A regenerated cellulose fiber with tunable surface hydrophobic groups, its preparation method and application
By introducing hydrophobic groups onto the surface of regenerated cellulose fibers, the heterogeneous modification method solves the problems of high surface energy and hydrophilicity limitations of regenerated cellulose fibers, achieving improved surface hydrophobicity and performance enhancement, and is suitable for a variety of high-end material applications.
Patent Information
- Application Number
- CN202611333847.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-10
AI Technical Summary
The high surface energy and strong hydrophilicity of regenerated cellulose fibers limit their application in high-end waterproof fabrics, oil-proof and barrier materials, medical protective drapes, functional oil-water separation filters, and special filter materials. Existing integral bulk modification methods damage the fiber structure and make it difficult to precisely control surface properties.
Hydrophobic groups were introduced onto the surface of regenerated cellulose fibers using a heterogeneous reaction. Nucleophilic substitution reactions were then carried out through spraying with an activator solution and impregnation with a mixed solvent to prepare regenerated cellulose fibers with tunable surface hydrophobic groups. A hydrophobic layer was constructed only on the surface, while retaining the internal hydrophilic and mechanical properties.
It improves the hydrophobicity of regenerated cellulose fiber surface, enhances waterproof and oil-proof properties, and maintains the original structure and mechanical properties of the fiber. It is suitable for waterproof fabrics, oil-proof isolation materials, medical protective sheets and oil-water separation filter materials, especially smoke filter rods, and has a sensory quality superior to traditional materials.
Smart Images

Figure CN123064003A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of surface modification technology of regenerated cellulose fibers, and relates to a regenerated cellulose fiber with tunable surface hydrophobic groups, its preparation method and application. Background Technology
[0002] Regenerated cellulose fibers are a type of fiber material produced from natural plant cellulose (such as wood pulp and cotton linters) through processes such as dissolution and spinning. These fibers retain the excellent moisture absorption, breathability, and biodegradability of natural cellulose fibers, while also achieving strength and dimensional stability close to synthetic fibers through process control. They have broad application prospects in textiles, apparel, medical and health applications, filtration and separation, and protective materials. However, the densely distributed hydroxyl groups (-OH) on the molecular chains of regenerated cellulose fibers endow them with high surface energy, strong hydrophilicity, and relatively weak hydrophobicity. This inherent property limits their application in high-end waterproof fabrics, oil-repellent materials, medical protective drapes, functional oil-water separation filtration, and special filter materials (such as cigarette filter rods). Therefore, improving the hydrophobicity of fibers while maintaining their original morphology and mechanical properties is a key technological direction for expanding their application scenarios and increasing their added value. Summary of the Invention
[0003] Therefore, it is necessary to provide a regenerated cellulose fiber with tunable surface hydrophobic groups, its preparation method, and its application.
[0004] In some embodiments, a method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups is provided, comprising the following steps:
[0005] An activator solution is sprayed onto the surface of regenerated cellulose fibers and allowed to stand for activation reaction to prepare surface-activated regenerated cellulose fibers. The activator solution contains an activator and a solvent, wherein the solvent includes an aqueous ethanol solution.
[0006] The surface-activated regenerated cellulose fibers are impregnated in a mixed solvent to carry out a nucleophilic substitution reaction. The reaction is terminated with an acid aqueous solution, and the fibers are washed and dried to prepare the regenerated cellulose fibers with tunable surface hydrophobic groups. The mixed solvent contains propylene oxide and chloromethane.
[0007] In some embodiments, the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups satisfies one or more of the following conditions:
[0008] (1) The activator includes at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide and benzyltrimethylammonium hydroxide;
[0009] (2) The volume fraction of ethanol in the aqueous ethanol solution is 50% to 95%; optionally, the volume fraction of ethanol in the aqueous ethanol solution is 60% to 80%.
[0010] (3) The activator in the activator solution has a mass percentage of 2% to 12%, and optionally, the activator in the activator solution has a mass percentage of 4% to 10%;
[0011] (4) The mass ratio of the mixed solvent to the regenerated cellulose fiber is (15~20):1;
[0012] (5) In the mixed solvent, the volume ratio of propylene oxide to chloromethane is (1~8):(9~2).
[0013] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the mass of the activator in the activator solution is 5% to 20% of the mass of the regenerated cellulose fibers. Optionally, the mass of the activator in the activator solution is 5% to 10% of the mass of the regenerated cellulose fibers.
[0014] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the activation reaction time is 5 min to 30 min, and the activation reaction temperature is 5 °C to 30 °C.
[0015] In some embodiments, the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups satisfies one or more of the following conditions:
[0016] (1) The surface-activated regenerated cellulose fibers are impregnated in a mixed solvent to carry out a nucleophilic substitution reaction. The reaction temperature is 25℃~65℃ and the reaction time is 0.5h~2.5h; optionally, the reaction temperature is 35℃~55℃ and the reaction time is 1.0h~2.0h.
[0017] (2) In the washing step, anhydrous ethanol and / or water are used for washing. The washing method includes repeated washing by suction filtration or centrifugation until the pH value of the filtrate is neutral.
[0018] (3) The acidic aqueous solution includes an acetic acid aqueous solution with a concentration of 10% (v / v) to 20% (v / v);
[0019] (4) The drying temperature is 50℃~80℃.
[0020] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the regenerated cellulose fibers are obtained by dissolving natural cellulose fibers in a solvent and then spinning them; optionally, the regenerated cellulose fibers include one or more of lyocell fibers, viscose fibers, and modal fibers.
[0021] In some embodiments, a regenerated cellulose fiber with tunable surface hydrophobic groups is provided, which is prepared by the aforementioned preparation method.
[0022] In some embodiments, the provided regenerated cellulose fibers with tunable surface hydrophobic groups satisfy one or both of the following conditions:
[0023] (1) The surface of the regenerated cellulose fiber with adjustable hydrophobic groups has hydroxypropyl and methyl groups, wherein the mass percentage of hydroxypropyl groups in the regenerated cellulose fiber with adjustable hydrophobic groups is 1% to 5%, and the mass percentage of methyl groups in the regenerated cellulose fiber with adjustable hydrophobic groups is 1% to 5%;
[0024] (2) The water contact angle of the regenerated cellulose fiber with adjustable surface hydrophobic groups is 100°~140°.
[0025] In some embodiments, the regenerated cellulose fibers with tunable surface hydrophobic groups are provided for use in the preparation of at least one of waterproof fabrics, oil-resistant materials, medical protective drapes, oil-water separation filter materials, and cigarette filter rods.
[0026] In some embodiments, a waterproof fabric, an oil-proof barrier material, a medical protective drape, an oil-water separation filter material, or a cigarette filter rod is provided, the raw materials for which include regenerated cellulose fibers with adjustable surface hydrophobic groups.
[0027] The provided method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups yields fibers with hydrophobic functional groups (e.g., methyl groups) on their surface, exhibiting excellent surface hydrophobicity. The method employs a heterogeneous reaction at the solid-liquid interface, where reagents only contact the surface hydroxyl groups. The fiber remains solid throughout the modification process, with only the surface reacting, eliminating the need to dissolve the fiber in a solvent system. This reduces solvent costs and eliminates the complexity of solvent recovery processes. It avoids the defects of complete dissolution and remodeling of cellulose, which can damage the original appearance and structure of fibers, sheets, and films, while preserving the original hydrophilic and mechanical properties of the cellulose's internal structure. The surface hydrophobic modification process is simplified, resulting in lower energy and reagent consumption. The surface hydrophobicity can be flexibly controlled by switching the type and quantity of hydrophilic and hydrophobic groups, adjusting the hydrophobicity level and interfacial compatibility as needed, enabling precise control and customization of the surface hydrophobic groups. The surface modification process produces less waste liquid and has a lower pollution load.
[0028] The regenerated cellulose fibers with tunable surface hydrophobic groups prepared by the method of this invention possess excellent surface hydrophobicity. For example, in one embodiment, the modified lyocell fiber has a surface hydroxypropyl content of up to 4.11%, a methyl content of up to 4.86%, a water contact angle of up to 139.7°, and a water vapor transmission coefficient of 8.96 g·cm / (cm²). 2 The tar content (·s·Pa) of the modified lyocell fiber was higher than that of the unmodified blank sample, indicating that the modified lyocell fiber surface contains a certain amount of hydrophobic functional groups and has good surface hydrophobicity. When the modified lyocell fiber was used to prepare tobacco filter rods, the smoke filtration performance of the lyocell fiber tobacco filter rods was comparable to that of cellulose acetate, indicating that it has good tar reduction and harm reduction functions. Furthermore, its sensory quality score was significantly higher than that of cellulose acetate filter rods, demonstrating great application potential. Attached Figure Description
[0029] To more clearly illustrate the technical solutions in the embodiments and examples of this application, and to more completely understand this application and its beneficial effects, the accompanying drawings used in the description of the embodiments or examples will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of this application. Those skilled in the art can obtain other drawings based on these drawings without any creative effort.
[0030] Figure 1 Microscopic morphology of unmodified lyocell fiber surface;
[0031] Figure 2 The image shows the surface microstructure of the modified Lyocell fiber obtained in Example 1.
[0032] Figure 3 Infrared spectra of modified lyocell fibers, where “Control” is “blank control”, i.e., “unmodified lyocell fibers of Comparative Example 1”; “low” is “low dose group”, i.e., “modified lyocell fibers of Example 1”; “mid” is “medium dose group”, i.e., “modified lyocell fibers of Example 3”; “high” is “high dose group”, i.e., “modified lyocell fibers of Example 5”; “Transmittance” is “transmittance”; and “Wavenumber” is “wavenumber”. Detailed Implementation
[0033] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Preferred embodiments of the invention are shown in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the invention.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0035] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings:
[0036] The terms "and / or," "or / and," and "and / or" as used in this application encompass any one of two or more related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected using at least two conjunctions selected from "and / or," "or / and," and "and / or," it should be understood that in this application, the technical solution undoubtedly includes solutions connected by "logical AND," and also undoubtedly includes solutions connected by "logical OR." For example, "A and / or B" includes three parallel solutions: A, B, and "a combination of A and B."
[0037] In this application, the terms "multiple", "various", "multiple times", "multi-dimensional", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more than or equal to two.
[0038] The terms “combinations thereof,” “any combination thereof,” and “any combination thereof” as used in this application include all suitable combinations of any two or more of the listed items.
[0039] In this application, terms such as "further," "even further," and "particularly" are used to describe purposes and indicate differences in content, but should not be construed as limiting the scope of protection of this application.
[0040] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, each "optional" entry shall be independent.
[0041] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.
[0042] In this application, numerical intervals (i.e., numerical ranges) are involved. Unless otherwise specified, the selected numerical distributions within the aforementioned numerical intervals are considered continuous and include the two endpoints (i.e., the minimum and maximum values) of the numerical range, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints. In this document, this is equivalent to directly listing every integer. For example, if t is an integer selected from 1 to 10, it means that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10. Furthermore, when multiple ranges are provided to describe features or characteristics, these ranges can be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges to which they are included.
[0043] Unless otherwise specified, the temperature parameters in this application are permitted to be either constant-temperature treatment or variations within a certain temperature range. It should be understood that the constant-temperature treatment allows temperature fluctuations within the precision range of the instrument control, such as ±5℃, ±4℃, ±3℃, ±2℃, or ±1℃.
[0044] In this application, % (w / w) and wt% both represent weight percentage, % (v / v) refers to volume percentage, and % (w / v) refers to mass-volume percentage.
[0045] In this application, "room temperature" generally refers to 5℃~30℃, and more preferably 25±5℃.
[0046] Traditional chemical modification of cellulose often employs a bulk modification approach, where cellulose is completely dissolved in a homogeneous reaction system, allowing the molecular chains to fully extend and introducing hydrophobic ester or ether groups at the molecular level. This method significantly reduces hydrophilicity and blocks hydroxyl activity, inhibiting fiber fibrillation and improving dimensional stability. Under appropriate processing conditions, the crystalline structure changes minimally, and mechanical properties are well-preserved. The resulting materials can be used in waterproof fabrics, membranes, and medical protective materials. However, this strategy has significant limitations: First, complete dissolution and remodeling of cellulose can damage the original appearance of the fiber, sheet, or membrane, making it difficult to maintain the structural integrity of the molded product. Second, bulk homogeneous grafting can easily lead to excessive and uneven substitution, causing fiber embrittlement and uneven reaction. Third, because hydrophobic groups are widely distributed along the molecular chain, the resulting material has a generally high degree of hydrophobicity, making it difficult to precisely achieve the functional zoning effect of "hydrophobic surface, hydrophilic interior," thus failing to meet the application requirements for precise control of surface properties. Current methods mostly involve homogeneous reactions for bulk modification, which are costly in terms of reagents, damage to fiber morphology, difficulty in controlling hydrophilicity, and challenging in hydrophobic modification. Furthermore, the preparation processes are cumbersome and complex. Therefore, this application is submitted.
[0047] In some embodiments, a method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups is provided, comprising the following steps:
[0048] An activator solution is sprayed onto the surface of regenerated cellulose fibers and allowed to stand for an activation reaction to prepare surface-activated regenerated cellulose fibers. The activator solution contains an activator and a solvent, the solvent of which includes an aqueous ethanol solution.
[0049] Surface-activated regenerated cellulose fibers were impregnated in a mixed solvent to carry out a nucleophilic substitution reaction. The reaction was terminated with an acid aqueous solution, and the fibers were washed and dried to prepare regenerated cellulose fibers with tunable surface hydrophobic groups. The mixed solvent contained propylene oxide and chloromethane.
[0050] In some embodiments, the activator in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups includes at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and benzyltrimethylammonium hydroxide. Using aliphatic esters such as isotridecyl stearate, sorbitan monooleate, or polyoxyethylene sorbitan monooleate as activators will result in a decrease in the water contact angle of the prepared product.
[0051] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the volume fraction of ethanol in the aqueous ethanol solution is 50% to 95%, for example, 50%, 60%, 70%, 80%, 90%, 95%, etc., or it can be a range composed of any two of the aforementioned values; optionally, the volume fraction of ethanol in the aqueous ethanol solution is 60% to 80%, for example, 60%, 65%, 70%, 75%, 80%, etc., or it can be a range composed of any two of the aforementioned values.
[0052] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the mass percentage of the activator in the activator solution can be 2% to 12%, or 4% to 10%, for example, 2%, 4%, 6%, 8%, 10%, 12%, etc., or any range of the aforementioned two values.
[0053] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the mass ratio of the mixed solvent to the regenerated cellulose fibers is (15~20):1, for example, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, etc., or it can be a range of any two of the aforementioned ratios.
[0054] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the volume ratio of propylene oxide to chloromethane in the mixed solvent is (1~8):(9~2), for example, 1:9, 2:8, 3:7, 4:6, 5:5, 6:4, 7:3, 8:2, etc., or it can be a range of any two of the aforementioned ratios.
[0055] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the mass of the activator in the activator solution is 5% to 20% of the mass of the regenerated cellulose fibers, or it can be 5% to 10%, for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc., or it can be a range composed of any two of the aforementioned values.
[0056] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the activation reaction time is 5 min to 30 min, and the activation reaction temperature is 5 °C to 30 °C. For example, the activation reaction time can be 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, etc., and the activation reaction temperature can be 5 °C, 10 °C, 15 °C, 20 °C, 25 °C, 30 °C, etc., and the values of each parameter can also be ranges composed of any two of the aforementioned values.
[0057] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the nucleophilic substitution reaction step of impregnating the surface-activated regenerated cellulose fibers in a mixed solvent can be carried out at a temperature of 25°C to 65°C or 35°C to 55°C, and at a reaction time of 0.5h to 2.5h or 1.0h to 2.0h. For example, the reaction temperature can be 25°C, 35°C, 45°C, 55°C, 65°C, etc., and the reaction time can be 0.5h, 1.0h, 1.5h, 2.0h, 2.5h, etc., and the values of each parameter can also be ranges composed of any two of the aforementioned values.
[0058] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the washing step involves washing with anhydrous ethanol and / or water, and the washing method includes repeated washing by vacuum filtration or centrifugation until the pH of the filtrate is neutral.
[0059] In some embodiments, the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups includes an aqueous solution of acetic acid with a concentration of 10% (v / v) to 20% (v / v), such as 10% (v / v), 12% (v / v), 14% (v / v), 16% (v / v), 18% (v / v), 20% (v / v), etc., or any range of two of the aforementioned values.
[0060] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the drying temperature is 50°C to 80°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc., or it can be a range composed of any two of the aforementioned values.
[0061] In some embodiments, in the method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, the regenerated cellulose fibers are obtained by dissolving natural cellulose fibers in a solvent and then spinning them; in some embodiments, the regenerated cellulose fibers include one or more of lyocell fibers, viscose fibers, and modal fibers.
[0062] In some embodiments, a regenerated cellulose fiber with tunable surface hydrophobic groups is provided, which is prepared by the aforementioned preparation method.
[0063] Traditional hydrophobic modification of cellulose uses homogeneous reactions, which can damage the original morphology of the fiber; for example, the resulting hydrophobic modified cellulose is in powder form. However, the regenerated cellulose fiber with tunable surface hydrophobic groups prepared in this application does not alter the overall structure and surface morphology compared to unmodified regenerated cellulose fiber, and it exhibits improved hydrophobicity and moisture permeability.
[0064] In some embodiments, the regenerated cellulose fiber with tunable hydrophobic groups provided has hydroxypropyl and methyl groups on its surface. The mass percentage of hydroxypropyl groups in the regenerated cellulose fiber with tunable hydrophobic groups is 1% to 5%, for example, 1%, 2%, 3%, 4%, 5%, etc., or it can be any range of two of the aforementioned values. The mass percentage of methyl groups in the regenerated cellulose fiber with tunable hydrophobic groups is 1% to 5%, for example, 1%, 2%, 3%, 4%, 5%, etc., or it can be any range of two of the aforementioned values.
[0065] In some embodiments, the water contact angle of the regenerated cellulose fiber with adjustable surface hydrophobic groups is 100°~140°, for example, 100°, 110°, 120°, 130°, 140°, etc., or it can be a range composed of any two of the aforementioned values.
[0066] In some embodiments, the aforementioned regenerated cellulose fibers with tunable surface hydrophobic groups are provided for use in the preparation of at least one of waterproof fabrics, oil-proof and insulating materials, medical protective drapes, oil-water separation filter materials, and cigarette filter rods.
[0067] In some embodiments, a waterproof fabric, an oil-proof barrier material, a medical protective drape, an oil-water separation filter material, or a cigarette filter rod is provided, the raw materials for which include the aforementioned regenerated cellulose fibers with tunable surface hydrophobic groups.
[0068] In some embodiments, a cigarette filter rod is provided, the raw material of which includes the aforementioned regenerated cellulose fibers with tunable surface hydrophobic groups.
[0069] In some embodiments, the provided cigarette filter rod includes regenerated cellulose fibers with adjustable surface hydrophobic groups and filter rod forming paper that wraps the regenerated cellulose fibers with adjustable surface hydrophobic groups.
[0070] The provided method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups employs surface modification to hydrophobically modify the regenerated cellulose fibers. Surface modification allows for targeted control of interfacial hydrophobic groups, resulting in greater precision. A hydrophobic layer is constructed only on the surface, while the original hydrophilic and mechanical properties of cellulose are retained internally. Surface hydrophobicity control allows for flexible switching of the type and quantity of hydrophilic and hydrophobic groups, adjusting the hydrophobicity level and interfacial compatibility as needed.
[0071] The following are specific embodiments. They are intended to provide a more detailed description of this application to help those skilled in the art and researchers better understand it. The technical conditions described do not constitute any limitation on this application. Any modifications made within the scope of the claims of this application are protected by the claims.
[0072] Unless otherwise stated, all raw materials and reagents used in the following examples are commercially available or can be prepared by known methods. Experimental methods not specifying particular conditions in the examples were performed under conventional conditions, such as those described in literature, books, or methods recommended by the manufacturer.
[0073] The concentration of dilute acetic acid used in the following examples is 10% (v / v).
[0074] Example 1
[0075] Lyocell fiber nonwoven fabric was cut into 5 cm × 5 cm square samples. A 2 wt% tetramethylammonium hydroxide solution (activator solution) was prepared using a 50% (v / v) ethanol aqueous solution as the solvent. The mass of the tetramethylammonium hydroxide solution sprayed was controlled to be 5% of the mass of the Lyocell fiber nonwoven fabric. The tetramethylammonium hydroxide solution was sprayed onto the surface of the Lyocell fiber nonwoven fabric and allowed to react in a sealed environment at room temperature for 10 min. After the activation reaction was completed, the fabric was placed in a distillation flask equipped with a reflux condenser, and a measured amount of a mixed solvent of propylene oxide and chloromethane was added, wherein the volume ratio of propylene oxide to chloromethane was 1:9, and the mass ratio of propylene oxide to nonwoven fabric was 15:1. The reaction was carried out at 50℃ for 1.5 hours. After the reaction was completed and cooled, the reaction was terminated with dilute acetic acid solution. The fabric was taken out, filtered, and thoroughly washed with deionized water until the pH of the filtrate was neutral. After being completely washed, it was dried in an oven at 60℃ to constant weight to obtain a surface-modified lyocell fiber sample, which was then sealed and stored.
[0076] Example 2
[0077] Lyocell fiber nonwoven fabric was cut into 5 cm × 5 cm square samples. A 4 wt% tetraethylammonium hydroxide solution (activator solution) was prepared using a 60% (v / v) ethanol aqueous solution as the solvent. The mass of the tetraethylammonium hydroxide sprayed was controlled to be 10% of the mass of the Lyocell fiber nonwoven fabric. The tetraethylammonium hydroxide solution was sprayed onto the surface of the Lyocell fiber nonwoven fabric and allowed to react in a sealed environment at room temperature for 15 min. After the activation reaction was completed, the fabric was placed in a distillation flask equipped with a reflux condenser, and a measured amount of a mixed solvent of propylene oxide and chloromethane was added, wherein the volume ratio of propylene oxide to chloromethane was 3:7, and the mass ratio of propylene oxide to nonwoven fabric was 20:1. The reaction was carried out at 50℃ for 1.5 hours. After the reaction was completed and cooled, the reaction was terminated with dilute acetic acid solution. The fabric was taken out, filtered, and thoroughly washed with deionized water until the pH of the filtrate was neutral. After being completely washed, it was dried in an oven at 60℃ to constant weight to obtain a surface-modified lyocell fiber sample, which was then sealed and stored.
[0078] Example 3
[0079] Lyocell fiber nonwoven fabric was cut into 5 cm × 5 cm square samples. A 6 wt% tetrapropylammonium hydroxide solution (activator solution) was prepared using a 75% (v / v) ethanol aqueous solution as the solvent. The mass of the tetrapropylammonium hydroxide solution to be sprayed was controlled to be 15% of the mass of the lyocell fiber nonwoven fabric. The tetrapropylammonium hydroxide solution was sprayed onto the surface of the lyocell fiber nonwoven fabric and allowed to react in a sealed environment at room temperature for 15 min. After the activation reaction was completed, the fabric was placed in a distillation flask equipped with a reflux condenser, and a measured amount of a mixed solvent of propylene oxide and chloromethane was added, wherein the volume ratio of propylene oxide to chloromethane was 5:5, and the mass ratio of propylene oxide to nonwoven fabric was 18:1. The reaction was carried out at 55℃ for 1.0 h. After the reaction was completed and cooled, the reaction was terminated with dilute acetic acid solution. The fabric was taken out, filtered, and washed thoroughly with deionized water until the pH of the filtrate was neutral. After being completely washed, it was dried in an oven at 60℃ to constant weight to obtain a surface-modified lyocell fiber sample, which was then sealed and stored.
[0080] Example 4
[0081] Lyocell fiber nonwoven fabric was cut into 5 cm × 5 cm square samples. An 8 wt% tetrabutylammonium hydroxide solution (activator solution) was prepared using an 80% (v / v) ethanol aqueous solution as the solvent. The mass of the tetrabutylammonium hydroxide solution was controlled to be 17% of the mass of the Lyocell fiber nonwoven fabric. The tetrabutylammonium hydroxide solution was sprayed onto the surface of the Lyocell fiber nonwoven fabric and allowed to react in a sealed environment at room temperature for 20 min. After the activation reaction was completed, the fabric was placed in a distillation flask equipped with a reflux condenser, and a measured amount of a mixed solvent of propylene oxide and chloromethane was added, wherein the volume ratio of propylene oxide to chloromethane was 7:3, and the mass ratio of propylene oxide to nonwoven fabric was 20:1. The reaction was carried out at 60℃ for 1.5 hours. After the reaction was completed and cooled, the reaction was terminated with dilute acetic acid solution. The fabric was taken out, filtered, and thoroughly washed with deionized water until the pH of the filtrate was neutral. After being completely washed, it was dried in an oven at 60℃ to constant weight to obtain a surface-modified lyocell fiber sample, which was then sealed and stored.
[0082] Example 5
[0083] Lyocell fiber nonwoven fabric was cut into 5 cm × 5 cm square samples. An 8 wt% benzyltrimethylammonium hydroxide solution (activator solution) was prepared using an 85% (v / v) ethanol aqueous solution as the solvent. The mass of the benzyltrimethylammonium hydroxide solution was controlled to be 20% of the mass of the lyocell fiber nonwoven fabric. The benzyltrimethylammonium hydroxide solution was sprayed onto the surface of the lyocell fiber nonwoven fabric and allowed to react in a sealed environment at room temperature for 25 min. After the activation reaction was completed, the fabric was placed in a distillation flask equipped with a reflux condenser, and a measured amount of a mixed solvent of propylene oxide and chloromethane was added, wherein the volume ratio of propylene oxide to chloromethane was 8:2, and the mass ratio of propylene oxide to nonwoven fabric was 20:1. The reaction was carried out at 65℃ for 2.0 h. After the reaction was completed and cooled, the reaction was terminated with dilute acetic acid solution. The fabric was taken out, filtered, and thoroughly washed with deionized water until the pH of the filtrate was neutral. After being completely washed, it was dried in an oven at 60℃ to constant weight to obtain a surface-modified lyocell fiber sample, which was then sealed and stored.
[0084] Comparative Example 1
[0085] Unmodified lyocell fiber was used as a blank control.
[0086] Performance testing
[0087] (1) Microscopic morphology detection
[0088] The surface microstructure of unmodified and surface-modified lyocell fiber samples was observed using a Hitachi S-4800 scanning electron microscope (SEM). Figure 1 It is unmodified Lyocell fiber. Figure 2 The sample is a surface-modified lyocell fiber obtained in Example 1. It can be seen that the overall structure and surface morphology of the surface-modified lyocell fiber sample remained unchanged, indicating that the heterogeneous surface hydrophobic modification method used in this application effectively controlled the hydrophobic groups on the fiber surface without damaging the fiber's bulk structure, resulting in lyocell fibers with improved hydrophobicity and moisture permeability.
[0089] (2) Test for hydroxypropyl and methyl content
[0090] The hydroxypropyl content in surface-modified lyocell fiber samples was determined using the spectrophotometric method specified in GB / T 40998-2021 "Determination of hydroxypropyl content in modified starch". The hydroxypropyl content is shown in Table 1.
[0091] The methyl content in the surface-modified lyocell fiber samples was determined using the method in GB 1886.256-2024, and the methyl content is shown in Table 1.
[0092] (3) Testing of hydrophobic properties
[0093] For the modified samples of Examples 1-5, the water contact angle of the samples was tested according to GB / T 42694-2023 "Detection and evaluation of the surface anti-wetting properties of textiles - contact angle and rolling angle method". Five different points were tested for each sample and the average value was taken as the test result. The contact angle of each sample is shown in Table 1.
[0094] (4) Water vapor permeability
[0095] For the modified samples of Examples 1-5, the water vapor permeability was tested using the pseudo-cup method according to GB 1037-2021. The water vapor permeability of each sample is shown in Table 1. The test results showed that the water vapor permeability coefficient of the modified lyocell fiber was higher than that of the unmodified lyocell fiber sample. This indicates that the surface hydrophobic modification improved the permeability of the lyocell fiber, which is beneficial for the transfer of aroma components in the smoke and thus improves the sensory quality of the cigarette.
[0096] Table 1 Performance Tests of Modified Lyocell Fibers
[0097]
[0098] As shown in Table 1, the test results indicate that, compared to the blank control in Comparative Example 1, the modified lyocell fibers exhibit significantly increased hydroxypropyl and methyl content, ranging from 1% to 5%. By adjusting the activation reaction conditions, such as the concentration of the activator, the amount of coating applied, the activation time, and the reaction temperature and time with the mixed solvent (a mixture of propylene oxide and chloromethane), precise control of the surface hydrophobic groups can be achieved. Compared to the blank sample, the modified lyocell fibers show significantly improved hydrophobic properties, with contact angles ranging from 100° to 140°. This demonstrates that the preparation method described in this invention, by introducing hydrophobic hydroxypropyl groups onto the fiber surface, achieves a superior hydrophobic modification effect.
[0099] (5) Analysis of mainstream cigarette smoke components
[0100] Using modified lyocell fiber and cellulose acetate from Examples 1-5 as raw materials, cigarette filter rods were prepared by a filter rod forming machine and then attached to cigarette segments to form cigarettes. The conventional chemical components of the cigarette smoke were tested according to GB / T19609-2004, GB / T23203.1-2013, GB / T23355-2009, and GB / T23356-2009. Sensory quality was evaluated according to GB 5606.4-2005 "Sensory Technical Requirements for Cigarettes Part 4" and YC / T 497-2014 "Sensory Evaluation Method for Chinese-style Cigarettes," and compared with cellulose acetate filter rods to evaluate the cigarette smoke filtration performance and sensory quality of the modified lyocell fiber. The total score for sensory quality is 100 points; a higher score indicates a better overall sensory quality of the cigarette. The test results are shown in Table 2.
[0101] Table 2. Cigarette smoke filtration performance of modified lyocell fiber
[0102]
[0103] As shown in Table 2, compared with cellulose acetate filter rods, the modified lyocell fiber filter rods of Examples 1-5 all exhibited significantly lower levels of major smoke components. This indicates that the modified lyocell fiber filter rods possess excellent adsorption, retention, and filtration capabilities for major smoke components, meeting the basic requirements for reducing tar and harm in cigarettes. Furthermore, the sensory quality scores of Examples 1-5 were all higher than those of cellulose acetate filter rods, indicating that the modified lyocell fiber filter rods are suitable for tobacco filter rods and have significant application potential.
[0104] (6) Structural characterization
[0105] For the samples of Examples 1, 3, and 5, structural analysis was performed using infrared spectroscopy, such as... Figure 3 As shown in the figure, compared with the blank control in Comparative Example 1, all three modified samples exhibited a methyl (-CH3) bending vibration peak (~1370 cm⁻¹). -1 ), ether bond (COC) stretching vibration peak (~1060 cm⁻¹) -1 Unmodified Lyocell fiber samples at 1370 cm⁻¹ -1 The absorption at 2960 cm⁻¹ is extremely weak, with no obvious characteristic peak. After modification, the peak intensity increases significantly in the low, medium, and high modification groups, and the peak shape gradually becomes sharper and clearer from a flat state. This is because the modification reaction grafts methyl-containing side chains onto the fiber. The bending vibrations of these newly added methyl groups produce obvious absorption signals, and the higher the degree of modification, the more methyl groups are grafted, and the higher the peak intensity. The change in this peak is related to the 2960 cm⁻¹. -1 The CH stretching vibration peaks corroborated each other, jointly proving the successful introduction of the alkyl side chain.
[0106] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0107] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention should be determined by the appended claims, and the specification and drawings can be used to interpret the content of the claims.
Claims
1. A method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups, characterized in that, Includes the following steps: An activator solution is sprayed onto the surface of regenerated cellulose fibers and allowed to stand for activation reaction to prepare surface-activated regenerated cellulose fibers. The activator solution contains an activator and a solvent, wherein the solvent includes an aqueous ethanol solution. The surface-activated regenerated cellulose fibers are impregnated in a mixed solvent to carry out a nucleophilic substitution reaction. The reaction is terminated with an acid aqueous solution, and the fibers are washed and dried to prepare the regenerated cellulose fibers with tunable surface hydrophobic groups. The mixed solvent contains propylene oxide and chloromethane.
2. The method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups according to claim 1, characterized in that, One or more of the following conditions must be met: (1) The activator includes at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide and benzyltrimethylammonium hydroxide; (2) The volume fraction of ethanol in the aqueous ethanol solution is 50% to 95%; optionally, the volume fraction of ethanol in the aqueous ethanol solution is 60% to 80%. (3) The activator in the activator solution has a mass percentage of 2% to 12%, and optionally, the activator in the activator solution has a mass percentage of 4% to 10%; (4) The mass ratio of the mixed solvent to the regenerated cellulose fiber is (15~20):1; (5) In the mixed solvent, the volume ratio of propylene oxide to chloromethane is (1~8):(9~2).
3. The method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups according to claim 1, characterized in that, The mass of the activator in the activator solution is 5% to 20% of the mass of the regenerated cellulose fiber. Optionally, the mass of the activator in the activator solution is 5% to 10% of the mass of the regenerated cellulose fiber.
4. The method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups according to any one of claims 1 to 3, characterized in that, The activation reaction time is 5 min to 30 min, and the activation reaction temperature is 5℃ to 30℃.
5. The method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups according to any one of claims 1 to 3, characterized in that, One or more of the following conditions must be met: (1) The surface-activated regenerated cellulose fibers are impregnated in a mixed solvent to carry out a nucleophilic substitution reaction. The reaction temperature is 25℃~65℃ and the reaction time is 0.5h~2.5h; optionally, the reaction temperature is 35℃~55℃ and the reaction time is 1.0h~2.0h. (2) In the washing step, anhydrous ethanol and / or water are used for washing. The washing method includes repeated washing by suction filtration or centrifugation until the pH value of the filtrate is neutral. (3) The acidic aqueous solution includes an acetic acid aqueous solution with a concentration of 10% (v / v) to 20% (v / v); (4) The drying temperature is 50℃~80℃.
6. The method for preparing regenerated cellulose fibers with tunable surface hydrophobic groups according to any one of claims 1 to 3, characterized in that, The regenerated cellulose fiber is obtained by dissolving natural cellulose fiber in a solvent and then spinning it; optionally, the regenerated cellulose fiber includes one or more of lyocell fiber, viscose fiber and modal fiber.
7. A regenerated cellulose fiber with tunable surface hydrophobic groups, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 6.
8. The regenerated cellulose fiber with tunable surface hydrophobic groups according to claim 7, characterized in that, One or both of the following conditions must be met: (1) The surface of the regenerated cellulose fiber with adjustable hydrophobic groups has hydroxypropyl and methyl groups, wherein the mass percentage of hydroxypropyl groups in the regenerated cellulose fiber with adjustable hydrophobic groups is 1% to 5%, and the mass percentage of methyl groups in the regenerated cellulose fiber with adjustable hydrophobic groups is 1% to 5%; (2) The water contact angle of the regenerated cellulose fiber with adjustable surface hydrophobic groups is 100°~140°.
9. The use of the regenerated cellulose fiber with tunable surface hydrophobic groups as described in claim 7 or 8 in the preparation of at least one of waterproof fabrics, oil-proof isolation materials, medical protective drapes, oil-water separation filter materials, and cigarette filter rods.
10. A waterproof fabric, oil-proof barrier material, medical protective sheet, oil-water separation filter material, or smoke filter rod, characterized in that, The raw materials for its preparation include regenerated cellulose fibers with tunable surface hydrophobic groups as described in claim 7 or 8.