A wear-resistant and non-deformable fabric and its manufacturing method
By performing smoothing, alkali treatment, and low-shrinkage treatment on nylon fibers, combined with a nano-sheet tungsten disulfide coating and polyester melt bonding, the problem of twisting and deformation of lightweight fabrics after washing is solved, achieving a wear-resistant and non-deformable effect.
Patent Information
- Application Number
- CN202611234164.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-10
AI Technical Summary
Thin fabrics are prone to twisting and deformation after home washing, have poor abrasion resistance, and are difficult to control in terms of dimensional stability.
Nylon fibers are treated with a fiber lubricant, mixed and spun, and then subjected to alkali treatment and low shrinkage treatment. They are then coated with nano-sheet tungsten disulfide, waterborne polyurethane, and liquid wax. Finally, the polyester fibers are melted and bonded by baking, which eliminates internal stress and improves abrasion resistance.
The fabric is less prone to deformation after friction and washing, has improved abrasion resistance, enhanced dimensional stability, reduced slip resistance between fibers, and maintains a good hand feel and breathability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a wear-resistant and non-deformable fabric and its manufacturing method, belonging to the textile field. Background Technology
[0002] Lightweight clothing is becoming increasingly popular, offering a light and comfortable wearing experience. Due to its thinness, the fabric is breathable and cool to wear; however, it also suffers from poor abrasion resistance and presents technical challenges in controlling and maintaining consistent fabric shrinkage.
[0003] Lightweight fabrics typically use yarns with a higher yarn count (S), which leads to significant skew problems. The internal stress accumulated during the twisting process cannot be balanced in conventional finishing processes, causing garments to easily twist and deform after regular household washing. Summary of the Invention
[0004] In order to overcome the shortcomings of the prior art, the present invention provides a wear-resistant and non-deformable fabric and a method for manufacturing the same, and clothing made from the fabric is not easily deformed during household washing.
[0005] The technical solution adopted by this invention to solve its technical problem is: In a first aspect, this application provides a method for manufacturing a wear-resistant and non-deformable fabric, the steps of which include: Modified nylon is obtained by soaking heat-shrinkable nylon fibers in a fiber lubricant. The first yarn is obtained by mixing cotton fiber, modified nylon fiber and polyester fiber with a melting point of 90℃~120℃ and spinning them together. Weave the fabric blank using the first yarn; The fabric is then finished to obtain the wear-resistant and non-deformable fabric. The finishing processes include: alkali treatment, low shrinkage treatment, padding treatment, and baking treatment; The padding solution used in the padding process contains nano-sheet tungsten disulfide, waterborne polyurethane, liquid wax, and emulsifier.
[0006] The method for manufacturing abrasion-resistant and non-deformable fabric provided in this application involves treating nylon fibers with a fiber smoothing agent to make them smooth, while the cotton fibers remain untreated, ensuring sufficient yarn cohesion during blending. Spinning causes the yarn to accumulate internal stress; this method involves alkali treatment of the woven fabric to smooth the cotton fibers as well. Then, a low-shrinkage treatment is performed. The smooth cotton and modified nylon fibers allow the fabric to significantly eliminate internal stress during the low-shrinkage treatment, making it less prone to twisting and deformation during subsequent friction and household washing. The padding treatment coats the fabric with a coating containing nano-flake tungsten disulfide and liquid wax, making the fabric even smoother and thus more resistant to everyday wear friction. Finally, baking not only cures the coating, but more importantly, because both nylon and cotton fibers become smooth and easily slip between each other, this method uses baking to partially melt the polyester fibers, which has the effect of bonding the blended components, ensuring the strength of the fabric. In addition, the modified nylon has been heat-shrinked beforehand, so its shape and structure are stable during baking. The fabric has already eliminated most of the internal stress during the previous low-shrinkage treatment. Therefore, the fabric after bonding has a low shrinkage rate, a stable shrinkage rate, and is not easily deformed.
[0007] Furthermore, in the step of blending and spinning, the raw materials include 30% to 40% cotton fiber, 30% to 40% modified nylon fiber, and 20% to 30% polyester fiber.
[0008] Cotton fibers provide the fabric with moisture absorption and a soft hand feel. Before alkali treatment, their rough surface provides the cohesion needed for spinning; after alkali treatment, the surface becomes smooth and participates in stress release. Modified nylon fibers inherently possess excellent abrasion resistance. After lubrication treatment, the coefficient of friction is further reduced, allowing them to bear the main load when subjected to friction. Their smooth surface also contributes to reducing torque during spinning. Polyester fibers are uniformly dispersed in the yarn cross-section. During baking, the molten polyester forms a continuous bonding network, effectively locking in the stable fiber configuration after low-shrinkage treatment. If the proportion of polyester fibers is too low, insufficient melt bonding results in a weakly locked yarn structure, making the fibers prone to slippage under external force, thus degrading the fabric's dimensional stability and abrasion resistance. If the proportion is too high, excessive melt flow leads to large-area fiber adhesion, resulting in a stiff hand feel and affecting the moisture absorption of cotton fibers and the breathability of the fabric.
[0009] Furthermore, in the alkali treatment step, the Baume degree of the alkali solution is 16 Bé to 18 Bé, and the treatment time is 15 min to 25 min.
[0010] The alkali concentration and treatment time set for the alkali treatment ensure sufficient smoothing while avoiding overtreatment that could damage cotton fibers or severely corrode polyester fibers (mild corrosion is negligible, as polyester fibers primarily function as a melt bond). After alkali treatment, the cotton fibers become smooth, forming a low-friction interface system together with the already smooth modified nylon fibers. During low-shrinkage treatment, this fully smooth interface reduces the sliding resistance between fibers to extremely low levels, allowing the fabric to shrink freely and efficiently in a tension-free environment. Residual internal stress is completely released, and the yarn tends towards a stable configuration. If the alkali concentration is too low or the treatment time is insufficient, the cotton fibers will not be sufficiently smoothed. The rough parts of their surface will lock the movement between fibers during low-shrinkage treatment, resulting in incomplete release of internal stress. After multiple washes of thin fabrics, the gradual release of residual stress may lead to dimensional changes and skewness. The alkali treatment itself also stabilizes the dimensions of the cotton fibers, providing another layer of protection for the overall low shrinkage rate of the fabric.
[0011] Furthermore, prior to the alkali treatment, the finishing process also includes a tenter frame treatment, the requirements of which are: the tenter frame belt is overfed by 25% to 35%, and the machine speed is 50m / min to 60m / min.
[0012] Under overfeed conditions, the interlacing points of the warp and weft yarns loosen, widening the yarn gaps. This allows the alkali solution to quickly and evenly penetrate each yarn during subsequent alkali treatment, ensuring full contact with all cotton fibers and guaranteeing that all fibers undergo the same degree of smoothing. Appropriate machine speed and overfeed volume provide sufficient relaxation time for the fabric on the conveyor belt, allowing the expanded yarn gaps to fully develop without being pulled back to their original state by excessive running speed. After stretching, the fabric immediately enters the alkali treatment while in a structurally relaxed state. The swelling effect of the alkali solution fixes this open gap state and the morphological transformation of the cotton fibers, ensuring that fibers throughout the fabric have an equal opportunity to slip during subsequent low-shrinkage treatment.
[0013] Furthermore, the shrinkage treatment is carried out in an overflow machine at a temperature of 50℃~60℃ for 20min~30min.
[0014] The low-shrinkage treatment is carried out in an overflow machine, with appropriate treatment temperature and sufficient treatment time set. The low-tension environment provides ample free space for fiber sliding and rearrangement, releasing the physical internal stress accumulated during spinning and weaving. The selected treatment temperature accelerates fiber chain segment movement while remaining below the melting point of polyester fibers. After the low-shrinkage treatment, the fabric reaches a stable state with minimal stress. Subsequently, padding and baking are performed, and the polyester melts and bonds, fixing this stable structure. During washing, there is no more internal stress to release, resulting in dimensional stability and resistance to deformation of the fabric.
[0015] Furthermore, the dispersed phase of the padding liquid contains, by mass, 15 to 25 parts of nano-sheet tungsten disulfide dispersion, 40 to 60 parts of the aqueous polyurethane, 5 to 8 parts of the liquid wax, and 3 to 5 parts of the emulsifier. The preparation steps of the nano-sheet tungsten disulfide dispersion include: taking 60 to 80 parts by mass of N,N-dimethylformamide as the continuous phase of the nano-sheet tungsten disulfide dispersion, adding 3 to 5 parts of polyvinyl alcohol, 10 to 18 parts of tungsten disulfide powder, and 6 to 16 parts of dispersant, mixing and ultrasonically treating to obtain the nano-sheet tungsten disulfide dispersion.
[0016] In the preparation of this dispersion, N,N-dimethylformamide was used as the continuous phase, and polyvinyl alcohol was added. Tungsten disulfide powder was ultrasonically exfoliated to obtain thin sheet-like tungsten disulfide nanosheets. Polyvinyl alcohol plays a dual role in the dispersion: on the one hand, it encapsulates the exfoliated tungsten disulfide nanosheets, using steric hindrance to prevent them from recombinizing and maintaining the sheet-like dispersion; on the other hand, after padding, polyvinyl alcohol and N,N-dimethylformamide together slow down the solvent evaporation rate, allowing the tungsten disulfide nanosheets more time to spread evenly on the fiber surface during the waterborne polyurethane film formation process, forming a layered lubricating arrangement with overlapping surfaces. Liquid wax is present in a small amount, filling the spaces between the tungsten disulfide nanosheet layers and the interior of the polyurethane film. It responds rapidly in the initial stage of friction, providing boundary lubrication and reducing the starting friction coefficient; while the tungsten disulfide nanosheets, due to their low interlayer shear strength, slide between layers during continuous friction, bearing and dispersing the frictional load. The appropriate amount of emulsifier ensures that the liquid wax is stably dispersed into tiny droplets in the aqueous system, preventing the liquid wax from agglomerating into large particles that leave voids after baking, thus maintaining the dense and intact film layer.
[0017] Furthermore, the nylon fiber is Cordura fiber.
[0018] Cordura fiber is produced using a special spinning process, resulting in higher orientation and crystallinity than ordinary nylon, and superior fiber strength, abrasion resistance, and tear resistance. Heat shrinking treatment is also effective on Cordura fiber. The heat resistance of Cordura fiber is sufficient to withstand the temperatures of baking processes without degradation or performance decline. Its high strength is fully retained after polyester bonding, resulting in fabrics with high overall strength, fewer tears, abrasion resistance, and resistance to deformation.
[0019] Furthermore, the heat shrinking treatment involves boiling in water at 95℃~100℃ for 50min~60min.
[0020] These temperature and time parameters ensure that the Cordura fibers shrink evenly. If the heat shrinkage is incomplete, residual shrinkage will occur in the Cordura fibers during baking, and the dimensional changes will be frozen as the polyester cools and solidifies, resulting in wrinkles and dimensional deviations in the fabric.
[0021] Furthermore, the baking process is carried out at a temperature of 120℃~140℃ for a time of 5min~10min.
[0022] The baking process, with its set temperature range and duration, partially melts the polyester fibers. The baking temperature, exceeding the melting point of polyester, allows the dispersed polyester fibers within the yarn to fully soften and flow within a specified time, forming effective bonding points at fiber intersections. Simultaneously, this temperature is significantly lower than the melting temperature of nylon fibers and the thermal degradation temperature of cotton fibers, affecting only the polyester component without damaging the inherent properties of nylon and cotton fibers. Since nylon fibers have already undergone heat shrinkage treatment, they remain morphologically stable under these dry heat conditions, without additional shrinkage, and the overall dimensions of the fabric no longer change. The melt bonding of the polyester fibers occurs on a dimensionally stable matrix with fully released stress. After the bonding points cool and solidify, the stable fiber network structure obtained through the low-shrinkage treatment is firmly locked, preventing easy slippage between fibers. If the temperature is too high or the time too long, excessive melting and flow of the polyester can cause large-area adhesion between fibers, resulting in a stiff feel, and may also cause excessive evaporation or migration of liquid wax in the padding coating, weakening its lubrication and wear-resistant properties.
[0023] Secondly, this application provides a wear-resistant and non-deformable fabric, made by the wear-resistant and non-deformable fabric manufacturing method described in the first aspect.
[0024] The beneficial effects of this invention are as follows: First, the nylon fibers are made smooth. During blending, the untreated cotton fibers ensure tight cohesion between the fibers. After weaving, the alkali treatment makes the cotton fibers smooth as well. The internal stress accumulated during spinning and weaving can be greatly eliminated by the slippage of the smooth fibers during the low-shrinkage treatment. Then, a coating with nano-sheet tungsten disulfide and liquid wax is applied, which makes the fabric more slippery and wear-resistant. Finally, baking partially melts the polyester fibers and binds the yarn fibers, ensuring the strength of the fabric. The modified nylon has been heat-shrinked beforehand, and its shape and structure are stable during baking. The final fabric has a low shrinkage rate, a stable shrinkage rate, and is not easily deformed. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions of the embodiments of this disclosure are described clearly and completely below. Obviously, the described embodiments are only some, not all, of the embodiments of this disclosure. All other embodiments obtained by those skilled in the art based on the described embodiments of this disclosure without creative effort are within the scope of protection of this invention.
[0026] It should be understood that, without conflict, any and all embodiments of the present invention can be combined with technical features of any other embodiment or multiple other embodiments to obtain other embodiments. The present invention includes such combinations to obtain other embodiments.
[0027] In this specification, groups and their substituents may be selected by those skilled in the art to provide stable structural moieties and compounds. When a substituent is described by a conventional chemical formula written from left to right, the substituent also includes chemically equivalent substituents obtained when the structural formula is written from right to left.
[0028] Unless otherwise specified, all technical and scientific terms used herein have the standard meaning in the field to which the claimed subject matter pertains. Where multiple definitions exist for a term, the definition herein shall prevail.
[0029] In existing technologies, there are also cases of enhancing the abrasion resistance of fabrics through coatings. However, this usually involves adding abrasion-resistant substances, such as abrasive powder, to the coating. Although this can improve abrasion resistance, the abrasion-resistant substances have large particles, which can easily cause the coating surface to crack after long-term use. Furthermore, abrasive powder is also uncomfortable when it comes into contact with the skin.
[0030] This application provides a method for manufacturing a wear-resistant and non-deformable fabric, the steps of which include: S1: Modified nylon is obtained by soaking nylon fibers that have undergone heat shrinkage treatment in a fiber lubricant.
[0031] S2: The first yarn is obtained by mixing cotton fiber, modified nylon fiber and polyester fiber with a melting point of 90℃~120℃ and spinning them together.
[0032] S3: Weave the fabric blank using the first yarn.
[0033] S4: Perform finishing on the fabric to obtain a wear-resistant and non-deformable fabric.
[0034] The finishing processes include: alkali treatment, low shrinkage treatment, padding treatment, and baking treatment.
[0035] The padding solution used in the padding process contains nano-sheet tungsten disulfide, waterborne polyurethane, liquid wax, and emulsifier.
[0036] Specifically, the nylon fibers are first heat-shrinked by boiling in water at 95-100℃ for 50-60 minutes, followed by drying. This heat-shrinking treatment stabilizes the fiber morphology, effectively reducing dimensional changes in the fabric caused by heat deformation of the nylon fibers in subsequent processes. This treatment effectively maintains the fabric's stability. Then, the nylon fibers are treated with a fiber lubricant (POLYFIN501) to obtain modified nylon fibers (which are then cut into segments for easy blending).
[0037] Cotton fiber, modified nylon fiber, and low-melting-point polyester fiber are mixed and then spun (including opening, carding, drawing, roving, spinning, etc.) to obtain the first yarn. The surface of the low-melting-point polyester fiber is also relatively smooth. In the spinning process, the modified nylon fiber can avoid the problem of large single yarn torque due to high friction during the processing of the fiber, reduce the internal stress of the fiber in the yarn, and thus improve the dimensional stability of the yarn.
[0038] The first yarn obtained is used as warp and weft yarns, interwoven to form a fabric, and then finished off the machine.
[0039] The sorting process includes: Tensoring: The tenter frame belt is overfed by 25%–35%, and the machine speed is 50m / min–60m / min. After tentering, the gaps between the warp and weft yarns in the fabric are increased, which is beneficial for the next processing step.
[0040] Alkali treatment: Baumé degree 16 Bé~18 Bé, treatment time 15-25 min. After alkali treatment, the cotton fiber will change its shape, shrink, the radial cross section of the fiber will become round and the fiber surface will become relatively smooth, thereby enhancing the stability of the fabric structure.
[0041] Low-shrinkage treatment: The fabric undergoes a low-tension water washing process in an overflow machine at a temperature of 50-60℃ for 20-30 minutes. During this process, the fabric experiences minimal stress and can freely shrink in the overflow machine, eliminating some of the internal stress in the fibers. This allows for slight fiber transfer within the fabric, resulting in a more stable yarn state.
[0042] Padding treatment: First, prepare the treatment solution, which includes the following raw materials by weight: 15-25 parts of nano-flake tungsten disulfide dispersion, 40-60 parts of waterborne polyurethane resin, 5-8 parts of liquid wax (Dongguan Enke Chemical Co., Ltd. hydrophilic liquid wax AAG-42), and 3-5 parts of emulsifier (Guangdong Huana Chemical Co., Ltd.). The liquid wax can adhere to the fiber surface and provide lubrication. For the waterborne polyurethane, soft aliphatic polyurethane (Guangzhou Ruilin New Materials Co., Ltd.) is preferred, as it has good film-forming properties, is soft, and has good elongation and resilience.
[0043] The nano-sheet tungsten disulfide dispersion comprises the following raw materials by weight: 10-18 parts tungsten disulfide powder, 6-16 parts dispersant, 60-80 parts N,N-dimethylformamide, and 3-5 parts PVA (Guangzhou Zhonggao Chemical Co., Ltd.). These raw materials are mixed and ultrasonically treated with an ultrasonic power of 300-500W for 5-8 hours to obtain the nano-sheet tungsten disulfide dispersion.
[0044] N,N-Dimethylformamide is used as a stripping agent. Adding a small amount of PVA (polyvinyl alcohol) can reduce the volatilization rate of N,N-dimethylformamide and form a uniform film layer to encapsulate the stripped tungsten disulfide nanosheets. The steric hindrance effect is used to prevent them from re-aggregating, thereby obtaining a more stable dispersion.
[0045] The exfoliated nano-sheet tungsten disulfide has a layered structure with relatively weak interlayer bonding, resulting in low shear strength and excellent lubrication and friction reduction. It also provides better elasticity, a softer feel, and better bending resistance compared to abrasive powder when used in lightweight fabrics. A non-ionic aqueous dispersant (such as those available from Huangshan Zhonghao New Materials Co., Ltd.) is preferred as the dispersant. This dispersant improves the steric hindrance between the dispersions, preventing the tungsten disulfide powder from re-agglomerating and resulting in a more stable sheet-like structure.
[0046] After impregnation, a thin and elastic protective film is attached to the fiber surface, which can effectively reduce the friction of the fiber surface, making the fiber surface smoother and greatly reducing the coefficient of friction of the fabric surface.
[0047] The preferred nylon fiber is Cordura fiber. Compared with traditional nylon fiber, Cordura fiber has far superior strength, abrasion resistance and tear resistance. Furthermore, after heat shrinking treatment, the morphological structure of Cordura fiber is more stable. Combined with the effect of tungsten disulfide, the fabric has better abrasion resistance and bending resistance.
[0048] Baking treatment: Temperature 120-140℃, treatment time 5-10 minutes. Because the yarn contains low-melting-point fibers, the baking process causes partial melting of these fibers, creating a bonding effect that stabilizes the yarn, increases fabric strength, and improves tear resistance. Baking also solidifies the padding solution, forming a protective layer on the fiber surface, improving lubrication and abrasion resistance. Cordura fibers, having previously undergone heat shrinkage and being in a stable state, show minimal deformation during baking.
[0049] The finishing process significantly improves the fabric's abrasion resistance and reduces the probability of twisting due to internal stress in the yarn, ensuring the fabric's dimensional stability and preventing fiber transfer.
[0050] Example 1 The first yarn composition consists of 40% cotton fiber, 35% modified nylon fiber, and 25% polyester fiber. The modified nylon fiber is Cordura, which has undergone heat shrinking and fiber lubrication treatment. Spinning yields the 10S first yarn of Example 1.
[0051] The first yarn is woven into a fabric blank, and the finishing process after it comes off the machine includes: alkali treatment, low shrinkage treatment, padding treatment, and baking treatment, to obtain the fabric of Example 1.
[0052] Example 2 The first yarn composition consists of 30% cotton fiber, 40% modified nylon fiber, and 30% polyester fiber. The modified nylon fiber is Cordura that has undergone heat shrinking and fiber lubrication treatment. Spinning yields the 10S first yarn of Example 2.
[0053] The first yarn is woven into a fabric blank, and the finishing process after it comes off the machine includes: stretching treatment, alkali treatment, shrinkage reduction treatment, padding treatment, and baking treatment, to obtain the fabric of Example 2.
[0054] Comparative Example 1 The first yarn composition consists of 40% cotton fiber, 40% nylon fiber, and 20% polyester fiber. Spinning yields a 10S first yarn, similar to Comparison 1.
[0055] The first yarn is woven into a fabric blank, and the finishing process after it comes off the machine includes: padding treatment and baking treatment, to obtain the fabric of Comparative Example 1.
[0056] Comparative Example 2 The fabric blank after Example 2 was not finished after being removed from the machine and used as Comparative Example 2.
[0057] Comparative Example 3 The first yarn composition consists of 40% cotton fiber, 30% modified nylon fiber, and 30% polyester fiber. The modified nylon fiber is Cordura, which has undergone heat shrinking and fiber lubrication treatment. Spinning yields the 10S first yarn of Comparative Example 3.
[0058] The first yarn is woven into a fabric blank, and the finishing processes after it comes off the machine include: stretching treatment, alkali treatment, shrinkage reduction treatment, and baking treatment, to obtain the fabric of Comparative Example 3.
[0059] The following tests were performed on each embodiment and comparative example: Abrasion resistance was tested using Martindale, according to standard GB / T 21196.2-2007.
[0060] The breaking strength of the fabric was measured according to GB / T 3923.1-2013 Textiles - Tensile Properties of Fabrics - Part 1: Determination of Breaking Strength and Elongation at Break - Strip Method.
[0061] The YG821L fabric style tester was used to test the coefficient of friction of the fabric surface.
[0062] The results are shown in the table below:
[0063] This application employs a series of processes, including nylon pre-shrinkage, cotton fiber alkali smoothing, low-shrinkage stress release, synergistic lubrication coating of nano-tungsten disulfide and liquid wax, and low-melting-point polyester melt bonding, to significantly reduce the fabric's coefficient of friction, greatly improve its abrasion resistance, and substantially enhance its tensile strength. Compared to unmodified and uncoated fabrics, this invention exhibits significant advantages in abrasion resistance, tear resistance, and structural stability. The low-shrinkage treatment effectively eliminates internal fiber stress, and the melt-bonded polyester fixes a stable configuration, ensuring dimensional stability and resistance to deformation. It balances abrasion resistance, strength, and shape retention, making it suitable for lightweight, abrasion-resistant clothing.
[0064] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, material, or characteristic described in connection with the embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0065] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A method for manufacturing a wear-resistant and non-deformable fabric, characterized in that the steps include... include: Modified nylon is obtained by soaking heat-shrinkable nylon fibers in a fiber lubricant. The first yarn is obtained by mixing cotton fiber, modified nylon fiber and polyester fiber with a melting point of 90℃~120℃ and spinning them together. Weave the fabric blank using the first yarn; The fabric is then finished to obtain the wear-resistant and non-deformable fabric. The finishing processes include: alkali treatment, low shrinkage treatment, padding treatment, and baking treatment; The padding solution used in the padding process contains nano-sheet tungsten disulfide, waterborne polyurethane, liquid wax, and emulsifier.
2. The method for manufacturing a wear-resistant and non-deformable fabric according to claim 1, characterized in that, In the mixed spinning step, the raw materials include 30%~40% cotton fiber, 30%~40% modified nylon fiber, and 20%~30% polyester fiber.
3. The method for manufacturing a wear-resistant and non-deformable fabric according to claim 1, characterized in that, In the alkali treatment step, the Baume degree of the alkali solution is 16 Bé to 18 Bé, and the treatment time is 15 min to 25 min.
4. The method for manufacturing a wear-resistant and non-deformable fabric according to claim 1, characterized in that, Prior to the alkali treatment, the finishing process also includes a tenter frame treatment, which requires that the tenter frame belt be overfed by 25% to 35% and the machine speed be 50m / min to 60m / min.
5. The method for manufacturing a wear-resistant and non-deformable fabric according to claim 1, characterized in that, The shrinkage treatment is carried out in an overflow machine at a temperature of 50℃~60℃ for 20min~30min.
6. The method for manufacturing a wear-resistant and non-deformable fabric according to claim 1, characterized in that, The dispersed phase of the padding liquid contains, by mass, 15 to 25 parts of nano-sheet tungsten disulfide dispersion, 40 to 60 parts of the aqueous polyurethane, 5 to 8 parts of the liquid wax, and 3 to 5 parts of the emulsifier. The preparation steps of the nano-sheet tungsten disulfide dispersion include: taking 60 to 80 parts by mass of N,N-dimethylformamide as the continuous phase of the nano-sheet tungsten disulfide dispersion, adding 3 to 5 parts of polyvinyl alcohol, 10 to 18 parts of tungsten disulfide powder, and 6 to 16 parts of dispersant, mixing and ultrasonically treating to obtain the nano-sheet tungsten disulfide dispersion.
7. The method for manufacturing a wear-resistant and non-deformable fabric according to claim 1, characterized in that, The nylon fiber is Cordura fiber.
8. The method for manufacturing a wear-resistant and non-deformable fabric according to claim 7, characterized in that, The heat shrinking treatment involves boiling in water at 95℃~100℃ for 50 to 60 minutes.
9. The method for manufacturing a wear-resistant and non-deformable fabric according to claim 1, characterized in that, The baking process is carried out at a temperature of 120℃~140℃ for 5min~10min.
10. A wear-resistant and non-deformable fabric, characterized in that, Made by the method of manufacturing a wear-resistant and non-deformable fabric as described in any one of claims 1 to 9.