A production process for high flame retardant polyester fabric

By preparing bridging agents and grafting agents, and modifying polyester fabrics, nitrogen, phosphorus, and boron elements are introduced to form a branched long-chain structure. This solves the problems of complex equipment and weak bonding force in the flame retardant modification method of polyester fabrics, and achieves improved flame retardant performance and mechanical strength, thus expanding the application fields.

CN123063997APending Publication Date: 2026-11-10LIXIN COUNTY WANYUE TEXTILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611579742.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing flame-retardant modification methods for polyester fabrics have problems such as high equipment requirements, complex processes, impact on physical and mechanical properties, weak bonding force between post-treatment flame retardants and fibers, and poor durability.

Method used

A bridging agent was prepared by using γ-glycidyl etheroxypropyltrimethoxysilane, rancid acid, and chromium 2-ethylhexanoate, and then reacted with aluminum chloride and dimethylphosphonic acid to prepare a grafting agent. Combined with ultraviolet irradiation reaction, the polyester fabric was modified to introduce nitrogen, phosphorus, and boron elements, forming a branched long-chain structure, which enhanced the flame retardant and mechanical properties.

Benefits of technology

The prepared polyester fabric has excellent flame retardant properties and good mechanical strength, which solves the shortcomings of existing flame retardant modification methods and expands the application of polyester fabric in fire protection, military, aviation and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of fabric technology, specifically to a production process for a high flame-retardant polyester fabric. The process includes: pre-treatment of the polyester fabric with alkaline etching; then introducing phosphorus-containing reactive groups onto the polyester surface using a bridging agent; finally, grafting a silicon- and boron-containing grafting agent onto the polyester fabric under ultraviolet irradiation using the bridging agent. The bridging agent is prepared by reacting γ-glycidyl etheroxypropyltrimethoxysilane, rancid acid, and dimethylphosphonic acid, etc.; the grafting agent is prepared by reacting 3-mercaptopropyltrimethoxysilane with trimethoxyborane, etc. The polyester fabric produced by this invention not only has excellent flame-retardant properties but also good mechanical strength, effectively ensuring its quality and showing promising application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fabric technology, specifically to a production process for a high flame-retardant polyester fabric. Background Technology

[0002] Polyester, or polyethylene terephthalate (PET) fiber, is widely used in clothing, home textiles, and industrial textiles due to its excellent mechanical properties, chemical resistance, dimensional stability, and low price. However, polyester is a flammable fiber, and during combustion, it produces severe molten dripping, which can easily ignite other materials and cause a rapid spread of fire. This greatly limits the application of polyester in fields with strict requirements for flame retardant properties, such as fire fighting, military, and aerospace.

[0003] Therefore, flame-retardant modification of polyester fabrics to impart excellent flame-retardant and anti-dripping properties is of significant practical importance. Existing flame-retardant modification methods for polyester mainly include blending, copolymerization, and finishing. Blending and copolymerization methods require sophisticated equipment, involve complex processes, and may affect the original physical and mechanical properties of the fiber. While finishing methods are simple to operate, they generally suffer from weak bonding between the flame retardant and the fiber, poor durability, and problems such as easy migration and precipitation of the flame retardant during use.

[0004] Based on the above, the present invention provides a production process for high flame retardant polyester fabric, aiming to solve the technical problems mentioned above. Summary of the Invention

[0005] The purpose of this invention is to provide a production process for high flame retardant polyester fabric. The polyester fabric produced by this invention not only has excellent flame retardant properties, but also has good mechanical strength, effectively ensuring its quality and having good application prospects.

[0006] A production process for a high flame-retardant polyester fabric includes the following steps: The first step is to clean the surface of the polyester fabric. After cleaning, the polyester fabric is immersed in an alkaline solution at 30-50℃ for 40-60 minutes, and then rolled and dried to obtain the pretreated polyester fabric. The second step involves uniformly dispersing the pretreated polyester fabric in an ethanol aqueous solution with a volume concentration of 75-85 wt%, then adding a bridging agent with a mass of 0.6-1.2 times that of the pretreated polyester fabric. After reacting at 40-60℃ for 3-5 hours, the pretreated polyester fabric is filtered out, cleaned, and then vacuum dried at 70-80℃ to obtain the modified polyester fabric. Step 3: Disperse the modified polyester fabric evenly in tetrahydrofuran at a dosage ratio of 60-100 g / L, then add the grafting agent and initiator, and carry out the ultraviolet irradiation reaction for 2-3 hours under nitrogen protection. After the reaction is completed, filter out the modified polyester fabric, wash it with water, and then roll it dry under a pressure of 0.05-0.2 MPa. After drying, the high flame retardant polyester fabric is obtained. The mass ratio of grafting agent, modified polyester fabric and initiator is 0.6-1:1:0.02-0.04.

[0007] Furthermore, the specific operation of the cleaning process is as follows: ultrasonically clean the polyester fabric in deionized water for 30-40 minutes, then remove it and dry it at 80-100℃.

[0008] Furthermore, the alkaline solution is an inorganic alkaline aqueous solution with a concentration of 5-10 wt%, and the inorganic alkaline is either sodium hydroxide or potassium hydroxide.

[0009] Furthermore, the bridging agent is prepared as follows: Step 1: Under stirring conditions, γ-glycidoxypropyltrimethoxysilane, rancid acid, and chromium 2-ethylhexanoate are added to toluene. After reacting at 70-80℃ for 3-6 hours, the product is cooled to room temperature and filtered. The toluene in the filtrate is evaporated and recovered to obtain the intermediate product. The mass ratio of rancid acid, γ-glycidoxypropyltrimethoxysilane, and chromium 2-ethylhexanoate is 1:1.2-1.5:0.05-0.08, and the ratio of rancid acid to toluene is 50-60 g / L. Step 2: Under stirring conditions, add the intermediate product, aluminum chloride, and dimethylphosphonic acid to DMF. After reacting at 100-110℃ for 6-8 hours, cool the product to room temperature and filter. Evaporate and recover the DMF from the filtrate to obtain the modifier. The mass ratio of the intermediate product, aluminum chloride, and dimethylphosphonic acid is 1:0.3-0.4:0.2-0.3, and the ratio of dimethylphosphonic acid to DMF is 100-150 g / L.

[0010] Furthermore, the preparation method of the grafting agent is as follows: Under nitrogen protection, 3-mercaptopropyltrimethoxysilane, trimethoxyborane, deionized water and 4-methylbenzenesulfonic acid are added to the reactor in a weight ratio of 20-25:10-15:4-5:0.04-0.06 while stirring. After refluxing at 65-75℃ for 5-8 hours, under nitrogen protection, a mixed component with a volume of 2-3 times that of 3-mercaptopropyltriethoxysilane is added to the obtained product component. After refluxing at 70-90℃ for 6-10 hours, the reaction product is subjected to vacuum distillation. The crude product is washed with toluene to remove insoluble matter, and then evaporated and recovered by vacuum distillation. Finally, it is vacuum dried at 60-80℃ to obtain the grafting agent.

[0011] Furthermore, the mixed components are composed of trimethylsilane chloride, propanol and 1,4-epoxybutane in a volume ratio of 2-4:2:1.

[0012] Furthermore, the rolling pressure in the first step is 0.08-0.2 MPa, the drying temperature is 90-110℃, and the drying time is 40-80 min.

[0013] Furthermore, the drying temperature in the third step is 80-100℃, and the drying time is 50-90 minutes.

[0014] Furthermore, the initiator is benzoin dimethyl ether, and the rolling pressure in the third step is 0.05-0.15 MPa.

[0015] Furthermore, the wavelength of the ultraviolet irradiation reaction is 365 nm, and the light intensity is 90-110 mW / cm². 2 .

[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention uses 3-mercaptopropyltrimethoxysilane, trimethoxyborane, 4-methylbenzenesulfonic acid, 3-mercaptopropyltriethoxysilane, and trimethylsilane chloride as raw materials to prepare a grafting agent containing the reactive mercapto group through a chemical reaction. The prepared grafting agent has a large molecular weight and numerous branched structures, and its molecular chain contains silicon and boron elements. This gives the prepared grafting agent not only excellent reactivity but also a good synergistic flame retardant effect.

[0017] 2. This invention uses γ-glycidyl etheroxypropyltrimethoxysilane, rancid acid, and chromium 2-ethylhexanoate as raw materials to prepare an intermediate product through a ring-opening reaction. Then, using the intermediate product, aluminum chloride, and dimethylphosphonic acid as raw materials, a bridging agent is prepared through an esterification reaction. Alkali treatment can etch the surface of polyester fibers, increasing their specific surface area and reactive sites. The prepared bridging agent not only serves as a bridge connecting the polyester fabric and the modifier, but its molecular chain also contains phosphorus-containing groups with flame-retardant properties. When polyester fabric is dispersed in an ethanol-water solution and the bridging agent is added, the hydrolyzed bridging agent molecular chain can chemically react with the hydroxyl groups on the surface of the pretreated polyester fabric to form bonds, thus obtaining modified polyester fabric. The modified polyester fabric was then uniformly dispersed in tetrahydrofuran, followed by the addition of a grafting agent and initiator. Under the action of the initiator, the grafting agent reacted chemically with the unsaturated bonds at the free ends of the bridging agent molecules to form bonds, ultimately successfully "grafting" the grafting agent onto the modified polyester fabric. After washing, rolling, and drying, the finished polyester fabric was obtained. Due to the synergistic effect of the bridging agent and modifier, the prepared polyester fabric contains nitrogen, phosphorus, and boron elements. These three elements work synergistically to achieve a good flame-retardant effect. Furthermore, the branched long-chain structure introduced after the reaction of the bridging agent and grafting agent intertwines with the polyester fibers, further improving the mechanical properties of the polyester fabric.

[0018] In summary, the polyester fabric products produced by this invention not only have excellent flame retardant properties, but also good mechanical strength, effectively ensuring their quality and showing good application prospects. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0020] Example 1 A production process for a high flame-retardant polyester fabric includes the following steps: The first step is to clean the surface of the polyester fabric. After cleaning, the polyester fabric is immersed in an alkaline solution at 30°C for 60 minutes, and then subjected to rolling and drying to obtain the pretreated polyester fabric. The alkaline solution used is a 5wt% sodium hydroxide aqueous solution. The rolling pressure is 0.08MPa, the drying temperature is 90°C, and the drying time is 80 minutes. The second step is to uniformly disperse the pretreated polyester fabric in an ethanol aqueous solution with a volume concentration of 75wt%, and then add a bridging agent with a mass of 0.6 times that of the pretreated polyester fabric. After reacting at 40℃ for 5 hours, filter out the pretreated polyester fabric, clean it, and then vacuum dry it at 70℃ to obtain the modified polyester fabric. Step 3: The modified polyester fabric is evenly dispersed in tetrahydrofuran at a dosage ratio of 60 g / L. Then, the grafting agent and initiator are added, and the mixture is subjected to ultraviolet irradiation for 2 hours under nitrogen protection. After the reaction is complete, the modified polyester fabric is filtered out, washed with water, and then rolled dry under a pressure of 0.05 MPa. After further drying, the high flame-retardant polyester fabric is obtained. The mass ratio of grafting agent, modified polyester fabric, and initiator is 0.6:1:0.02; the drying temperature is 80℃, and the drying time is 90 min; the initiator is benzoin dimethyl ether, and the rolling pressure in step 3 is 0.05 MPa; the wavelength of the ultraviolet irradiation reaction is 365 nm, and the light intensity is 90 mW / cm². 2 .

[0021] The specific cleaning procedure is as follows: After ultrasonically cleaning the polyester fabric in deionized water for 30 minutes, remove it and then dry it at 80℃.

[0022] The preparation method of the bridging agent is as follows: Step 1: Under stirring conditions, γ-glycidoxypropyltrimethoxysilane, rancid acid, and chromium 2-ethylhexanoate were added to toluene. After reacting at 70°C for 6 hours, the product was cooled to room temperature and filtered. The toluene in the filtrate was evaporated and recovered to obtain the intermediate product. The mass ratio of rancid acid, γ-glycidoxypropyltrimethoxysilane, and chromium 2-ethylhexanoate was 1:1.2:0.05, and the ratio of rancid acid to toluene was 50 g / L. The temperature for evaporating toluene was 60°C, the rotation speed was 150 rpm, and the vacuum degree was 0.1 MPa. Step 2: Under stirring conditions, the intermediate product, aluminum chloride, and dimethylphosphonic acid are added to DMF. After reacting at 100℃ for 8 hours, the product is cooled to room temperature and filtered. The DMF in the filtrate is evaporated and recovered to obtain the modifier. The mass ratio of the intermediate product, aluminum chloride, and dimethylphosphonic acid is 1:0.3:0.2, and the ratio of dimethylphosphonic acid to DMF is 100 g / L. The temperature for evaporating DMF is 80℃, the rotation speed is 150 rpm, and the vacuum degree is 30 mbar.

[0023] The preparation method of the grafting agent is as follows: Under nitrogen protection, 3-mercaptopropyltrimethoxysilane, trimethoxyborane, deionized water and 4-methylbenzenesulfonic acid are added to the reactor in a weight ratio of 20:10:4:0.04 while stirring. After refluxing at 65°C for 8 hours, under nitrogen protection, a mixed component with a volume twice that of 3-mercaptopropyltriethoxysilane is added to the obtained product component. After refluxing at 70°C for 10 hours, the reaction product is subjected to vacuum distillation. The crude product is washed with toluene to remove insoluble matter, and then evaporated and recovered by vacuum distillation. Finally, it is dried under vacuum at 60°C to obtain the grafting agent. The mixed components are composed of trimethylsilane chloride, propanol and 1,4-epoxybutane in a volume ratio of 2:2:1.

[0024] Example 2 A production process for a high flame-retardant polyester fabric includes the following steps: The first step is to clean the surface of the polyester fabric. After cleaning, the polyester fabric is immersed in an alkaline solution at 40°C for 50 minutes, and then subjected to rolling and drying to obtain the pretreated polyester fabric. The alkaline solution used is an 8wt% potassium hydroxide aqueous solution. The rolling pressure is 0.1MPa, the drying temperature is 100°C, and the drying time is 60 minutes. The second step is to uniformly disperse the pretreated polyester fabric in an ethanol aqueous solution with a volume concentration of 80wt%, then add a bridging agent of the same mass as the pretreated polyester fabric, react at 50℃ for 4 hours, filter out the pretreated polyester fabric, clean it, and then vacuum dry it at 75℃ to obtain the modified polyester fabric. Step 3: The modified polyester fabric is evenly dispersed in tetrahydrofuran at a dosage ratio of 80 g / L. Then, the grafting agent and initiator are added, and the mixture is subjected to ultraviolet irradiation for 2 hours under nitrogen protection. After the reaction is complete, the modified polyester fabric is filtered out, washed with water, and then rolled dry under a pressure of 0.1 MPa. Following this, it undergoes further drying to obtain the high flame-retardant polyester fabric. The mass ratio of grafting agent, modified polyester fabric, and initiator is 0.8:1:0.03; the drying temperature is 90℃, and the drying time is 70 min; the initiator is benzoin dimethyl ether, and the rolling pressure is 0.1 MPa; the wavelength of the ultraviolet irradiation reaction is 365 nm, and the light intensity is 100 mW / cm². 2 ; The specific cleaning procedure is as follows: After ultrasonically cleaning the polyester fabric in deionized water for 35 minutes, remove it and then dry it at 90℃.

[0025] The preparation method of the bridging agent is as follows: Step 1: Under stirring conditions, γ-glycidoxypropyltrimethoxysilane, rancid acid, and chromium 2-ethylhexanoate were added to toluene. After reacting at 75°C for 5 hours, the product was cooled to room temperature and filtered. The toluene in the filtrate was evaporated and recovered to obtain the intermediate product. The mass ratio of rancid acid, γ-glycidoxypropyltrimethoxysilane, and chromium 2-ethylhexanoate was 1:1.3:0.06, and the ratio of rancid acid to toluene was 55 g / L. The temperature for evaporating toluene was 60°C, the rotation speed was 150 rpm, and the vacuum degree was 0.1 MPa. Step 2: Under stirring conditions, the intermediate product, aluminum chloride, and dimethylphosphonic acid are added to DMF. After reacting at 100℃ for 7 hours, the product is cooled to room temperature and filtered. The DMF in the filtrate is evaporated and recovered to obtain the modifier. The mass ratio of the intermediate product, aluminum chloride, and dimethylphosphonic acid is 1:0.3:0.3, and the ratio of dimethylphosphonic acid to DMF is 120 g / L. The temperature for evaporating DMF is 80℃, the rotation speed is 150 rpm, and the vacuum degree is 30 mbar.

[0026] The preparation method of the grafting agent is as follows: Under nitrogen protection, 3-mercaptopropyltrimethoxysilane, trimethoxyborane, deionized water and 4-methylbenzenesulfonic acid are added to the reactor in a weight ratio of 20:12:4:0.05 while stirring. After refluxing at 70°C for 6 hours, under nitrogen protection, a mixed component with a volume of 3 times that of 3-mercaptopropyltriethoxysilane is added to the obtained product component. After refluxing at 80°C for 8 hours, the reaction product is subjected to vacuum distillation. The crude product is washed with toluene to remove insoluble matter, and then evaporated and recovered by vacuum distillation. Finally, it is dried under vacuum at 70°C to obtain the grafting agent.

[0027] The mixed components are composed of trimethylsilane chloride, propanol and 1,4-epoxybutane in a volume ratio of 3:2:1.

[0028] Example 3 A production process for a high flame-retardant polyester fabric includes the following steps: The first step is to clean the surface of the polyester fabric. After cleaning, the polyester fabric is immersed in an alkaline solution at 50°C for 40 minutes, and then subjected to rolling and drying to obtain the pretreated polyester fabric. The alkaline solution used is a 10wt% sodium hydroxide aqueous solution. The rolling pressure is 0.2MPa, the drying temperature is 110°C, and the drying time is 40 minutes. The second step is to uniformly disperse the pretreated polyester fabric in an ethanol aqueous solution with a volume concentration of 85wt%, and then add a bridging agent with a mass of 1.2 times that of the pretreated polyester fabric. After reacting at 60℃ for 3 hours, filter out the pretreated polyester fabric, clean it, and then vacuum dry it at 80℃ to obtain the modified polyester fabric. Step 3: The modified polyester fabric is evenly dispersed in tetrahydrofuran at a dosage ratio of 100 g / L. Then, the grafting agent and initiator are added, and the mixture is subjected to ultraviolet irradiation for 3 hours under nitrogen protection. After the reaction is complete, the modified polyester fabric is filtered out, washed with water, and then rolled dry under a pressure of 0.2 MPa. After further drying, the high flame-retardant polyester fabric is obtained. The mass ratio of grafting agent, modified polyester fabric, and initiator is 1:1:0.04; the drying temperature is 100℃, and the drying time is 50 min; the initiator is benzoin dimethyl ether, and the rolling pressure in step 3 is 0.15 MPa; the wavelength of the ultraviolet irradiation reaction is 365 nm, and the light intensity is 110 mW / cm². 2 .

[0029] The specific cleaning procedure is as follows: After ultrasonically cleaning the polyester fabric in deionized water for 40 minutes, remove it and then dry it at 100℃.

[0030] The preparation method of the bridging agent is as follows: Step 1: Under stirring conditions, γ-glycidoxypropyltrimethoxysilane, rancid acid, and chromium 2-ethylhexanoate were added to toluene. After reacting at 80°C for 3 hours, the product was cooled to room temperature and filtered. The toluene in the filtrate was evaporated and recovered to obtain the intermediate product. The mass ratio of rancid acid, γ-glycidoxypropyltrimethoxysilane, and chromium 2-ethylhexanoate was 1:1.5:0.08, and the ratio of rancid acid to toluene was 60 g / L. The temperature for evaporating toluene was 60°C, the rotation speed was 150 rpm, and the vacuum degree was 0.1 MPa. Step 2: Under stirring conditions, the intermediate product, aluminum chloride, and dimethylphosphonic acid are added to DMF. After reacting at 110℃ for 6 hours, the product is cooled to room temperature and filtered. The DMF in the filtrate is evaporated and recovered to obtain the modifier. The mass ratio of the intermediate product, aluminum chloride, and dimethylphosphonic acid is 1:0.4:0.3, and the ratio of dimethylphosphonic acid to DMF is 150 g / L. The temperature, rotation speed, and vacuum degree for evaporating DMF are 80℃, 150 rpm, and 30 mbar.

[0031] The preparation method of the grafting agent is as follows: Under nitrogen protection, 3-mercaptopropyltrimethoxysilane, trimethoxyborane, deionized water and 4-methylbenzenesulfonic acid are added to the reactor in a weight ratio of 25:15:5:0.06 while stirring. After refluxing at 75°C for 5 hours, under nitrogen protection, a mixed component with a volume of 3 times that of 3-mercaptopropyltriethoxysilane is added to the obtained product component. After refluxing at 90°C for 6 hours, the reaction product is subjected to vacuum distillation. The crude product is washed with toluene to remove insoluble matter, and then evaporated and recovered by vacuum distillation. Finally, it is dried under vacuum at 80°C to obtain the grafting agent. The mixed components are composed of trimethylsilane chloride, propanol and 1,4-epoxybutane in a volume ratio of 4:2:1.

[0032] Comparative Example 1: The difference between this comparative example and Example 1 is that the polyester fabric produced in this comparative example has not undergone the third step of treatment, that is, the fabric product produced in this comparative example is the modified polyester fabric obtained in the second step.

[0033] Comparative Example 2: The difference between this comparative example and Example 1 is that an equal amount of vinyl silane coupling agent (specifically vinyltrimethoxysilane) is used instead of the bridging agent in this comparative example, and the steps are the same as in Example 1.

[0034] Performance testing The relevant properties of the high flame-retardant polyester fabrics produced in Examples 1-3 and Comparative Examples 1-2 were tested as follows, and the test data are recorded in the table below: 1. Flame Retardant Performance Test: The limiting oxygen index (LOI) of each high flame-retardant polyester fabric sample was tested according to GB / T 5454-1997 "Textiles - Test for Burning Performance - Oxygen Index Method". Simultaneously, the polyester fabric was subjected to standard washing according to the washing method of GB / T 20944.1-2007 "Test for Color Fastness to Wash". After 20 washes, the LIO of each high flame-retardant polyester fabric sample was tested. Additionally, the UL-94 vertical flammability rating (tested using a CZF-5 vertical flammability tester) was used to assist in the assessment.

[0035] 2. Bursting Strength Test: Following GB / T 19976-2005 "Determination of Bursting Strength of Textiles - Steel Ball Method", the high flame-retardant polyester fabric samples produced in Examples 1-3 and Comparative Examples 1-2, as well as high flame-retardant polyester fabric samples that had not undergone the first, second, and third steps of treatment (i.e., polyester fabrics that only underwent cleaning treatment, and these were used as a control group; their bursting strength was tested to be 316 N), were tested at 110 g / m². 2 Breakthrough strength test.

[0036] 3. Tensile Strength Test: According to GB / T3923-1997 standard, the high flame-retardant polyester fabric samples produced in Examples 1-3 and Comparative Examples 1-2, as well as the high flame-retardant polyester fabric samples without the first, second, and third steps of treatment (i.e., polyester fabrics that only underwent cleaning treatment, and these were used as a control group, with a tensile strength of 768 / N), were cut into 150×50mm pieces. 2 The breaking strength of the remaining high flame-retardant polyester fabric samples was measured using an electronic fabric strength tester at a rate of 100 mm / min.

[0037] The test data obtained above is recorded in the table below:

[0038] By comparing and analyzing the relevant data in the table, it can be seen that the high flame-retardant polyester fabric produced by this invention not only has excellent flame-retardant properties but also good mechanical strength, effectively ensuring its quality. This indicates that the production process for the high flame-retardant polyester fabric provided by this invention has a broader market prospect and is more suitable for promotion.

[0039] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0040] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A production process for a high flame-retardant polyester fabric, characterized in that, Includes the following steps: The first step is to clean the surface of the polyester fabric. After cleaning, the polyester fabric is immersed in an alkaline solution at 30-50℃ for 40-60 minutes, and then rolled and dried to obtain the pretreated polyester fabric. The second step involves uniformly dispersing the pretreated polyester fabric in an ethanol aqueous solution with a volume concentration of 75-85 wt%, then adding a bridging agent with a mass of 0.6-1.2 times that of the pretreated polyester fabric. After reacting at 40-60℃ for 3-5 hours, the pretreated polyester fabric is filtered out, cleaned, and then vacuum dried at 70-80℃ to obtain the modified polyester fabric. Step 3: Disperse the modified polyester fabric evenly in tetrahydrofuran at a dosage ratio of 60-100 g / L, then add the grafting agent and initiator, and carry out the ultraviolet irradiation reaction for 2-3 hours under nitrogen protection. After the reaction is completed, filter out the modified polyester fabric, wash it with water, and then roll it dry under a pressure of 0.05-0.2 MPa. After drying, the high flame retardant polyester fabric is obtained. The mass ratio of grafting agent, modified polyester fabric and initiator is 0.6-1:1:0.02-0.

04.

2. The production process of a high flame-retardant polyester fabric according to claim 1, characterized in that: The specific cleaning process is as follows: ultrasonically clean the polyester fabric in deionized water for 30-40 minutes, then remove it and dry it at 80-100℃.

3. The production process of a high flame-retardant polyester fabric according to claim 1, characterized in that: The alkaline solution is an inorganic alkaline aqueous solution with a concentration of 5-10 wt%, and the inorganic alkaline is either sodium hydroxide or potassium hydroxide.

4. The production process of a high flame-retardant polyester fabric according to claim 1, characterized in that, The bridging agent is prepared as follows: Step 1: Under stirring conditions, γ-glycidoxypropyltrimethoxysilane, rancid acid, and chromium 2-ethylhexanoate are added to toluene. After reacting at 70-80℃ for 3-6 hours, the product is cooled to room temperature and filtered. The toluene in the filtrate is evaporated and recovered to obtain the intermediate product. The mass ratio of rancid acid, γ-glycidoxypropyltrimethoxysilane, and chromium 2-ethylhexanoate is 1:1.2-1.5:0.05-0.08, and the ratio of rancid acid to toluene is 50-60 g / L. Step 2: Under stirring conditions, add the intermediate product, aluminum chloride, and dimethylphosphonic acid to DMF. After reacting at 100-110℃ for 6-8 hours, cool the product to room temperature and filter. Evaporate and recover the DMF from the filtrate to obtain the modifier. The mass ratio of the intermediate product, aluminum chloride, and dimethylphosphonic acid is 1:0.3-0.4:0.2-0.3, and the ratio of dimethylphosphonic acid to DMF is 100-150 g / L.

5. The production process of a high flame-retardant polyester fabric according to claim 1, characterized in that, The grafting agent is prepared as follows: Under nitrogen protection, 3-mercaptopropyltrimethoxysilane, trimethoxyborane, deionized water, and 4-methylbenzenesulfonic acid are added to a reactor at a weight ratio of 20-25:10-15:4-5:0.04-0.06 while stirring. After refluxing at 65-75℃ for 5-8 hours, under nitrogen protection, a mixed component with a volume of 2-3 times that of 3-mercaptopropyltriethoxysilane is added to the obtained product component. After refluxing at 70-90℃ for 6-10 hours, the reaction product is subjected to vacuum distillation. The crude product is washed with toluene to remove insoluble matter, and then distilled again under vacuum to remove and recover toluene. Finally, it is vacuum dried at 60-80℃ to obtain the grafting agent.

6. The production process of a high flame-retardant polyester fabric according to claim 5, characterized in that: The mixture is composed of trimethylsilane chloride, propanol and 1,4-epoxybutane in a volume ratio of 2-4:2:

1.

7. The production process of a high flame-retardant polyester fabric according to claim 1, characterized in that: The rolling pressure in the first step is 0.08-0.2 MPa, the drying temperature is 90-110℃, and the drying time is 40-80 min.

8. The production process of a high flame-retardant polyester fabric according to claim 1, characterized in that, The drying temperature in the third step is 80-100℃, and the drying time is 50-90 minutes.

9. The production process of a high flame-retardant polyester fabric according to claim 1, characterized in that: The initiator is benzoin dimethyl ether, and the rolling pressure in the third step is 0.05-0.15 MPa.

10. The production process of a high flame-retardant polyester fabric according to claim 1, characterized in that: The wavelength of the ultraviolet irradiation reaction is 365 nm, and the light intensity is 90-110 mW / cm². 2 .