A titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating and its preparation method
By using a dual-layer structure design of titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coatings, the problems of insufficient titanium anode adhesion, short lifespan and high cost of tin-antimony oxide coatings are solved, achieving a balance between high oxygen evolution potential, long lifespan and economy.
Patent Information
- Application Number
- CN202611574926.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-10
AI Technical Summary
Existing tin-antimony oxide coated titanium anodes have shortcomings in terms of adhesion, service life and cost. The coating is prone to cracking and peeling, the interfacial resistance increases, and the excessive use of precious metals leads to high costs, making it difficult to balance stability and economy.
A titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating is adopted. Through the double-layer structure design of the ruthenium-iridium-titanium oxide intermediate layer and the tin-antimony-tantalum oxide surface layer, combined with optimized component ratio, stepped drying and temperature-controlled calcination and in-situ annealing process, a gradient transition of thermal expansion coefficient, enhanced interface bonding, electrolyte penetration barrier and precious metal component shielding protection are formed.
It improves the adhesion of the coating and the service life of the electrode, maintains a high oxygen evolution potential, controls the amount of precious metals used, solves the problem of balancing stability and economy, extends the operational stability of the electrode and reduces costs.
Smart Images

Figure CN123063751A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite oxide coating technology on metal substrate surfaces, and particularly to a titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating and its preparation method. Background Technology
[0002] Titanium-based metal oxide coated anodes have been applied in chlor-alkali industries, electroplating, hydrometallurgy, and wastewater treatment due to their dimensional stability, strong corrosion resistance, and low overpotential. Among them, tin-antimony oxide coated titanium anodes have attracted attention in advanced oxidation processes due to their high oxygen evolution potential and strong oxidation ability against organic pollutants. However, in practical use, these anodes have revealed problems such as insufficient adhesion between the coating and the titanium substrate, easy cracking and peeling of the coating, and easy passivation of the titanium substrate.
[0003] The tin-antimony oxide coating has a different coefficient of thermal expansion than the titanium substrate. During electrolysis, the coating is prone to microcracks and gradual peeling due to bubble erosion and thermal cycling stress. The electrolyte and oxygen atoms penetrate along these microcracks to the titanium substrate surface, causing the formation of a non-conductive titanium dioxide passivation film at high potential. This leads to increased interfacial resistance, a continuous rise in tank voltage, and a significantly shortened anode lifespan. Furthermore, improving the conductivity and stability of the tin-antimony oxide coating typically requires the introduction of precious metal components or an increase in the amount of precious metals used, which significantly increases the anode manufacturing cost, making it difficult to balance stability and economic efficiency.
[0004] Therefore, existing tin-antimony oxide-coated titanium anodes still have significant shortcomings in terms of adhesion, service life, and cost. It is necessary to provide a composite oxide-coated titanium anode and its preparation method that has a strong bond with the titanium substrate, strong resistance to passivation, long service life, and controllable cost. Summary of the Invention
[0005] The main objective of this invention is to provide a titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating and its preparation method. The coating, by bonding firmly with the titanium substrate, can effectively suppress microcracks and electrolyte penetration, has strong resistance to substrate passivation, and improves the service life of the electrode.
[0006] To achieve the above objectives, the present invention provides a method for preparing a titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating, comprising the following steps: The titanium substrate was subjected to alkaline washing to remove oil, sandblasting to roughen it, and oxalic acid etching in sequence. It was then rinsed with deionized water until neutral, dehydrated with anhydrous ethanol, and dried. The pretreated titanium substrate was then coated. A precursor solution containing ruthenium, iridium and titanium ions was prepared. The molar ratio of ruthenium, iridium and titanium in the precursor solution, based on oxides, was 15:35:50 for ruthenium oxide, iridium oxide and titanium oxide. The precursor solution was coated on the surface of the pretreated titanium substrate. The coating, drying and calcination operations were repeated until a ruthenium-iridium titanium oxide intermediate layer with a thickness of 2-5 μm was formed. Then, the substrate was annealed at 500℃ for 1-2 h. A precursor solution containing tin, antimony, and tantalum ions was prepared. The molar ratio of tin, antimony, and tantalum in the precursor solution, calculated as oxides, was 25:1.2:4.5. The precursor solution was coated onto the surface of the ruthenium-iridium titanium oxide intermediate layer. The titanium substrate coated with the tin-antimony-tantalum precursor solution was kept at 50°C to allow the solvent in the coating to evaporate slowly and uniformly. The temperature was then increased to 100–120°C and kept at that temperature to form a uniform dry film. The dried titanium substrate was transferred to a muffle furnace and heated to 500–520°C at a rate of 5–10°C / min for calcination to form oxides. The process of coating with the tin-antimony-tantalum precursor solution, step drying, and calcination was repeated until the tin-antimony-tantalum oxide surface layer reached the target thickness. After the final calcination, the furnace temperature was maintained at 500–520°C for an extended holding period, and the substrate was cooled to room temperature with the furnace to obtain a titanium-based ruthenium-iridium titanium and tin-antimony-tantalum composite oxide coating.
[0007] Furthermore, the step of repeatedly coating the ruthenium-iridium titanium oxide intermediate layer after drying and calcination to form a thickness of 2-5 μm, followed by annealing, includes: The titanium substrate coated with the precursor solution was dried in an oven at 100-120°C to remove the solvent from the coating. After drying, the titanium matrix is transferred into a muffle furnace and calcined at 500°C to allow the precursor to thermally decompose and form oxides. Repeat the process of coating the precursor solution, drying, and calcining until the thickness of the ruthenium-iridium titanium oxide intermediate layer on the surface of the titanium substrate reaches 2-5 μm; After the final calcination, maintain the temperature inside the muffle furnace at 500℃ for an extended holding period, and then cool the furnace to room temperature.
[0008] Furthermore, the repeated coating of precursor solution, drying, and calcination operations are performed 8 to 12 times, with each drying time being 20 minutes and each calcination time being 15 minutes.
[0009] Furthermore, in the step drying process, the temperature is maintained at 50°C for 5 minutes, and then raised to 100-120°C and maintained for 5-10 minutes; the holding time for calcination is 12-15 minutes.
[0010] Furthermore, the process of repeatedly coating the tin-antimony-tantalum precursor solution, step drying, and calcining is repeated 5 to 9 times.
[0011] Furthermore, the steps of sequentially performing alkaline washing to remove oil, sandblasting to roughen, and oxalic acid etching on the titanium substrate, rinsing with deionized water until neutral, dehydrating with anhydrous ethanol, and drying include: The titanium matrix was immersed in a 1 mol / L sodium hydroxide solution at 90°C for 1 hour, and then rinsed with deionized water. Using 80-120 mesh white corundum sand, under a compressed air pressure of 0.4-0.6 MPa, the nozzle is 100-150 mm away from the titanium substrate to blast the surface of the titanium substrate until the surface roughness Ra is 3.0-5.0 μm; The sandblasted titanium substrate was immersed in a 10%–18% oxalic acid solution and boiled at a constant temperature of 55–65°C for 2 hours. After being removed, it was rinsed with deionized water until neutral, dehydrated with anhydrous ethanol, and dried in an oven at 60°C. The pretreated titanium substrate is coated with the precursor solution within 4 hours.
[0012] Furthermore, the precursor solutions containing ruthenium ions, iridium ions, and titanium ions, and the precursor solutions containing tin ions, antimony ions, and tantalum ions, are all prepared using a mixed solvent consisting of isopropanol and concentrated hydrochloric acid at a volume ratio of 9:1.
[0013] Furthermore, the total metal ion concentration in the precursor solution containing ruthenium ions, iridium ions, and titanium ions is 0.1–0.2 mol / L, and the total metal ion concentration in the precursor solution containing tin ions, antimony ions, and tantalum ions is 0.08–0.10 mol / L.
[0014] The present invention also provides a titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating, comprising a titanium substrate, and a ruthenium-iridium-titanium oxide intermediate layer and a tin-antimony-tantalum oxide surface layer sequentially attached to the surface of the titanium substrate; In the ruthenium-iridium titanium oxide intermediate layer, the molar ratio of ruthenium oxide, iridium oxide and titanium oxide is 15:35:50 based on oxides, and the thickness of the intermediate layer is 2-5 μm; In the tin-antimony-tantalum oxide surface layer, the molar ratio of tin oxide, antimony oxide and tantalum oxide, based on oxides, is 25:1.2:4.5.
[0015] Furthermore, the surface in contact with the titanium substrate and the ruthenium-iridium titanium oxide intermediate layer is a surface that has been roughened by sandblasting and etched with oxalic acid, and the roughness Ra of the surface after sandblasting and etching is 3.0 to 5.0 μm.
[0016] The method for preparing a titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating provided in the above embodiments has the following beneficial effects: By designing the composition ratio of the ruthenium-iridium titanium oxide interlayer, the thermal expansion coefficient of the interlayer is controlled to be highly matched with that of the titanium substrate, thus alleviating the interfacial thermal stress. Combined with the in-situ isothermal annealing process after calcination, the internal stress of the coating is eliminated, grain growth and interfacial bonding are promoted, and the risk of microcrack generation and coating peeling under thermal cycling and bubble erosion is reduced. Employing a reverse sequence structure with a noble metal active layer inside and a non-noble metal shielding layer outside, the dense tin-antimony-tantalum oxide surface layer can effectively prevent electrolyte and oxygen atoms from penetrating into the interior. Combined with a stepped drying and controlled-rate heating calcination process for the surface layer, pinhole defects in the coating are reduced, preventing electrolyte from penetrating along the defects to the titanium substrate surface and causing passivation. This stabilizes the interface resistance and cell voltage, and the electrode lifespan is improved compared to conventional single-layer tin-antimony oxide anodes. By confining the precious metals ruthenium and iridium to the inner middle layer, there is no need to add a large amount of precious metals to the surface layer. The outer tin-antimony-tantalum oxide has both high oxygen evolution potential and chemical stability. It can shield and protect the inner precious metals and reduce their dissolution and loss rate, while also ensuring the oxidation treatment capability of the anode. This improves operational stability while controlling the total amount of precious metals used and maintenance costs, solving the problem of the difficulty in balancing stability and economy in existing technologies. Attached Figure Description
[0017] Figure 1 This is a flowchart of a method for preparing a titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating provided in an embodiment of the present invention; Figure 2 This is a performance test comparison table of various comparative examples and embodiments in this invention; Figure 3 This is a SEM image of the surface morphology of Embodiment 1 in this invention; Figure 4 This is a schematic diagram of the coating layer structure in this invention; The realization of the objective, functional features and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0019] Reference Figure 1 This is a schematic flowchart of a method for preparing a titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating proposed in this invention, including the following steps: S1, the titanium substrate is subjected to alkaline washing to remove oil, sandblasting to roughen it and oxalic acid etching in sequence, rinsed with deionized water until neutral, dehydrated with anhydrous ethanol and dried, and then coated on the pretreated titanium substrate. S2. Prepare a precursor solution containing ruthenium ions, iridium ions and titanium ions. The molar ratio of ruthenium, iridium and titanium in the precursor solution is 15:35:50 based on oxides. Coat the precursor solution onto the surface of the pretreated titanium substrate. Repeat the coating, drying and calcining operations until a ruthenium-iridium titanium oxide intermediate layer with a thickness of 2-5 μm is formed. Then, perform annealing treatment by extending the holding time at 500℃ for 1-2 hours. S3. Prepare a precursor solution containing tin, antimony, and tantalum ions. The molar ratio of tin, antimony, and tantalum in the precursor solution, based on oxides, is 25:1.2:4.5 for tin oxide, antimony oxide, and tantalum oxide. Coat the surface of the ruthenium-iridium titanium oxide intermediate layer with the precursor solution. Place the titanium substrate coated with the tin-antimony-tantalum precursor solution at 50°C and keep it warm to allow the solvent in the coating to evaporate slowly and uniformly. Raise the temperature to 100-120°C and continue to keep it warm to form a uniform dry film. Transfer the dried titanium substrate into a muffle furnace and calcine it at a rate of 5-10°C / min to 500-520°C to form oxides. Repeat the coating of the tin-antimony-tantalum precursor solution, the step drying, and the calcination operation until the surface layer of the tin-antimony-tantalum oxide reaches the target thickness. After the final calcination, maintain the furnace temperature at 500-520°C for an extended holding period and cool it to room temperature with the furnace to obtain a titanium-based ruthenium-iridium titanium and tin-antimony-tantalum composite oxide coating.
[0020] As described in step S1 above, a thin oxide film will naturally form on the surface of the titanium substrate. Grease and impurities will also adhere to the substrate surface. Directly applying the precursor solution will damage the interfacial bonding state of the coating. Alkali washing is used to remove the processing oil stains remaining on the surface of the titanium substrate. The titanium substrate is immersed in a sodium hydroxide solution and the set temperature is maintained to complete the soaking. After the oil stains are fully removed, the residual alkali solution on the substrate surface is rinsed with deionized water. Sandblasting roughens the surface microstructure of the titanium substrate. Compressed air carries white corundum sand to impact the substrate surface at high speed. The sand particle size and spray pressure are controlled within a suitable range. A fixed distance is maintained between the nozzle and the workpiece. The substrate surface forms a uniform uneven morphology, and the surface roughness within the target range is obtained, increasing the actual contact area between the substrate and the coating. After sandblasting, the titanium substrate is transferred to an oxalic acid solution system. The immersion temperature and duration are controlled. The oxalic acid etches the surface of the titanium substrate, dissolving the brittle oxide layer generated during sandblasting. Microscopic interfaces are formed, creating a textured structure conducive to coating anchoring. After etching is complete, the titanium substrate is continuously rinsed until the rinsing water is neutral. Ethanol replaces the moisture remaining in the substrate pores, reducing interface defects caused by residual water film. Drying removes the ethanol components from the substrate surface. The pretreated titanium substrate needs to be coated promptly. Exposure to air will cause the titanium substrate to spontaneously form a passivating oxide film again. Exceeding the specified time interval will weaken the bonding strength between the coating and the substrate. The pretreated substrate then proceeds to the next precursor solution coating process.
[0021] As described in step S2 above, the precursor solution uses a mixture of isopropanol and concentrated hydrochloric acid (volume ratio 9:1) as the solvent. Ruthenium, iridium, and titanium sources are added to the solvent, based on oxides, to achieve a molar ratio of ruthenium oxide, iridium oxide, and titanium oxide of 15:35:50. The total metal ion concentration in the precursor solution is adjusted to 0.1~0.2 mol / L, and the solution is stirred until it is homogeneous and clear. The precursor solution is uniformly coated onto the pretreated titanium substrate surface, controlling the coating amount to prevent film dripping. After coating, the titanium substrate is placed in an oven and dried at 100~120℃ to remove the solvent components from the coating, forming a uniform dry film. The dried titanium substrate is then transferred to a muffle furnace and calcined at 500℃ to allow the metal precursor to completely decompose and transform into an oxide crystalline phase, completing the sintering and curing of the single-layer coating. Repeat the coating, drying, and calcining operations to gradually accumulate the coating thickness until the total thickness of the ruthenium-iridium titanium oxide intermediate layer reaches 2~5μm. After the final calcination, the titanium substrate is not removed from the muffle furnace. The furnace temperature is maintained at 500℃ for an extended holding time of 1~2h to complete the in-situ annealing treatment. After the holding time, the substrate is cooled to room temperature with the furnace to release the residual stress inside the coating, promote the growth of interfacial grains, and strengthen the bonding strength between the coating and the titanium substrate.
[0022] As described in step S3 above, the precursor solution uses a mixture of isopropanol and concentrated hydrochloric acid (volume ratio 9:1) as the solvent. Tin, antimony, and tantalum sources are added to the solvent based on the oxide content, resulting in a molar ratio of tin oxide, antimony oxide, and tantalum oxide of 25:1.2:4.5. The total metal ion concentration in the precursor solution is controlled to be 0.08~0.10 mol / L, and the solution is stirred until it is uniform and clear. The precursor solution is uniformly coated onto the surface of the ruthenium-iridium titanium oxide intermediate layer. The amount of coating per coat is controlled to prevent film flow. After coating, the titanium substrate is placed in an oven and kept at 50°C to allow the solvent in the coating to evaporate slowly and uniformly. The temperature is then raised to 100~120°C and kept at that temperature to completely remove any residual solvent from the coating, forming a dense dry film. The dried titanium substrate is then transferred to a muffle furnace and heated at a rate of 5~10°C / min to 500~520°C for calcination, causing the metal precursor to completely decompose and transform into an oxide crystalline phase, completing the sintering and curing of the single-layer coating. Repeated coating, step drying, and calcination operations are performed to gradually accumulate the coating thickness. The operation is repeated 5 to 9 times. After the final calcination, the titanium substrate is not removed from the muffle furnace. The furnace temperature is maintained at 500 to 520°C for extended holding to complete the in-situ annealing treatment. After the holding period, the substrate is cooled to room temperature with the furnace to release the residual stress inside the coating and improve the surface density and structural integrity.
[0023] The present invention will be specifically described below through examples and comparative examples. Example 1
[0024] This embodiment prepares a titanium-based ruthenium-iridium-titanium / tin-antimony-tantalum composite oxide coating, the layered structure of which is as follows: Figure 4As shown, it is composed of a titanium substrate, a ruthenium-iridium titanium oxide intermediate layer, and a tin-antimony-tantalum oxide surface layer stacked sequentially. The intermediate layer is located between the titanium substrate and the surface layer to match the coefficient of thermal expansion and provide conductive catalytic activity. The surface layer is located on the outermost side and has both high oxygen evolution potential and shielding protection functions.
[0025] Gr1 pure titanium sheet was selected as the titanium substrate and subjected to degreasing, sandblasting roughening, oxalic acid etching and cleaning preservation treatment in sequence.
[0026] The titanium substrate was placed in a 1 mol / L NaOH solution and immersed at 90°C for 1 hour to remove surface processing oil stains; after removal, it was rinsed with deionized water to remove residual alkali solution.
[0027] Use 80-120 mesh white corundum sand, and under a compressed air pressure of 0.4-0.6MPa, control the nozzle distance from the workpiece to 100-150mm, and spray sand evenly perpendicular to the substrate surface until the surface has a uniform silver-gray matte finish. After sandblasting, the surface roughness Ra is controlled at 3.0-5.0μm. After sandblasting, use compressed air to blow away the loose sand on the surface.
[0028] The sandblasted titanium substrate is immersed in a 10%–18% (w / w) oxalic acid solution and kept at a constant temperature of 55–65°C for 2 hours to form a uniform micro-textured structure on the titanium surface. Immediately after etching, it is rinsed with plenty of deionized water until neutral, then dehydrated with anhydrous ethanol and dried in a 60°C oven. The pretreated titanium substrate is then coated within 4 hours to prevent re-oxidation and the formation of a passivation film on the titanium surface.
[0029] According to the oxide molar ratio RuO2:IrO2:TiO2=15:35:50, RuCl3・xH2O, IrCl3・xH2O and tetrabutyl titanate were weighed out and dissolved in a mixed solvent of isopropanol and concentrated hydrochloric acid with a volume ratio of 9:1. The total metal ion concentration was adjusted to 0.1-0.2 mol / L and stirred until completely dissolved to obtain the intermediate layer precursor solution.
[0030] The precursor solution was uniformly coated onto the pretreated titanium substrate surface using a brush. The coating was applied in a thin layer in a single direction, and the amount of each coating was controlled to ensure that the wet film evenly covered the surface without dripping. After coating, the substrate was immediately placed in an oven at 100-120℃ for 20 minutes to allow the solvent to evaporate fully. After drying, the substrate was transferred to a muffle furnace and calcined at 500℃ for 15 minutes to thermally decompose the metal precursor into oxides.
[0031] Repeat the above coating, drying, and calcination steps 8 to 12 times until the total thickness of the intermediate layer reaches 2 to 5 μm. After the last calcination, without removing the titanium substrate, keep it at 500°C for 1 to 2 hours, and then cool it to room temperature in the furnace to complete the in-situ annealing treatment of the intermediate layer, eliminate the internal stress of the coating, and enhance the adhesion between the coating and the substrate.
[0032] Measure 90 mL of isopropanol and 10 mL of 37% concentrated hydrochloric acid, and mix thoroughly to obtain an isopropanol-hydrochloric acid mixed solvent with a volume ratio of 9:1. Weigh out 2.167 g of SnCl₄·5H₂O, 0.135 g of SbCl₃, and 0.797 g of TaCl₅, and add them sequentially to the mixed solvent, stirring until completely dissolved. Make up the volume to 100 mL with the mixed solvent; the total metal ion concentration in the solution is approximately 0.09 mol / L. Continue stirring for 30 min, then allow to stand to allow the metal ions to fully complex and homogenize, obtaining the surface precursor solution. The corresponding molar ratio of oxides in this precursor solution is SnO₂:Sb₂O₃:Ta₂O₅ = 25:1.2:4.5. The precursor solution was uniformly coated onto the surface of the ruthenium-iridium titanium oxide intermediate layer using a brush. Immediately after coating, a step-by-step drying process was carried out: the first stage was baking at 50°C for 5 minutes to allow the solvent to evaporate slowly and evenly, avoiding wet film flow or surface skin formation; the second stage was heating to 100-120°C and baking for 5-10 minutes to ensure that the residual solvent was completely evaporated, and the coating was transformed from a wet film to a uniform light gray dry film.
[0033] The dried titanium substrate is immediately transferred to a muffle furnace for high-temperature calcination, with the temperature increased from room temperature to 500-520°C at a rate of 5-10°C / min and held for 12-15 minutes to thermally decompose the metal chloride precursor into oxides. After the holding period, the titanium substrate is removed and allowed to cool naturally to room temperature in the air.
[0034] Repeat the above steps of coating, step drying, calcination, and air cooling 5 to 9 times; after completing the final coating and calcination, perform final annealing treatment in the furnace at 500 to 520°C, and obtain the target composite oxide coating after furnace cooling.
[0035] The surface morphology and performance of the composite oxide coating prepared in this embodiment were characterized and compared with those of other embodiments and comparative samples.
[0036] The surface microstructure of the coating in this embodiment is as follows: Figure 3 As shown, the coating surface exhibits a uniform micro-uneven morphology, with no obvious pinholes, cracks, or peeling defects, and good density; this structure can both ensure the shielding and protection of the interior by the surface layer and provide sufficient electrochemical reaction active sites.
[0037] This embodiment underwent bonding strength testing, oxygen evolution potential testing, and enhanced lifetime testing. The test results are as follows: Figure 2As shown, the adhesion test was conducted using the 180° peel-off method with 3M transparent tape. In this embodiment, the coating surface showed no peeling and the tape showed no black marks, indicating a good adhesion level. The oxygen evolution potential (OE) test was performed using a three-electrode system in a 0.5 mol / L H₂SO₄ electrolyte. In this embodiment, the OE potential was 2.01 V vs. RHE, maintaining a high OE potential and meeting the requirements of advanced oxidation treatment. The enhanced life test employed a constant current accelerated aging method, electrolyzing at a current density of 100 mA / cm². In this embodiment, the initial cell voltage was 2.98 V, and after 2 hours of operation, the cell voltage reached 3.02 V. The rate of increase in cell voltage was gradual, indicating an enhanced life of 24 hours. Example 2
[0038] This embodiment prepares a titanium-based ruthenium-iridium-titanium / tin-antimony composite oxide coating, whose layered structure is similar to... Figure 4 The three-layer stacked structure shown is identical, the only difference being that the surface layer is a tin-antimony binary oxide and no tantalum component is added. The titanium substrate pretreatment and the preparation process and parameters of the ruthenium-iridium titanium oxide intermediate layer are exactly the same as those in Example 1.
[0039] Measure 90 mL of isopropanol and 10 mL of 37% concentrated hydrochloric acid, mix them evenly to obtain an isopropanol-hydrochloric acid mixed solvent with a volume ratio of 9:1. Weigh 2.167 g of SnCl4・5H2O and 0.135 g of SbCl3, add them to the mixed solvent in sequence and stir until completely dissolved. Make up the volume to 100 mL with the mixed solvent. Continue stirring for 30 min and let stand to allow the metal ions to fully complex and become uniform, thus obtaining the tin-antimony oxide surface precursor solution.
[0040] The precursor liquid was uniformly coated onto the surface of the ruthenium-iridium titanium oxide intermediate layer using a brush. The step drying, heating and calcination, number of coating cycles and final annealing processes were the same as in Example 1, and a titanium-based ruthenium-iridium titanium / tin-antimony composite oxide coating was finally obtained.
[0041] The coating prepared in this embodiment was subjected to performance testing, and the test results are as follows: Figure 2 As shown.
[0042] The adhesion test was conducted using the same tape peeling method as in Example 1. In this example, the coating surface showed no peeling and the tape showed no black marks, indicating a good adhesion level, which was comparable to the adhesion performance of Example 1. This shows that the adjustment of the surface layer components did not affect the interfacial bonding strength between the intermediate layer and the titanium substrate.
[0043] The oxygen evolution potential (OE) test results show that the OE potential in this embodiment is 1.92 V vs. RHE, which is slightly lower than 2.02 V vs. RHE in Example 1, and can meet the potential requirements of conventional advanced oxidation treatment.
[0044] In the enhanced life test, the initial cell voltage in this embodiment was 2.75V, and the cell voltage was 2.82V after 2 hours of operation. The cell voltage rise rate was slow, and the enhanced life reached 21 hours. The results show that when the surface layer is not doped with tantalum, the coating can still have excellent structural stability and long-term service performance. The appropriate surface layer composition scheme can be selected according to the potential and life requirements of the actual working conditions.
[0045] Comparative Example 1 This comparative example is a single-layer tin-antimony oxide coated titanium anode without an intermediate layer, used to compare and verify the effect of the ruthenium-iridium titanium oxide intermediate layer on the interfacial bonding performance and service life. The pretreatment process parameters of the titanium substrate are exactly the same as those in Example 1. The difference is that the preparation process of the ruthenium-iridium titanium oxide intermediate layer is omitted, and the tin-antimony oxide surface layer is directly prepared on the surface of the pretreated titanium substrate. The composition of the surface layer precursor solution, the step drying, the calcination, the number of cyclic coatings, and the final annealing process are all consistent with those in Example 1.
[0046] The coating prepared in this comparative example was subjected to performance testing, and the test results are as follows: Figure 2 As shown.
[0047] The adhesion test results showed that the coating in this comparative example had poor adhesion, and localized peeling of the coating occurred after the tape was removed. The reason is that the thermal expansion coefficients of tin-antimony oxide and titanium substrate are significantly different, lacking the thermal expansion transition and interfacial bonding strengthening effect of the intermediate layer. During calcination and thermal cycling, the residual stress at the interface is large, making the coating prone to cracking and peeling.
[0048] The oxygen evolution potential test result was 1.85V vs. RHE, which was lower than that of Examples 1 and 2. The catalytic activity of the monolayer tin-antimony oxide was limited, and the oxidation treatment capacity under high potential conditions was insufficient.
[0049] In the enhanced life test, the initial cell voltage of this comparative example was 2.68V, and the enhanced life was only 1.6h, far lower than that of the other examples. The failure was due to poor coating adhesion, which easily led to microcracks and peeling. The electrolyte and oxygen atoms directly penetrated to the surface of the titanium substrate, rapidly forming a non-conductive titanium dioxide passivation film at a high potential. This caused a sharp increase in interface resistance and cell voltage, resulting in rapid electrode deactivation.
[0050] Comparative Example 2 In this comparative example, the pretreatment process parameters of the titanium substrate are exactly the same as those in Example 1. The layered design of the intermediate layer and the surface layer is omitted, and a single-layer coating of iridium oxide and tantalum oxide is directly prepared on the surface of the titanium substrate. The molar ratio of iridium to tantalum is 7:3 based on oxides, the total coating thickness is controlled to be 5 μm, and the coating is prepared by a conventional coating, drying, and calcination cycle process, and finally annealed.
[0051] The coating prepared in this comparative example was subjected to performance testing, and the test results are as follows: Figure 2As shown in the figure. Adhesion test results show that the coating in this comparative example has good adhesion, with no peeling after the tape is removed, indicating good interfacial bonding between the iridium tantalum oxide and the titanium substrate. The oxygen evolution potential (OE) test result is 1.48V vs. RHE, significantly lower than 2.15V in Example 1 and 1.92V in Example 2. This type of anodic OE potential is too low and cannot meet the high-potential requirements of advanced oxidation treatment. In the enhanced life test, the initial tank voltage of this comparative example was 2.30V, and after 2 hours of operation, the tank voltage was 2.33V, showing good tank voltage stability. The enhanced life reached 32.0 hours, longer than Example 1 of this invention. However, this scheme requires a large amount of the precious metal iridium, with an iridium loading of approximately 15g / m², resulting in a preparation cost approximately 35% higher than Example 1. The large amount of precious metal used and the high risk of price fluctuations present a challenge in balancing stability and economy.
[0052] Comparative Example 3 This comparative example is a titanium anode with a single-layer ruthenium-iridium titanium oxide coating. Only the ruthenium-iridium titanium oxide intermediate layer structure is retained as in Example 1; the outer tin-antimony-tantalum oxide surface layer is not prepared. This is used to compare and verify the shielding and protective effect of the tin-antimony-tantalum oxide surface layer on the internal noble metal active components, and its impact on the long-term service performance of the electrode. The titanium substrate pretreatment process, the composition of the precursor solution for the ruthenium-iridium titanium oxide coating, the coating, drying, and calcination cycle process, thickness control, and final annealing parameters are all completely consistent with the intermediate layer preparation process in Example 1.
[0053] The coating prepared in this comparative example was subjected to performance testing, and the test results are as follows: Figure 2 As shown.
[0054] The adhesion test results show that the coating in this comparative example has good adhesion, and there is no peeling after the tape is removed. The thermal expansion coefficients of the ruthenium-iridium titanium oxide and the titanium substrate are well matched, and the interfacial bonding strength is excellent.
[0055] The oxygen evolution potential test result was 1.47V vs. RHE, which was significantly lower than that of Examples 1 and 2, and slightly lower than that of Comparative Example 2. The oxygen evolution potential of the monolayer ruthenium iridium titanium oxide was too low and could not meet the high potential requirements of advanced oxidation treatment.
[0056] In the enhanced life test, the initial cell voltage of this comparative example was 2.32V, and after 2 hours of operation, it rose to 2.45V. The rate of voltage rise was significantly higher than that of the other double-layer structure examples, and the enhanced life was only 10.0 hours, far lower than the 24 hours of Example 1 and the 21 hours of Example 2. The failure was due to the lack of shielding protection from the tin-antimony-tantalum oxide surface layer. The ruthenium-iridium-titanium oxide was directly exposed to the highly oxidizing electrolyte, and the ruthenium oxide component gradually dissolved and was lost at high potential, resulting in a continuous decline in catalytic activity. At the same time, the electrolyte and oxygen atoms could more easily penetrate into the interface region, accelerating the degradation of interface performance and ultimately leading to a significant reduction in electrode life. The test results show that adding a tin-antimony-tantalum oxide surface layer on the outside of the ruthenium-iridium-titanium intermediate layer is a necessary means to improve the electrode oxygen evolution potential, inhibit the dissolution of noble metals, and extend service life.
[0057] In summary, combining Figure 2 The test results, through a horizontal comparison of various embodiments and comparative examples, show that the differences in coating structure, layer sequence arrangement and component formulation directly determine the performance differentiation of the electrode in terms of interfacial bonding force, oxygen evolution potential, service life and economy. The double-layer composite coating structure proposed in this invention systematically solves the inherent shortcomings of various existing single-layer coatings through the synergistic effect of different functional layers, and achieves a balanced improvement in multi-dimensional performance.
[0058] Regarding interfacial bonding performance, only Comparative Example 1 showed localized coating detachment, while the bonding strength of the remaining samples was good. The core reason for the difference lies in the significant difference in the coefficients of thermal expansion between tin-antimony oxide and the titanium substrate. Direct bonding results in high residual stress at the interface, which easily leads to crack initiation and peeling under thermal cycling and bubble erosion. The ruthenium-iridium titanium oxide intermediate layer introduced in this invention has a coefficient of thermal expansion between that of the titanium substrate and the tin-antimony oxide, forming a continuous gradient transition. Combined with in-situ annealing to release interfacial stress, this fundamentally strengthens the bonding strength between the coating and the substrate, avoiding the failure mode of easy detachment of single-layer tin-antimony oxide coatings.
[0059] Regarding the oxygen evolution potential (OE potential), Examples 1 and 2 showed significantly higher potentials than the three comparative examples, with Example 1, doped with tantalum, exhibiting the highest potential. Comparative Examples 2 and 3, being typical noble metal oxide coatings, generally had low OE potentials, making them unsuitable for the high-potential conditions of advanced oxidation processes. The monolayer tin-antimony oxide in Comparative Example 1 exhibited limited catalytic activity, and its potential level remained insufficient. This invention employs a reverse sequence design, placing the tin-antimony oxide with high OE potential on the outermost layer in direct contact with the electrolyte, fully leveraging its high OE potential advantage. Simultaneously, tantalum doping optimizes the surface electronic structure, further enhancing the OE potential to meet the requirements of strong oxidation processes.
[0060] In terms of service life and economy, the samples exhibited significant performance differentiation and different failure mechanisms. Comparative Example 1 had the shortest service life, with failure stemming from the lack of a barrier effect from the intermediate layer. This led to rapid propagation of microcracks in the coating, electrolyte penetration causing passivation of the titanium substrate, and a sharp increase in tank voltage. Comparative Example 3 also had a short service life, with failure due to the lack of surface shielding protection. The precious metal ruthenium oxide was directly exposed to the electrolyte, gradually dissolving and leaching at high potentials, resulting in a continuous decline in catalytic activity. Although Comparative Example 2 had the longest service life, it relied on a high amount of the precious metal iridium, resulting in a preparation cost approximately 35% higher than Example 1. This also led to high material cost and price fluctuation risks, making it difficult to balance stability and economy. The double-layer structure of this invention achieves a dual protective effect. The intermediate layer blocks electrolyte penetration into the substrate and inhibits passivation of the titanium substrate, while the surface layer shields against a strong oxidizing environment and reduces the dissolution and loss of the precious metal components. With a much lower amount of precious metal than Comparative Example 2, it achieved a service life far superior to Comparative Examples 1 and 3, while maintaining a high oxygen evolution potential. This resulted in the optimal combination of bonding performance, electrochemical performance, service life, and preparation cost.
[0061] In summary, this invention employs a double-layer composite coating structure consisting of a ruthenium-iridium titanium oxide intermediate layer and a tin-antimony-tantalum oxide surface layer, combined with optimized component ratios, step-by-step drying, segmented temperature-controlled calcination, and in-situ annealing processes. This achieves multiple synergistic effects, including gradient transition of thermal expansion coefficients, enhanced interfacial bonding, electrolyte penetration barrier, and shielding protection from noble metal components. While maintaining a high oxygen evolution potential to adapt to advanced oxidation conditions, it significantly improves coating adhesion and electrode service life, effectively controls the amount of noble metal used and preparation costs, and solves the technical problem of existing titanium-based oxide coatings that struggle to balance bonding performance, oxygen evolution potential, service life, and economy.
[0062] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, apparatus, article, or method that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, apparatus, article, or method. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, apparatus, article, or method that includes that element.
[0063] The above description is only a preferred embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A method for preparing a titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating, characterized in that, Includes the following steps: The titanium substrate was subjected to alkaline washing to remove oil, sandblasting to roughen it, and oxalic acid etching in sequence. It was then rinsed with deionized water until neutral, dehydrated with anhydrous ethanol, and dried. The pretreated titanium substrate was then coated. A precursor solution containing ruthenium, iridium and titanium ions was prepared. The molar ratio of ruthenium, iridium and titanium in the precursor solution, based on oxides, was 15:35:50 for ruthenium oxide, iridium oxide and titanium oxide. The precursor solution was coated on the surface of the pretreated titanium substrate. The coating, drying and calcination operations were repeated until a ruthenium-iridium titanium oxide intermediate layer with a thickness of 2-5 μm was formed. Then, the substrate was annealed at 500℃ for 1-2 h. A precursor solution containing tin, antimony, and tantalum ions was prepared. The molar ratio of tin, antimony, and tantalum in the precursor solution, calculated as oxides, was 25:1.2:4.
5. The precursor solution was coated onto the surface of the ruthenium-iridium titanium oxide intermediate layer. The titanium substrate coated with the tin-antimony-tantalum precursor solution was kept at 50°C to allow the solvent in the coating to evaporate slowly and uniformly. The temperature was then increased to 100–120°C and kept at that temperature to form a uniform dry film. The dried titanium substrate was transferred to a muffle furnace and heated to 500–520°C at a rate of 5–10°C / min for calcination to form oxides. The process of coating with the tin-antimony-tantalum precursor solution, step drying, and calcination was repeated until the tin-antimony-tantalum oxide surface layer reached the target thickness. After the final calcination, the furnace temperature was maintained at 500–520°C for an extended holding period, and the substrate was cooled to room temperature with the furnace to obtain a titanium-based ruthenium-iridium titanium and tin-antimony-tantalum composite oxide coating.
2. The method for preparing the titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating according to claim 1, characterized in that, The step of repeatedly coating the ruthenium-iridium titanium oxide intermediate layer after drying and calcination to form a thickness of 2-5 μm, followed by annealing, includes: The titanium substrate coated with the precursor solution was dried in an oven at 100-120°C to remove the solvent from the coating. After drying, the titanium matrix is transferred to a muffle furnace and calcined at 500°C to allow the precursor to thermally decompose and form oxides. Repeat the process of coating the precursor solution, drying, and calcining until the thickness of the ruthenium-iridium titanium oxide intermediate layer on the surface of the titanium substrate reaches 2-5 μm; After the final calcination, maintain the temperature inside the muffle furnace at 500℃ for an extended holding period, and then cool the furnace to room temperature.
3. The method for preparing the titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating according to claim 2, characterized in that, The repeated coating of precursor solution, drying, and calcination are performed 8 to 12 times, with each drying time being 20 minutes and each calcination time being 15 minutes.
4. The method for preparing the titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating according to claim 1, characterized in that, In the stepped drying process, the temperature is maintained at 50°C for 5 minutes, and then raised to 100-120°C and maintained for 5-10 minutes; the holding time for calcination is 12-15 minutes.
5. The method for preparing the titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating according to claim 1, characterized in that, The number of times the tin-antimony-tantalum precursor solution is repeatedly coated, the step drying process is repeated, and the calcination is carried out is 5 to 9.
6. The method for preparing the titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating according to claim 1, characterized in that, The steps of sequentially performing alkaline washing to remove oil, sandblasting to roughen, and oxalic acid etching on the titanium substrate, rinsing with deionized water until neutral, dehydrating with anhydrous ethanol, and drying include: The titanium matrix was immersed in a 1 mol / L sodium hydroxide solution at 90°C for 1 hour, and then rinsed with deionized water. Using 80-120 mesh white corundum sand, under a compressed air pressure of 0.4-0.6 MPa, the nozzle is 100-150 mm away from the titanium substrate to blast the surface of the titanium substrate until the surface roughness Ra is 3.0-5.0 μm; The sandblasted titanium substrate was immersed in a 10%–18% oxalic acid solution and boiled at a constant temperature of 55–65°C for 2 hours. After being removed, it was rinsed with deionized water until neutral, dehydrated with anhydrous ethanol, and dried in an oven at 60°C. The pretreated titanium substrate is coated with the precursor solution within 4 hours.
7. The method for preparing the titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating according to claim 1, characterized in that, The precursor solutions containing ruthenium, iridium, and titanium ions, and the precursor solutions containing tin, antimony, and tantalum ions, are all prepared using a mixed solvent consisting of isopropanol and concentrated hydrochloric acid at a volume ratio of 9:
1.
8. The method for preparing the titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating according to claim 1, characterized in that, The total metal ion concentration in the precursor solution containing ruthenium, iridium and titanium ions is 0.1-0.2 mol / L, and the total metal ion concentration in the precursor solution containing tin, antimony and tantalum ions is 0.08-0.10 mol / L.
9. A titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating, characterized in that, It includes a titanium substrate, and a ruthenium-iridium titanium oxide intermediate layer and a tin-antimony-tantalum oxide surface layer sequentially attached to the surface of the titanium substrate; In the ruthenium-iridium titanium oxide intermediate layer, the molar ratio of ruthenium oxide, iridium oxide and titanium oxide is 15:35:50 based on oxides, and the thickness of the intermediate layer is 2-5 μm; In the tin-antimony-tantalum oxide surface layer, the molar ratio of tin oxide, antimony oxide and tantalum oxide, based on oxides, is 25:1.2:4.
5.
10. The titanium-based ruthenium-iridium-titanium and tin-antimony-tantalum composite oxide coating according to claim 9, characterized in that, The surface in contact with the titanium substrate and the ruthenium-iridium titanium oxide intermediate layer is a surface that has been roughened by sandblasting and etched with oxalic acid, and the roughness Ra of the surface after sandblasting and etching is 3.0 to 5.0 μm.