Preparation method and application of high-load, water-washable quaternary ammonium salt-silica composite material
By employing a synergistic approach combining a two-step double-drop method and acidic nano-silica sol capture, the problems of low quaternary ammonium salt loading, high wastewater COD, and poor washability were solved, enabling the preparation of high-load, wash-resistant quaternary ammonium salt-silica composite materials suitable for high-efficiency antibacterial textile finishing.
Patent Information
- Application Number
- CN202611516637.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies suffer from limitations in quaternary ammonium salt loading, high wastewater treatment pressure, and insufficient textile adhesion and washability, resulting in poor antibacterial effects and difficulty in meeting the high requirements of textile applications.
A two-step double-drop method was adopted, combining excessive quaternary ammonium salt feeding with acidic nano-silica sol capture. By controlling the drop acceleration rate and stirring conditions, a dense composite structure was formed, which increased the quaternary ammonium salt loading and enhanced adhesion.
It significantly increases the quaternary ammonium salt loading to 28%-32%, reduces the COD value of wastewater to below 300mg/L, increases the number of water washes to more than 45, and significantly enhances antibacterial properties, making it suitable for industrial production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of antibacterial finishing materials for textiles, specifically relating to a method for preparing a high-load, washable quaternary ammonium salt-silica composite material and its application. Background Technology
[0002] Existing technologies have disclosed various preparation processes for quaternary ammonium salt-silica composite antibacterial materials. The core idea is to use a silicon source and a quaternary ammonium salt to prepare a composite antibacterial powder. This type of powder can achieve basic antibacterial and antifungal functions when used in textile finishing. Among them, conventional processes often use water glass (sodium silicate) as the silicon source, and generate a silica matrix through acidification treatment, while simultaneously loading quaternary ammonium salts (such as hexadecyltrimethylammonium chloride CTAC and hexadecyltrimethylammonium bromide CTAB), and obtain the finished product through subsequent separation, drying and other processes.
[0003] However, existing technologies and processes suffer from the following core pain points in actual industrial production, limiting product competitiveness and application scenarios: 1. Limited quaternary ammonium salt loading: During the formation of the silica matrix, the surface adsorption sites are limited, and the quaternary ammonium salt loading has a saturation limit (usually not exceeding 20%). If excessive quaternary ammonium salt is added, the uncoated free quaternary ammonium salt will be lost in large quantities during the washing process, failing to effectively improve the antibacterial activity of the product and causing raw material waste. 2. High wastewater treatment pressure: Free quaternary ammonium salt is a recalcitrant organic compound, and its large-scale loss into the washing wastewater leads to a sharp increase in the COD value of the wastewater (usually reaching over 800 mg / L), increasing environmental treatment costs and contradicting the green and low-carbon development trend of the dyeing and printing industry. 3. Textile adhesion and washability need improvement: Products prepared by existing technologies rely solely on the physical adsorption and bonding between the silica matrix and textile fibers. After drying, there is no significant anchoring effect, and the antibacterial components are easily detached after multiple washes. The number of washes is usually only 20-30, which is insufficient to meet the long-term use requirements of close-fitting textiles (such as underwear and towels). 4. Insufficient antibacterial long-term effect: In existing technology products, quaternary ammonium salts are only released through a single matrix. After long-term use or repeated washing, the encapsulation structure is easily damaged, and the quaternary ammonium salts are quickly lost, resulting in an excessively rapid decline in antibacterial effect.
[0004] Currently, most improvement solutions for increasing quaternary ammonium salt loading involve increasing the amount of quaternary ammonium salt added or optimizing the reaction pH, but none of these solutions address the core issue of free quaternary ammonium salt loss. Solutions for improving washability often involve adding fixatives during finishing, which is a complicated process that can affect the feel and absorbency of textiles, and cannot achieve simultaneous improvements in "loading capacity, washability, and environmental friendliness".
[0005] Therefore, there is an urgent need for an improvement solution that can address the above pain points, adapt to existing processes, and be easily industrialized. Summary of the Invention
[0006] This invention aims to at least partially solve one of the technical problems in related technologies. This invention provides a method for preparing a high-load, wash-resistant quaternary ammonium salt-silica composite material. This method is an improvement on existing processes, employing a two-step double-drop method that combines excessive quaternary ammonium salt feeding with the synergistic effect of acidic nano-silica sol capture. This significantly increases the quaternary ammonium salt loading to 28%~32%, improves wash resistance to over 45 cycles, and reduces wastewater COD to below 300mg / L. It is suitable for antibacterial finishing of textiles with high antibacterial efficiency, high wash resistance, and low environmental impact, and can be widely applied to antibacterial and antifungal modification of various textiles such as cotton, polyester, and blended fabrics.
[0007] Specifically, the present invention provides the following technical solution: The first aspect of the present invention provides a method for preparing a high-load water-resistant quaternary ammonium salt-silica composite material, comprising: (1) Provide a base mother liquor, wherein the base mother liquor comprises quaternary ammonium salt and water glass, and the mass ratio of quaternary ammonium salt to water glass in the base mother liquor is (1.2~1.5):10; (2) Add a first mixture and water glass to the base mother liquor. The first mixture includes dilute sulfuric acid and quaternary ammonium salt. The mass ratio of quaternary ammonium salt to dilute sulfuric acid in the first mixture is (1.8~2.5):50. React at a predetermined temperature and a predetermined stirring speed to obtain a composite gel. (3) The composite gel and acidic nano silica sol are mixed under stirring conditions for 20-40 minutes to obtain the composite material; (4) Filter, wash, dry and crush to obtain the high-load quaternary ammonium salt-silica composite material.
[0008] The method provided does not employ complex modifiers or post-processing techniques. It solves the three core pain points of low load capacity, wastewater pollution, and poor washability simultaneously through a simple synergistic feeding design. The technical route is simpler, lower in cost, and more practical, and has significant industrial application value and patent innovation.
[0009] According to an embodiment of the present invention, the loading of quaternary ammonium salt in the high-load quaternary ammonium salt-silica composite material is 22%~28%.
[0010] According to an embodiment of the present invention, the quaternary ammonium salt is composed of a cation and an anion; wherein the cation is selected from at least one of alkyltrimethylammonium ion, alkyldimethylbenzylammonium ion, and dialkyldimethylammonium ion, and the alkyl group is a C12-C16 long-chain alkyl group, preferably C12-C16. 12 Long-chain alkyl or C 16 Long-chain alkyl; the anion is selected from at least one of chloride ion, bromide ion, and iodide ion.
[0011] According to embodiments of the present invention, the quaternary ammonium salt may be selected from at least one of dodecyltrimethylammonium chloride (DTAC), dodecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride (CTAC), hexadecyltrimethylammonium bromide, dodecyl dimethyl benzyl ammonium chloride, hexadecyl dimethyl benzyl ammonium chloride, bis(dodecyl dimethyl ammonium chloride), bis(hexadecyl dimethyl ammonium chloride), dodecyltrimethylammonium iodide, hexadecyltrimethylammonium iodide, etc.
[0012] According to an embodiment of the present invention, the mass concentration of the dilute sulfuric acid is 2~5% w / w.
[0013] According to an embodiment of the present invention, the predetermined temperature is 25~35 degrees Celsius.
[0014] According to an embodiment of the present invention, the predetermined stirring speed is 500-600 r / min.
[0015] According to an embodiment of the present invention, the reaction is maintained at pH 2-3.
[0016] According to an embodiment of the present invention, the acidic nano-silica sol has a particle size of 10-20 nm and a solid content of 20%~30%.
[0017] According to an embodiment of the present invention, the amount of acidic nano-silica sol added is 12%-20% of the dry basis mass of the composite powder. In this invention, the amount of acidic nano-silica sol added is not arbitrarily determined, but is optimized based on the material balance results of the quaternary ammonium salt. Specifically, after the water glass acidification gelation and quaternary ammonium salt composite reaction are completed, in addition to the quaternary ammonium salt already embedded in the silica framework, a certain amount of free quaternary ammonium salt remains in the system. The actual loading of quaternary ammonium salt is determined by filtering, washing, and drying the gelation product; the difference between the total amount of quaternary ammonium salt added and the actual loading is the mass of free quaternary ammonium salt that can be lost during the washing process. Based on this loss, the minimum amount of acidic nano-silica sol required to effectively adsorb / capture this portion of free quaternary ammonium salt is calculated. Combined with the rheological properties and filtration performance of the gel system, the final determination of the acidic nano-silica sol addition range is 12%-20% of the dry basis mass of the composite powder. This range ensures that free quaternary ammonium salts are fully captured (wastewater COD≤300mg / L) without causing abnormal gel viscosity or filtration difficulties due to excessive silica sol, thus achieving a balance between performance and process feasibility.
[0018] According to an embodiment of the present invention, in step (3), the acidic silica sol is slowly added to the composite gel in batches, with each batch not exceeding 1 / 3 of the total amount, and the interval between each batch is at least 5 minutes.
[0019] According to an embodiment of the present invention, the water glass is an aqueous solution of sodium silicate with a modulus of 2.8 to 3.2.
[0020] A second aspect of the present invention provides a high-load, water-washable quaternary ammonium salt-silica composite material, obtained by the preparation method described in the first aspect of the present invention.
[0021] According to an embodiment of the present invention, the quaternary ammonium salt loading of the composite material is 28% to 32%, the wastewater COD value is ≤300 mg / L, and the number of water washes is ≥45 (antibacterial retention rate ≥80%).
[0022] The third aspect of the invention provides the use of the high-load, wash-resistant quaternary ammonium salt-silica composite material described in the first aspect in antibacterial finishing of textiles.
[0023] The beneficial effects achieved by this invention are at least as follows: The method provided by this invention, through the synergistic design of excessive quaternary ammonium salt feeding and acidic nano-silica sol capture, combined with the structural advantages of the two-step double-drop method, overcomes the limitations of existing technologies and achieves a triple improvement in raw material utilization, product performance, and environmental friendliness, as detailed below: (1) Breakthrough in quaternary ammonium salt loading, significantly improved antibacterial activity: The synergistic strategy of two-step double drop, quaternary ammonium salt excess and acidic nano silica sol capture provided by this invention increases the embedding amount by using the framework structure prepared by the two-step double drop method and captures free quaternary ammonium salt by acidic nano silica sol, thereby increasing the effective loading of quaternary ammonium salt to 28%-32%, breaking through the upper limit of loading saturation of a single gel; the antibacterial MIC (minimum inhibitory concentration) value of the product is optimized from <50ppm in the prior art to <25ppm, the antibacterial rate is increased by more than 40%, and the broad-spectrum antibacterial (bacteria, fungi) effect is better.
[0024] (2) Green and environmentally friendly, significantly reducing wastewater treatment costs: By capturing free quaternary ammonium salts through acidic nano silica sol, the loss of quaternary ammonium salts during the washing process is reduced by 60%-70%, the COD value of wastewater is reduced to below 300mg / L, and the environmental treatment cost is reduced by 30%-40%, which meets the requirements of green and low-carbon development in the printing and dyeing industry and solves the industry pain point of excessively high COD in existing process wastewater.
[0025] (3) Double-layer composite structure, double the adhesion and water resistance: The method of the present invention can form a double-layer structure in which silica gel is embedded with quaternary ammonium salt (as the core, playing a long-term sustained-release role) and acidic nano silica sol adsorbs quaternary ammonium salt (as the outer layer, realizing the anchoring and film formation role). After drying, the silanol of the outer silica sol dehydrates and condenses to form dense silicon-oxygen bonds, which not only realizes the stable agglomeration between composite particles, but also forms chemical bonds with the hydroxyl groups of textile fibers, thereby increasing the adhesion between the product and the fiber by more than 70%; the number of water washes is increased to 45-55 times, and the antibacterial retention rate is still more than 90% after 20 water washes, which is far superior to existing similar products.
[0026] (4) Strong process compatibility and easy industrialization: Based on the two-step double-drop method, only two additional steps are added: the addition of excess quaternary ammonium salt and the addition of acidic nano-sized silica sol. No new complex equipment is needed, and the original production process does not need to be overturned. The industrialization transformation is easy and cost-effective. At the same time, the number of water washings can be simplified, the production cycle can be shortened, and the production efficiency can be improved.
[0027] (5) Wider product application adaptability: The obtained product has better dispersibility. After grinding to D50 800nm-1.5μm, when used for textile padding, the fabric surface has no white spots and the hand feel is soft. It does not affect the original water absorption of textiles and can be widely used in intimate apparel, towels, home textiles and other scenarios with high requirements for water resistance and hand feel. Detailed Implementation
[0028] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0029] This invention solves the core problems of low quaternary ammonium salt loading, high wastewater COD, poor water washability, and insufficient adhesion in conventional one-pot or two-step double-drop methods by using a two-step double-drop method combined with the synergistic improvement of excessive quaternary ammonium salt feeding and acidic nano-silica sol capture, without changing the core process of existing technologies or adding complex equipment. It maximizes the content of effective substances in quaternary ammonium salt, while improving the antibacterial long-lasting effect and environmental performance of the product.
[0030] The conventional one-pot method involves pre-mixing quaternary ammonium salts with water glass, then slowly adding dilute sulfuric acid dropwise to the mixture to complete the in-situ gelation reaction. Products obtained through this method exhibit uneven particle size, loose structure, disordered pores, and a tendency to agglomerate; uneven distribution of quaternary ammonium salts, with surface enrichment and low internal content; easy saturation of quaternary ammonium salt loading, with a loading rate of only 13%–18%; resistance to water washing only 15–25 times, with antibacterial components easily detaching; viscous gel during filtration, slow filtration, and easy clumping; wastewater COD ≥ 800 mg / L, with high levels of free quaternary ammonium salts; and antibacterial retention rate below 60% after 20 water washes.
[0031] The two-step double-drop method involves first preparing a base mother liquor (nucleation solution) by mixing a small amount of quaternary ammonium salt with water glass. Then, a dilute sulfuric acid-quaternary ammonium salt mixture and water glass are simultaneously added dropwise to the base mother liquor, with continuous temperature and pH control to complete the in-situ growth and composite reaction. The product prepared by this method has uniform particles, a dense structure, regular amorphous shape, and good dispersibility; the quaternary ammonium salt is uniformly embedded in the framework with consistent internal and external distribution; the loading capacity can reach 22%–28%; it can withstand 40–50 washes and is stably embedded; it has good filtration performance, with compact particles, fast filtration, and easy drying; the wastewater COD is ≤350 mg / L, with low free quaternary ammonium salt content; and the antibacterial retention rate is higher than 90% after 20 washes.
[0032] To further maximize the effective content of quaternary ammonium salt in the product, this invention adds an excess of quaternary ammonium salt to both the base mother liquor and the dilute sulfuric acid-quaternary ammonium salt mixture based on the two-step double-drop method. After the in-situ gelation reaction is completed, acidic nano silica sol is then uniformly added to the system.
[0033] Therefore, the method provided by the present invention includes: (1) Preparation of basic mother liquor: Mix quaternary ammonium salt and water glass evenly, with a mass ratio of quaternary ammonium salt to water glass of (1.2~1.5):10; (2) Double drop reaction: At the same time, two titrants are added to the base mother liquor: the first mixture (a mixture of dilute sulfuric acid and quaternary ammonium salt, with a mass ratio of quaternary ammonium salt to dilute sulfuric acid of (1.8-2.5):50) and water glass. The reaction temperature is controlled at 25-35℃ and the pH is kept stable at 2-3. The mixture is stirred until the in-situ gelation reaction is completed, and a composite gel containing free quaternary ammonium salt is obtained. (3) Subsequent composite: Add acidic nano silica sol to the above composite gel in batches and stir continuously for 30-40 min to allow the acidic silica sol to fully capture the free quaternary ammonium salts that are not embedded in the system. (4) Post-processing: Filter, wash, dry and pulverize according to conventional process to obtain high-load quaternary ammonium salt-silica composite antibacterial powder.
[0034] The well-defined framework formed by the two-step double-drop method can accommodate more quaternary ammonium salts, and most of the excess feed can be embedded in the framework, reducing the amount of free quaternary ammonium salts. The strong negative charge on the surface of the acidic silica sol and the silanol groups can capture free quaternary ammonium salts through electrostatic adsorption and hydroxyl bonding, converting them into effective loading components. Excess feed ensures sufficient embedding, and silica sol capture achieves zero free quaternary ammonium salts, synergistically exceeding the upper limit of the loading capacity. At the same time, the silica sol forms a dense coating layer on the surface of the composite gel, enhancing the adhesion to fibers without affecting dispersibility and stability.
[0035] Compared to the double-drop method, the method provided by this invention further improves the effective loading of quaternary ammonium salts: from 22%-28% to 28%-32%, maximizing the effective substance content; the free quaternary ammonium salt content approaches zero: the acidic silica sol fully captures the unembedded free quaternary ammonium salts, further reducing the COD of the washing wastewater to ≤300mg / L, significantly alleviating environmental pressure; the wash resistance and adhesion are further enhanced: the coating layer formed by the acidic silica sol works synergistically with the silica skeleton, increasing the number of washes to 45-55 times and improving the adhesion to textile fibers by more than 70%; the antibacterial performance is superior: the effective content of quaternary ammonium salts is increased, the antibacterial MIC value is optimized to <25ppm, and the antibacterial rate and long-lasting effect are more significant; the production feasibility is strong: it only adds two steps after the acidic silica sol and the excessive quaternary ammonium salt feeding to the two-step double-drop method, without adding complex equipment, adapting to industrial production, and without affecting the production efficiency of filtration, drying, etc.
[0036] The acidic nanohydrogels used have a particle size of 10-20 nm, pH=2-4, solid content of 20%-30%, and are added at 12%-20% of the dry basis mass of the final composite powder.
[0037] Although quaternary ammonium salts can be used in excess, they should not be used excessively. For example, the quaternary ammonium salt in the base mother liquor should not be excessive by 1.2-1.5 times to avoid abnormal system viscosity, gel agglomeration, and increased filtration difficulty. The quaternary ammonium salt in the first mixture should not be excessively used (more than 3 times) to avoid abnormal system viscosity, gel agglomeration, and increased filtration difficulty.
[0038] Acidic silica sol should be added slowly in batches, with each batch not exceeding 1 / 3 of the total amount, with a 5-minute interval between each batch. Stirring should be continuous to avoid local flocculation and agglomeration, and to ensure full capture of free quaternary ammonium salts.
[0039] According to the specific implementation method, the pH is maintained at 2-3 throughout the process in step (3) to avoid the desorption of quaternary ammonium salt and the agglomeration and failure of silica sol due to excessively high pH.
[0040] During the double-drop reaction stage, the stirring speed is 500-600 r / min. After adding the silica sol, the stirring speed is maintained at 400-500 r / min to ensure that the system is mixed evenly and the quaternary ammonium salt is distributed uniformly.
[0041] The water glass mentioned in this article refers to sodium silicate or potassium silicate, with a modulus of 1.5-3.5.
[0042] The quaternary ammonium salt-silica composite material prepared by the method provided in this invention can be widely used in the antibacterial finishing of various textiles, especially suitable for scenarios with high requirements for washability, long-lasting antibacterial effect, and environmental friendliness, including but not limited to intimate apparel textiles requiring washability, low irritation, and a soft feel: underwear, towels, socks, etc.; home textile products requiring antibacterial and mildew-proof properties and resistance to multiple washes: bed sheets, duvet covers, curtains, etc.; and industrial textiles requiring highly effective antibacterial properties and long-lasting stability: work clothes, medical textiles, etc. The provided composite material can be applied through conventional textile finishing processes such as padding, coating, and printing, without the need for additional specialized equipment, and is compatible with existing textile mill production processes.
[0043] The technical solution of the present invention will be described below through specific embodiments. It should be noted that these embodiments are only used to facilitate understanding by those skilled in the art and should not be considered as limiting the scope of protection of the present invention. Unless otherwise specified, the reagents used in the embodiments are commercially available. The modulus of the water glass used is 3.0.
[0044] The amount of acidic nano-silica sol added in each embodiment was determined based on previous material balance experiments. Previous experimental results showed that the gel prepared using the two-step double-drop method (1.3 times excess of the quaternary ammonium salt base mother liquor and 2.0 times excess of mixed solution A), after washing and drying, had an actual quaternary ammonium salt loading of approximately 25%–26% as measured by the EA method. Compared to the total feed amount, the loss of free quaternary ammonium salt accounted for approximately 15%–20% of the total quaternary ammonium salt feed amount (equivalent to 12%–15% of the final dry basis mass). Therefore, the amount of acidic nano-silica sol added was selected as 12%–20% of the final composite powder dry basis mass to ensure sufficient capture of free quaternary ammonium salt while avoiding process problems caused by excessive addition.
[0045] Example 1 Example 1 describes the preparation of a quaternary ammonium salt-silica composite material using the following method. The raw materials include: CTAC (for basal stock solution, 1.3 times excess, normal dosage 8g, actual dosage 10.4g). CTAC (for Mixture A, 2.0 times excess, standard dosage 10g, actual dosage 20g); Acidic nano-silica sol with a particle size of 15nm, pH=3, solid content of 25%, is added at 15% of the dry basis weight of the final composite powder. Water glass (for base mother liquor) 80 g; 20 g of water glass (for titrant B).
[0046] The preparation steps are as follows: (1) Preparation of basic mother liquor: Mix 10.4g CTAC with 80g water glass and 200g deionized water to dilute and stir evenly to obtain basic mother liquor; (2) Preparation of mixture A: Mix 20g CTAC with 500g 2.7% dilute sulfuric acid to obtain dilute sulfuric acid-quaternary ammonium salt mixture A; (3) Double drop reaction: Mixture A and 20g water glass are added dropwise to the base mother liquor at the same time and separately. The temperature is controlled at 30℃, the stirring speed is 550r / min, the pH of the system is kept stable at 2.5, and the mixture is continuously added and stirred until the in-situ gelation reaction is completed. (4) Subsequent composite: Add acidic nano silica sol dropwise to the composite gel system in batches (1 / 3 of the total amount added in each batch, with an interval of 5 min), reduce the stirring speed to 450 r / min, and continue stirring for 35 min; (5) Filter, wash twice with water, dry at 130℃ for 2.5h, and pulverize to obtain composite powder.
[0047] Example 2 The difference between this embodiment and Example 1 is that cetyltrimethylammonium bromide (CTAB) is used instead of CTAC, the amount of quaternary ammonium salt added is slightly lower, and acidic nano silica sol with a smaller particle size (particle size 10 nm, pH=2.5, solid content 20%, added at 12% of the dry basis mass of the final composite powder) is selected.
[0048] The preparation steps are as follows: (1) Preparation of basic mother liquor: 9.6g CTAB, 80g water glass and 200g deionized water were added to the reaction vessel in sequence and stirred evenly to obtain the basic mother liquor.
[0049] (2) Preparation of mixture A: Dissolve 18.0g CTAB in 500.0g 2.0% dilute sulfuric acid and stir until completely dissolved to obtain dilute sulfuric acid-quaternary ammonium salt mixture A.
[0050] (3) Double-drop reaction: Mixture A and 20.0 g of water glass were placed in two constant-pressure dropping funnels and added dropwise to the base mother liquor simultaneously and separately under stirring. The reaction temperature was controlled at 25℃ and the stirring speed at 500 r / min. The pH of the system was kept stable at 2.0 by adjusting the dropping speed. The addition was continued and stirred until the in-situ gelation reaction was complete, and a composite gel was obtained.
[0051] (4) Subsequent composite: acidic nano silica sol is slowly added to the composite gel in batches. The amount added in each batch is 1 / 3 of the total amount of silica sol. The interval between each batch is 5 min. The stirring speed is reduced to 400 r / min. After the addition is completed, stirring is continued for 30 min.
[0052] (5) Post-processing: Filter, wash the filter cake twice with deionized water, dry at 130℃ for 2.5h, crush and sieve to obtain composite powder.
[0053] Example 3 The difference between this embodiment and Example 1 is that the excess of quaternary ammonium salt is greater, and acidic nano silica sol with a larger particle size (particle size 20 nm, pH=4.0, solid content 30%) is selected. The reaction temperature and pH value are also adjusted accordingly (added at 20% of the dry basis mass of the final composite powder).
[0054] The preparation steps are as follows: (1) Preparation of basic mother liquor: 12.0g CTAC, 80g water glass and 200g deionized water are added to the reaction vessel in sequence and stirred evenly to obtain basic mother liquor.
[0055] (2) Preparation of mixture A: Dissolve 25.0g CTAC in 500.0g 5.0% dilute sulfuric acid and stir until completely dissolved to obtain dilute sulfuric acid-quaternary ammonium salt mixture A.
[0056] (3) Double-drop reaction: Mixture A and 20.0 g of water glass were placed in two constant-pressure dropping funnels and added dropwise to the base mother liquor simultaneously and separately under stirring. The reaction temperature was controlled at 35℃ and the stirring speed was 600 r / min. The pH of the system was kept stable at 3.0 by adjusting the dropping speed. The addition was continued and stirred until the in-situ gelation reaction was complete, and a composite gel was obtained.
[0057] (4) Subsequent composite: acidic nano silica sol is slowly added to the composite gel in batches. The amount added in each batch is 1 / 3 of the total amount of silica sol. The interval between each batch is 5 min. The stirring speed is reduced to 500 r / min. After the addition is completed, stirring is continued for 40 min.
[0058] (5) Post-processing: Filter, wash the filter cake twice with deionized water, dry at 130℃ for 2.5h, crush and sieve to obtain composite powder.
[0059] Comparative Example 1 Comparative Example 1 prepared a quaternary ammonium salt-silica composite material by the following method, which did not add excessive CTAC or acidic silica sol.
[0060] The raw materials used include: CTAC (8g of basal stock solution); CTAC (10g of mixture A); Water glass (for base mother liquor) 80 g; 20 g of water glass (for titrant B).
[0061] The preparation methods specifically include: (1) Preparation of basic mother liquor: Mix 8g CTAC with 80g water glass and 200g deionized water to dilute and stir evenly to obtain basic mother liquor; (2) Preparation of mixture A: Mix 10g CTAC with 500g 2.7% dilute sulfuric acid to obtain dilute sulfuric acid-quaternary ammonium salt mixture A; (3) Double drop reaction: Mixture A and 20g water glass are added dropwise to the base mother liquor at the same time and separately. The temperature is controlled at 30℃, the stirring speed is 550r / min, the pH of the system is kept stable at 2.5, and the mixture is continuously added and stirred until the in-situ gelation reaction is completed. (4) After filtration, washing twice with water, drying at 130℃ for 2.5h, and pulverizing, a composite powder is obtained.
[0062] Comparative Example 2 Comparative Example 2 prepared a quaternary ammonium salt-silica composite material using a conventional one-pot method. The quaternary ammonium salt and water glass were premixed evenly to obtain a mixed system. Then, dilute sulfuric acid was slowly added dropwise to the mixed system to complete the in-situ gelation reaction, thereby achieving silica gel formation and quaternary ammonium salt loading.
[0063] The raw materials used include: 100 g of water glass; 500 g of 2.7% dilute sulfuric acid; CTAC 18 g.
[0064] The preparation methods specifically include: (1) Mix 18g CTAC with 100g water glass and 500g deionized water to dilute and stir evenly to obtain a mixed system; (2) Slowly add 500g of 2.7% dilute sulfuric acid to the mixture to complete the in-situ gelation reaction and obtain a composite gel; (3) Filter, wash twice with water, dry at 130℃ for 2.5h, and pulverize to obtain composite powder.
[0065] The composite powders prepared in each embodiment and comparative example were evaluated as follows: (1) Effective loading of quaternary ammonium salt: The percentage content of nitrogen was tested using an organic elemental analyzer (EA), and the effective loading of quaternary ammonium salt was calculated based on the nitrogen content. The specific test conditions were as follows: the elemental analyzer was an Elementar VarioEL Cube or an instrument of equivalent precision, the high-temperature combustion-thermal conductivity detection method was used, the combustion temperature was set to 950~1050℃, helium was used as the carrier gas and oxygen was used as the combustion-supporting gas, the sample weight was about 2~5mg, each sample was measured in parallel 3 times, and the average value was taken as the final nitrogen content determination result.
[0066] The formula for calculating the effective loading rate (%) of quaternary ammonium salt is as follows: Effective loading of quaternary ammonium salt (%) = N% × (M quaternary ammonium salt / (number of N atoms × 14.01)) × 100% in: N% represents the mass percentage of nitrogen element measured by the elemental analyzer; M represents the relative molecular mass of the selected quaternary ammonium salt (e.g., the relative molecular mass of hexadecyltrimethylammonium chloride CTAC is 319.5). The number of N atoms is the number of nitrogen atoms in each quaternary ammonium salt molecule; 14.01 is the molar mass of nitrogen atom (g / mol).
[0067] The above method can accurately determine the actual effective loading of quaternary ammonium salt in the final composite powder, thereby evaluating the loading efficiency of quaternary ammonium salt by different preparation processes.
[0068] (2) Wastewater COD value: The COD value of wastewater was determined by spectrophotometry.
[0069] The chemical oxygen demand (COD) of wastewater generated during filtration and washing was determined by rapid digestion spectrophotometry, in accordance with the standard "Determination of Chemical Oxygen Demand in Water - Rapid Digestion Spectrophotometry" (HJ / T 399-2007).
[0070] (3) Minimum inhibitory concentration (MIC) determination: The MIC value was determined by the agar dilution method, referring to the "Clinical Microbiology Laboratory Operation Specifications" and the relevant standards of CLSI (Clinical and Laboratory Standards Institute).
[0071] (4) Determination of wash fastness and antibacterial retention rate: The tests were conducted in accordance with GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles - Part 3: Shaking method" and AATCC 61-2013 "Color fastness to washing: Accelerated method". The finished textiles were washed repeatedly according to the standard washing procedure. Samples were taken every 5 washes as one cycle, and the antibacterial rate was determined. The maximum number of washes when the antibacterial retention rate was ≥80% was taken as the wash fastness.
[0072] (5) Evaluation of fabric appearance: The prepared composite powder is ground to a D50 of 800nm~1.5μm and then prepared into a finishing solution (solid content 1~3%). It is then applied to a standard cotton fabric through a one-dip-one-pinch process (pinch-off rate 70~80%). After baking at 120℃ for 3min, the fabric surface is visually observed under a standard light source to see if there are any defects such as white spots or color spots. The hand feel (soft / hard / rough) is evaluated by touch. The water absorption test (capillary effect method) is carried out in accordance with GB / T 8629-2017 to evaluate whether the basic performance of the textile after finishing is negatively affected.
[0073] The measurement results of each embodiment and comparative example are shown in Table 1 below: Table 1 Measurement Results
[0074] To evaluate the bactericidal kinetics of the composite material prepared in this invention against common pathogenic bacteria, the quantitative bactericidal test methods in GB / T20944.3-2008 "Evaluation of Antimicrobial Properties of Textiles - Part 3: Shaking Method" and "Disinfection Technical Specifications" (2002 edition) were used to determine the bactericidal effect of the antimicrobial material on the test strains at different contact times, and the antimicrobial rate constant was calculated. Test strains: Escherichia coli and Staphylococcus aureus.
[0075] To evaluate the inhibitory effect of the composite material prepared in this invention on common molds, the petri dish method in GB / T 24346-2009 "Evaluation of Antifungal Properties of Textiles" (or AATCC 30-2017 "Evaluation of Antifungal Properties of Textiles: Antifungal and Antiseptic Properties of Textiles") was used for testing. The test strain used was Aspergillus niger.
[0076] Table 2. Determination of bactericidal performance
[0077] Experimental results show that the method provided in Example 1 of this invention has significantly better core performance than Comparative Examples 1 and 2, maximizing the effective loading of quaternary ammonium salt, thus verifying the effectiveness, feasibility, and advancement of the improved scheme. The results of Examples 2 and 3 are comparable to those of Example 1.
[0078] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a high-load, water-washable quaternary ammonium salt-silica composite material, characterized in that, include: (1) Provide a base mother liquor, wherein the base mother liquor comprises quaternary ammonium salt and water glass, and the mass ratio of quaternary ammonium salt to water glass in the base mother liquor is (1.2~1.5):10; (2) Add a first mixture and water glass to the base mother liquor. The first mixture includes dilute sulfuric acid and quaternary ammonium salt. The mass ratio of quaternary ammonium salt to dilute sulfuric acid in the first mixture is (1.8~2.5):
50. React at a predetermined temperature and a predetermined stirring speed to obtain a composite gel. (3) The composite gel and acidic nano silica sol are mixed under stirring conditions for 20-40 minutes to obtain the composite material; (4) Filter, wash, dry and crush to obtain the high-load quaternary ammonium salt-silica composite material.
2. The preparation method according to claim 1, characterized in that, The loading of quaternary ammonium salt in the high-load quaternary ammonium salt-silica composite material is 28%~32%.
3. The preparation method according to claim 1, characterized in that, The cation of the quaternary ammonium salt is selected from at least one of alkyltrimethylammonium ion, alkyldimethylbenzylammonium ion, and dialkyldimethylammonium ion; the alkyl group is C10. 12 ~C 16 Long-chain alkyl group; the anion is independently selected from at least one of chloride ion, bromide ion, and iodide ion; Optionally, the quaternary ammonium salt is selected from at least one of dodecyltrimethylammonium chloride, dodecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, dodecyldimethylbenzylammonium chloride, hexadecyldimethylbenzylammonium chloride, didodecyldimethylammonium chloride, and dihexadecyldimethylammonium chloride; Optionally, the mass concentration of the dilute sulfuric acid is 2-5% (w / w).
4. The preparation method according to claim 1, characterized in that, The predetermined temperature is 25~35 degrees Celsius; The predetermined stirring speed is 500-600 r / min; Optionally, the reaction is maintained at pH 2-3.
5. The preparation method according to claim 1, characterized in that, The acidic nano-silica sol has a particle size of 10-20 nm and a solid content of 20%~30%.
6. The preparation method according to claim 1, characterized in that, The amount of acidic nano-silica sol added is 12%-20% of the dry basis mass of the composite powder.
7. The preparation method according to claim 1, characterized in that, Step (3) The acidic silica sol is slowly added to the composite gel in batches, with each batch not exceeding 1 / 3 of the total amount, and the interval between each batch is at least 5 minutes.
8. A high-load, water-washable quaternary ammonium salt-silica composite material, characterized in that, Obtained by the preparation method according to any one of claims 1 to 7.
9. The high-load, water-washable quaternary ammonium salt-silica composite material according to claim 8, characterized in that, The composite material has a quaternary ammonium salt loading of 28% to 32%; wastewater COD value ≤ 300 mg / L; and can withstand ≥ 45 washes, with an antibacterial retention rate ≥ 80%.
10. The use of the high-load water-resistant quaternary ammonium salt-silica composite material according to claim 9 in antibacterial finishing of textiles.