A boron nitride thin film, its preparation method and application

By using bipolar high-power pulsed magnetron sputtering technology to ignite boron targets at low temperatures, the problems of poor conductivity and low plasma ionization rate of boron targets in traditional methods are solved, and high-density and high-adhesion boron nitride films are prepared, which are suitable for electronic devices, wear-resistant protection, high-temperature insulation and aerospace fields.

CN123063733APending Publication Date: 2026-11-10GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611051791.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-15
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies make it difficult to ignite boron targets at low temperatures, resulting in poor target conductivity during the preparation of boron nitride films. An insulating layer is easily formed on the target surface, affecting discharge stability and film quality. Furthermore, traditional magnetron sputtering technology has a low plasma ionization rate, leading to insufficient film density and poor adhesion.

Method used

The technology employs bipolar high-power pulsed magnetron sputtering (BP-HiPIMS), which uses two external boron targets that act as anode and cathode to ignite the boron targets at low temperatures using a high-frequency pulsed power supply. The high plasma density and ionization rate improve the film density and adhesion, while avoiding target poisoning.

Benefits of technology

This technology enables efficient ignition of boron targets at low temperatures, significantly improving the density and adhesion of boron nitride films to the substrate, thereby enhancing the quality and application performance of the films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063733A_ABST
    Figure CN123063733A_ABST
Patent Text Reader

Abstract

This invention discloses a boron nitride thin film, its preparation method, and its applications. The preparation method of the boron nitride thin film includes the following steps: S1: substrate pretreatment; S2: using a bipolar high-power pulsed magnetron sputtering power supply connected to two boron targets, sputtering the boron targets in a nitrogen-containing discharge atmosphere, and depositing a boron nitride thin film on the substrate after the pretreatment in step S1. The bipolar high-power pulsed magnetron sputtering method used in this invention can reach the mid-frequency range. With two boron targets connected to the power supply, the boron targets can be ignited at a relatively low temperature, solving the problem in existing technologies where high temperatures are required to ignite the boron targets. Furthermore, BP-HiPIMS has extremely high plasma density and ionization rate, which can significantly improve the density of the boron nitride thin film and enhance the adhesion between the boron nitride thin film and the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor technology, and in particular to a boron nitride thin film, its preparation method, and its applications. Background Technology

[0002] Boron nitride (BN) films, as important functional materials of group III-V compounds, have shown broad application prospects in electronic devices, wear-resistant protection, high-temperature insulation, and aerospace due to their excellent mechanical properties, thermal properties, and chemical stability. Depending on their crystal structure, BN mainly includes various phases such as hexagonal boron nitride (h-BN), cubic boron nitride (c-BN), and amorphous boron nitride (a-BN). Among them, h-BN has a graphite-like layered structure, exhibiting excellent lubrication properties, high-temperature resistance, and electrical insulation characteristics, and is widely used in two-dimensional electronic devices, heat dissipation insulation layers, and high-temperature lubrication applications.

[0003] Magnetron sputtering technology has been widely used in industry due to its ability to precisely control the composition and structure of BN thin films. However, the preparation of BN thin films, especially high-quality c-BN thin films, still faces many challenges. On the one hand, h-BN is thermodynamically more stable, while the formation of c-BN requires high-energy ion bombardment to promote sputtering. 3 The formation of bond structures during conventional DC magnetron sputtering (DCMS) and RF magnetron sputtering (RFMS) deposition processes often leads to the formation of amorphous BN or h-BN structures, making it difficult to obtain high-content c-BN phases. Furthermore, the B4C targets used in conventional boron nitride film deposition introduce impurities, affecting phase purity for functional coatings used in semiconductors / optoelectronics and resulting in decreased film dielectric properties. Boron targets, on the other hand, have poor conductivity and are difficult to ignite on the target surface, requiring temperatures above 500°C for ignition. Simultaneously, reactive sputtering using boron targets easily forms an insulating BN layer, leading to "target poisoning," resulting in unstable discharge, decreased deposition rate, and film quality fluctuations. Moreover, due to the low plasma ionization rate in conventional magnetron sputtering, most deposited particles reaching the substrate surface are low-energy neutral atoms, resulting in insufficient film density, disordered crystal structure, and poor film-substrate adhesion, limiting the practical application of BN films in high-load and high-temperature environments.

[0004] In recent years, the development of High Power Impulse Magnetron Sputtering (HIPIMS) technology has provided a new research direction for the preparation of high-performance boron (BN) thin films. HIPIMS significantly increases plasma density by applying high-power pulses in an extremely short time, thereby greatly improving the ionization rate of target atoms. Compared to the less than 1% ionization rate in traditional magnetron sputtering, HIPIMS technology can increase the boron ionization rate to over 50%. Simultaneously, high-energy ion bombardment can effectively improve the interfacial bonding between the thin film and the substrate, enhancing film adhesion and wear resistance. However, due to the poor conductivity and difficulty in ignition of boron targets, HIPIMS still requires heating the boron target to over 100 degrees Celsius for successful ignition, posing a challenge to both the heating method and the instrument. Summary of the Invention

[0005] The present invention aims to at least solve one of the aforementioned technical problems existing in the prior art. Therefore, the first objective of the present invention is to provide a method for preparing a boron nitride thin film. The second objective of the present invention is to provide a boron nitride thin film prepared by this method. The third objective of the present invention is to provide applications of this boron nitride thin film.

[0006] The inventive concept of this invention addresses the problem that existing technologies require high temperatures to ignite boron targets. This invention discovers that connecting two boron targets with alternating anode and cathode to a mid-frequency power supply can successfully ignite the boron target at a lower temperature. Furthermore, the bipolar pulsed high-power magnetron sputtering (BP-HiPIMS) power supply frequency can reach the mid-frequency range, and BP-HiPIMS possesses extremely high plasma density and ionization rate. Therefore, this invention provides a method for preparing boron nitride thin films using BP-HiPIMS sputtering of boron targets. This method can ignite boron targets at lower temperatures and significantly improves the density of boron nitride thin films and enhances the adhesion between the boron nitride thin film and the substrate. This results in boron nitride thin films with excellent applications in electronic devices, wear-resistant protection, high-temperature insulation, and aerospace fields.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a method for preparing a boron nitride thin film, comprising the following steps: S1: Substrate pretreatment; S2: Two boron targets are connected to a bipolar high-power pulsed magnetron sputtering power supply. The boron targets are sputtered using the bipolar high-power pulsed magnetron sputtering power supply in a discharge atmosphere containing nitrogen. A boron nitride thin film is deposited on the substrate pretreated in step S1.

[0008] The bipolar pulsed high-power magnetron sputtering (BP-HiPIMS) employed in this invention can reach the mid-frequency range. With two boron targets connected to its power supply, it can ignite the boron targets at relatively low temperatures, solving the problem of requiring high temperatures for ignition in existing technologies. Simultaneously, BP-HiPIMS exhibits extremely high plasma density and ionization rate, significantly improving the density of boron nitride films and enhancing their adhesion to the substrate. Furthermore, under the control of the bipolar high-power pulsed magnetron sputtering power supply, the two boron targets alternately act as cathode and anode. When one target is the cathode and the other the anode, the potential is positive. At this point, the charge accumulated on the target surface is pushed away from the target surface under the influence of the positive potential, effectively avoiding the "target poisoning" problem and achieving stable film deposition.

[0009] Preferably, the substrate in step S1 is selected from one of the following: silicon substrate, sapphire substrate, diamond substrate, quartz substrate, glass substrate, nickel substrate, and cobalt substrate.

[0010] Preferably, the pretreatment method in step S1 is glow etching of the substrate under a protective atmosphere. The substrate is cleaned using glow etching.

[0011] Preferably, the protective atmosphere includes at least one of argon (Ar), helium (He), neon (Ne), and krypton (Kr).

[0012] Preferably, the glow etching pressure is 2~5 Pa; more preferably, the glow etching pressure is 2.2~4 Pa; even more preferably, the glow etching pressure is 2.4~3.5 Pa; and even more preferably, the glow etching pressure is 2.8~3.2 Pa.

[0013] Preferably, the bias voltage for glow etching is 600~1000V; more preferably, the bias voltage for glow etching is 650~950V; even more preferably, the bias voltage for glow etching is 700~900V; and even more preferably, the bias voltage for glow etching is 750~850V.

[0014] Preferably, the glow etching time is 10-20 min; more preferably, the glow etching time is 12-18 min; and even more preferably, the glow etching time is 13-17 min.

[0015] Preferably, the nitrogen-containing discharge atmosphere in step S2 is a mixture of nitrogen and an inert gas, wherein the inert gas includes at least one of He, Ne, Ar, and Kr.

[0016] Preferably, the volume ratio of nitrogen to inert gas is 1:(0.1~30); more preferably, the volume ratio of nitrogen to inert gas is any one of 1:19, 1:9, 3:17, 1:4, 1:3, 3:7, 7:13, 2:3, 9:11, 1:1, 11:9, 3:2 or any range formed by both.

[0017] Preferably, the peak current density on the surface of the boron target in step S2 is 0.1~1.0 A / cm². 2 More preferably, the peak current density on the surface of the boron target in step S2 is 0.2~0.8 A / cm². 2 Furthermore, preferably, the peak current density on the surface of the boron target in step S2 is 0.4~0.6 A / cm². 2 .

[0018] Preferably, the positive and negative pulse widths of the bipolar high-power pulsed magnetron sputtering power supply are the same in step S2.

[0019] Preferably, the positive and negative pulse widths of the bipolar high-power pulsed magnetron sputtering power supply in step S2 are 5~500 μs; more preferably, the positive and negative pulse widths of the bipolar high-power pulsed magnetron sputtering power supply in step S2 are 10~400 μs; even more preferably, the positive and negative pulse widths of the bipolar high-power pulsed magnetron sputtering power supply in step S2 are 15~300 μs; even more preferably, the positive and negative pulse widths of the bipolar high-power pulsed magnetron sputtering power supply in step S2 are 20~200 μs.

[0020] Preferably, the positive and negative pulse interval in step S2 is set to 50~2000μs; more preferably, the positive and negative pulse interval in step S2 is set to 200~1500μs; and even more preferably, the positive and negative pulse interval in step S2 is set to 800~1000μs.

[0021] Preferably, the pulse frequency of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 100~5000 Hz; more preferably, the pulse frequency of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 200~4500 Hz; even more preferably, the pulse frequency of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 500~4000 Hz. The pulse frequency of the bipolar high-power pulsed magnetron sputtering power supply is a medium frequency, avoiding the problem of decreased ionization rate caused by excessively high frequencies.

[0022] Preferably, the operating voltage of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 800-1000V; more preferably, the operating voltage of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 820-980V; and even more preferably, the operating voltage of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 850-950V.

[0023] Preferably, the power density of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 2~15 W / cm². 2 More preferably, the power density of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 3~13W / cm². 2 Furthermore, preferably, the power density of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 5~10 W / cm². 2 .

[0024] Preferably, the substrate bias voltage of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is -500~0V; more preferably, the substrate bias voltage of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is -400~0V; even more preferably, the substrate bias voltage of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is -300~0V; and even more preferably, the substrate bias voltage of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is -200~0V.

[0025] Preferably, the target-substrate distance of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 10~200 mm; more preferably, the target-substrate distance of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 15~180 mm; even more preferably, the target-substrate distance of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 20~150 mm; and even more preferably, the target-substrate distance of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 40~100 mm.

[0026] Preferably, the deposition pressure in step S2 is 0.1~5.0 Pa; more preferably, the deposition pressure in step S2 is 0.2~4.0 Pa; even more preferably, the deposition pressure in step S2 is 0.3~3.0 Pa; and even more preferably, the deposition pressure in step S2 is 0.4~2.0 Pa.

[0027] Preferably, the deposition temperature in step S2 is 20~800℃; more preferably, the deposition temperature in step S2 is 50~750℃; even more preferably, the deposition temperature in step S2 is 100~720℃; and even more preferably, the deposition temperature in step S2 is 150~700℃.

[0028] Preferably, the deposition time in step S2 is 80-200 min; more preferably, the deposition time in step S2 is 90-170 min; even more preferably, the deposition time in step S2 is 100-150 min; and even more preferably, the deposition time in step S2 is 110-130 min.

[0029] Preferably, the temperature of the boron target in step S2 is 20~100℃; more preferably, the temperature of the boron target in step S2 is 30~90℃; and even more preferably, the temperature of the boron target in step S2 is 40~80℃.

[0030] Preferably, during deposition in step S2, the pretreated substrate from step S1 is placed on a rotatable sample stage.

[0031] Preferably, the rotation speed of the sample stage is 2~20 r / min; more preferably, the rotation speed of the sample stage is 4~15 r / min.

[0032] In a second aspect, the present invention provides a boron nitride thin film prepared by the preparation method described in the first aspect.

[0033] Thirdly, the present invention provides the application of the boron nitride thin film described in the second aspect in the fields of electronic devices, wear-resistant protection, high-temperature insulation, and aerospace technology.

[0034] The beneficial effects of this invention are: (1) The bipolar pulsed high-power pulsed magnetron sputtering (BP-HiPIMS) used in this invention can reach the mid-frequency range. After connecting two boron targets to its power supply, it can ignite the boron targets at a relatively low temperature, solving the problem that the boron targets need to be ignited at high temperatures in the prior art. In addition, BP-HiPIMS has extremely high plasma density and ionization rate, which can significantly improve the density of boron nitride films and enhance the adhesion between boron nitride films and substrates.

[0035] (2) The boron nitride thin film prepared by the present invention has high density, high hardness, high elastic modulus and strong bonding ability with the substrate, and can be well applied in fields such as electronic devices, wear-resistant protection, high temperature insulation and aerospace. Attached Figure Description

[0036] Figure 1 The image shows the cross-sectional SEM morphology of the BN thin film prepared in Example 2. Figure 2 The image shows the cross-sectional SEM morphology of the BN thin film prepared in Example 4. Figure 3 The cross-sectional SEM image of the BN thin film prepared in Example 8; Figure 4The image shows the cross-sectional SEM morphology of the BN thin film prepared for Comparative Example 1. Detailed Implementation

[0037] To enable those skilled in the art to better understand this application, the present invention will be further described in detail below with reference to embodiments. However, it should be understood that the following embodiments are merely preferred embodiments of the present invention, and the scope of protection of the present invention should be determined by the scope defined in the claims.

[0038] In the description of this invention, it should be noted that unless specific conditions are specified in the examples, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0039] The boron target material used in the embodiments of the present invention has a purity of 3N.

[0040] Furthermore, to better illustrate the present invention, numerous specific details are provided in the following detailed embodiments. Those skilled in the art should understand that the present invention can be practiced without certain specific details. In some embodiments, materials, methods, and means well-known to those skilled in the art are not described in detail in order to highlight the spirit of the invention.

[0041] Unless otherwise expressly stated, throughout the specification and claims, the term "comprising" or its variations such as "including" or "comprising" shall be understood to include the stated elements or components without excluding other elements or other components.

[0042] Example 1 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (nitrogen to argon volume ratio of 1:19) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect two boron targets to the bipolar high-power pulsed magnetron sputtering power supply and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0043] Example 2 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (nitrogen to argon volume ratio of 1:9) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2 The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0044] Example 3 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (nitrogen to argon volume ratio of 3:17) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0045] Example 4 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (the volume ratio of nitrogen to argon is 1:4) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2 The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0046] Example 5 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (the volume ratio of nitrogen to argon is 1:3) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0047] Example 6 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (nitrogen to argon volume ratio of 3:7) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa; Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2 The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0048] Example 7 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (the volume ratio of nitrogen to argon is 7:13) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0049] Example 8 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (nitrogen to argon volume ratio of 2:3) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2 The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0050] Example 9 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (the volume ratio of nitrogen to argon is 9:11) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0051] Example 10 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (nitrogen to argon volume ratio of 1:1) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2 The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0052] Example 11 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (nitrogen to argon volume ratio of 11:9) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa. Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition time was 120 minutes, the deposition chamber temperature was 300℃, the target temperature was 30℃, and a boron nitride thin film was obtained after deposition.

[0053] Example 12 This embodiment provides a method for preparing a boron nitride thin film, including the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (the volume ratio of nitrogen to argon is 3:2) into the deposition chamber and control the pressure in the deposition chamber to 0.6 Pa; Step 3: Connect the bipolar high-power pulsed magnetron sputtering power supply to the two boron targets, and set the power density of the bipolar high-power pulsed magnetron sputtering power supply to 7 W / cm³. 2 The substrate bias was -100V, the target-substrate distance was 100mm, the operating voltage was 900V, the positive pulse width (discharge time) was 25μs and the charging time was 75μs in one complete pulse cycle, the negative pulse width (discharge time) was 25μs and the charging time was 75μs, and the total frequency was 5000Hz; the deposition chamber temperature was 300℃, the target temperature was 30℃, the deposition time was 120 minutes, and a boron nitride thin film was obtained after deposition.

[0054] Comparative Example 1 This comparative example provides a method for preparing a boron nitride thin film, comprising the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber, and set the rotation speed of the rotating sample stage to 5 r / min; introduce a mixture of nitrogen and argon gas (nitrogen to argon volume ratio of 1:4) into the deposition chamber, control the deposition chamber pressure to 0.6 Pa, the deposition chamber temperature to 300℃, the target temperature to 30℃, the substrate bias voltage to -100V, the target-substrate distance to 100mm, the operating voltage to 900V, and use a DC magnetron sputtering boron target (single boron target) with a DC sputtering power density of 1W / cm³. 2(The highest power density that can be achieved using DC sputtering is this), and the deposition time is 120 minutes to obtain a boron nitride film.

[0055] Comparative Example 2 This comparative example provides a method for preparing a boron nitride thin film, comprising the following steps: Step 1: In a pure Ar atmosphere, place the silicon substrate in the deposition chamber, control the deposition chamber pressure to 3.0 Pa, the bias voltage to -800 V, and perform glow discharge etching on the silicon substrate for 15 minutes. Step 2: Place the pretreated silicon substrate on the rotating sample stage in the deposition chamber, setting the stage speed to 5 r / min; introduce a mixture of nitrogen and argon (nitrogen to argon volume ratio 1:4) into the deposition chamber, controlling the chamber pressure to 0.6 Pa, chamber temperature to 300 °C, target temperature to 30 °C, substrate bias to -100 V, target-substrate distance to 100 mm, and operating voltage to 900 V. Use a mid-frequency magnetron sputtering boron target (dual boron targets with alternating anode and cathode, frequency 5 kHz) at a sputtering power density of 7 W / cm². 2 The deposition time was 120 minutes, and a boron nitride thin film was obtained.

[0056] Morphological characteristics The cross-sections of the BN thin films in Examples 1-12 and Comparative Example 1 were characterized using field emission scanning electron microscopy. Examples 1-12 have similar morphology and film thickness; Examples 2, 4, and 8 are used as examples in this invention. The characterization results are as follows: Figures 1-4 As shown.

[0057] Figure 1 This is a SEM image of the cross-section of the BN thin film prepared in Example 2. Figure 2 This is a SEM image of the cross-section of the BN thin film prepared in Example 4. Figure 3 This is a SEM image of the cross-section of the BN thin film prepared in Example 8. Figure 4 The image shows the cross-sectional SEM morphology of the BN thin film prepared for Comparative Example 1.

[0058] contrast Figures 1-4 It can be seen that the BN film thickness of Comparative Example 1, prepared by DC magnetron sputtering, is approximately 40 nm. This is due to the low deposition rate of DC magnetron sputtering, resulting in insufficient film density. In contrast, the BN films prepared by bipolar high-power pulsed magnetron sputtering in Examples 2, 4, and 8 are approximately 900 nm thick. These examples demonstrate high deposition rates and high cross-sectional density of the prepared BN films. Furthermore, due to the insulating properties of pure boron targets, the power density of DC magnetron sputtering can only reach 1 W / cm². 2Traditional methods improve the conductivity of pure boron by increasing the target temperature, thereby increasing the target power density. This invention employs bipolar high-power pulsed magnetron sputtering, where the two targets act as anode and cathode, neutralizing the positive charge accumulated on the target surface and lowering the ignition voltage threshold, thus achieving low-temperature ignition. Therefore, this invention can increase the target power density to 7 W / cm² even without heating the target. 2 This enables the low-temperature ignition of pure boron targets.

[0059] Performance Characterization This invention utilizes an AntonPaar TTX-NHT2 nanoindenter to test the mechanical properties of boron nanofiber (BN) films. This device is equipped with a high-sensitivity sensor with a displacement resolution of approximately 0.1-0.2 nm and a load resolution of approximately 0.5-2 mN. A Berkovich diamond indenter was used in the test. The load-displacement curves during the indentation process were recorded, and the hardness and elastic modulus of the BN film were calculated using the Oliver-Pharr method. An appropriate maximum load was selected based on the BN film thickness to avoid significant influence of matrix effects on the results. Both the loading and unloading rates were set to 5.0 mN / min, and the maximum load was maintained for 10 seconds. To improve data reliability, each sample was tested nine times at different locations, and the average results were analyzed.

[0060] This invention employs a scratch test to assess the adhesion between a BN film and its substrate. The specific process involves applying a positive load and then tracing the surface of the BN film with a scratching needle until the film is penetrated. During this process, changes in acoustic emission signals are observed in real-time using an optical microscope to determine the critical load value Lc at which the BN film is penetrated. The scratch test is categorized into Lc1 (critical load for cracking) and Lc2 (critical load for localized peeling). In this invention, the critical load (Lc2) corresponding to the first peeling point (critical load for localized peeling) between the BN film and the substrate is used as the adhesion strength of the BN film. To ensure data accuracy and reliability, five tests are performed on each sample, and the average of these five test results is taken as the final data characterizing the adhesion strength between the BN film and the substrate. The testing instrument used in this experiment is an Anton Paar RST3. The hardness, elastic modulus, adhesion strength Lc1, and adhesion strength Lc2 of the BN films from Comparative Examples 1-2 and Examples 2, 4, and 8 are tested respectively. The test results are shown in Table 1.

[0061] Table 1. Performance data of BN thin films in Comparative Examples 1-2 and Examples 2, 4, and 8

[0062] As shown in Table 1, the hardness, elastic modulus, adhesion force Lc1, and adhesion force Lc2 of the BN films in Examples 2, 4, and 8 are all higher than those in Comparative Examples 1 and 2. This is because, compared with DC magnetron sputtering (Comparative Example 1), Examples 2, 4, and 8 have higher target power densities and use bipolar high-power pulsed magnetron sputtering power supplies (BP-HiPIMS) with higher ionization rates. Therefore, the density and uniformity of the prepared BN films are much better than those prepared by DC magnetron sputtering. Compared with conventional medium-frequency magnetron sputtering (Comparative Example 2), although Comparative Example 2 can achieve lower temperature ignition of the boron target, the boron nitride films prepared in Examples 2, 4, and 8 have higher hardness and elastic modulus, and better adhesion between the boron nitride films and the substrate, due to the extremely high plasma density and ionization rate of BP-HiPIMS.

[0063] In summary, the bipolar pulsed high-power pulsed magnetron sputtering (BP-HiPIMS) employed in this invention can reach the mid-frequency range. With two external boron targets connected to its power supply, it can ignite the boron targets at relatively low temperatures, solving the problem in existing technologies where high temperatures are required for target ignition. Compared to DC magnetron sputtering and conventional mid-frequency magnetron sputtering, BP-HiPIMS exhibits extremely high plasma density and ionization rate, which can significantly improve the density of boron nitride films and enhance the adhesion between the boron nitride film and the substrate.

[0064] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A method for preparing a boron nitride thin film, characterized in that, Includes the following steps: S1: Substrate pretreatment; S2: Two boron targets are connected to a bipolar high-power pulsed magnetron sputtering power supply. The boron targets are sputtered using the bipolar high-power pulsed magnetron sputtering power supply in a discharge atmosphere containing nitrogen. A boron nitride thin film is deposited on the substrate pretreated in step S1.

2. The method for preparing boron nitride thin films according to claim 1, characterized in that, The substrate in step S1 is selected from one of the following: silicon substrate, sapphire substrate, diamond substrate, quartz substrate, glass substrate, nickel substrate, and cobalt substrate.

3. The method for preparing boron nitride thin films according to claim 1, characterized in that, The pretreatment method described in step S1 is to perform glow etching on the substrate under a protective atmosphere.

4. The method for preparing boron nitride thin films according to claim 1, characterized in that, The nitrogen-containing discharge atmosphere mentioned in step S2 is a mixed atmosphere of nitrogen and an inert gas, wherein the inert gas includes at least one of He, Ne, Ar, and Kr.

5. The method for preparing boron nitride thin films according to claim 1, characterized in that, The peak current density on the surface of the boron target in step S2 is 0.1~1.0 A / cm². 2 .

6. The method for preparing boron nitride thin film according to claim 1, characterized in that, In step S2, the positive and negative pulse widths of the bipolar high-power pulsed magnetron sputtering power supply are 5~500 μs; And / or, in step S2, the pulse frequency of the bipolar high-power pulsed magnetron sputtering power supply is 100~5000 Hz; And / or, the operating voltage of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 800~1000V; And / or, the power density of the bipolar high-power pulsed magnetron sputtering power supply in step S2 is 2~15W / cm². 2 ; And / or, in step S2, the substrate bias voltage of the bipolar high-power pulsed magnetron sputtering power supply is -500~0V; And / or, in step S2, the target-substrate distance of the bipolar high-power pulsed magnetron sputtering power supply is 10~200 mm.

7. The method for preparing boron nitride thin films according to claim 1, characterized in that, The deposition pressure in step S2 is 0.1~5.0 Pa; And / or, the deposition temperature in step S2 is 20~800℃; And / or, the deposition time in step S2 is 80~200 min.

8. The method for preparing boron nitride thin films according to claim 1, characterized in that, In step S2, the temperature of the boron target is 20~100℃.

9. A boron nitride thin film, characterized in that, The boron nitride thin film was prepared using the method described in any one of claims 1 to 8.

10. The method for preparing the boron nitride thin film according to any one of claims 1 to 8, or the application of the boron nitride thin film according to claim 9 in the fields of electronic devices, wear-resistant protection, high-temperature insulation, and aerospace technology.