder being Fe and unavoidable inclusions.
3. The seamless pipeline pipe according to claim 1, characterized in that, The performance of the seamless pipeline is as follows: tensile strength 460~650MPa, elongation ≥30%, transverse full-size impact energy greater than 200J at -20℃, hardness ≤250HV10, yield strength ratio ≤0.92, and ductile-brittle transition temperature ≤-60℃.
4. The seamless pipeline pipe according to claim 1, characterized in that, The metallographic structure of the seamless pipeline is a bidirectional structure of tempered bainite and ferrite.
5. The method for preparing a seamless pipeline according to any one of claims 1-4, characterized in that, The steps are as follows: (1) The ingredients are prepared according to the chemical composition and weight percentage content, and then smelted using a short process, followed by die casting and forging to obtain a round billet; (2) The round billet is rolled by MPM continuous rolling mill, PQF continuous rolling mill or 720REM skew rolling mill, including: cold centering, walking beam ring furnace heating, billet descaling, hot centering, piercing-continuous rolling, tube removal, high pressure water descaling, hot sizing, cold straightening and flaw detection processes to obtain rolled tube; (3) The rolled tube is heated and then quenched at high temperature. The quenched seamless pipeline is sent to a tempering furnace for high-temperature tempering. After tempering, the steel pipe is hot straightened at high temperature and then air-cooled to room temperature on a cooling bed to obtain a seamless pipeline.
6. The preparation method according to claim 5, characterized in that, The outer diameter tolerance of the round blank is ±1.2%D, the curvature per meter should be ≤3mm / m, and the total curvature should be ≤25mm.
7. The preparation method according to claim 5, characterized in that, The outer diameter tolerance of the rolled tube is ≤ ±1.6 mm, the wall thickness tolerance is ±11.5%t, and the out-of-roundness of the outer diameter of the tube end is ≤ 3 mm.
8. The preparation method according to claim 5, characterized in that, Heating temperature: 910~980℃, quenching temperature: 890~980℃, cooling rate: 8~20℃ / s, tempering temperature: 670~720℃.
9. The preparation method according to claim 5, characterized in that, High-pressure water descaling devices are installed at the outlet of the quenching furnace and the high-temperature tempering furnace. The descaling water pressure is 14~25MPa. During the heat treatment process, the pressure inside the furnace is controlled in a slightly positive pressure state, with a pressure of 3~5Pa.
Citation Information
Patent Citations
Pipeline steel with resistance to microbial corrosion
CN106337104B
A pipeline steel resistant to microbial and carbon dioxide corrosion and its preparation method
CN115558856B