A process and equipment for producing unbleached chemimechanical pulp from mixed hardwoods.
By screening, washing, and dewatering the mixed hardwood raw materials, combined with pre-steaming, pressure impregnation, fiber separation, and graded pulping, the problem of inconsistent impregnation and softening states of the mixed hardwood raw materials during the production of natural-colored chemimechanical pulp was solved, resulting in a more stable pulping process and high-quality pulping effect.
Patent Information
- Application Number
- CN202611386925.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies for producing unbleached mechanical pulp using mixed wood as raw material suffer from inconsistent impregnation and softening states due to the mixing of different wood chip types, resulting in fluctuations in pulping load, unstable pulp strength, and an excessive number of fiber bundles.
After screening, washing and dewatering, the wood chips undergo pre-steaming, pressure impregnation, fiber separation, reaction, graded pulping and anti-fouling washing to ensure stable impregnation and softening before entering the pulping process, reducing the impact of differences in wood properties and different penetration rates of the chemical solution.
It achieves uniform pretreatment of mixed hardwood raw materials, reduces pulping load fluctuations, improves the stability and continuity of pulp quality, reduces the occurrence of fiber bundles, and enhances the stability of the production process.
Smart Images

Figure CN123064032A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of pulp and paper technology, specifically to a process and equipment for producing unbleached chemimechanical pulp from mixed hardwoods. Background Technology
[0002] Wood fiber is an important fiber raw material for the paper industry. Currently, fast-growing woods such as poplar and eucalyptus are widely used as raw materials for wood pulping. With the increasing demand for wood pulping raw materials, the purchase price and supply stability of commercial wood chips have a certain impact on the production costs of pulping enterprises. On the other hand, thinning timber, small-diameter timber, branches, and mixed mixed hardwoods formed during logging and tending processes have a certain resource volume. These raw materials have historically been primarily used as fuel for charcoal production, with relatively limited utilization in the pulping and papermaking sector. Utilizing readily available mixed hardwoods locally or nearby can serve as a way to diversify wood pulping raw materials.
[0003] However, compared to commercial wood chips made from relatively single tree species, mixed hardwoods have a more complex raw material composition. Different tree species exhibit variations in wood density, hardness, and tissue structure. Even when chips are processed to similar sizes, under the same treatment conditions, their heating rates, liquid absorption rates, and the rate at which the chemical penetrates the chips may still differ. When thinned timber, small-diameter timber, branches, and chips from multiple tree species are mixed, some chips may soften faster than others, resulting in inconsistent material conditions before the subsequent pulping process.
[0004] Meanwhile, the raw material after mixed hardwood chipping may contain excessively large wood chips, scraps, mud, sand, and iron impurities. Differences in the size, cleanliness, and moisture content of the wood chips can also affect subsequent continuous feeding, impregnation, and pulping processes. If the wood chips differ significantly in their state before entering the impregnation process, the degree of softening can easily vary under the same chemical solution, temperature, and mechanical treatment conditions. Insufficiently softened wood chips need to withstand greater mechanical forces during pulping, which can easily increase the pulping load and may also result in more fiber bundles and fluctuations in pulp quality.
[0005] To address the issues of mixed wood chip types and chemimechanical pulp production, existing technologies have proposed various treatment methods. For example, patent CN104711880B discloses a chemimechanical pulping process. In this process, softened wood chips are processed by an extrusion shredder and then enter an impregnator to absorb the chemical solution. They then enter a reaction chamber and are conveyed via a feed screw conveyor to a high-consistency mill for pulping. The process includes vortex separation, bleaching and washing, anti-latency treatment, and subsequent pulping. This technology can improve the impregnation conditions of wood chips through extrusion shredding and provides corresponding treatment for pulping processes involving mixed wood chip types. However, its main approach involves extrusion shredding followed by impregnation, and then high-consistency pulping. For mixed woods with significant differences in hardness, there is still room for further optimization in how to improve the fiber separation and softening uniformity of different materials before the formal high-consistency pulping.
[0006] For example, Chinese invention patent application CN112176750A discloses a P-RC APMP pulping method for hardwood blends. This method can adapt to a certain proportion of hardwood blend raw materials, but its technical route mainly revolves around extrusion delamination, segmented chemical preimpregnation, and P-RC APMP bleaching processes. For mixed hardwood raw materials with diverse tree species and significant differences in hardness, ensuring that the wood chips achieve a relatively uniform impregnation, fiber separation, and softening state before entering the formal pulping process still requires appropriate treatment based on the characteristics of the mixed hardwood raw materials.
[0007] For example, Chinese invention patent application CN119711233A discloses a production process for high-quality hardwood chemimechanical pulp. This process primarily relies on pre-cooking, multi-stage extrusion tearing, and pre-impregnation for softening and impregnation, involving relatively many steps and incorporating bleaching treatment. Further research and improvement are needed in the production of unbleached chemimechanical pulp to improve the impregnation state of different hardwood chips under continuous pressure treatment conditions and to further loosen the chips before formal pulping, allowing the chemical solution to continue interacting with the materials and thus reducing the differences in state between different hardwoods entering the pulping process.
[0008] As can be seen from the existing technologies described above, for the problems of preparing chemimechanical pulp from mixed wood species, hardwood blends, and hardwood-mixed wood, existing technologies mainly employ methods such as wood chip screening and washing, pre-steaming, extrusion tearing or disintegration, chemical pre-impregnation, and multi-stage refining to improve the impregnation and refining performance of raw materials. These processes can improve the adaptability of mixed wood chips to a certain extent; however, due to differences in the species composition, hardness, and chemical penetration rate of mixed wood raw materials, the impregnation and softening state of the wood chips before formal refining may still vary under continuous production conditions.
[0009] Therefore, when using thinned timber, small-diameter timber, branch timber, and mixed mixed hardwoods to produce natural-colored mechanical pulp, it is still necessary to rationally connect the processes of raw material screening, chip washing, continuous feeding, impregnation, fiber separation, reaction, and subsequent pulping. This will ensure that different hardwood chips receive sufficient and stable treatment before entering the pulping process, thereby reducing problems such as fluctuations in pulping load, unstable pulp strength, and excessive fiber bundles caused by differences in the hardness of raw materials and different penetration rates of the chemical solution. Summary of the Invention
[0010] The technical problem to be solved by this invention is to overcome the shortcomings of the existing technology and provide a process and equipment for producing unbleached mechanical pulp from mixed hardwoods. By screening, washing and dewatering the mixed hardwood chips, and then sequentially performing pre-steaming, pressure impregnation, fiber separation, reaction, graded grinding, desulfurization and washing and concentration treatment, the mixed hardwood chips of different species and different hardness are subjected to more sufficient and stable impregnation, fiber separation and softening treatment before entering the grinding process. This reduces the problems of grinding load fluctuation, unstable pulp strength and more fiber bundles caused by differences in the properties of mixed hardwoods and different penetration rates of the chemical solution. It can effectively solve the problems in the background technology.
[0011] To achieve the above objectives, the present invention provides the following technical solution: a device for producing unbleached mechanical pulp from mixed hardwoods, comprising a pre-steaming spiral, a spiral feeder, a T-tube, an expansion joint, a vertical steaming pipe, a feeder, a discharge spiral, a fiber separator, a cyclone separator, a feed plug spiral, a No. 1 reaction chamber, a No. 1 mill feed spiral, a No. 1 high-consistency mill, a No. 1 mill discharge spiral, a No. 2 reaction chamber, a No. 2 mill feed spiral, and a No. 2 high-consistency mill; the discharge end of the pre-steaming spiral is connected to the inlet of the spiral feeder, the spiral feeder includes a transmission mechanism, a feed plug pipe, and a spiral shaft, the transmission mechanism is connected to the spiral shaft, the spiral shaft is a variable diameter and variable pitch spiral with a compression ratio of 1:2 to 1:2.5, the discharge end of the feed plug pipe is connected to the T-tube, the T-tube is provided with a liquid and steam addition section, and is connected to the vertical steaming pipe through an expansion joint; The feeder is located at the bottom of the vertical steaming pipe. The discharge side of the feeder is connected to the fiber separator via a discharge screw. The fiber separator includes a feed screw, a stationary grinding disc, a moving grinding disc, and a discharge port. The feed screw is a double-headed screw forced feeding structure. The stationary and moving grinding discs are large-toothed grinding discs for fiber separation. The moving grinding disc can move forward and backward relative to the stationary grinding disc. During operation, the gap between the stationary and moving grinding discs is 2-2.5 mm. The discharge port of the fiber separator is connected to the hydrocyclone separator, the material outlet of the hydrocyclone separator is connected to the No. 1 reaction chamber through the feed plug screw, the flash steam outlet of the hydrocyclone separator is connected to the pre-steam screw, the feed plug screw is a variable diameter and variable pitch screw, and the No. 1 reaction chamber is a horizontal flow bed reaction chamber. The No. 1 reaction chamber is connected to the No. 1 high-concentration mill via the No. 1 mill feed screw. The No. 1 high-concentration mill is connected to the No. 2 reaction chamber via the No. 1 mill discharge screw. The No. 2 reaction chamber is connected to the No. 2 high-concentration mill via the No. 2 mill feed screw. Both the No. 1 and No. 2 high-concentration mills are atmospheric pressure high-concentration mills. During operation, the gap between the fixed plate and the moving plate is 0.2-0.4 mm.
[0012] Furthermore, upstream of the pre-steaming screw, along the material conveying direction, are sequentially arranged a metering hopper, a conveyor belt, a cylindrical screen, an electromagnet, a feeding belt, a washing machine, and a dewatering screw. The metering hopper is equipped with two variable frequency speed-regulating discharge screws, and the dewatering screw is a screw dewatering device with a filter screen and an inclination angle of 30°.
[0013] Furthermore, the cylindrical screen includes a feed inlet, a large-piece outlet, a qualified-piece outlet, a crushed-piece outlet, a drum, a large-aperture screen, a small-aperture screen, and a drum drive mechanism; the drum drive mechanism is connected to the drum drive and is used to drive the drum to rotate; the large-aperture screen and the small-aperture screen are arranged inside the drum, the screen aperture of the large-aperture screen is φ40~45mm, and the screen aperture of the small-aperture screen is φ6~8mm; the mixed wood chips entering the drum are screened into large pieces, qualified pieces, and crushed-pieces by the large-aperture screen and the small-aperture screen during the rotation of the drum, and the large pieces, qualified pieces, and crushed-pieces are discharged from the large-piece outlet, the qualified-piece outlet, and the crushed-piece outlet, respectively.
[0014] Furthermore, it also includes a fine screen, a sedimentation tank, a clarification tank, a washing water pump, and a sludge discharge pump. The drain end of the dewatering spiral is connected to the fine screen, the outlet end of the fine screen is connected to the sedimentation tank, the upper part of the sedimentation tank is connected to the clarification tank, the clarification tank is connected to the washing water inlet of the washing machine through the washing water pump, and the bottom of the sedimentation tank is connected to the water treatment system through the sludge discharge pump. The fine screen is a drum screen with a 0.5mm sieve opening, and the sedimentation tank is a vertical flow sedimentation tank.
[0015] Furthermore, the T-shaped tube is equipped with an anti-backflow device consisting of a cylinder and a cone sealing device; the vertical steam pipe is equipped with a feed inlet, a pressure detection port, a temperature detection port 1, a material level detection port 1, a material level detection port 2, a material level detection port 3, a steam inlet, and a temperature detection port 2. The material level detection ports 1, 2, and 3 are arranged along the height direction of the vertical steam pipe and are respectively equipped with tension gauges for outputting material level signals. The feeder includes a scraper, which is used to evenly push the material at the bottom of the vertical steam pipe to the discharge screw.
[0016] Furthermore, the discharge end of the No. 2 high-consistency mill is sequentially connected to the No. 2 mill discharge screw, the lifting screw, the anti-submersion tank feed screw, and the anti-submersion tank. The anti-submersion tank is connected to the No. 1 rotary drum extruder via a slurry pump. The No. 1 rotary drum extruder is connected to the No. 2 rotary drum extruder via a dilution screw. The discharge end of the No. 2 rotary drum extruder is connected to the slurry discharge screw. Both the No. 1 and No. 2 rotary drum pulping machines include a feed inlet, a gravity dewatering zone, an angle between the upper and lower screens, a rotary drum, 3-4 stage pressing rollers, and a pulp scraper. They are also equipped with a screen top, a screen bottom, and a pneumatic tensioning device. The gravity dewatering zone, the angle between the upper and lower screens, the rotary drum, and the pressing rollers are arranged sequentially along the pulp conveying direction.
[0017] Furthermore, a process for producing unbleached phenolic pulp from mixed hardwoods, implemented using the equipment described in claim 1, is characterized by comprising the following steps: Step 1, Pre-treatment of miscellaneous wood chips: Thinnings, small-diameter timber, branches, or mixed miscellaneous wood of multiple species are chipped into miscellaneous wood chips. The miscellaneous wood chips are screened, iron removed, washed, and dehydrated. The dehydrated miscellaneous wood chips are then fed into a pre-steaming spiral for preheating and softening. Step 2, Pressure Impregnation: The preheated and softened hardwood chips are fed into the screw feeder. Under the pushing and compression of the variable diameter and variable pitch screw shaft with a compression ratio of 1:2 to 1:2.5, the hardwood chips form a plug in the plug tube to block the vapor-liquid pressure in the vertical steam pipe. After the plug is formed, the hardwood chips enter the T-tube, mix with the medicine and steam added through the T-tube, and then enter the vertical steam pipe through the expansion joint. Pressure impregnation is carried out at 135 to 165°C for 6 to 10 minutes. Step 3, Filament Separation and Reaction: The pressure-impregnated hardwood chips are evenly discharged from the feeder at the bottom of the vertical steam pipe and fed into the filament separator by the discharge screw. The feed screw then feeds the hardwood chips between the stationary and moving grinding discs. Filament separation is performed under the condition that the gap between the stationary and moving grinding discs is 2-2.5mm, so that the hardwood chips are formed into fine filaments. The filaments are sprayed into the hydrocyclone separator under the system pressure and auxiliary compressed air to separate the material from the flash steam. The separated flash steam is returned to the pre-steam screw for preheating the hardwood chips. The separated material is fed into the No. 1 reaction chamber by the feed plug screw and reacted for 60-90 minutes. Step 4, coarse grinding, reaction and fine grinding: The material after reaction in reaction chamber 1 is fed into high-consistency mill 1 for coarse grinding via the feed screw of mill 1. The coarsely ground material is fed into reaction chamber 2 via discharge screw of mill 1 for reaction for 60 minutes, and then fed into high-consistency mill 2 via feed screw of mill 2 for fine grinding. Both high-consistency mill 1 and high-consistency mill 2 use atmospheric pressure high-consistency grinding slurry. During the grinding process, the gap between the stationary disc and the moving disc is 0.2-0.4 mm. Step 5, Submersion Removal: The finely ground slurry is sent to a submersion removal tank for submersion removal treatment; Step 6, washing and concentration: The pulp after de-potting is washed and concentrated sequentially through the No. 1 rotary drum pulper, the dilution screw, and the No. 2 rotary drum pulper, and then discharged through the pulp discharge screw to obtain the uncolored mechanical pulp.
[0018] Further, in step one, the miscellaneous wood chips are quantitatively fed from the metering hopper to the conveyor belt, enter the drum through the feed inlet of the cylindrical screen, and the drum drive mechanism drives the drum to rotate. During the rotation of the drum, the miscellaneous wood chips are screened sequentially through a large-hole screen with a screen size of φ40~45mm and a small-hole screen with a screen size of φ6~8mm. The qualified miscellaneous wood chips obtained by screening are discharged from the qualified chip outlet. After iron impurities are removed by an electromagnet, they enter the chip washing machine. After washing, the miscellaneous wood chips are dewatered by a dewatering spiral with an inclination angle of 30° to remove free water.
[0019] The washing water discharged from the dewatering spiral passes through a fine screen with 0.5mm gaps to remove large particles of impurities and then enters a vertical flow sedimentation tank. The sedimentation tank settles for 60-70 minutes. The clarified liquid overflows from the top of the sedimentation tank to the clarification tank and is returned to the washing system by the washing water pump. The silt and heavy impurities at the bottom of the sedimentation tank are discharged into the water treatment system by the sludge discharge pump.
[0020] Furthermore, in step two, the pressure and temperature inside the vertical steaming pipe are detected through the pressure detection port and temperature detection port one, and the material level is detected through the tension gauges on material level detection ports one, two and three, and the material level inside the vertical steaming pipe is kept within the height range corresponding to material level detection ports one and three, so as to ensure the pressure impregnation time of the wood chips inside the vertical steaming pipe.
[0021] Furthermore, in step five, the finely ground slurry is fed into the anti-submersion tank via the discharge screw of mill #2, the lifting screw, and the feed screw of the anti-submersion tank. Hot water is used to adjust the slurry concentration to 4-5%, the slurry temperature is maintained at 72-75℃, and the anti-submersion time is 60-80 minutes. In step six, the dewatered pulp is pumped into the No. 1 rotary drum press with an initial pulp concentration of 4-5%. After passing through the gravity dewatering zone, the pulp concentration increases to 7-8%. It then enters the rotary drum dewatering zone through the angle between the upper and lower screens. After rotary drum dewatering and pressing by the 3rd to 4th stage press rollers, the concentration increases to 30-35%. The pulp is then discharged into the dilution screw by the pulp scraper. Washing water is added to the dilution screw to adjust the pulp concentration to 6-8%. The pulp then enters the No. 2 rotary drum press for further washing and dewatering, increasing the pulp concentration to 33-38%. Finally, the pulp is discharged through the discharge screw.
[0022] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention addresses the characteristics of mixed hardwood raw materials, which include a variety of tree species and significant differences in hardness. Before entering the pressure impregnation process, the hardwood chips undergo quantitative feeding, grading and screening, iron removal, chip washing, and dehydration. A cylindrical sieve separates large chips, qualified chips, and fragments using both large and small mesh screens, ensuring a relatively uniform chip size for subsequent processes. The chip washing and dehydration processes simultaneously remove mud, heavy impurities, and free water. Through this pretreatment, the impact of differences in chip size, cleanliness, and moisture content on subsequent impregnation and pulping processes can be reduced, providing more uniform raw material conditions for the continuous and stable processing of mixed hardwood species.
[0023] 2. In this invention, a pre-steaming spiral, a spiral feeder, a T-tube, an expansion joint, and a vertical steaming pipe are continuously coordinated in the pressure impregnation section. After pre-steaming and softening, the hardwood chips are compressed by a variable-diameter, variable-pitch spiral to form a plug, sealing the vapor-liquid pressure inside the vertical steaming pipe while continuously feeding. The wood chips, chemical solution, and steam are mixed at the T-tube and then enter the vertical steaming pipe, where they are pressure impregnated at 135–165°C for 6–10 minutes. The vertical steaming pipe controls the material level through multi-point material level detection, and the bottom feeder evenly discharges the material, ensuring a relatively stable pressure impregnation time for the wood chips during continuous operation. This structure integrates continuous feeding, pressure sealing, chemical mixing, impregnation, and stable discharge, which helps to reduce fluctuations in the impregnation and softening degree caused by differences in the properties of different hardwood chips.
[0024] 3. The main feature of this invention is that the wood chips after pressure impregnation do not directly enter the conventional high-consistency pulping process, but instead first enter a fiber separator for decomposition. The fiber separator uses a large-toothed grinding disc for decomposition, with a relatively large working gap of 2-2.5 mm between the moving and stationary discs. This allows the impregnated wood chips to form fine filaments under the kneading action, and ensures that the chemical solution continues to be in full contact with the material during the fiber separation process. Subsequently, the material enters the No. 1 reaction chamber for 60-90 minutes to further impregnate and soften the fiberized material before it enters the formal pulping process. Through the continuous treatment of "pressure impregnation - large-gap fiber separation - post-fiber reaction", the wood chips can be decomposed and further softened under lower intensity mechanical action, reducing the dependence on high-intensity pulping treatment. The power consumption of this fiber separator is about 1 / 3 to 1 / 4 of that of a traditional high-consistency mill.
[0025] 4. This invention adopts a graded treatment method of "coarse grinding - reaction - fine grinding". The material after being fully impregnated and softened by fiber separation is first coarsely ground by No. 1 high-consistency mill, then enters No. 2 reaction chamber for 60 minutes of further reaction, and is then finely ground by No. 2 high-consistency mill. Both high-consistency mills use atmospheric pressure high-consistency pulping, with a working gap of 0.2-0.4 mm. This process does not concentrate all mechanical processing in one pulping process, but sets a reaction stage between two pulping processes, so that the softening and fiberization processes of the material are carried out in stages. This helps to reduce the fluctuation of pulping load caused by the difference in hardness and impregnation state of different hardwoods, and improves the problem of more fiber bundles and unstable pulp quality in the pulp.
[0026] 5. This invention provides a continuous system for energy utilization after pressure impregnation and fiber separation, as well as for post-grinding pulp treatment. After fiber separation, the material is separated from flash steam via a cyclone separator. The flash steam is returned to the pre-steaming screw for preheating the wood chips, while the material enters subsequent reaction processes, thus achieving the reuse of flash steam heat. The finely ground pulp is de-latented at a concentration of 4-5% and a temperature of 72-75°C for 60-80 minutes, allowing the fibers that have curled, twisted, and have residual internal stress after high-consistency grinding to relax. Subsequently, the pulp undergoes a second dewatering and concentration process after intermediate dilution and washing using two series-connected rotary drum extruders, ensuring continuous washing and concentration. This treatment, combined with the front-end pressure impregnation, fiber separation, and graded grinding, improves the continuity and stability of the entire mixed hardwood natural-colored mechanical pulp production process. Attached Figure Description
[0027] Figure 1 This is a schematic diagram of the overall process flow of the process and equipment for producing unbleached chemimechanical pulp using miscellaneous wood as raw material according to the present invention; Figure 2 This is a schematic diagram of the cylindrical sieve in this invention; Figure 3 This is a schematic diagram of the screw feeder in this invention; Figure 4 This is a schematic diagram of the vertical steam pipe in this invention; Figure 5 This is a schematic diagram of the fiber splitting machine in this invention; Figure 6 This is a schematic diagram of the rotary drum pulper in this invention.
[0028] In the diagram: 1. Metering hopper; 2. Conveyor belt; 3. Cylindrical screen; 4. Electromagnet; 5. Feeding belt; 6. Washing machine; 7. Dewatering screw; 8. Pre-steaming screw; 9. Screw feeder; 10. T-tube; 11. Expansion joint; 12. Vertical steaming pipe; 13. Feeder; 14. Discharge screw; 15. Fiber separator; 16. Hydrocyclone separator; 17. Plug screw; 18. Reaction chamber #1; 19. Feed screw for mill #1; 20. High-concentration mill #1 Mill; 21. Discharge screw of No. 1 mill; 22. Reaction chamber No. 2; 23. Feed screw of No. 2 mill; 24. High-consistency mill No. 2; 25. Discharge screw of No. 2 mill; 26. Lifting screw; 27. Feed screw of submersion elimination tank; 28. Submersion elimination tank; 29. Slurry pump; 30. Rotary drum slurry press No. 1; 31. Dilution screw; 32. Rotary drum slurry press No. 2; 33. Slurry discharge screw; 34. Fine screen; 35. Sedimentation tank; 36. Clarification tank; 37. Washing... 38. Sludge pump; 301. Feed inlet; 302. Large piece outlet; 303. Qualified piece outlet; 304. Crushed material outlet; 305. Drum; 306. Large-hole screen; 307. Small-hole screen; 308. Drum drive mechanism; 901. Feed inlet; 902. Transmission mechanism; 903. Material plug tube; 904. Screw shaft; 1201. Feed inlet; 1202. Pressure detection port; 1203. Temperature detection port one; 1204. 1205. Material level detection port 1; 1206. Material level detection port 2; 1207. Steam inlet; 1208. Temperature detection port 2; 2001. Feed screw; 2002. Stationary grinding disc; 2003. Moving grinding disc; 2004. Discharge port; 3001. Feed inlet; 3002. Gravity dewatering zone; 3003. Angle between upper and lower screens; 3004. Rotary drum; 3005. Press roller; 3006. Slurry scraper. Detailed Implementation
[0029] The technical solution of the present invention will be further described below with reference to the accompanying drawings. It should be noted that the following embodiments are used to illustrate the equipment composition, connection relationship and process operation of the present invention, so that those skilled in the art can implement the present invention accordingly, and are not intended to impose additional limitations on the scope of protection of the present invention.
[0030] like Figures 1-6 As shown, this invention provides a process and equipment for producing unbleached mechanical pulp from mixed hardwoods. The mixed hardwoods used include thinnings, small-diameter timber, branch timber, and mixed hardwoods of multiple species. The entire production system includes, in sequence along the material conveying direction, a dry and wet material preparation section, a pressure impregnation and fiber separation section, a pulping section, and a desulfurization and washing section, and is equipped with a washing water treatment system. The hardwood chips are sequentially subjected to screening, iron removal, washing, dewatering, pre-steaming, pressure impregnation, fiber separation, reaction, coarse grinding, re-reaction, fine grinding, desulfurization, and washing and concentration treatment to finally obtain unbleached mechanical pulp.
[0031] I. Dry and wet preparation methods and treatment of washing water The mixed wood is first processed into wood chips by a chipper, and the wood chips are fed into the metering silo 1 by a loader. The metering silo 1 includes a silo body and two variable frequency speed control discharge screws. By adjusting the speed of the two discharge screws, the amount of wood chips fed is controlled, thereby realizing continuous quantitative feeding to the subsequent pulping system and providing a material quantity basis for the processing capacity of the subsequent pulping system and the amount of chemical solution added.
[0032] The discharge end of the metering hopper 1 is connected to the conveyor belt 2, and the wood chips are conveyed to the cylindrical screen 3 via the conveyor belt 2; the cylindrical screen 3 is used to screen the wood chips by particle size before they enter the subsequent washing and impregnation processes.
[0033] like Figure 2 As shown, the cylindrical screen 3 includes a feed inlet 301, a large-piece outlet 302, a qualified-piece outlet 303, a crushed material outlet 304, a drum 305, a large-hole screen 306, a small-hole screen 307, and a drum drive mechanism 308. The drum drive mechanism 308 is connected to the drum 305 for driving the drum 305 to rotate. The large-hole screen 306 and the small-hole screen 307 are arranged inside the drum 305, wherein the screen aperture of the large-hole screen 306 is φ40~45mm, and the screen aperture of the small-hole screen 307 is φ6~8mm.
[0034] After the mixed wood chips enter the drum 305 through the feed inlet 301, the drum 305 rotates at a constant speed under the drive of the drum drive mechanism 308. The mixed wood chips are tumbled with the drum 305 and move towards the discharge end. The qualified chips and scraps in the mixed wood chips pass through the large-hole screen 306. The large-sized wood chips are intercepted by the large-hole screen 306 and discharged from the large-chip outlet 302 during the rotation of the drum 305. The material passing through the large-hole screen 306 continues to be screened. The scraps pass through the small-hole screen 307 and are discharged from the scrap outlet 304. The qualified wood chips are intercepted by the small-hole screen 307 and discharged from the qualified chip outlet 303. The two-stage screening by the large-hole screen 306 and the small-hole screen 307 separates the large chips, qualified chips and scraps, so that the wood chips entering the subsequent process are relatively concentrated in size.
[0035] Wood chips discharged from qualified chip outlet 303 fall onto feeding belt 5 and pass through electromagnet 4 during their transport to the chip washer 6. Electromagnet 4 removes iron impurities from the wood chips. After iron removal, the wood chips enter the chip washer 6 and are thoroughly mixed with washing water. Through water washing and gravity, dust on the surface of the wood chips and heavy impurities such as mud and sand mixed in the wood chips are removed, while the moisture content of different wood chips is initially balanced.
[0036] After washing, the wood chips enter the dewatering spiral 7; the dewatering spiral 7 is an inclined spiral dewatering device with a filter screen, and its inclination angle is 30°; during the conveying process in the dewatering spiral 7, the free water carried by the wood chips is discharged through the filter screen, and the wood chips after the free water is removed are conveyed by the dewatering spiral 7 to the pre-steaming spiral 8.
[0037] The washing water separated by the dewatering spiral 7 enters the washing water treatment system; the washing water treatment system includes a fine screen 34, a sedimentation tank 35, a clarification tank 36, a washing water pump 37, and a sludge discharge pump 38; the drain end of the dewatering spiral 7 is connected to the fine screen 34, which is a drum screen with a screen opening of 0.5 mm, used to remove sawdust and other larger particulate impurities from the washing water.
[0038] The washing water after being treated by the fine screen 34 enters the sedimentation tank 35. The sedimentation tank 35 adopts a vertical flow sedimentation structure. The washing water undergoes sedimentation treatment in the sedimentation tank 35 for 60 to 70 minutes. The silt and other heavy impurities settle to the bottom of the sedimentation tank 35, and the clarified liquid overflows from the top of the sedimentation tank 35 to the clarification tank 36. The clarified water in the clarification tank 36 is returned to the washing machine 6 for recycling via the washing water pump 37. The silt and other heavy impurities at the bottom of the sedimentation tank 35 are discharged into the water treatment system via the sludge discharge pump 38.
[0039] II. Pressure Impregnation and Splitting After dehydration, qualified wood chips enter the pre-steaming screw 8. The pre-steaming screw 8 is a screw conveyor with a steam inlet pipe. The wood chips are heated while being conveyed in the pre-steaming screw 8. The pre-steaming screw 8 uses the flash steam separated by the subsequent cyclone separator 16 to preheat the wood chips, so that the wood chips are initially heated and softened, which is beneficial to the subsequent screw feeding. At the same time, it reduces fiber damage caused by extrusion and tearing during the compression feeding process, and reuses the flash steam generated by the fiber separation spray.
[0040] The discharge end of the pre-steaming screw 8 is connected to the screw feeder 9; for example Figure 3 As shown, the screw feeder 9 includes a feed inlet 901, a transmission mechanism 902, a feed plug tube 903, and a screw shaft 904; the transmission mechanism 902 is connected to the screw shaft 904 for driving the screw shaft 904 to rotate; the screw shaft 904 adopts a variable diameter and variable pitch screw structure with a compression ratio of 1:2 to 1:2.5.
[0041] After being preheated and softened, the wood chips enter the screw feeder 9 through the inlet 901. Driven by the transmission mechanism 902, the screw shaft 904 rotates and conveys the wood chips toward the feed plug tube 903. Under the action of the variable diameter and pitch screw and the corresponding compression space, the wood chips are gradually compressed and form a feed plug in the feed plug tube 903. The feed plug is used to seal the steam-liquid pressure inside the vertical steam pipe 12, preventing steam and liquid from backflowing toward the screw feeder 9, while ensuring that the wood chips can continuously enter the subsequent pressure impregnation system.
[0042] The discharge end of the feed plug tube 903 is connected to the T-tube 10, which is located between the screw feeder 9 and the vertical steaming tube 12. The wood chips conveyed by the screw feeder 9 enter the T-tube 10. The material, medicine, and some steam converge and mix at the T-tube 10 before entering the pressure impregnation system. The T-tube 10 is also equipped with an anti-backflow device consisting of a cylinder and a cone sealing device. The anti-backflow device cooperates with the feed plug formed by the screw feeder 9 to maintain a dynamic balance of pressure on the feed side and inside the vertical steaming tube 12, so as to ensure that the pressure impregnation process is continuous.
[0043] T-shaped pipe 10 is connected to vertical steam pipe 12 via expansion joint 11. Expansion joint 11 is used to compensate for the thermal expansion displacement generated during the process of vertical steam pipe 12 rising from room temperature to working temperature, so as to reduce the impact of thermal expansion on the normal operation of screw feeder 9 and upstream and downstream connected equipment of vertical steam pipe 12.
[0044] like Figure 4 As shown, the vertical steam pipe 12 is arranged vertically. The vertical steam pipe 12 is equipped with a feed inlet 1201, a pressure detection port 1202, a temperature detection port 1203, a material level detection port 1204, a material level detection port 2 1205, a material level detection port 3 1206, a steam inlet 1207, and a temperature detection port 2 1208. Wood chips, medicine liquid, and some steam enter the vertical steam pipe 12 through the feed inlet 1201, and steam is added through the steam inlet 1207 to further heat up the material.
[0045] The immersion temperature inside the vertical steam tube 12 is controlled at 135-165℃, and the holding time is 6-10 minutes. The pressure detection port 1202 is used to detect the pressure inside the vertical steam tube 12, and the temperature detection port 1203 is used to detect the temperature at the corresponding position inside the vertical steam tube 12. The vertical steam tube 12 is also equipped with a second temperature detection port 1208 for monitoring the working status of the vertical steam tube 12.
[0046] Material level detection ports 1204, 1205, and 1206 are set along the height of the vertical steam pipe 12. Each material level detection port is equipped with a tension meter and outputs a material level signal. During production, the material level in the vertical steam pipe 12 is kept within the height range corresponding to material level detection ports 1204 and 1206 to maintain a relatively stable material quantity and ensure that the wood chips have the appropriate pressure impregnation time.
[0047] A feeder 13 is installed at the bottom of the vertical steaming tube 12. The main working part of the feeder 13 is a scraper. After the wood chips that have completed pressure impregnation run to the bottom of the vertical steaming tube 12, the feeder 13 continuously and evenly pushes out the bottom material and sends it to the discharge screw 14, so that the wood chips fall at a uniform speed in the vertical steaming tube 12. The discharge screw 14 is set between the feeder 13 and the splitting machine 15, and is used to continuously transport the wood chips that have completed pressure impregnation to the splitting machine 15.
[0048] like Figure 5 As shown, the main body of the fiber separator 15 includes a feeding mechanism and a fiber separating mechanism; the feeding mechanism includes a feeding screw 2001, which adopts a double-headed screw forced feeding structure; the fiber separating mechanism includes a stationary grinding disc 2002 and a moving grinding disc 2003 that can move forward and backward relative to the stationary grinding disc 2002; the fiber separator 15 is also provided with a discharge port 2004.
[0049] The main structure of the fiber separator 15 is similar to that of the high-consistency pressure mill, but it is mainly used to separate and loosen wood chips after pressure impregnation. The stationary grinding disc 2002 and the moving grinding disc 2003 are loosening type large tooth groove grinding discs with fiber separation as the main function. During operation, the working gap between the stationary grinding disc 2002 and the moving grinding disc 2003 is 2 to 2.5 mm.
[0050] Wood chips conveyed by the discharge screw 14 are forcibly fed into the splitting area between the stationary grinding disc 2002 and the moving grinding disc 2003 by the feed screw 2001. Under the kneading action of the moving and stationary grinding discs, the wood chips are split into fine filaments. The wood chips have been treated with liquid and steam before splitting. During the splitting process, the internal structure of the wood chips is further opened up, and the liquid can continue to fully contact and mix with the material, creating conditions for subsequent softening reaction. Since the splitting machine 15 uses large toothed grinding discs that are mainly used for disintegration and splitting, and maintains a large working gap of 2 to 2.5 mm, its power consumption is about 1 / 3 to 1 / 4 of that of a traditional high-concentration mill.
[0051] The material after shaving is discharged from the outlet 2004 and sprayed into the cyclone separator 16 under the pressure of the vertical steam pipe 12 system and the action of auxiliary compressed air. The cyclone separator 16 separates the sprayed material from the flash steam. The separated material enters the feed plug screw 17, while the flash steam returns to the pre-steaming screw 8 through the pipeline for preheating and softening of newly entered wood chips.
[0052] The feed plug screw 17 adopts a variable diameter and variable pitch screw structure. The material is compressed during the conveying process and forms a feed plug. The feed plug blocks the flash steam, allowing the flash steam to enter the pre-steaming screw 8 along the return pipeline. At the same time, the material is conveyed by the feed plug screw 17 to the No. 1 reaction chamber 18.
[0053] Reaction chamber 18 adopts a horizontal flow bed reaction chamber. The material after filament separation is kept at a constant temperature in reaction chamber 18 for 60-90 minutes, so that the chemical solution can further act on the material that has formed fine filaments, so that the material can continue to be impregnated and softened, creating conditions for subsequent high-concentration pulping.
[0054] III. Pulping After the reaction in reaction chamber 18 is completed, the material is fed into high-concentration mill 20 via feed screw 19 of mill 1.
[0055] The No. 1 high-consistency mill 20 is an atmospheric pressure high-consistency mill. Its main body includes a feeding mechanism and a grinding mechanism. The feeding mechanism adopts a double-headed spiral forced feeding. The grinding mechanism includes a fixed plate and a moving plate that can be adjusted forward and backward. During operation, the grinding gap between the fixed plate and the moving plate is controlled at 0.2 to 0.4 mm.
[0056] After pressure impregnation, fiber separation, and a 60-90 minute heat preservation reaction, the material is first coarsely ground in the No. 1 high-concentration mill 20 to further mechanically fiberize the fine filament strip material.
[0057] The discharge end of the No. 1 high-concentration mill 20 is connected to the No. 2 reaction chamber 22 through the discharge screw 21 of the No. 1 mill; the coarsely ground material enters the No. 2 reaction chamber 22 through the discharge screw 21 of the No. 1 mill and is kept at a temperature for 60 minutes in the No. 2 reaction chamber 22.
[0058] After the intermediate reaction is completed, the material is fed into the No. 2 high-consistency mill 24 via the feed screw 23 of the No. 2 mill. The No. 2 high-consistency mill 24 also adopts the atmospheric pressure high-consistency grinding method. Its feeding mechanism adopts double-headed screw forced feeding. The grinding mechanism includes a fixed plate and a moving plate that can be adjusted forward and backward. During operation, the grinding gap between the fixed plate and the moving plate is 0.2-0.4mm. After being finely ground by the No. 2 high-consistency mill 24, the material reaches the pulp state required for subsequent pulp processing.
[0059] Therefore, in the formal grinding stage, the material is successively subjected to coarse grinding in No. 1 high-consistency mill 20, intermediate reaction in No. 2 reaction chamber 22, and fine grinding in No. 2 high-consistency mill 24, so that the reaction softening and mechanical grinding are carried out in stages.
[0060] IV. Anti-flammation and washing concentration The slurry after fine grinding in the No. 2 high-consistency mill 24 is discharged through the No. 2 mill discharge screw 25, and then conveyed to the submersion elimination tank 28 through the lifting screw 26 and the submersion elimination tank feed screw 27.
[0061] The anti-sublimation tank 28 is used to treat the high-consistency refined slurry to remove sublimation. After the slurry enters the anti-sublimation tank 28, hot water is used to adjust the slurry concentration to 4-5%, the slurry temperature is maintained at 72-75℃, and the anti-sublimation time is 60-80 minutes.
[0062] During the high-consistency pulping process, the fibers are subjected to mechanical kneading and temperature effects, and some fibers will curl, twist, and form certain internal residual stress. The pulp is kept in a warm and low-concentration state in the subsidence tank 28, which allows the internal stress of the fibers to be gradually released and the fibers to be stretched, thereby improving the state of the pulp.
[0063] After the anti-submersion treatment is completed, the slurry is transported by slurry pump 29 to the No. 1 rotary drum slurry press 30.
[0064] like Figure 6As shown, the rotary drum press includes a feed inlet 3001, a gravity dewatering zone 3002, an angle between the upper and lower screens 3003, a rotary drum 3004, 3-4 stage pressing rollers 3005, and a pulp scraper 3006, and is equipped with a screen top, a screen bottom, and a pneumatic tensioning device.
[0065] After dewatering, the pulp, with a concentration of 4-5%, enters the No. 1 rotary drum pulper 30 through the feed inlet 3001. It first enters the gravity dewatering zone 3002, where some water is removed by gravity, increasing the pulp concentration from 4-5% to 7-8%. The pulp then enters the rotary drum dewatering zone through the angle between the upper and lower screens 3003, where it is dewatered by both the lower screen and the rotary drum 3004. Afterward, it continues to be pressed by the 3-4 stage press rollers 3005, increasing the pulp concentration to 30-35%.
[0066] After the first stage of pulping, the pulp is discharged into the dilution spiral 31 under the action of the pulp scraper 3006. The dilution spiral 31 is set between the No. 1 rotary drum pulper 30 and the No. 2 rotary drum pulper 32. Washing water is added into the dilution spiral 31 to fully mix the pulp with the washing water and adjust the pulp concentration from 30-35% to 6-8%.
[0067] After dilution and washing, the pulp enters the No. 2 rotary drum pulper 32, where it is dewatered and washed again, and finally concentrated to 33-38%. The pulp processed by the No. 2 rotary drum pulper 32 enters the pulp discharge screw 33 and is discharged from the screw, thus completing the production process of the natural color mechanical pulp of miscellaneous wood.
[0068] Through the continuous coordination of the No. 1 rotary drum pulper 30, the dilution screw 31 and the No. 2 rotary drum pulper 32, the pulp is first subjected to primary pulping and concentration, then diluted and washed with washing water, and then subjected to secondary pulping and concentration, thus completing the washing and concentration of the pulp in the continuous operation process.
[0069] V. Overall Operation Process In operation, thinned timber, small-diameter timber, branches and branches, and mixed mixed wood are chipped into wood chips. The wood chips first enter the metering silo 1, and are continuously and quantitatively fed into the conveyor belt 2. The conveyor belt 2 feeds the wood chips into the cylindrical screen 3. After two-stage screening by the large-hole screen 306 and the small-hole screen 307, the large-sized wood chips are discharged from the large chip outlet 302, the crushed material is discharged from the crushed material outlet 304, and the qualified wood chips are discharged from the qualified chip outlet 303.
[0070] Qualified wood chips are conveyed by the feeding belt 5 and iron impurities are removed by the electromagnet 4 before entering the chip washer 6. Dust and heavy impurities are removed in the chip washer 6 and the moisture content is initially balanced. After that, free water is removed by the dewatering spiral 7. The dewatered wood chips enter the pre-steaming spiral 8 and are preheated and softened by the flash steam returned by the cyclone separator 16.
[0071] The preheated wood chips enter the screw feeder 9 and are compressed by the variable diameter and pitch screw shaft 904. After forming a material plug in the material plug tube 903, they are continuously fed into the T-tube 10. The wood chips are fully contacted and mixed with the medicine and some steam at the T-tube 10, and then enter the vertical steaming tube 12 through the expansion joint 11. They are then pressure impregnated at 135-165℃ for 6-10 minutes. The vertical steaming tube 12 detects the material level through tension gauges corresponding to three material level detection ports, keeping the material level between material level detection port 1204 and material level detection port 1206.
[0072] The wood chips that have completed pressure impregnation are evenly discharged from the feeder 13 at the bottom of the vertical steam pipe 12, so that the wood chips fall at a uniform speed in the vertical steam pipe 12 and are fed into the splitting machine 15 through the discharge screw 14. The wood chips are split into fine strips by working gap of 2 to 2.5 mm between the stationary grinding disc 2002 and the moving grinding disc 2003.
[0073] After the material is separated into fibers, it is sprayed into the hydrocyclone separator 16 under the action of system pressure and auxiliary compressed air. The hydrocyclone separator 16 separates the material from the flash steam. The flash steam is returned to the pre-steaming screw 8 for preheating of the newly entered wood chips. The material enters the No. 1 reaction chamber 18 through the feed plug screw 17 and is kept at a temperature for 60-90 minutes in the No. 1 reaction chamber 18.
[0074] After the reaction, the material enters the No. 1 high-consistency mill 20 through the feed screw 19 of the No. 1 mill for coarse grinding. The coarsely ground material enters the No. 2 reaction chamber 22 through the discharge screw 21 of the No. 1 mill for heat preservation and reaction for 60 minutes, and then enters the No. 2 high-consistency mill 24 through the feed screw 23 of the No. 2 mill for fine grinding. Both the No. 1 high-consistency mill 20 and the No. 2 high-consistency mill 24 are atmospheric pressure high-consistency mills, and their grinding gap is 0.2-0.4 mm.
[0075] The finely ground slurry enters the de-deposition tank 28 via the discharge screw 25 of mill #2, the lifting screw 26, and the de-deposition tank feed screw 27. Under the conditions of slurry concentration of 4-5% and temperature of 72-75℃, the de-deposition is eliminated for 60-80 minutes. The de-deposition slurry is then pumped by slurry pump 29 to mill #1 rotary drum press 30, where it is concentrated to 30-35% after gravity dewatering, rotary drum dewatering, and pressing. Subsequently, it enters the dilution screw 31, where washing water is added and the slurry concentration is adjusted to 6-8%. Then, it enters mill #2 rotary drum press 32 for further washing and dewatering, and finally, it is concentrated to 33-38% and discharged via the discharge screw 33.
[0076] In the above production process, the flash steam separated by the propeller separator 16 is returned to the pre-steaming spiral 8 for wood chip preheating; the washing water discharged from the dewatering spiral 7 is treated by the fine screen 34, the sedimentation tank 35 and the clarification tank 36, and then returned to the washing machine 6 for recycling via the washing water pump 37; the mud and other heavy impurities at the bottom of the sedimentation tank 35 are discharged by the sludge discharge pump 38.
[0077] Thus, the present invention forms a continuous production process consisting of quantitative feeding of miscellaneous wood chips, screening and washing, preheating and softening, continuous pressure feeding with a feed plug, pressure impregnation in a vertical steam tube, large gap splitting, reaction after splitting, coarse grinding, intermediate reaction, fine grinding, desulfurization, and two-stage washing and concentration, while also forming a flash steam reuse and chip washing water recycling process.
[0078] The foregoing has shown and described the basic principles, main features and advantages of the present invention. Various changes and modifications can be made to the present invention without departing from the spirit and scope thereof, and all such changes and modifications fall within the scope of the present invention as claimed.
Claims
1. A device for producing unbleached chemimetallic pulp from mixed hardwoods, characterized in that, The system includes, sequentially arranged along the material conveying direction, a pre-steaming spiral (8), a spiral feeder (9), a T-tube (10), an expansion joint (11), a vertical steaming pipe (12), a feeder (13), a discharge spiral (14), a fiber separator (15), a cyclone separator (16), a feed plug spiral (17), a No. 1 reaction chamber (18), a No. 1 mill feed spiral (19), a No. 1 high-consistency mill (20), a No. 1 mill discharge spiral (21), a No. 2 reaction chamber (22), a No. 2 mill feed spiral (23), and a No. 2 high-consistency mill (24); the pre-steaming spiral (8) The discharge end of the screw feeder (9) is connected to the inlet (901) of the screw feeder (9). The screw feeder (9) includes a transmission mechanism (902), a material plug tube (903) and a screw shaft (904). The transmission mechanism (902) is connected to the screw shaft (904). The screw shaft (904) is a variable diameter and variable pitch screw with a compression ratio of 1:2 to 1:2.
5. The discharge end of the material plug tube (903) is connected to the T-tube (10). The T-tube (10) is provided with a liquid medicine and steam addition part and is connected to the vertical steam pipe (12) through an expansion joint (11). The feeder (13) is located at the bottom of the vertical steam pipe (12). The discharge side of the feeder (13) is connected to the fiber separator (15) through the discharge screw (14). The fiber separator (15) includes a feed screw (2001), a stationary grinding disc (2002), a moving grinding disc (2003), and a discharge port (2004). The feed screw (2001) is a double-headed spiral forced feeding structure. The stationary grinding disc (2002) and the moving grinding disc (2003) are large-tooth groove grinding discs for fiber separation. The moving grinding disc (2003) can move forward and backward relative to the stationary grinding disc (2002). During operation, the gap between the stationary grinding disc (2002) and the moving grinding disc (2003) is 2 to 2.5 mm. The discharge port (2004) of the fiber separator (15) is connected to the cyclone separator (16). The material outlet of the cyclone separator (16) is connected to the No. 1 reaction chamber (18) through the feed plug screw (17). The flash steam outlet of the cyclone separator (16) is connected to the pre-steam screw (8). The feed plug screw (17) is a variable diameter and variable pitch screw. The No. 1 reaction chamber (18) is a horizontal flow bed reaction chamber. The No. 1 reaction chamber (18) is connected to the No. 1 high-concentration mill (20) via the No. 1 mill feed screw (19). The No. 1 high-concentration mill (20) is connected to the No. 2 reaction chamber (22) via the No. 1 mill discharge screw (21). The No. 2 reaction chamber (22) is connected to the No. 2 high-concentration mill (24) via the No. 2 mill feed screw (23). Both the No. 1 high-concentration mill (20) and the No. 2 high-concentration mill (24) are atmospheric pressure high-concentration mills. During operation, the gap between the fixed plate and the moving plate is 0.2 to 0.4 mm.
2. The equipment for producing unbleached phenolic pulp from miscellaneous wood as raw material according to claim 1, characterized in that, Upstream of the pre-steaming spiral (8) along the material conveying direction are arranged a metering hopper (1), a conveyor belt (2), a cylindrical screen (3), an electromagnet (4), a feeding belt (5), a film washer (6), and a dewatering spiral (7). The metering hopper (1) is equipped with two variable frequency speed-regulating discharge spirals. The dewatering spiral (7) is a spiral dewatering device with a filter screen and an inclination angle of 30°.
3. The equipment for producing unbleached phenolic pulp from mixed hardwoods according to claim 2, characterized in that, The cylindrical screen (3) includes a feed inlet (301), a large-piece outlet (302), a qualified-piece outlet (303), a crushed material outlet (304), a drum (305), a large-hole screen (306), a small-hole screen (307), and a drum drive mechanism (308); the drum drive mechanism (308) is connected to the drum (305) for driving the drum (305) to rotate; the large-hole screen (306) and the small-hole screen (307) are arranged on the drum (305). Inside the drum (305), the mesh size of the large-hole screen (306) is φ40~45mm, and the mesh size of the small-hole screen (307) is φ6~8mm. The wood chips entering the drum (305) are screened into large pieces, qualified pieces and broken pieces by the large-hole screen (306) and the small-hole screen (307) during the rotation of the drum (305). The large pieces, qualified pieces and broken pieces are discharged from the large piece outlet (302), the qualified piece outlet (303) and the broken piece outlet (304) respectively.
4. The equipment for producing unbleached phenolic pulp from miscellaneous wood as raw material according to claim 2, characterized in that, It also includes a fine screen (34), a sedimentation tank (35), a clarifier (36), a washing water pump (37), and a sludge pump (38). The drain end of the dewatering spiral (7) is connected to the fine screen (34), the outlet end of the fine screen (34) is connected to the sedimentation tank (35), the upper part of the sedimentation tank (35) is connected to the clarifier (36), the clarifier (36) is connected to the washing water inlet of the washing machine (6) through the washing water pump (37), and the bottom of the sedimentation tank (35) is connected to the water treatment system through the sludge pump (38). The fine screen (34) is a drum screen with a screen opening of 0.5 mm, and the sedimentation tank (35) is a vertical flow sedimentation tank.
5. The equipment for producing unbleached phenolic pulp from mixed hardwoods according to claim 1, characterized in that, The T-shaped pipe (10) is equipped with an anti-backflow device consisting of a cylinder and a cone sealing device; the vertical steam pipe (12) is equipped with a feed inlet (1201), a pressure detection port (1202), a temperature detection port one (1203), a material level detection port one (1204), a material level detection port two (1205), a material level detection port three (1206), a steam inlet (1207), and a temperature detection port two (1208). The material level detection ports one (1204), two (1205), and three (1206) are arranged along the height direction of the vertical steam pipe (12) and are respectively equipped with tension gauges for outputting material level signals. The feeder (13) includes a scraper plate, which is used to uniformly push the material at the bottom of the vertical steam pipe (12) to the discharge screw (14).
6. The equipment for producing unbleached phenolic pulp from miscellaneous wood as raw material according to claim 1, characterized in that, The discharge end of the No. 2 high-consistency mill (24) is connected in sequence to the No. 2 mill discharge screw (25), the lifting screw (26), the anti-submersion tank feed screw (27) and the anti-submersion tank (28). The anti-submersion tank (28) is connected to the No. 1 rotary drum extruder (30) through the slurry pump (29). The No. 1 rotary drum extruder (30) is connected to the No. 2 rotary drum extruder (32) through the dilution screw (31). The discharge end of the No. 2 rotary drum extruder (32) is connected to the discharge screw (33). Both the No. 1 rotary drum pulper (30) and the No. 2 rotary drum pulper (32) include a feed inlet (3001), a gravity dewatering zone (3002), an angle between the upper and lower screens (3003), a rotary drum (3004), a 3-4 stage pressing roller (3005), and a pulp scraper (3006), and are equipped with a screen feeding device, a screen lowering device, and a pneumatic tensioning device. The gravity dewatering zone (3002), the angle between the upper and lower screens (3003), the rotary drum (3004), and the pressing roller (3005) are arranged sequentially along the pulp conveying direction.
7. A process for producing unbleached phenolic pulp from mixed hardwoods, implemented using the equipment described in claim 1, characterized in that, Includes the following steps: Step 1, Pre-treatment of miscellaneous wood chips: Thinnings, small-diameter timber, branches or mixed miscellaneous wood are chipped to form miscellaneous wood chips. The miscellaneous wood chips are screened, iron removed, washed and dehydrated. The dehydrated miscellaneous wood chips are sent into a pre-steaming spiral (8) for preheating and softening. Step 2, pressure impregnation: The preheated and softened wood chips are fed into the screw feeder (9). Under the pushing and compression of the variable diameter and variable pitch screw shaft (904) with a compression ratio of 1:2 to 1:2.5, the wood chips form a plug in the plug tube (903) to seal the vapor-liquid pressure in the vertical steam tube (12). After the plug is formed, the wood chips enter the T-tube (10) and are mixed with the medicine and steam added by the T-tube (10). Then, they enter the vertical steam tube (12) through the expansion joint (11) and are pressure impregnated at 135 to 165°C for 6 to 10 minutes. Step 3, fiber separation and reaction: The pressure-impregnated hardwood chips are evenly discharged from the feeder (13) at the bottom of the vertical steam pipe (12), and fed into the fiber separator (15) by the discharge screw (14). The feed screw (2001) feeds the hardwood chips between the stationary grinding disc (2002) and the moving grinding disc (2003). Fiber separation is performed under the condition that the gap between the stationary grinding disc (2002) and the moving grinding disc (2003) is 2-2.5mm, so that the hardwood chips form fine filaments. The fiber separated material is sprayed into the hydrocyclone separator (16) under the action of system pressure and auxiliary compressed air, so that the material is separated from the flash steam. The separated flash steam is returned to the pre-steaming screw (8) for preheating of the hardwood chips. The separated material is sent into the No. 1 reaction chamber (18) via the feed plug screw (17) for reaction for 60-90 minutes. Step 4, coarse grinding, reaction and fine grinding: The material after reaction in reaction chamber 1 (18) is fed into high-consistency mill 1 (20) through feed screw (19) of mill 1 for coarse grinding. The coarsely ground material is fed into reaction chamber 2 (22) through discharge screw (21) of mill 1 for reaction for 60 minutes, and then fed into high-consistency mill 2 (24) through feed screw (23) of mill 2 for fine grinding. Both high-consistency mill 1 (20) and high-consistency mill 2 (24) use atmospheric pressure high-consistency grinding slurry. The gap between the fixed plate and the moving plate during the grinding process is 0.2 to 0.4 mm. Step 5, Submersion removal: The finely ground slurry is sent to the submersion removal tank (28) for submersion removal treatment; Step 6, washing and concentration: The pulp after de-flaking is washed and concentrated in sequence through the No. 1 rotary drum pulper (30), the dilution screw (31) and the No. 2 rotary drum pulper (32), and discharged through the pulp discharge screw (33) to obtain the uncolored mechanical pulp.
8. The process for producing unbleached phenolic pulp from mixed hardwoods according to claim 7, characterized in that, In step one, the wood chips are quantitatively fed from the metering hopper (1) to the conveyor belt (2), and enter the drum (305) through the feed inlet (301) of the cylindrical screen (3). The drum drive mechanism (308) drives the drum (305) to rotate. During the rotation of the drum (305), the wood chips are screened in sequence through the large hole screen (306) with a screen size of φ40~45mm and the small hole screen (307) with a screen size of φ6~8mm. The qualified wood chips obtained by screening are discharged from the qualified chip outlet (303). After the iron impurities are removed by the electromagnet (4), they enter the chip washing machine (6). After washing, the wood chips are dewatered by the dewatering spiral (7) with an inclination angle of 30°. The washing water discharged from the dewatering spiral (7) passes through a fine screen (34) with a 0.5 mm sieve to remove large particles of impurities and then enters a vertical flow sedimentation tank (35). The sedimentation tank (35) settles for 60-70 minutes. The clarified liquid overflows from the top of the sedimentation tank (35) to the clarification tank (36) and is returned to the washing system by the washing water pump (37). The mud and heavy impurities at the bottom of the sedimentation tank (35) are discharged into the water treatment system by the sludge discharge pump (38).
9. The process for producing unbleached chemimetallic pulp from mixed hardwoods according to claim 7, characterized in that, In step two, the pressure and temperature inside the vertical steam pipe (12) are detected by pressure detection port (1202) and temperature detection port one (1203). The material level is detected by tension gauges on material level detection port one (1204), material level detection port two (1205) and material level detection port three (1206). The material level inside the vertical steam pipe (12) is kept within the height range corresponding to material level detection port one (1204) and material level detection port three (1206) to ensure the pressure impregnation time of the wood chips inside the vertical steam pipe (12).
10. The process for producing unbleached phenolic pulp from mixed hardwoods according to claim 7, characterized in that, In step five, the finely ground slurry is fed into the submersion elimination tank (28) through the discharge screw (25) of the No. 2 mill, the lifting screw (26) and the feed screw (27) of the submersion elimination tank. Hot water is used to adjust the slurry concentration to 4-5%, the slurry temperature is maintained at 72-75℃, and the submersion elimination time is 60-80 minutes. In step six, the pulp after de-sublimation is pumped into the No. 1 rotary drum extruder (30) by the pulp pump (29). The initial pulp concentration is 4-5%. After passing through the gravity dewatering zone (3002), the pulp concentration increases to 7-8%. Then, it enters the rotary drum dewatering zone through the angle between the upper and lower screens (3003). After dewatering by the rotary drum (3004) and pressing by the 3-4 stage press rollers (3005), the concentration increases to 30-35%. The pulp is then discharged into the dilution screw (31) by the pulp scraper (3006). Washing water is added to the dilution screw (31) to adjust the pulp concentration to 6-8%. The pulp then enters the No. 2 rotary drum extruder (32) for washing and dewatering again, increasing the pulp concentration to 33-38%. The pulp is then discharged through the discharge screw (33).
Citation Information
Patent Citations
A chemical mechanical pulping process
CN104711880B
P-RC APMP pulping method of broadleaf wood mixed material
CN112176750A