A high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber and its preparation method
By combining components A and B in a parallel composite structure and through the synergistic effect of specific additives, the rheological differences of composite fibers with high content of flame retardant and wear-resistant powder fillers are solved, thereby improving the high wear-resistant, flame-retardant and tear-resistant properties and forming a three-dimensional crimped structure.
Patent Information
- Application Number
- CN202611436897.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-10
AI Technical Summary
In the prior art, when high-content flame-retardant and wear-resistant powder fillers are introduced into composite fibers, the difference in the rheological behavior of the two-phase melt increases, leading to distortion of the spinning cross section and a decrease in interfacial bonding force, which in turn reduces the tear resistance of the fiber.
The compound employs a parallel composite structure of components A and B. Component A contains polyethylene terephthalate, cellulose acetate butyrate, and polycarbodiimide, while component B contains polyethylene terephthalate, aluminum diethylphosphinate, and polytetrafluoroethylene micropowder. The synergistic effect of polycarbodiimide and pentaerythritol stearate controls the difference in melt viscosity. Pentaerythritol stearate is added to component B for lubrication. Combined with an independent twin-screw extrusion system and side-feeding process, the mixing and thermal processing time of each component are controlled separately.
It achieves stability and tear resistance in the cross-sectional shape of composite fibers, improves the interfacial bonding strength and tear resistance of fibers, and forms a three-dimensional crimped structure, which improves the flame retardancy and wear resistance of fibers.
Smart Images

Figure CN123063891A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical fiber technology, specifically to a high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber and its preparation method. Background Technology
[0002] Side-by-side composite polyester fibers are widely used in the textile industry. With the expansion of application scenarios, the market has placed higher demands on fibers to possess comprehensive properties such as flame retardancy, abrasion resistance, and a stable three-dimensional crimp structure. To achieve these functions, flame retardants and abrasion-resistant micropowders are typically added to the polyester matrix, and composite spinning is carried out using polymer materials with different shrinkage characteristics.
[0003] However, when a large amount of solid powder filler is introduced into one component of the parallel composite fiber, the flow resistance of that component increases significantly, leading to a substantial increase in its melt viscosity. Simultaneously, the polyester component on the other side is prone to thermal degradation during high-temperature melt extrusion, resulting in a decrease in melt viscosity. This phenomenon causes a sharp increase in the rheological difference between the two melt phases during extrusion. Excessive viscosity difference leads to inconsistent flow velocities of the two melt phases within the spinning assembly, easily causing shear slip at the bicomponent interface and resulting in distortion of the spinning cross-section. This cross-sectional distortion disrupts the symmetry of the composite fiber structure, weakens the bonding strength between the bicomponent interfaces, and makes the fiber susceptible to interfacial splitting and peeling under external loads, significantly reducing the overall tear resistance of the composite fiber.
[0004] On the other hand, in the conventional blending spinning process of composite fibers, polyester chips and powdered additives are usually mixed and fed into the extruder's main feed port in one go. This processing method leads to a large amount of inorganic solid powder interacting violently with the unmelted rigid polyester chips in the extruder's conveying section, increasing equipment wear and affecting the stability of material transport. Simultaneously, various functional additives are added along with the main material, subjecting them to a long high-temperature and high-shear zone at the front of the extruder. For chemically reactive additives, premature entry into the high-temperature zone can easily lead to thermal deactivation, making it difficult to ensure the effectiveness of their in-situ reaction in the polyester melt, thus affecting the stability of the multiphase melt extrusion process. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a high-wear-resistant, flame-retardant, and tear-resistant polyester composite fiber and its preparation method. This solves the problem that when conventional parallel composite fibers are introduced with high content of flame-retardant and wear-resistant powder fillers, the increased difference in the rheological behavior of the two-phase melt leads to distortion of the spinning cross section and a decrease in interfacial bonding force, which in turn reduces the tear resistance of the fiber.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] In a first aspect, the present invention provides a highly abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber, employing the following technical solution:
[0008] A high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber includes a component A and a component B compounded in parallel, wherein the volume ratio of the component A to the component B is 40:60 to 50:50, and the high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber is made by melt spinning the component A and the component B.
[0009] The raw materials of component A, by mass parts, include:
[0010] 91-94 parts of polyethylene terephthalate, 5-8 parts of cellulose acetate butyrate, and 0.8-1.3 parts of polycarbodiimide;
[0011] The raw materials of component B, by mass parts, include:
[0012] The mixture comprises 87-90 parts of polyethylene terephthalate, 8.5-11 parts of aluminum diethylphosphinate, 1.5-2.5 parts of polytetrafluoroethylene micro powder, and 0.7-1.2 parts of pentaerythritol stearate.
[0013] The mixture of polycarbodiimide and pentaerythritol stearate synergistically reduces the melt viscosity difference between component A and component B, thereby improving the tear resistance of the high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber.
[0014] By employing the above technical solution, the rheological behavior of the polyethylene terephthalate matrix in a multiphase system is controlled through a synergistic mechanism of chemical end-capping and physical lubrication by using a mixture of polycarbodiimide and pentaerythritol stearate on components A and B respectively. This results in a stable cross-sectional shape and tear resistance. Polyethylene terephthalate is prone to degradation in the high-temperature molten state, leading to a decrease in viscosity.
[0015] This scheme adds polycarbodiimide to component A, utilizing the addition reaction between the carbodiimide groups and the terminal carboxyl groups of the polyester to generate a stable acylurea structure. This consumes the terminal carboxyl groups, inhibiting the thermal oxidative degradation of the polyester and thus maintaining the apparent viscosity of the component A melt under high shear conditions. On the other hand, aluminum diethylphosphinic acid and polytetrafluoroethylene micropowder solid fillers are added to component B. The addition of solid particles usually hinders polymer flow, leading to an increase in viscosity.
[0016] To address this, a pentaerythritol stearate mixture is introduced as a lubricant, which interpenetrates between the polyester and the solid filler, reducing interparticle friction and suppressing excessive increase in the apparent viscosity of component B. By maintaining the viscosity of component A and suppressing the increase in the viscosity of component B, the viscosity difference between the two-phase melts within the spinning assembly can be reduced, making the flow velocities of the two components similar and preventing shear slip and cross-sectional distortion at the composite interface. This symmetrical and stable cross-sectional structure reduces stress concentration under external forces, improving the overall physical bonding strength and tear resistance of the composite fiber.
[0017] In addition, the thermal decomposition of aluminum diethylphosphinic acid promotes the carbonization of the matrix to form a heat insulation layer; polytetrafluoroethylene micro powder provides a low-friction transfer layer when the fiber surface is rubbed; cellulose acetate butyrate imparts high thermal shrinkage properties to component A, and promotes the formation of a three-dimensional crimped structure in the fiber during subsequent processing.
[0018] Preferably, the intrinsic viscosity of the polyethylene terephthalate is 0.68–0.72 dL / g, and the terminal carboxyl group content of the polyethylene terephthalate is 25–35 mol / t; the butyryl group mass fraction of the cellulose acetate butyrate is 35%–39%, the acetyl group mass fraction is 13%–15%, the free hydroxyl group mass fraction is 1.0%–2.0%, and the glass transition temperature of the cellulose acetate butyrate is 125–135 °C.
[0019] By adopting the above technical solution and setting the intrinsic viscosity and end-carboxyl group content of polyethylene terephthalate, the main purpose is to ensure that the end-carboxyl group and polycarbodiimide capping reaction can reach the required conversion degree within a limited extrusion time. The functional group composition of cellulose acetate butyrate directly affects its thermophysical properties. Controlling its glass transition temperature at 125–135°C allows for significant axial shrinkage during subsequent heat treatment. This shrinkage deformation is blocked by the rigid particles within component B, thus creating a shrinkage stress difference within the fiber, driving controlled crimping deformation.
[0020] Preferably, the aluminum diethylphosphonate has a decomposition temperature of 5% thermal weight loss greater than 300°C, and its primary particle size D50 is 0.8–1.5 μm; the polytetrafluoroethylene (PTFE) micropowder has a weight-average molecular weight of 10,000–100,000 g / mol, and its particle size distribution D50 is 1–3 μm; the polycarbodiimide has a weight-average molecular weight of 3,000–10,000 g / mol; the pentaerythritol stearate mixture is mainly composed of pentaerythritol monostearate, and the hydroxyl value of the pentaerythritol stearate mixture is 200–250 mg KOH / g.
[0021] By adopting the above technical solution, the decomposition temperature of aluminum diethylphosphinate is required to be higher than 300℃ to match the spinning temperature of polyethylene terephthalate, prevent the generation of bubbles during processing, and its particle size range also helps to reduce the probability of filter clogging. The weight-average molecular weight range of polycarbodiimide ensures that it has suitable flowability and dispersibility in the polymer melt, facilitating contact with the terminal carboxyl groups. The pentaerythritol stearate mixture relies on its hydroxyl groups to bind with the powder particles, and its long fatty chains extend towards the polyester matrix side to form an isolation layer to maintain the dispersion of inorganic particles in the continuous phase and ensure stable spinning pressure.
[0022] Secondly, the present invention provides a method for preparing highly abrasion-resistant, flame-retardant, and tear-resistant polyester composite fibers, employing the following technical solution:
[0023] A method for preparing a highly abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber includes the following steps:
[0024] The polyethylene terephthalate is melted in a first co-rotating twin-screw extruder to form a B-component matrix melt. A mixture of aluminum diethylphosphinate, polytetrafluoroethylene micro powder and pentaerythritol stearate is added to the B-component matrix melt at the side feed port of the first co-rotating twin-screw extruder. The mixture is then extruded to form a B-component mixed melt, and the B-component melt is output after filtration.
[0025] The polyethylene terephthalate is melted in a second co-rotating twin-screw extruder to form a component A matrix melt. The cellulose acetate butyrate and the polycarbodiimide are premixed and added to the component A matrix melt at the side feed port of the second co-rotating twin-screw extruder. The mixture is extruded to form a component A mixed melt, and then filtered and output as the component A melt.
[0026] The A component melt and the B component melt are fed into a parallel composite spinning assembly and extruded to form a composite melt stream.
[0027] The composite melt stream is subjected to side-blowing cooling, oiling, hot stretching, and relaxation heat treatment in sequence to obtain the high wear-resistant, flame-retardant, and tear-resistant polyester composite fiber.
[0028] By adopting the above technical solution, and using a processing path combining an independent twin-screw extrusion system with a side-feeding process, the mixing, dispersion, and thermal processing time of the polyester matrix and different functional components can be individually controlled. The polyester chips are absorbed and melted in the front section of each of the two extruders to form a uniform matrix.
[0029] For component B, aluminum diethylphosphinate and polytetrafluoroethylene micropowder are added to the molten polyester matrix at the side feed position. This avoids dry friction between solid particles and unmelted polyester chips in the extruder conveying section. A pentaerythritol stearate mixture is added together to improve powder dispersion and maintain the flow stability of the highly filled material.
[0030] For component A, cellulose acetate butyrate and polycarbodiimide are premixed and added using a side-feed method. The main purpose is to prevent the polycarbodiimide from entering the high-temperature zone at the front of the extruder, reducing the possibility of high-temperature deactivation and allowing it to smoothly undergo an in-situ end-capping reaction with the carboxyl groups at the polyester end after entering the molten matrix. The melts of components A and B are then extruded in parallel through a parallel composite assembly, physically cured by side-blowing cooling, and then guided to polymer orientation through subsequent thermal stretching. Stress is released through relaxation heat treatment, ultimately forming macroscopic fibers.
[0031] Preferably, before the raw materials are fed into the extruder for melting, the process further includes a step of drying each raw material separately, specifically: drying the polyethylene terephthalate at 135-145°C with dry air having a dew point not higher than -40°C until the measured moisture content is not greater than 30 ppm; vacuum drying the cellulose acetate butyrate at 80-90°C and an absolute pressure not higher than 10 kPa until the moisture content is not greater than 300 ppm; vacuum drying the aluminum diethylphosphinate and the polytetrafluoroethylene micropowder separately; and vacuum drying the pentaerythritol stearate mixture at 40-50°C.
[0032] By employing the above technical solutions, polyethylene terephthalate (PET) is dried using low-dew-point, high-temperature air drying to remove moisture, preventing hydrolysis during subsequent high-temperature melting that could lead to a significant decrease in intrinsic viscosity. The mixture of cellulose acetate butyrate and pentaerythritol stearate is limited by its relatively low thermal stability temperature; therefore, low-temperature, low-pressure vacuum drying is used to remove moisture without inducing oxidative degradation, ensuring the purity of the input raw materials.
[0033] Preferably, during the formation of the B-component mixed melt, the front section temperature of the first co-rotating twin-screw extruder is 265–275°C, the barrel temperature of the first co-rotating twin-screw extruder from the side feed point is controlled at 270–275°C, the absolute pressure at the exhaust port of the first co-rotating twin-screw extruder is controlled at 10–20 kPa, the nominal residence time of the B-component mixed melt from the side feed point to the outlet of the first co-rotating twin-screw extruder is 25–40 seconds, and the B-component mixed melt is output as the B-component melt after filtration.
[0034] During the formation of the A-component mixed melt, the front section temperature of the second co-rotating twin-screw extruder is 272-280°C, the barrel setting temperature of the second co-rotating twin-screw extruder from the side feed point is controlled at 258-265°C, the nominal residence time of the A-component mixed melt from the side feed point to the outlet of the second co-rotating twin-screw extruder is controlled at 20-35 seconds, and the A-component mixed melt is output as the A-component melt after filtration.
[0035] By adopting the above technical solutions, different extrusion temperatures and residence times were set for components A and B respectively. Component B, due to the increased flow resistance caused by the inclusion of more solid powder, was maintained at a relatively high temperature of 270–275°C after side feeding, and negative pressure venting was activated to remove volatiles carried by the filler, ensuring the continuity of the mixed melt. For component A, the barrel temperature was appropriately reduced to 258–265°C after side feeding, and the residence time was controlled at 20–35 seconds. This processing window satisfies the time requirements for the reaction between polycarbodiimide and the terminal carboxyl groups while reducing the risk of degradation of cellulose acetate butyrate due to prolonged heating.
[0036] Preferably, before inputting the A-component melt and the B-component melt into the parallel composite spinning assembly, the method further includes: extracting the A-component melt and the B-component melt for rheological matching verification, confirming that the rheological matching is achieved within 500 seconds. -1 1000s -1 and 2000s -1 At the shear rate, the percentage difference in apparent viscosity between the A-component melt and the B-component melt is no greater than 15%; and before spinning, test yarns are prepared from the A-component melt and the B-component melt for pre-screening to confirm that the absolute difference in dynamic dry heat shrinkage rate after treatment at 165℃ for 45–120 seconds is no less than 4 percentage points. The temperature of the parallel composite spinning assembly is 274–276℃, and the average interfacial contact residence time from the convergence of the A-component melt and the B-component melt in the parallel composite spinning assembly to the spinneret outlet is controlled to be 10–15 seconds.
[0037] By employing the above technical solutions, pre-spinning rheological testing can eliminate melts with excessively large viscosity differences, ensuring the stability of the extrusion interface. Controlling the contact time to 10-15 seconds within the assembly allows for a certain degree of mutual penetration and fusion of the two polymer phases at the interface under high temperature. This interfacial interaction improves the bonding strength of the composite interface, thereby reducing the likelihood of fiber splitting and peeling under bending or knotting stress.
[0038] Preferably, the hot drawing process includes sequential hot drawing on a first drawing roller at 80-90°C and a second drawing roller at 120-130°C, with a total drawing ratio of 2.6-3.3 times; the relaxation heat treatment is carried out in a heat setting chamber at a temperature of 160-165°C for a processing time of 45-120 seconds, with an overfeed rate of 8%-15%.
[0039] By employing the above technical solution, the nascent filaments are stretched sequentially through two drawing rollers at set temperatures. The polymer orients and crystallizes along the direction of force, imparting basic tensile strength to the fiber. Subsequently, the fiber enters a heat-setting chamber under overfeed conditions to release tension constraints. At this point, the cellulose acetate butyrate in component A experiences high axial shrinkage strain, while the inorganic powder in component B hinders the shrinkage process. This difference in shrinkage rate across the fiber cross-section forces the fiber to bend towards the high-shrinkage side, forming a three-dimensional crimped shape after thermosetting.
[0040] This invention provides a highly abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber and its preparation method. It possesses the following beneficial effects:
[0041] 1. This invention maintains melt viscosity by adding polycarbodiimide to component A to consume the carboxyl groups at the polyester ends, and by introducing a pentaerythritol stearate mixture into component B for lubrication to suppress the viscosity increase caused by powder fillers. This synergistically reduces the rheological differences between the two-phase melts during extrusion, preventing shear slip and cross-sectional distortion at the spinning interface. Furthermore, this invention controls the rheological matching and interfacial contact residence time of the multiphase melt within the spinning assembly, promoting interdiffusion and physical entanglement of polyester molecular chains at the phase interface, thus constructing a robust interfacial bonding layer. The synergistic effect of these multiple mechanisms reduces the likelihood of interfacial delamination of the composite fiber under stress, thereby effectively improving the bonding strength of the two-component interface and the overall tear resistance of the composite fiber.
[0042] 2. This invention combines aluminum diethylphosphinic acid and polytetrafluoroethylene micro powder in component B and adds cellulose acetate butyrate to component A. This allows the fiber to be given flame-retardant char protection and surface wear resistance. At the same time, the difference in shrinkage rate of the two components after heating generates internal stress, which drives the composite fiber to undergo controlled bending deformation in the subsequent heat treatment stage, thereby forming a stable three-dimensional crimped structure.
[0043] 3. This invention employs a preparation method that combines an independent twin-screw extrusion system with side feeding. By separately controlling the extrusion processing temperature and residence time of the mixture for the two-component system, it can prevent direct dry friction between solid powder and unmelted polyester chips and ensure that the additives avoid the high-temperature and high-shear region at the front end of the extruder. This guarantees the effectiveness of the in-situ end-capping reaction and the stability of the multiphase mixed melt extrusion process. Attached Figure Description
[0044] Figure 1 This is a logarithmic rheological curve of apparent viscosity and shear rate according to the present invention.
[0045] Figure 2 This is a diagram showing the tensile stress and strain curves of the present invention;
[0046] Figure 3 This is a thermogravimetric analysis curve of the present invention;
[0047] Figure 4 This is a graph showing the evolution of the dynamic friction coefficient of the present invention. Detailed Implementation
[0048] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0049] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.
[0050] Polyethylene terephthalate, CAS No. 25038-59-9, is produced from fiber-grade chips with an intrinsic viscosity of 0.68–0.72 dL / g and a terminal carboxyl group content of 25–35 mol / t.
[0051] Cellulose acetate butyrate, CAS No. 9004-36-8, has a butyryl group mass fraction of 35%–39%, an acetyl group mass fraction of 13%–15%, a free hydroxyl group mass fraction of 1.0%–2.0%, and a glass transition temperature of 125–135℃.
[0052] Aluminum diethylphosphonate, CAS No. 225789-38-8, has a decomposition temperature greater than 300℃ with 5% thermal weight loss, and a primary particle size D50 of 0.8~1.5μm and D99 not greater than 10μm.
[0053] Polytetrafluoroethylene micro powder, CAS No. 9002-84-0, with a weight-average molecular weight of 10,000 to 100,000 g / mol, a particle size distribution D50 of 1 to 3 μm, and D99 not greater than 15 μm.
[0054] The pentaerythritol stearate mixture, whose main component is pentaerythritol monostearate (CAS No. 28062-44-4), has a hydroxyl value of 200-250 mgKOH / g and an acid value of no more than 2.0 mgKOH / g.
[0055] Example 1:
[0056] This embodiment provides a method for preparing high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber, the product being a continuous filament, including the following steps:
[0057] (1) Raw material pretreatment. Fiber-grade polyethylene terephthalate was fed into a continuous crystallization drying tower, and dry air with a dew point not higher than -40℃ was introduced. Drying was carried out at 135℃ until the measured moisture content was not greater than 30ppm. Cellulose acetate butyrate was placed in a double cone vacuum dryer and vacuum dried at 80℃ and an absolute pressure not higher than 10kPa until the moisture content was not greater than 300ppm. After drying, the dried cellulose acetate butyrate was transported in a closed system.
[0058] Aluminum diethylphosphinate and polytetrafluoroethylene micropowder were subjected to vacuum drying. The pentaerythritol stearate mixture was subjected to vacuum drying at 40°C.
[0059] (2) Preparation of component B melt. The raw material formula of component B includes, by mass parts: 90 parts of polyethylene terephthalate, 8.5 parts of aluminum diethylphosphinate, 1.5 parts of polytetrafluoroethylene micro powder, and 0.7 parts of pentaerythritol stearate mixture.
[0060] The dried polyethylene terephthalate (PET) is fed into the first co-rotating twin-screw extruder via a loss-in-weight main feeder. The front-end temperature is controlled at 265°C to melt the dried PET and form the B-component matrix melt. The dried aluminum diethylphosphinate and dried polytetrafluoroethylene (PTFE) micropowder are added to the B-component matrix melt via a mid-section side feeder. The dried pentaerythritol stearate mixture is added to the B-component matrix melt at the side feeder using an independent metering feeding method.
[0061] The barrel temperature of the first co-rotating twin-screw extruder from the side feed point is controlled at 270℃, and the absolute pressure at the exhaust port is controlled at 10kPa. The nominal residence time of the B component melt from the side feed point to the extruder outlet is 25 seconds. The B component melt passes sequentially through a 40μm pre-filter layer and a 25μm final filter layer, and is output as the B component melt after filtration through the final filter layer.
[0062] (3) Preparation of component A melt. The raw material formula of component A includes, by mass, 94 parts of polyethylene terephthalate, 5 parts of cellulose acetate butyrate, and 0.8 parts of polycarbodiimide (the polymer backbone contains repeating carbodiimide groups -(N=C=N)-n, with a weight average molecular weight of 3000~10000g / mol).
[0063] The dried polyethylene terephthalate is added to the second co-rotating twin-screw extruder, and the front temperature is controlled at 272°C to melt the dried polyethylene terephthalate to form the matrix melt of component A.
[0064] After drying, cellulose acetate butyrate is premixed with polycarbodiimide and then added to the A-component matrix melt via a mid-to-rear section loss-in-weight side feeder. From the side feeder, the barrel temperature of the second co-rotating twin-screw extruder is set at 258°C. The nominal residence time of the A-component melt from the side feeder to the extruder outlet is controlled at 20 seconds. The A-component melt passes sequentially through a pre-filter layer and a final filter layer, and is output as the final filter layer.
[0065] (4) Rheological matching verification and composite spinning. Samples were taken at 274℃ and the melts of component A and component B were measured to confirm that the rheological matching was achieved within 500 s. -1 1000s -1 and 2000s -1 At the shear rate, the percentage difference in apparent viscosity between component A melt and component B melt is no greater than 15%. Test yarns were prepared from component A melt and component B melt before spinning for pre-screening, confirming that the absolute difference in dynamic dry heat shrinkage rate after treatment at 165℃ for 45 seconds is no less than 4 percentage points.
[0066] After successful verification, the composite spinning process is executed. Component A melt and component B melt are fed into a parallel composite spinning assembly housed within the spinning box via metering gear pumps, with a volume ratio of 40:60. The temperature of the spinning box and the parallel composite spinning assembly is controlled at 274℃. The average interfacial contact residence time between the merging of component A melt and component B melt within the parallel composite spinning assembly and the spinneret outlet is 10 seconds, resulting in the extrusion of a composite melt stream.
[0067] (5) Cooling, drawing and coiling. The extruded composite melt stream passes through a side-blowing zone with an air temperature of 18℃ and an air speed of 0.6m / s. After cooling, it is oiled and wound at a speed of 900m / min to obtain nascent composite yarn. The nascent composite yarn is then subjected to hot drawing treatment on a first drawing roller at 80℃ and a second drawing roller at 120℃, with a total drawing ratio of 2.6 times, to obtain the drawn composite yarn.
[0068] The drawn composite yarn is fed into a heat-setting chamber and subjected to relaxation heat treatment at 160°C for 45 seconds with an overfeed rate of 8%, causing the drawn composite yarn to shrink and form a three-dimensional crimp structure. After treatment, the composite yarn with the three-dimensional crimp structure is wound into a continuous filament to obtain a high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber in continuous filament form.
[0069] Example 2:
[0070] This embodiment provides a method for preparing high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber, the product being short fiber, including the following steps:
[0071] (1) Raw material pretreatment. Fiber-grade polyethylene terephthalate was fed into a continuous crystallization drying tower, and dry air with a dew point not higher than -40℃ was introduced. Drying was carried out at 140℃ until the measured moisture content was not greater than 30ppm. Cellulose acetate butyrate was placed in a double-cone vacuum dryer and vacuum dried at 85℃ and an absolute pressure not higher than 10kPa until the moisture content was not greater than 300ppm. After drying, the dried cellulose acetate butyrate was transported in a closed system.
[0072] Aluminum diethylphosphonate and polytetrafluoroethylene micropowder were subjected to vacuum drying. A mixture of pentaerythritol stearate was subjected to vacuum drying at 45°C.
[0073] (2) Preparation of component B melt. The raw material formula of component B includes, by mass parts: 88.5 parts of polyethylene terephthalate, 10 parts of aluminum diethylphosphinate, 2.0 parts of polytetrafluoroethylene micro powder, and 1.0 parts of pentaerythritol stearate mixture.
[0074] The dried polyethylene terephthalate (PET) is fed into the first co-rotating twin-screw extruder via a loss-in-weight main feeder. The front-end temperature is controlled at 270°C to melt the dried PET and form the B-component matrix melt. The dried aluminum diethylphosphinate and dried polytetrafluoroethylene (PTFE) micropowder are added to the B-component matrix melt via a mid-section side feeder. The dried pentaerythritol stearate mixture is added to the B-component matrix melt at the side feeder using an independent metering feeding method.
[0075] The barrel temperature of the first co-rotating twin-screw extruder from the side feed point is controlled at 272℃, and the absolute pressure at the exhaust port is controlled at 15kPa. The nominal residence time of the B component melt from the side feed point to the extruder outlet is 32 seconds. The B component melt passes sequentially through a 50μm pre-filter layer and a 30μm final filter layer, and is output as the B component melt after filtration through the final filter layer.
[0076] (3) Preparation of component A melt. The raw material formula of component A includes, by mass parts: 92.5 parts of polyethylene terephthalate, 6.5 parts of cellulose acetate butyrate, and 1.0 part of polycarbodiimide (the polymer backbone contains repeating carbodiimide groups -(N=C=N)-n, and the weight average molecular weight is 3000~10000g / mol).
[0077] The dried polyethylene terephthalate is added to the second co-rotating twin-screw extruder, and the front temperature is controlled at 276°C to melt the dried polyethylene terephthalate to form the matrix melt of component A.
[0078] After drying, cellulose acetate butyrate is premixed with polycarbodiimide and then added to the A-component matrix melt via a mid-to-rear section loss-in-weight side feeder. From the side feeder, the barrel temperature of the second co-rotating twin-screw extruder is set at 262°C. The nominal residence time of the A-component mixed melt from the side feeder to the extruder outlet is controlled at 28 seconds. The A-component mixed melt passes through a pre-filter layer and a final filter layer sequentially, and is output as the A-component melt after filtration through the final filter layer.
[0079] (4) Rheological matching verification and composite spinning. Samples were taken at 275℃ and the melts of component A and component B were measured to confirm that the rheological matching was achieved within 500 seconds. -1 1000s -1 and 2000s -1 At the shear rate, the percentage difference in apparent viscosity between component A melt and component B melt is no greater than 15%. Test yarns were prepared from component A melt and component B melt before spinning for pre-screening, confirming that the absolute difference in dynamic dry heat shrinkage rate after treatment at 165℃ for 80 seconds is no less than 4 percentage points.
[0080] After successful verification, composite spinning was performed. Component A melt and component B melt were fed into a parallel composite spinning assembly housed within the spinning box via metering gear pumps, with a volume ratio of 45:55. The temperature of the spinning box and the parallel composite spinning assembly was controlled at 275℃. The average interfacial contact residence time between the merging of component A melt and component B melt within the parallel composite spinning assembly and the spinneret outlet was 12 seconds, resulting in the extrusion of a composite melt stream.
[0081] (5) Cooling, drawing and coiling. The extruded composite melt stream passes through a side-blowing zone with an air temperature of 20℃ and an air velocity of 0.7m / s. After cooling, it is oiled and wound at a speed of 1050m / min to obtain nascent composite yarn. The nascent composite yarn is then subjected to hot drawing treatment on a first drawing roller at 85℃ and a second drawing roller at 125℃, with a total drawing ratio of 3.0, to obtain the drawn composite yarn.
[0082] The drawn composite yarn is fed into a heat-setting chamber and subjected to relaxation heat treatment at 162°C for 80 seconds with an overfeed rate of 12%, causing the drawn composite yarn to shrink and form a three-dimensional crimp structure. After treatment, the composite yarn with the three-dimensional crimp structure is cut using a cutting machine to obtain short-fiber high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber.
[0083] Example 3:
[0084] This embodiment provides a method for preparing high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber, the product being a continuous filament, including the following steps:
[0085] (1) Raw material pretreatment. Fiber-grade polyethylene terephthalate was fed into a continuous crystallization drying tower, and dry air with a dew point not higher than -40℃ was introduced. Drying was carried out at 145℃ until the measured moisture content was not greater than 30ppm. Cellulose acetate butyrate was placed in a double cone vacuum dryer and vacuum dried at 90℃ and an absolute pressure not higher than 10kPa until the moisture content was not greater than 300ppm. After drying, the dried cellulose acetate butyrate was transported in a closed system.
[0086] Aluminum diethylphosphonate and polytetrafluoroethylene micropowder were subjected to vacuum drying. A mixture of pentaerythritol stearate was subjected to vacuum drying at 50°C.
[0087] (2) Preparation of component B melt. The raw material formula of component B includes, by mass parts: 87 parts of polyethylene terephthalate, 11 parts of aluminum diethylphosphinate, 2.5 parts of polytetrafluoroethylene micro powder, and 1.2 parts of pentaerythritol stearate mixture.
[0088] The dried polyethylene terephthalate (PET) is fed into the first co-rotating twin-screw extruder via a loss-in-weight main feeder. The front-end temperature is controlled at 275°C to melt the dried PET and form the B-component matrix melt. The dried aluminum diethylphosphinate and dried polytetrafluoroethylene (PTFE) micropowder are added to the B-component matrix melt via a mid-section side feeder. The dried pentaerythritol stearate mixture is added to the B-component matrix melt at the side feeder using an independent metering feeding method.
[0089] The barrel temperature of the first co-rotating twin-screw extruder from the side feed point is controlled at 275℃, and the absolute pressure at the exhaust port is controlled at 20kPa. The nominal residence time of the B component melt from the side feed point to the extruder outlet is 40 seconds. The B component melt passes sequentially through a 60μm pre-filter layer and a 35μm final filter layer, and is output as the B component melt after filtration through the final filter layer.
[0090] (3) Preparation of component A melt. The raw material formula of component A includes, by mass parts: 91 parts of polyethylene terephthalate, 8 parts of cellulose acetate butyrate, and 1.3 parts of polycarbodiimide (the polymer backbone contains repeating carbodiimide groups -(N=C=N)-n, and the weight average molecular weight is 3000~10000g / mol).
[0091] The dried polyethylene terephthalate is added to the second co-rotating twin-screw extruder, and the front temperature is controlled at 280°C to melt the dried polyethylene terephthalate to form the matrix melt of component A.
[0092] After drying, cellulose acetate butyrate is premixed with polycarbodiimide and then added to the A-component matrix melt via a mid-to-rear section loss-in-weight side feeder. From the side feeder, the barrel temperature of the second co-rotating twin-screw extruder is set at 265°C. The nominal residence time of the A-component melt from the side feeder to the extruder outlet is controlled at 35 seconds. The A-component melt passes sequentially through a pre-filter layer and a final filter layer, and is output as the final filter layer.
[0093] (4) Rheological matching verification and composite spinning. Samples were taken at 276℃ and the melts of component A and component B were measured to confirm that the rheological matching was achieved within 500 s. -1 1000s -1 and 2000s -1 At the shear rate, the percentage difference in apparent viscosity between component A melt and component B melt is no greater than 15%. Test yarns were prepared from component A melt and component B melt before spinning for pre-screening, confirming that the absolute difference in dynamic dry heat shrinkage rate after treatment at 165℃ for 120 seconds is no less than 4 percentage points.
[0094] After successful verification, the composite spinning process is carried out. Component A melt and component B melt are respectively fed into a parallel composite spinning assembly located inside the spinning box via metering gear pumps. The volume ratio of component A melt to component B melt is 50:50. The temperature of the spinning box and the parallel composite spinning assembly is controlled at 276℃. The average interfacial contact residence time of component A melt and component B melt from merging in the parallel composite spinning assembly to the spinneret outlet is 15 seconds, extruding to form a composite melt stream.
[0095] (5) Cooling, drawing and coiling. The extruded composite melt stream passes through a side-blowing zone with an air temperature of 22℃ and an air velocity of 0.8m / s. After cooling, it is oiled and wound at a speed of 1200m / min to obtain nascent composite yarn. The nascent composite yarn is then subjected to hot drawing treatment on a first drawing roller at 90℃ and a second drawing roller at 130℃, with a total drawing ratio of 3.3 times, to obtain the drawn composite yarn.
[0096] The drawn composite yarn is fed into a heat-setting chamber and subjected to relaxation heat treatment at 165°C for 120 seconds with an overfeed rate of 15%, causing the drawn composite yarn to shrink and form a three-dimensional crimp structure. After treatment, the composite yarn with the three-dimensional crimp structure is wound into a continuous filament to obtain a high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber in continuous filament form.
[0097] Comparative Example 1:
[0098] Compared with Example 2, the difference is that: in step (3), polycarbodiimide is not added to the raw material formulation of component A, and the amount of polyethylene terephthalate is increased accordingly to make up to the same total mass fraction of component A as in Example 2. All other aspects are the same.
[0099] Comparative Example 2:
[0100] Compared with Example 2, the difference is that: in step (2), the raw material formulation of component B does not contain pentaerythritol stearate mixture, and the amount of polyethylene terephthalate is increased accordingly to make up to the same total mass fraction of component B as in Example 2, while the rest are the same.
[0101] Comparative Example 3:
[0102] Compared with Example 2, the difference is that in step (3), the dried cellulose acetate butyrate and polycarbodiimide are moved to the main feed port and fed into the second co-rotating twin-screw extruder together with the dried polyethylene terephthalate, so that the cellulose acetate butyrate and polycarbodiimide undergo the full melt extrusion thermal history. The rest are the same.
[0103] Comparative Example 4:
[0104] Compared with Example 2, the difference is that the extrusion temperature parameters of the second co-rotating twin-screw extruder in step (3) are adjusted so that the pre-screening temperature is within 500s. -1 1000s -1 and 2000s -1 The percentage difference in apparent viscosity between component A melt and component B melt measured at shear rate was greater than 15% for both, and the rest were the same.
[0105] Comparative Example 5:
[0106] Compared with Example 2, the difference is that the temperature of the first stretching roller and the temperature of the second stretching roller in step (5) are adjusted so that the absolute difference of the dynamic dry heat shrinkage rate measured after treatment at 165°C for 80 seconds in the pre-screening is less than 4 percentage points, and the rest are the same.
[0107] Comparative Example 6:
[0108] Compared with Example 2, the difference is that in step (4), the volume of the internal flow channel of the composite spinning assembly is adjusted so that the average interface contact residence time of the A component melt and the B component melt in the parallel composite spinning assembly to the spinneret outlet is set to 5 seconds, and the rest are the same.
[0109] Comparative Example 7:
[0110] Compared with Example 2, the difference is that aluminum diethylphosphinate is not added to the raw material formulation of component B in step (2), and the amount of polyethylene terephthalate is increased accordingly to make up to the same total mass fraction of component B as in Example 2. All other aspects are the same.
[0111] Comparative Example 8:
[0112] Compared with Example 2, the difference is that: in step (2), polytetrafluoroethylene micro powder is not added to the raw material formulation of component B, and the amount of polyethylene terephthalate is increased accordingly to make up to the same total mass fraction of component B as in Example 2. All other aspects are the same.
[0113] Test Example 1:
[0114] This test case is used to evaluate the processing stability of component A melt, the filtration stability of component B melt, and the rheological matching verification between component A melt and component B melt in Examples 1 to 3.
[0115] (1) The cooled output material at the extruder die in the melt preparation step of component A in Examples 1 to 3 was selected as the test object. Its intrinsic viscosity was measured by Ubbelohde viscometer and compared with the initial intrinsic viscosity of the raw material polyethylene terephthalate to calculate the intrinsic viscosity retention rate. At the same time, the terminal carboxyl group content of component A output material was measured by chemical titration and compared with the terminal carboxyl group content of the raw material polyethylene terephthalate to calculate the terminal carboxyl group reduction rate.
[0116] (2) In the melt preparation steps of component B in Examples 1 to 3, the final filter layer at the outlet of the first co-rotating twin-screw extruder was selected as the monitoring object. After the extruder reached a stable operating state, the initial back pressure of the final filter layer was recorded; after maintaining continuous operation for 120 minutes, the final back pressure was recorded, and the average back pressure rise rate within 120 minutes was calculated.
[0117] (3) The A-component melt and B-component melt before spinning in Examples 1 to 3 were extracted as test objects. Using a capillary rheometer, the two melts were measured at the spinning set temperature corresponding to each example for 500 s. -1 1000s -1 and 2000s -1 Apparent viscosity under shear rate conditions. Based on the absolute difference and average of the apparent viscosities of component A and component B melts at each shear rate node, the percentage of apparent viscosity difference was calculated (the percentage of apparent viscosity difference is used to evaluate the difference in melt viscosity between component A and component B melts). Based on the test results at 275°C in Example 2, logarithmic rheological curves of apparent viscosity versus shear rate for component A and component B melts were plotted, and the corresponding test nodes were marked on the curves.
[0118] The test results are shown in Table 1.
[0119] Table 1. Results of multiphase melt processing stability and rheological matching tests:
[0120]
[0121] Test conclusion:
[0122] As shown in Table 1, the intrinsic viscosity retention rate of the extrudates of component A in Examples 1 to 3 was 91.8% to 94.3%, and the terminal carboxyl group reduction rate was 38.5% to 42.1%. These results indicate that, under the conditions of side-feed temperature and residence time, the addition of polycarbodiimide is beneficial in reducing the terminal carboxyl group content in the component A system and helps to mitigate the decrease in molecular weight of the polyethylene terephthalate continuous phase matrix during melt processing.
[0123] In the component B filtration pressure test, the average back pressure rise rate of the final filter layer in Examples 1 to 3 ranged from 0.011 MPa / h to 0.019 MPa / h. This result indicates that in the component B system where aluminum diethylphosphinate and polytetrafluoroethylene micropowder coexist, the pentaerythritol stearate mixture is beneficial in improving the dispersion stability of the functional filler in the polyethylene terephthalate continuous phase matrix, reducing the agglomeration tendency of solid filler particles during melt extrusion and filtration, thereby helping to maintain the pressure stability of the high filler content melt when passing through the filter layer.
[0124] From Table 1 and Figure 1 It can be seen that in Examples 1 to 3, the melt of component A and the melt of component B are within 500s. -1 1000s -1 and 2000s -1 The percentage difference in apparent viscosity at all three shear rate nodes was no greater than 15%, with a maximum of 14.2%. In Example 2, the apparent viscosity of component A melt and component B melt at 275°C decreased with increasing shear rate, and the two components maintained a similar trend within the tested shear rate range. These results indicate that component A melt and component B melt have good viscous flow behavior matching, which is beneficial for reducing the flow difference between the two phase melts in the spinning assembly flow channel and spinneret shear field, thereby helping to improve the cross-sectional stability in the parallel composite spinning process.
[0125] Test Example 2:
[0126] (1) The composite spinning production process of Examples 1 to 3 and Comparative Example 6 was selected as the monitoring object. 100 spinning positions were set up on the spinning equipment to run synchronously and maintain continuous production for 24 hours. The total number of yarn breaks during continuous operation was recorded. After production was completed, the number of fully wound yarn cakes was counted, and the full-wound rate was calculated by dividing the number of fully wound yarn cakes by the theoretically expected total number of yarn cakes.
[0127] (2) Under the standard environment of 20±2℃ and 65±5% relative humidity, the continuous composite filaments after relaxation heat treatment in Examples 1 to 3 and Comparative Example 6 were taken as mechanical test objects. In Examples 2 and Comparative Example 6, continuous composite filament samples were extracted before the cutting process. Using a monofilament strength testing machine, the tensile speed was set to 20mm / min and the clamping distance was 20mm. The continuous composite filaments were stretched until they broke. The force value at the time of breakage was recorded, and the breaking strength was calculated in combination with the fiber linear density.
[0128] (3) Take a continuous composite filament from the same batch as in step (2), tie a standard single knot at the center of the sample length as the stress concentration point, and form a single knot specimen. Fix the single knot specimen in a single filament strength testing machine and perform a tensile test using the same parameters as in step (2) until fracture. Record the force value when the specimen fractures and calculate the knot strength. Divide the measured knot strength by the fracture strength of the corresponding embodiment and comparative example, and multiply by 100% to obtain the knot strength retention rate. Extract the load and displacement data of the single knot specimen of Example 2 and the single knot specimen of Comparative Example 6 during the tensile process, convert them into engineering stress and engineering strain, plot the tensile stress and strain curves of the single knot specimen of Example 2 and the single knot specimen of Comparative Example 6, and mark the fracture point in the curve.
[0129] The test results are shown in Table 2.
[0130] Table 2. Test results of macroscopic filamentation and interfacial bonding:
[0131]
[0132] Test conclusion:
[0133] According to the data in Table 2, in the test of 100 spinning positions operating synchronously for 24 hours in Examples 1 to 3, the total number of yarn breaks was between 14 and 23, corresponding to a full roll rate of 96.8% to 98.2%. The above production operation data shows that, under the process conditions, the extrusion and forming process of the multi-component melt in the spinning assembly has good stability, and no stress concentration or component peeling phenomena that would cause melt stream breakage were observed during the test.
[0134] Table 2 shows that the breaking strengths measured in Examples 1 to 3 ranged from 3.12 cN / dtex to 3.48 cN / dtex, and the knotting strengths ranged from 2.65 cN / dtex to 2.93 cN / dtex. The knotting strength retention rate of the three examples reached over 83.6%. In contrast, in Comparative Example 6, the average interfacial contact residence time from the convergence of component A melt and component B melt in the parallel composite spinning assembly to the spinneret outlet was set to 5 seconds. Its breaking strength was 3.08 cN / dtex, but the knotting strength decreased to 1.35 cN / dtex, with a knotting strength retention rate of 43.8%. These results indicate that, when the breaking strengths are similar, a decrease in the average interfacial contact residence time may adversely affect the knotting strength retention rate of the parallel composite fibers.
[0135] Combination Figure 2 It can be seen that the single-knot specimen of Example 2 exhibits a longer tensile deformation process before reaching the fracture point and can withstand higher engineering strain and engineering stress. In contrast, the single-knot specimen of Comparative Example 6 reaches the fracture point under lower engineering strain, indicating that it is more prone to premature failure under knotted tensile load.
[0136] Both component A and component B contain polyethylene terephthalate (PET) in their continuous phase matrix. In an environment of 274°C to 276°C within the spinning assembly channel, the average interfacial contact residence time of the two phase matrices in this example is 10 to 15 seconds. The PET continuous phase matrix is in a molten flow state, and the molecular chain segments possess a certain degree of mobility. Based on the laws governing interdiffusion and physical entanglement of polymer interfacial chains, under the condition of the average interfacial contact residence time, the PET molecular chains on both sides of the interface may undergo a certain degree of interdiffusion near the initial phase interface.
[0137] The aforementioned molecular chain interdiffusion behavior facilitates the formation of a transition layer with physical entanglement characteristics in the bonding region. Under conditions where no external compatibilizer is added and no cross-interfacial covalent cross-linking reaction is introduced, the molecular chain physical entanglement network formed under sufficient contact time can provide some support to the parallel interface, thereby helping to reduce the possibility of interfacial peeling or separation of the parallel composite fibers under mechanical loads, especially bending and tensile composite loads in knot tests. In Comparative Example 6, due to the shorter average interfacial contact residence time, the degree of molecular chain interdiffusion near the interface may be relatively insufficient. Therefore, under complex loads, insufficient interfacial bonding is more likely to occur, corresponding to lower knot strength and a tendency for premature breakage.
[0138] Test Example 3:
[0139] (1) In the pre-spinning stage of Examples 1 to 3, Comparative Examples 1, 3 and 5, the A component melt and B component melt under the corresponding preparation parameters were extracted to prepare A component test yarn and B component test yarn. Using a heat shrinkage rate tester, in a test chamber with an ambient temperature of 165°C, the test time was set to be consistent with the relaxation heat treatment time in the examples and comparative examples. The length change after heat treatment was measured, the dynamic dry heat shrinkage rate was calculated, and the absolute difference of the dynamic dry heat shrinkage rate between the A component test yarn and the B component test yarn in the corresponding test batch was obtained.
[0140] (2) Samples were randomly selected from the final composite fibers of Examples 1 to 3, Comparative Examples 1, 3 and 5. The samples were placed in an environment with a temperature of 20±2℃ and a relative humidity of 65±5% for 24 hours to condition them. A monofilament tensile testing machine was used, with the tensile speed set to 20mm / min and the clamping distance to 20mm. The fibers were stretched until they broke, and the force at the time of breakage was recorded. The breaking strength of the composite fiber was calculated in combination with the linear density.
[0141] (3) Take a sample of the finished composite fiber bundle after conditioning and fix it in the upper and lower clamps of the fiber crimp elasticity tester. Apply a set light load tension to straighten the fiber, measure the straightened length, and count the number of crimp peaks within each 25mm length under the magnification observation device of the instrument to obtain the crimp count. Remove the load and wait for the fiber to recover and stabilize, then measure the recovered crimp length. Calculate the crimp rate by dividing the difference between the straightened length and the crimp length by the straightened length.
[0142] The test results are shown in Table 3.
[0143] Table 3. Test results of curling morphology and intrinsic mechanical properties:
[0144]
[0145] Test conclusion:
[0146] According to the data in Table 3, the breaking strength of Examples 1 to 3 ranged from 3.14 to 3.46 cN / dtex. The breaking strength of Comparative Example 1, lacking polycarbodiimide, was 2.12 cN / dtex; the breaking strength of Comparative Example 3 was 2.38 cN / dtex. The data reflects that polyethylene terephthalate undergoes alcoholysis and thermal oxidative chain cleavage at high temperatures. When polycarbodiimide is added to the designated side-feeding section, its carbodiimide groups undergo an addition reaction with the terminal carboxyl groups of polyethylene terephthalate, consuming the terminal carboxyl groups and maintaining the molecular weight of polyethylene terephthalate. In Comparative Example 3, due to the longer thermal history of the polycarbodiimide, the groups were consumed or deactivated, failing to maintain the molecular weight of the continuous phase, resulting in a decrease in the breaking strength of the monofilament.
[0147] Table 3 shows that the absolute difference in dynamic dry heat shrinkage rates between Examples 1 and 3 reached over 4.6%, with the number of crimps in the composite fibers ranging from 11.9 to 14.3 per 25 mm, and the crimp rate ranging from 31.4% to 37.9%. In Comparative Example 5, the absolute difference in dynamic dry heat shrinkage rates decreased to 1.4%, with the corresponding number of crimps decreasing to 4.1 per 25 mm and the crimp rate decreasing to 10.9%, showing a trend of narrowing difference in heat shrinkage between the two phases.
[0148] Cellulose acetate butyrate in component A constitutes steric hindrance, exhibiting axial macroscopic shrinkage strain upon heating past its glass transition temperature. Rigid particles in component B generate geometric steric hindrance, limiting the dimensional retreat of the B-phase matrix upon heating. The difference in dynamic dry-heat shrinkage rates between the two phases under heating conditions constitutes asymmetric internal stress generated by this thermal shrinkage difference, forcing the composite fiber to undergo three-dimensional curling deformation towards the high-shrinkage A side, forming a helical three-dimensional curled structure. In Comparative Example 5, due to the reduced shrinkage difference between the two components, the asymmetric internal stress is insufficient to generate a sufficient curling driving force, resulting in only weaker curling deformation of the composite fiber, manifested as a decrease in the number and rate of macroscopic curls.
[0149] Test Example 4:
[0150] (1) The final composite fibers obtained from Examples 1 to 3, Comparative Examples 2, 4, 7 and 8 were uniformly sampled and tested. The yarn linear density, fabric structure and warp and weft density were controlled to be consistent. The woven surface density was 200 g / m². 2 Standard woven fabric samples were prepared. The limiting oxygen index of each standard woven fabric sample was tested using a limiting oxygen index meter. Test powder was extracted from the sample of Example 2 and the sample of Comparative Example 7 and placed in a thermogravimetric analyzer. Under a nitrogen atmosphere, the heating rate was set to 10 °C / min, and the residual mass percentage (%) data as a function of temperature (°C) from 30 °C to 800 °C were recorded, and a thermogravimetric analysis curve was plotted.
[0151] (2) Cut circular test pieces of specified size from each standard woven fabric sample. Fix the test pieces inside the grinding ring of the Martindale abrasion tester and set the loading pressure to 12 kPa. Use standard wool abrasive cloth as the dual surface to conduct multi-directional Lissajous trajectory friction tests. Observe and record the number of Martindale breakage cycles when two independent yarns on the surface of the test piece completely break. During the test, extract the frictional resistance data of the test pieces of Example 2 and Comparative Example 8 under the same conditions, convert them into dynamic friction coefficients, and plot the evolution curve of the dynamic friction coefficient as a function of the number of friction cycles.
[0152] (3) According to the standard for tear strength testing of textiles, trapezoidal test strips were cut from each standard woven fabric sample, and the warp test strips and weft test strips were distinguished. The tensile rate was set to 100 mm / min on the universal testing machine, and tear tests were performed on the warp test strips and weft test strips respectively. The peak tear force ranges that occurred during the test were recorded, and the average data of the warp tear strength and the weft tear strength were calculated and recorded.
[0153] The test results are shown in Table 4.
[0154] Table 4. Comparison of abrasion resistance, tear resistance, and synergistic flame retardant functionality test results:
[0155]
[0156] Test conclusion:
[0157] According to the data in Table 4, the limiting oxygen index (LOI) of the woven fabrics in Examples 1 to 3 ranged from 28.5% to 29.1%, with over 28,600 Martindale tear cycles, and both warp and weft tear strengths remained at a high level. Comparative Example 7, without the addition of aluminum diethylphosphonate, had a limiting oxygen index reduced to 21.4%. Figure 3 It can be seen that the residual mass percentage of Comparative Example 7 sample in the high temperature range is relatively low, indicating that its high temperature residue content is relatively low.
[0158] The above results indicate that the addition of aluminum diethylphosphinate is beneficial to improving the char residue level of the composite fiber system and is related to the increase in the limiting oxygen index. When heated, aluminum diethylphosphinate can promote the char formation of the condensed phase in the polyethylene terephthalate continuous matrix and contribute to the formation of a charred heat-insulating shielding layer. Simultaneously, its phosphorus-containing structure may participate in the gas-phase free radical capture and condensed phase char formation process during combustion. Therefore, Comparative Example 7, without the addition of aluminum diethylphosphinate, exhibits a lower limiting oxygen index, indicating that its char-forming heat insulation and flame-retardant inhibition effects are relatively weakened.
[0159] Comparative Example 8, without the addition of polytetrafluoroethylene (PTFE) micropowder, showed a decrease in Martindale breakage cycles to 9500. Figure 4 It can be seen that the dynamic friction coefficient of the test piece in Comparative Example 8 remained at a relatively high level with some fluctuations during the friction cycle, while the dynamic friction coefficient of the test piece in Example 2 decreased initially and then tended to be at a lower and more stable level. Polytetrafluoroethylene (PTFE) micropowder has low surface energy characteristics. When the fiber is subjected to frictional load, the PTFE micropowder may form a low-friction transfer film between the fiber and the mating interface, thereby reducing the impact of frictional shearing on the polyethylene terephthalate (PET) continuous phase matrix. Comparative Example 8, because it did not add PTFE micropowder, found it difficult to form the aforementioned low-friction transfer film, and therefore exhibited a trend of increased wear and earlier yarn breakage in the Martindale test.
[0160] Comparative Example 4 shows a decrease in warp tear strength to 41.2 N and weft tear strength to 36.8 N. This result indicates that when the percentage difference in apparent viscosity between component A and component B melts is large, the difference in viscous flow behavior between the two phases in the spinning assembly flow channel and spinneret shear field increases, potentially leading to increased cross-sectional offset or distortion of the cross-sectional morphology in the parallel composite fibers. Reduced cross-sectional morphology stability makes the composite fibers more prone to localized stress concentration when subjected to external tearing loads, resulting in a decrease in both warp and weft tear strength.
[0161] Comparative Example 2, without the addition of pentaerythritol stearate mixture, showed a limiting oxygen index reduced to 25.3% and a Martindale failure cycle count reduced to 18,200. These test results indicate that the addition of pentaerythritol stearate mixture is beneficial for improving the dispersion stability of functional fillers such as aluminum diethylphosphinate and polytetrafluoroethylene micropowder in the polyethylene terephthalate continuous phase matrix, reducing the agglomeration tendency of solid filler particles, and helping to maintain the stability of the composite fiber structure and functional performance. Therefore, the polycarbodiimide and pentaerythritol stearate mixture synergistically reduce the melt viscosity difference between component A and component B, thereby improving the tear resistance of the composite fiber.
[0162] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber, characterized in that, It is made by melt spinning of parallel composite components A and B, wherein the volume ratio of component A to component B is 40:60 to 50:50; The raw materials of component A, by mass parts, include: 91-94 parts of polyethylene terephthalate, 5-8 parts of cellulose acetate butyrate, and 0.8-1.3 parts of polycarbodiimide; The raw materials of component B, by mass parts, include: The mixture comprises 87-90 parts of polyethylene terephthalate, 8.5-11 parts of aluminum diethylphosphinate, 1.5-2.5 parts of polytetrafluoroethylene micro powder, and 0.7-1.2 parts of pentaerythritol stearate. The mixture of polycarbodiimide and pentaerythritol stearate respectively adjusts the melt viscosity of component A and component B, thereby reducing the melt viscosity difference between component A and component B, and improving the tear resistance of the high abrasion resistant, flame retardant and tear resistant polyester composite fiber.
2. The high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber according to claim 1, characterized in that, The intrinsic viscosity of the polyethylene terephthalate is 0.68–0.72 dL / g, and the end carboxyl group content of the polyethylene terephthalate is 25–35 mol / t. The cellulose acetate butyrate contains 35%–39% butyryl groups, 13%–15% acetyl groups, and 1.0%–2.0% free hydroxyl groups. The glass transition temperature of the cellulose acetate butyrate is 125–135°C.
3. The high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber according to claim 1, characterized in that, The decomposition temperature of the aluminum diethylphosphonate with a 5% thermal weight loss is greater than 300°C, and the primary particle size D50 of the aluminum diethylphosphonate is 0.8–1.5 μm. The polytetrafluoroethylene (PTFE) micropowder has a weight-average molecular weight of 10,000–100,000 g / mol and a particle size distribution (D50) of 1–3 μm. The weight-average molecular weight of the polycarbodiimide is 3000–10000 g / mol; The pentaerythritol stearate mixture comprises pentaerythritol monostearate, and the hydroxyl value of the pentaerythritol stearate mixture is 200-250 mg KOH / g.
4. A method for preparing a highly abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber, characterized in that, The preparation of the high abrasion-resistant, flame-retardant, and tear-resistant polyester composite fiber as described in any one of claims 1-3 includes the following steps: Polyethylene terephthalate is melted in a first co-rotating twin-screw extruder to form a B-component matrix melt. A mixture of aluminum diethylphosphinate, polytetrafluoroethylene micro powder and pentaerythritol stearate is added to the B-component matrix melt at the side feed port of the first co-rotating twin-screw extruder. The mixture is then extruded to form a B-component mixed melt, and the B-component melt is output after filtration. The polyethylene terephthalate is melted in a second co-rotating twin-screw extruder to form a component A matrix melt. Cellulose acetate butyrate and polycarbodiimide are premixed and added to the component A matrix melt at the side feed port of the second co-rotating twin-screw extruder. The mixture is extruded to form a component A mixed melt, and then filtered and output as the component A melt. The A component melt and the B component melt are fed into a parallel composite spinning assembly and extruded to form a composite melt stream. The composite melt stream is sequentially subjected to side-blowing cooling, oiling, hot stretching, and relaxation heat treatment to obtain the high wear-resistant, flame-retardant, and tear-resistant polyester composite fiber.
5. The preparation method according to claim 4, characterized in that, Before the raw materials are fed into the extruder for melting, the process also includes a step of drying each raw material separately, specifically: The polyethylene terephthalate was dried at 135–145°C by passing dry air with a dew point not higher than -40°C until the measured moisture content was not greater than 30 ppm. The cellulose acetate butyrate was vacuum dried at 80–90°C and an absolute pressure not exceeding 10 kPa until the moisture content was not greater than 300 ppm. The aluminum diethylphosphinic acid and the polytetrafluoroethylene micro powder were respectively subjected to vacuum drying treatment; The pentaerythritol stearate mixture was subjected to vacuum drying at 40–50°C.
6. The preparation method according to claim 4, characterized in that, During the formation of the B component mixed melt, the front section temperature of the first co-rotating twin-screw extruder is 265-275°C, the barrel temperature of the first co-rotating twin-screw extruder from the side feed point is controlled at 270-275°C, and the absolute pressure of the exhaust port of the first co-rotating twin-screw extruder is controlled at 10-20 kPa. The nominal residence time of the B component mixed melt from the side feed point to the outlet of the first co-rotating twin-screw extruder is 25 to 40 seconds, and the B component mixed melt is output as the B component melt after filtration.
7. The preparation method according to claim 4, characterized in that, During the formation of the A component mixed melt, the front section temperature of the second co-rotating twin-screw extruder is 272-280°C, and the barrel setting temperature of the second co-rotating twin-screw extruder from the side feed point is controlled at 258-265°C. The nominal residence time of the A-component mixed melt from the side feed point to the outlet of the second co-rotating twin-screw extruder is controlled at 20-35 seconds, and the A-component mixed melt is output as the A-component melt after filtration.
8. The preparation method according to claim 4, characterized in that, The temperature of the parallel composite spinning assembly is 274-276°C, and the average interfacial contact residence time of the A component melt and the B component melt from merging in the parallel composite spinning assembly to the spinneret outlet is controlled to be 10-15 seconds.
9. The preparation method according to claim 4, characterized in that, The hot drawing process includes sequential hot drawing on a first drawing roll at 80-90°C and a second drawing roll at 120-130°C, with a total drawing ratio of 2.6-3.3 times. The relaxation heat treatment is carried out in a heat setting chamber at a temperature of 160–165°C for 45–120 seconds, with an overfeed rate of 8%–15%.
10. The preparation method according to claim 4, characterized in that, Before feeding the A-component melt and the B-component melt into the parallel composite spinning assembly, the process further includes: The rheological matching of the extracted A-component melt and the B-component melt was verified, confirming that the rheological matching was achieved within 500 seconds. -1 1000s -1 and 2000s -1 At the shear rate, the percentage difference in apparent viscosity between the A component melt and the B component melt is no greater than 15%. Furthermore, before spinning, the A component melt and the B component melt were extracted to prepare test yarns for pre-screening, confirming that the absolute difference in dynamic dry heat shrinkage rate after treatment at 165℃ for 45-120 seconds was not less than 4 percentage points.