An acrylate-paraffin composite fluorine-free waterproofing agent, its preparation method and application

By compounding octadecyl acrylate with paraffin and using low-temperature crosslinking technology, an interpenetrating network of silicone-polyurethane-acrylate is formed, which solves the problems of easy damage and poor mechanical stability of fluorine-free waterproofing agents at high temperatures, and achieves low-temperature molding, excellent waterproofing effect and smooth feel.

CN123064009APending Publication Date: 2026-11-10GUANGDONG HONGHAO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611499743.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing fluorine-free waterproofing agents have problems such as high energy consumption, poor mechanical stability and poor fabric hand feel in printing and dyeing processes. In particular, they are prone to damage to heat-sensitive fabrics at high temperatures, and the contradiction between washability and softness is caused by micro-phase separation and weak covalent bond anchoring.

Method used

It is made by compounding octadecyl acrylate with paraffin wax with a melting point of 50℃~60℃, combining it with a blocked isocyanate acrylate crosslinking agent and γ-(methacryloyloxy)propyltrimethoxysilane, and using strong cationic surfactants and nonionic surfactants as emulsifiers. Through low-temperature crosslinking, an organosilicon-polyurethane-acrylate interpenetrating network is formed, which improves mechanical stability and wash resistance while maintaining a soft hand feel.

Benefits of technology

A low-temperature molding process was achieved for an acrylate-paraffin composite fluorine-free waterproofing agent, which exhibits excellent mechanical stability, waterproofing effect, and smooth hand feel. This solves the problems of fabric damage and poor mechanical stability at high temperatures, and improves washability and waterproofing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses an acrylate-paraffin composite fluorine-free waterproofing agent, its preparation method, and its application. The acrylate-paraffin composite fluorine-free waterproofing agent of this invention, by weight, comprises 35-45 parts octadecyl acrylate, 12-18 parts paraffin wax, 3-6 parts blocked isocyanate acrylate crosslinking agent, 1.5-4 parts γ-(methacryloyloxy)propyltrimethoxysilane, 0.2-0.5 parts aliphatic thiol chain transfer agent, 3-8 parts organic co-solvent, 4-7 parts composite emulsifier, 100-140 parts deionized water, and 0.1-1 parts initiator. The composite emulsifier includes octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether. The melting point of the paraffin wax is 50℃-60℃. The acrylate-paraffin composite fluorine-free waterproofing agent of this invention can be baked and molded at a relatively low temperature (110℃-120℃), exhibiting excellent mechanical stability. Fabrics treated with it have good hand feel, waterproof effect, and wash resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of textile processing auxiliaries, and in particular to an acrylate-paraffin composite fluorine-free waterproofing agent, its preparation method, and its application. Background Technology

[0002] With increasingly stringent global environmental regulations on perfluorinated and polyfluorinated alkyl substances (PFAS), the development of efficient and green fluorine-free waterproofing agents has become the absolute mainstream in the textile chemicals field. Current fluorine-free waterproofing agents mainly rely on the orderly crystalline arrangement of long-chain alkyl acrylates (such as octadecyl acrylate, SA) and the low surface energy of paraffinic hydrocarbon groups to provide hydrophobic properties. However, traditional physical blending or conventional crosslinking copolymerization systems of "long-chain alkyl acrylate + paraffin" suffer from three major unresolved industrial pain points in dyeing and printing processing and practical use: First, high curing energy consumption and damage to sensitive fibers: To achieve a certain level of wash resistance, traditional systems often require the introduction of hydroxymethylacrylamide (MAM) or conventional weakly capped isocyanates as crosslinking agents. The deactivation temperature of these crosslinking agents is usually above 150°C. Such high baking temperatures not only consume enormous amounts of heat energy but also easily lead to a decrease in tensile strength, elastic fatigue, and severe yellowing in heat-sensitive fabrics such as nylon and spandex. Secondly, poor high-shear mechanical stability (sticking to rollers in continuous processing in dyeing and printing plants): The long chain of octadecyl acrylate monomers is prone to microscopic high crystallinity, while paraffin is a non-polar physical filler. During the continuous liquid-bearing rolling process of the setting machine in dyeing and printing plants, the emulsion is subjected to the continuous high shear force of the rollers, which easily leads to microscopic phase separation or thermal demulsification, causing polymer precipitation and agglomeration on the roller surface (commonly known as "sticking to rollers"), forcing the production line to frequently stop for cleaning. Thirdly, the inherent contradiction between wash fastness and the soft hand feel of the fabric: The covalent bond anchoring between conventional fluorine-free waterproof membranes and fibers is relatively weak. If the wash fastness is ensured by simply increasing the amount of crosslinking agent, the cured film will be too rigid, resulting in a stiff, rough hand feel of the fabric, obvious slippage defects, and loss of the original soft touch of the clothing fabric.

[0003] Therefore, there is an urgent need for an acrylate-paraffin composite fluorine-free waterproofing agent, its preparation method, and its application, in order to overcome the shortcomings of existing technologies. Summary of the Invention

[0004] In view of the above problems, the purpose of this invention is to provide an acrylate-paraffin composite fluorine-free waterproofing agent, its preparation method, and its application. The acrylate-paraffin composite fluorine-free waterproofing agent of this invention can be baked and molded at a relatively low temperature (110℃~120℃), exhibits excellent mechanical stability, and fabrics treated with it have good hand feel, waterproof effect, and wash resistance.

[0005] To achieve the above objectives, the first aspect of this invention provides an acrylate-paraffin composite fluorine-free waterproofing agent, comprising, by weight, 35-45 parts octadecyl acrylate, 12-18 parts paraffin, 3-6 parts blocked isocyanate acrylate crosslinking agent, 1.5-4 parts γ-(methacryloyloxy)propyltrimethoxysilane, 0.2-0.5 parts aliphatic thiol chain transfer agent, 3-8 parts organic cosolvent, 4-7 parts composite emulsifier, 100-140 parts deionized water, and 0.1-1 parts initiator. The composite emulsifier comprises octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether, and the paraffin has a melting point of 50°C-60°C.

[0006] Compared with the prior art, the acrylate-paraffin composite fluorine-free waterproofing agent of the present invention has at least the following beneficial effects: (1) The present invention uses octadecyl acrylate and paraffin wax with a melting point of 50℃~60℃ in combination. Both contain highly crystalline nonpolar hydrophobic groups. At the same time, under the condition of aliphatic thiol chain transfer agent, a macromolecular polymer with appropriate and uniform molecular weight can be obtained, thereby effectively avoiding local gelation caused by multifunctional group reaction. It can effectively increase the chain segment flexibility and molecular chain inversion ability of polymer film during heat setting, thereby effectively improving the initial hydrostatic pressure and waterproof effect of the fabric after it is treated, and bringing a smooth hand feel.

[0007] (2) The present invention contains both a blocked isocyanate acrylate crosslinking agent and γ-(methacryloyloxy)propyltrimethoxysilane. The blocked isocyanate acrylate crosslinking agent can deblock and release active isocyanate groups at a lower temperature. The isocyanate groups can form covalent bonds with hydroxyl or amino groups on the fiber surface, and can also undergo polycondensation crosslinking with silanols generated by in-situ hydrolysis of γ-(methacryloyloxy)propyltrimethoxysilane in the aqueous phase. This promotes the forward progress of the deblocking equilibrium reaction of the blocked isocyanate acrylate crosslinking agent. Therefore, the two work together to form an organosilicon-polyurethane-acrylate interpenetrating network on the fabric surface at a lower temperature (110℃~120℃), thereby effectively improving the wash resistance of the fabric after treatment.

[0008] (3) The present invention uses octadecyltrimethylammonium chloride, a strong cationic surfactant, and isomeric tridecyl alcohol polyoxyethylene ether, a nonionic surfactant, as a compound emulsifier. At the same time, an organic co-solvent is introduced. The three work together to effectively improve the mechanical stability of the acrylate-paraffin composite fluorine-free waterproofing agent of the present invention, and can effectively solve the technical problem of waterproofing agent breaking emulsion and sticking to rollers during the finishing process of fabric.

[0009] Specifically, the weight percentages of octadecyl acrylate may be, but are not limited to, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, or 45 parts; the weight percentages of paraffin may be, but are not limited to, 12, 13, 14, 15, 16, 17, or 18 parts; the weight percentages of the blocked isocyanate acrylate crosslinking agent may be, but are not limited to, 3, 4, 5, or 6 parts; and the weight percentages of γ-(methacryloyloxy)propyltrimethoxysilane may be, but are not limited to, 1.5, 2, 2.5, 3, or 3.5 parts. The weight percentages of aliphatic thiol chain transfer agents can be, but are not limited to, 0.2, 0.3, 0.4, or 0.5 parts; the weight percentages of organic cosolvents can be, but are not limited to, 3, 4, 5, 6, 7, or 8 parts; the weight percentages of composite emulsifiers can be, but are not limited to, 4, 5, 6, or 7 parts; the weight percentages of deionized water can be, but are not limited to, 100, 110, 120, 130, or 140 parts; and the weight percentages of initiators can be, but are not limited to, 0.1, 0.2, 0.4, 0.6, 0.8, or 1 part.

[0010] Furthermore, the composite emulsifier of the present invention is composed of octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether.

[0011] Further, the mass ratio of octadecyltrimethylammonium chloride to isotrimethylene tridecyl alcohol polyoxyethylene ether in this invention is 1:0.5~2. Specifically, the mass ratio of octadecyltrimethylammonium chloride to isotrimethylene tridecyl alcohol polyoxyethylene ether can be, but is not limited to, 1:0.5, 1:0.8, 1:1.0, 1:1.2, 1:1.4, 1:1.6, 1:1.8, or 1:2.0.

[0012] Furthermore, the blocked isocyanate acrylate crosslinking agent of the present invention is selected from pyrazole-blocked isocyanate ethyl acrylate. Specifically, the pyrazole-blocked isocyanate ethyl acrylate is 2-[(3,5-dimethyl-1-H-pyrazole)carboxyamino]ethyl acrylate (AOI-BP).

[0013] Furthermore, the paraffin of the present invention is selected from at least one of paraffin No. 52, paraffin No. 54 and paraffin No. 56.

[0014] Furthermore, the organic co-solvent of the present invention is selected from at least one of ethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol.

[0015] Furthermore, the aliphatic thiol chain transfer agent of the present invention is selected from at least one of n-dodecyl mercaptan, tert-dodecyl mercaptan, mercaptoethanol, mercaptoacetic acid, and mercaptopropionic acid.

[0016] A second aspect of this invention provides a method for preparing the aforementioned acrylate-paraffin composite fluorine-free waterproofing agent, comprising the steps of: S1. The paraffin wax, organic co-solvent, composite emulsifier and part of deionized water in the formula are heated and mixed evenly, and then subjected to high pressure homogenization to obtain paraffin wax microemulsion; the octadecyl acrylate, blocked isocyanate acrylate crosslinking agent, γ-(methacryloyloxy)propyltrimethoxysilane and aliphatic thiol chain transfer agent in the formula are mixed and stirred evenly to obtain premix; the initiator in the formula is mixed evenly with the remaining part of deionized water to obtain initiator solution; S2. Under a protective atmosphere, the premix and initiator solution are simultaneously added dropwise to the paraffin microemulsion, and the addition time is controlled to be 2.5h~3h. After the addition is completed, a ripening reaction is carried out. S3. After the reaction is complete, cool down and adjust the pH of the reaction system to 4.5~5.5 with glacial acetic acid before filtering.

[0017] This invention first heats and melts paraffin wax, organic co-solvent, composite emulsifier, and a portion of deionized water, then homogenizes them under high pressure to form a paraffin wax microemulsion. A monomer premix is ​​then added dropwise to this microemulsion for polymerization. This process encapsulates the paraffin wax within the polymer, while the crosslinking reactive groups are distributed on the surface. This synthesis method not only further enhances the high shear mechanical stability (anti-sticking to rollers) of the waterproofing agent emulsion but also ensures that the active groups (-NCO and silanol) are exposed to the maximum extent on the surface of the waterproofing agent particles, thereby enabling rapid interfacial grafting and network curing during the baking process.

[0018] Furthermore, the heating and mixing temperature of the present invention is 75°C to 80°C. Specifically, the heating and mixing temperature can be, but is not limited to, 75°C, 76°C, 77°C, 78°C, 79°C, or 80°C.

[0019] Furthermore, the pressure of the high-pressure homogenization process in this invention is 40MPa~45MPa. Specifically, the pressure of the high-pressure homogenization process can be, but is not limited to, 40MPa, 41MPa, 42MPa, 43MPa, 44MPa, or 45MPa.

[0020] Furthermore, the dropping temperature of the present invention is 70°C to 72°C. Specifically, the dropping temperature can be, but is not limited to, 70°C, 71°C, or 72°C.

[0021] Furthermore, the curing temperature of the present invention is 73°C to 75°C. Specifically, the curing temperature can be, but is not limited to, 73°C, 74°C, or 75°C. The curing time is 3 hours to 6 hours, specifically, the curing time can be, but is not limited to, 3 hours, 4 hours, 5 hours, or 6 hours.

[0022] The third aspect of the present invention provides the application of the aforementioned acrylate-paraffin composite fluorine-free waterproofing agent or the acrylate-paraffin composite fluorine-free waterproofing agent prepared according to the aforementioned method for preparing the acrylate-paraffin composite fluorine-free waterproofing agent in textile finishing, wherein the baking temperature of the acrylate-paraffin composite fluorine-free waterproofing agent is 110℃~120℃ and the baking time is 0.5min~2min. Detailed Implementation

[0023] To better illustrate the purpose, technical solution, and beneficial effects of this invention, the invention will be further described below with reference to specific embodiments. It should be noted that the methods described below are further explanations of this invention and should not be construed as limiting it.

[0024] Example 1 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0025] The preparation method of the acrylate-paraffin composite fluorine-free waterproofing agent in this embodiment includes the following steps: S1. 15g of No. 52 paraffin wax, 5g of tripropylene glycol, 5g of composite emulsifier, and 60g of deionized water are stirred and melted at 78℃, and then homogenized in a high-pressure homogenizer at a pressure of 40MPa for 3 times to obtain a paraffin microemulsion base material; 40g of octadecyl acrylate, 4.5g of AOI-BP crosslinking agent, 2.5g of γ-(methacryloyloxy)propyltrimethoxysilane, and 0.3g of n-dodecyl mercaptan are mixed and stirred evenly at 35℃ to obtain a premix; 60g of deionized water and 0.4g of ammonium persulfate are mixed evenly to obtain an initiator solution; S2. The paraffin microemulsion was placed in a four-necked flask and heated to 71°C under a protective atmosphere. The premix and initiator solution were simultaneously added to the paraffin microemulsion through a constant pressure dropping funnel. The dropping time was controlled to be 2.5 h. After the dropping was completed, the mixture was aged at 74°C for 5 h. S3. After the reaction is complete, cool to 35°C, add acetic acid to adjust the pH of the reaction system to 5.0, and filter using a 300-mesh pipeline filter to obtain an acrylate-paraffin composite fluorine-free waterproofing agent.

[0026] Example 2 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 36g octadecyl acrylate, 13g No. 52 paraffin, 3.5g AOI-BP crosslinking agent, 1.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 3.5g tripropylene glycol, 4g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 100g deionized water and 0.3g ammonium persulfate.

[0027] The acrylate-paraffin composite fluorine-free waterproofing agent of this embodiment was prepared according to the preparation method of Example 1.

[0028] Example 3 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent. The raw materials for preparation include 44g octadecyl acrylate, 17g No. 52 paraffin wax, 6g AOI-BP crosslinking agent, 4g γ-(methacryloyloxy)propyltrimethoxysilane, 0.5g n-dodecyl mercaptan, 7g tripropylene glycol, 6g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 140g deionized water, 0.2 parts glacial acetic acid, and 0.6g ammonium persulfate.

[0029] The acrylate-paraffin composite fluorine-free waterproofing agent of this embodiment was prepared according to the preparation method of Example 1.

[0030] Example 4 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 54 paraffin, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0031] The acrylate-paraffin composite fluorine-free waterproofing agent of this embodiment was prepared according to the preparation method of Example 1.

[0032] Example 5 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g propylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0033] The acrylate-paraffin composite fluorine-free waterproofing agent of this embodiment was prepared according to the preparation method of Example 1.

[0034] Example 6 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:2), 120g deionized water and 0.4g ammonium persulfate.

[0035] The acrylate-paraffin composite fluorine-free waterproofing agent of this embodiment was prepared according to the preparation method of Example 1.

[0036] Example 7 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:3), 120g deionized water and 0.4g ammonium persulfate.

[0037] The acrylate-paraffin composite fluorine-free waterproofing agent of this embodiment was prepared according to the preparation method of Example 1.

[0038] Example 8 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 4.5g butanone oxime blocked isocyanate ethyl acrylate crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isotridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0039] The acrylate-paraffin composite fluorine-free waterproofing agent of this embodiment was prepared according to the preparation method of Example 1.

[0040] Example 9 This embodiment provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin wax, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g mercaptoethanol, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0041] The acrylate-paraffin composite fluorine-free waterproofing agent of this embodiment was prepared according to the preparation method of Example 1.

[0042] Comparative Example 1 This comparative example provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0043] The acrylate-paraffin composite fluorine-free waterproofing agent of this comparative example was prepared according to the preparation method of Example 1.

[0044] Comparative Example 2 This comparative example provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin wax, 4.5g AOI-BP crosslinking agent, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0045] The acrylate-paraffin composite fluorine-free waterproofing agent of this comparative example was prepared according to the preparation method of Example 1.

[0046] Comparative Example 3 This comparative example provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin wax, 4.5g AOI-BP crosslinking agent, 2.5g vinyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0047] The acrylate-paraffin composite fluorine-free waterproofing agent of this comparative example was prepared according to the preparation method of Example 1.

[0048] Comparative Example 4 This comparative example provides an acrylate-paraffin composite fluorine-free waterproofing agent. The raw materials for preparation include 40g octadecyl acrylate, 15g No. 52 paraffin wax, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether in a mass ratio of 1:1), 120g deionized water, and 0.4g ammonium persulfate.

[0049] The acrylate-paraffin composite fluorine-free waterproofing agent of this comparative example was prepared according to the preparation method of Example 1.

[0050] Comparative Example 5 This comparative example provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g octadecyltrimethylammonium chloride, 120g deionized water and 0.4g ammonium persulfate.

[0051] The acrylate-paraffin composite fluorine-free waterproofing agent of this comparative example was prepared according to the preparation method of Example 1.

[0052] Comparative Example 6 This comparative example provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g isomeric tridecyl alcohol polyoxyethylene ether, 120g deionized water and 0.4g ammonium persulfate.

[0053] The acrylate-paraffin composite fluorine-free waterproofing agent of this comparative example was prepared according to the preparation method of Example 1.

[0054] Comparative Example 7 This comparative example provides an acrylate-paraffin composite fluorine-free waterproofing agent. The raw materials for preparation include 40g octadecyl acrylate, 15g No. 52 paraffin wax, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (the mass ratio of hexadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether is 1:1), 120g deionized water, and 0.4g ammonium persulfate.

[0055] The acrylate-paraffin composite fluorine-free waterproofing agent of this comparative example was prepared according to the preparation method of Example 1.

[0056] Comparative Example 8 This comparative example provides an acrylate-paraffin composite fluorine-free waterproofing agent, the raw materials of which include 40g octadecyl acrylate, 15g No. 52 paraffin, 4.5g AOI-BP crosslinking agent, 2.5g γ-(methacryloyloxy)propyltrimethoxysilane, 0.3g n-dodecyl mercaptan, 5g tripropylene glycol, 5g composite emulsifier (octadecyltrimethylammonium chloride and Span 80 in a mass ratio of 1:1), 120g deionized water and 0.4g ammonium persulfate.

[0057] The acrylate-paraffin composite fluorine-free waterproofing agent of this comparative example was prepared according to the preparation method of Example 1.

[0058] The acrylate-paraffin composite fluorine-free waterproofing agents prepared in the examples and comparative examples were diluted with water to 30 g / L, and nylon fabrics were subjected to one dip and one nip test with a nip-off rate of 72%, followed by baking at 115°C for 2 min. The treated nylon fabrics were then subjected to waterproof performance tests, wash resistance tests, hydrostatic pressure tests, anti-sticking roller processing performance tests, hand feel tests, and yellowing index tests. The test methods are as follows, and the test results are shown in Table 1.

[0059] Waterproof performance: Tested according to AATCC-22 spray test; Washability: Washing was performed according to AATCC-135 standard, 40℃ for 15 minutes, tumble dried, and then the water resistance was tested after 10 and 20 washes. Initial hydrostatic pressure: according to AATCC-127 standard; Mechanical stability: The acrylate-paraffin composite fluorine-free waterproofing agents prepared in the examples and comparative examples were diluted with water to 30 g / L, and then injected into a high-speed mechanical rolling shear tester. The tester was run continuously for 4 hours under the conditions of 4000 rpm and 0.5 MPa shear pressure. During the operation, it was observed whether the working fluid exhibited precipitation, wall adhesion, gelation, or roller sticking. Hand feel test: The evaluation was conducted according to the AATCC EP5 fabric hand feel evaluation program, with level 1 being the softest and level 5 being the stiffest. Table 1 Performance test results of the examples and comparative examples

[0060] As can be seen from the test results in Table 1, compared with Comparative Examples 1 to 8, Examples 1 to 9 of the present invention have superior mechanical stability, waterproof performance, washability and hand feel overall.

[0061] Specifically, a comparison of Example 1 and Comparative Examples 1-2 shows that at a setting temperature of 115°C, without AOI-BP or γ-(methacryloyloxy)propyltrimethoxysilane, the water resistance score of the fabric drops to 60 points or even completely loses its water resistance after 20 standard washes. However, Example 1 maintains a stable score of 80 points, indicating that the low-temperature unsealing characteristics of AOI-BP and the in-situ hydrolysis of γ-(methacryloyloxy)propyltrimethoxysilane must produce synergistic polycondensation to achieve excellent wash resistance at lower processing temperatures. Furthermore, a comparison of Example 1 and Comparative Example 3 shows that replacing γ-(methacryloyloxy)propyltrimethoxysilane with vinyltrimethoxysilane may be due to the relatively low copolymerization activity of vinyltrimethoxysilane with the water-repellent agent system of this invention, resulting in a significant deterioration in its wash resistance.

[0062] As can be seen from the comparison between Example 1 and Comparative Example 4, when the chain transfer agent is absent, the hydrostatic pressure drops significantly from 3.2 kPa to 1.9 kPa, and the initial waterproofing performance also deteriorates. This indicates that the addition of the chain transfer agent can effectively improve the waterproofing performance of the waterproofing agent of the present invention.

[0063] As can be seen from Examples 1 and Comparative Examples 5-8, although they have a waterproof effect that is basically equivalent to that of Examples 1, their mechanical stability under high shear conditions is significantly worse. This indicates that the compound emulsion system composed of octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether is more compatible with the waterproofing agent system of the present invention and is more conducive to improving mechanical stability.

[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. An acrylate-paraffin composite fluorine-free waterproofing agent, characterized in that, The raw materials, by weight, include 35-45 parts octadecyl acrylate, 12-18 parts paraffin wax, 3-6 parts blocked isocyanate acrylate crosslinking agent, 1.5-4 parts γ-(methacryloyloxy)propyltrimethoxysilane, 0.2-0.5 parts aliphatic thiol chain transfer agent, 3-8 parts organic cosolvent, 4-7 parts composite emulsifier, 100-140 parts deionized water, and 0.1-1 parts initiator. The composite emulsifier includes octadecyltrimethylammonium chloride and isotridecyl alcohol polyoxyethylene ether. The paraffin wax has a melting point of 50°C-60°C.

2. The acrylate-paraffin composite fluorine-free waterproofing agent according to claim 1, characterized in that, The composite emulsifier is composed of octadecyltrimethylammonium chloride and isomeric tridecyl alcohol polyoxyethylene ether.

3. The acrylate-paraffin composite fluorine-free waterproofing agent according to claim 2, characterized in that, The mass ratio of the octadecyltrimethylammonium chloride to isomeric tridecyl alcohol polyoxyethylene ether is 1:0.5~2.

4. The acrylate-paraffin composite fluorine-free waterproofing agent according to claim 1, characterized in that, The blocked isocyanate acrylate crosslinking agent is selected from pyrazole blocked isocyanate ethyl acrylate.

5. The acrylate-paraffin composite fluorine-free waterproofing agent according to claim 1, characterized in that, The paraffin wax is selected from at least one of paraffin wax No. 52, paraffin wax No. 54 and paraffin wax No.

56.

6. The acrylate-paraffin composite fluorine-free waterproofing agent according to claim 1, characterized in that, The organic co-solvent is selected from at least one of ethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol.

7. The acrylate-paraffin composite fluorine-free waterproofing agent according to claim 1, characterized in that, The aliphatic thiol chain transfer agent is selected from at least one of n-dodecyl mercaptan, tert-dodecyl mercaptan, mercaptoethanol, mercaptoacetic acid, and mercaptopropionic acid.

8. A method for preparing an acrylate-paraffin composite fluorine-free waterproofing agent according to any one of claims 1 to 7, characterized in that, Including the following steps: S1. The paraffin wax, the organic co-solvent, the composite emulsifier, and a portion of the deionized water in the prescribed amounts are heated and mixed evenly, and then subjected to high-pressure homogenization to obtain a paraffin wax microemulsion; the octadecyl acrylate, the blocked isocyanate acrylate crosslinking agent, the γ-(methacryloyloxy)propyltrimethoxysilane, and the aliphatic thiol chain transfer agent in the prescribed amounts are mixed and stirred evenly to obtain a premix; the initiator in the prescribed amounts is mixed evenly with the remaining portion of the deionized water to obtain an initiator solution; S2. Under a protective atmosphere, the premix and the initiator solution are simultaneously added dropwise to the paraffin microemulsion, and the dropping time is controlled to be 2.5h~3h. After the dropping is completed, a ripening reaction is carried out. S3. After the reaction is complete, cool down and adjust the pH of the reaction system to 4.5~5.5 with glacial acetic acid before filtering.

9. The preparation method of the acrylate-paraffin composite fluorine-free waterproofing agent according to claim 8, characterized in that, The temperature at which the drops are added is 70℃~72℃, and the temperature at which the curing is performed is 73℃~75℃.

10. The application of an acrylate-paraffin composite fluorine-free waterproofing agent prepared by the preparation method of the acrylate-paraffin composite fluorine-free waterproofing agent according to any one of claims 1 to 7 or according to any one of claims 8 to 9 in textile finishing, characterized in that, The baking temperature of the acrylate-paraffin composite fluorine-free waterproofing agent is 110℃~120℃, and the time is 0.5min~2min.