A method for preparing composite filler for acid-free paper used in cultural relic preservation

By preparing porous calcium silicate/calcium carbonate composite fillers, the problems of low retention rate and high wear of acid-free paper fillers were solved, improving the stability of paper machine operation and the effect of cultural relic protection, and achieving efficient acid environment control.

CN123064047APending Publication Date: 2026-11-10CHINA NAT PULP & PAPER RES INST CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510600856.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The existing acid-free paper uses a single filler system with small particle size, low retention rate, and high abrasion, which leads to decreased paper machine performance, low porosity, low bulk, and inability to effectively mitigate the acidic environment, thus affecting the preservation of cultural relics.

Method used

A porous calcium silicate suspension was reacted with an inorganic salt solution to generate calcium silicate/calcium carbonate composite filler in situ. After filtration, washing, deflocculation and drying, a composite filler with high whiteness, low wear and good pH control effect was prepared for use in acid-free paper for cultural relic preservation.

Benefits of technology

It improves the porosity and bulk of acid-free paper, enhances its ability to control the slow release of acidic environments, improves the stability of paper machine operation, extends the preservation life of cultural relics, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123064047A_ABST
    Figure CN123064047A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a composite filler for acid-free paper used in cultural relic preservation. Using porous calcium silicate filler, which is stable (without pH control), soft in texture, high in porosity, and abundant in source, as a carrier, the method involves preparing a porous calcium silicate suspension, preparing an inorganic salt solution, preparing a calcium silicate / calcium carbonate composite filler suspension via in-situ generation, filtration, washing, deflocculation, and drying. This process yields a novel composite functional filler with high whiteness, low abrasion, good pH control, and high paper retention, meeting the requirements for use in acid-free paper for cultural relic preservation. The calcium silicate / calcium carbonate composite filler prepared by this invention can be used as a filler for acid-free lining paper, acid-free lining paperboard, and acid-free corrugated paper for cultural relic preservation, replacing traditional buffers such as calcium carbonate and magnesium carbonate, and improving the performance of cultural relic preservation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing a composite filler for acid-free paper used in the preservation of cultural relics, belonging to the field of papermaking technology. Background Technology

[0002] As one of the world's four ancient civilizations, my country boasts a history of over 5,000 years, leaving behind numerous precious historical relics throughout its splendid cultural heritage. These relics, as historical legacies, possess immense research and conservation value. However, with the passage of time and environmental changes, a large number of my country's cultural relics have suffered from aging or corrosion. According to statistics from the State Administration of Cultural Heritage, my country currently has over 33 million cultural relics in its collections, of which more than 50% exhibit varying degrees of corrosion, and over 2.3 million are severely corroded—a heartbreaking situation. Inappropriate preservation methods have severely accelerated the aging, deterioration, or destruction of cultural relics. Once these relics are damaged or lost, the cultural and historical significance they embody is also lost, representing an irreparable and enormous loss for my country and the world.

[0003] To ensure the long-term preservation and protection of cultural relics, professional and effective conservation materials are crucial. Among various conservation materials, acid-free paper is a very important carrier. It contains no acidic substances and, when used for conservation, will not cause acidic damage to the relics. Furthermore, its weakly alkaline buffer neutralizes acidic substances within the relics or in the external environment, thus reducing corrosion and extending the lifespan of the relics. The type, content, and slow-release effect of the weakly alkaline buffer used in acid-free paper largely determine its protective performance. Currently, the most commonly used buffer in acid-free paper is micron-sized calcium carbonate filler, which has advantages such as suitable alkalinity, wide availability, and high cost-effectiveness. Invention patent ZL201610899369.X (A method for manufacturing acid-free inner lining paper for cultural relic protection) and literature (Xu Wenjuan, Wu Laiming, Dai Hongqi. Performance study of acid-free paper for packaging cultural relics in museums. Cultural Relics Protection and Archaeological Science. 2014; 26(4): 25-9; Zhang Meiyun, Li Peiyi, Xia Xinxing. Application and research progress of durable acid-free paper. China Pulp & Paper. 2010(10): 71-4.) reported the application of calcium carbonate filler in the preparation of acid-free paper.

[0004] Although traditional acid-free paper using fillers such as calcium carbonate can slow down the acidification process of cultural relics by providing a weakly alkaline environment, it still has certain limitations. These include a single filler system, small filler particle size, low retention rate during filling, high abrasion and significant wear on the paper machine, uneven filler distribution leading to decreased paper machine performance, and the resulting acid-free paper having low bulk, low porosity, and requiring further improvement in its ability to control the slow release of acidic environments. Against this backdrop, developing new fillers for acid-free paper used in cultural relic preservation, and improving the production operability and performance of acid-free paper for cultural relic preservation, is of great significance to both the paper industry and the cause of cultural relic preservation. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing a composite filler for acid-free paper used in cultural relic preservation. Using porous calcium silicate filler, which is stable (without pH control), soft in texture, high in porosity, and abundant in source, as a carrier, the method involves preparing a porous calcium silicate suspension, preparing an inorganic salt solution, preparing a calcium silicate / calcium carbonate composite filler suspension via in-situ generation, filtration, washing, deflocculation, and drying. This process yields a novel composite functional filler with high whiteness, low abrasion, good pH control, and high paper retention, meeting the requirements for use in acid-free paper for cultural relic preservation. To achieve the above objective, this invention provides the following technical solution:

[0006] A method for preparing a composite filler for acid-free paper used in the preservation of cultural relics includes the following steps:

[0007] al. Preparation of porous calcium silicate suspension: The selected porous calcium silicate raw material is uniformly dispersed in water under stirring conditions to prepare a suspension with a mass concentration of 5-15% for later use;

[0008] a2. Preparation of aqueous solutions of inorganic salts:

[0009] (1) Preparation of calcium salt aqueous solution: Water-soluble calcium salts such as calcium chloride, calcium nitrate, and calcium gluconate are used as raw materials. They are completely dissolved in water at a certain concentration under stirring and then set aside.

[0010] (2) Preparation of carbonate aqueous solution: Sodium carbonate, potassium carbonate, ammonium carbonate and other water-soluble carbonates are used as raw materials and completely dissolved in water at a certain concentration under stirring.

[0011] a3. Preparation of calcium silicate / calcium carbonate composite filler suspension by in-situ generation method: Slowly add the calcium salt aqueous solution prepared in step a2 to the porous calcium silicate suspension prepared in step a1, stir thoroughly for 15-30 minutes, mix evenly, and while stirring, slowly add the carbonate aqueous solution prepared in step a2 to the above porous calcium silicate / calcium salt mixture, and after reacting thoroughly for 30-45 minutes, nano or micron calcium carbonate is generated in-situ in the pores and surface of the porous calcium silicate, thus obtaining a suspension of porous calcium silicate / calcium carbonate composite filler;

[0012] a4. Filtration, washing, deflocculation, and drying: Filtration and washing are performed to fully remove residual soluble inorganic salt ions from the calcium silicate / calcium carbonate composite filler. Then, moderate grinding, deflocculation, and drying are carried out to obtain a composite filler for cultural relic preservation with high whiteness, low abrasion, high retention rate, and good pH control performance. The filler has a whiteness ≥90% ISO, an average particle size of 3-15 μm, a pH value (10% concentration) of 8.0-9.5, an abrasion value ≤5 mg / 2000 times, and a calcium silicate to calcium carbonate mass ratio of 10:1-1:1.

[0013] Preferably, the molar ratio of calcium ions to calcium silicate in the water-soluble calcium salt added in step a3 is in the range of 0.116-1.160.

[0014] Preferably, the molar ratio of calcium ions in the water-soluble calcium salt added in step a3 to carbonate ions in the water-soluble carbonate added is 1:1.

[0015] Preferably, the prepared calcium silicate / calcium carbonate composite filler can be used as a filler for acid-free lining paper, acid-free lining paperboard, and acid-free corrugated paper for cultural relic protection, replacing traditional buffers such as calcium carbonate and magnesium carbonate, and improving the performance of cultural relic protection.

[0016] Preferably, the prepared calcium silicate / calcium carbonate composite filler accounts for 5%-30% of the total weight relative to the oven-dry acid-free paper.

[0017] Beneficial effects:

[0018] (1) Compared with traditional single-system fillers such as calcium carbonate for acid-free paper, the porous calcium silicate / calcium carbonate composite filler prepared by the present invention has advantages such as soft texture, low wear, high porosity, and better pH control effect. The acid-free paper for cultural relic protection prepared by adding it has high porosity, good looseness and thickness, good pH control for acidic substances generated by the cultural relic itself or the external environment, strong pressure buffering capacity, and can significantly improve the protection performance of cultural relics.

[0019] (2) When using the porous calcium silicate / calcium carbonate composite filler prepared by the present invention to produce paper for cultural relic protection, the operating stability of the wet and dry parts of the paper machine will be significantly improved, such as significantly increasing the filler retention rate, reducing wear on paper machine equipment (wire, sizing roll, calender roll, etc.), reducing steam consumption, reducing the number of paper breaks, and improving operating efficiency.

[0020] (3) The raw materials required for the preparation of porous calcium silicate / calcium carbonate composite filler of the present invention are widely available, low in cost, and simple in production process, making it easy to expand production and application. For example, porous calcium silicate can be an industrial by-product extracted from fly ash waste residue, and inorganic salts can be extracted from inorganic salt waste liquid in industrial production, which can effectively solve the pollution caused by industrial waste and achieve comprehensive utilization. Attached Figure Description

[0021] Figure 1 This is a scanning electron microscope (SEM) image of the calcium silicate / calcium carbonate composite filler prepared according to the present invention (taking a CaSiO3 / CaCO3 mass ratio of 2:1 as an example). Detailed Implementation

[0022] Example 1:

[0023] Add 9000 kg of tap water to a stainless steel container equipped with a stirrer. Slowly add 1000 kg of porous calcium silicate raw material (whiteness ≥90% ISO, average particle size 20-25 μm, porosity ≥0.35 mL / g, settling volume ≥5.0 mL / g, abrasion value ≤5 mg / 2000 times) extracted from high-alumina fly ash while stirring at 500 rpm to prepare a 10% calcium silicate suspension for later use. While stirring, add an aqueous solution containing 222 kg of calcium chloride to the above calcium silicate suspension. After stirring thoroughly for 30 minutes, slowly add an aqueous solution containing 211.8 kg of sodium carbonate. After stirring thoroughly for 45 minutes, silicic acid is generated. Calcium / calcium carbonate composite filler suspension: The above calcium silicate / calcium carbonate composite filler suspension is filtered and washed to fully remove soluble inorganic salt ions (based on chloride ion detection, washed until chloride ions are undetectable). Then, the concentration is adjusted to 10%, and the composite filler is moderately ground and deflocculated using a sand mill. The deflocculated composite filler is then spray-dried to obtain a high-whiteness, low-abrasion, high-retention rate, and good pH control performance composite filler for cultural relic preservation with a whiteness ≥90% ISO, an average particle size of 12-15 μm, a pH value (10% concentration) of 8.0-9.5, an abrasion value ≤5 mg / 2000 times, and a calcium silicate:calcium carbonate mass ratio of 5:1.

[0024] The above composite filler is used in acid-free backing paper for cultural relic preservation (basis weight 20-25 g / m³). 2 Through the addition of fillers and papermaking processes, including pulping, mixing, screening, purification, forming, pressing, drying, calendering and curling, acid-free lining paper for cultural relic protection with a composite filler content of 10-15% is produced. It has advantages such as high whiteness, good bulk, good pH control effect, and strong compression and buffering capacity. It can be used for lining, wrapping, isolation and repair of cultural relics, which can effectively improve the preventive protection effect of cultural relics and extend their life.

[0025] Example 2:

[0026] Add 4500 kg of tap water to a stainless steel container equipped with a stirrer. While stirring, slowly add 500 kg of porous calcium silicate raw material extracted from high-alumina fly ash to prepare a 10% concentration suspension. While stirring, add an aqueous solution containing 410 kg of calcium nitrate to the calcium silicate suspension. After stirring thoroughly for 30 minutes, slowly add an aqueous solution containing 345 kg of potassium carbonate. After stirring thoroughly for 45 minutes, a calcium silicate / calcium carbonate composite filler suspension is generated. The calcium silicate / calcium carbonate composite filler... The material suspension is filtered and washed to fully remove soluble inorganic salt ions. Then, the concentration is adjusted to 10%, and the composite filler is moderately ground and deflocculated using a sand mill. The deflocculated composite filler is then spray-dried to obtain a high-whiteness, low-abrasion, high-retention rate, and good pH control performance composite filler for cultural relic protection with a whiteness ≥90% ISO, an average particle size of 8-10 μm, a pH value (10% concentration) of 8.0-9.5, an abrasion value ≤5mg / 2000 times, and a calcium silicate:calcium carbonate mass ratio of 2:1.

[0027] The above composite filler is used in acid-free paperboard for cultural relic preservation (basis weight 120-250 g / m³). 2 Through the addition of fillers and papermaking processes, including pulping, mixing, screening, purification, forming, pressing, drying, calendering, and curling, a high-performance acid-free paperboard for cultural relic preservation with a composite filler content of 20-25% is produced. This paperboard boasts advantages such as high whiteness, good bulkiness, effective pH control, and strong compression buffering capacity. It can be used for preparing cultural relic cases, lining boards, and mounting, effectively enhancing the preventative protection of cultural relics and extending their lifespan.

[0028] Example 3:

[0029] Add 4500 kg of tap water to a stainless steel container equipped with a stirrer. While stirring, slowly add 500 kg of porous calcium silicate raw material synthesized by a hydrothermal method to prepare a 10% concentration suspension for later use. While stirring, add an aqueous solution containing 2247 kg of calcium gluconate to the above calcium silicate suspension. After stirring thoroughly for 30 minutes, slowly add an aqueous solution containing 530 kg of sodium carbonate. After stirring thoroughly for 45 minutes, a calcium silicate / calcium carbonate composite filler suspension is generated. The above calcium silicate / calcium carbonate composite filler... The material suspension is filtered and washed to fully remove soluble inorganic salt ions. Then, the concentration is adjusted to 10%, and the composite filler is moderately ground and deflocculated using a sand mill. The deflocculated composite filler is then spray-dried to obtain a high-whiteness, low-abrasion, high-retention rate, and good pH control performance composite filler for cultural relic protection with a whiteness ≥90% ISO, an average particle size of 5-8 μm, a pH value (10% concentration) of 8.0-9.5, an abrasion value ≤5 mg / 2000 times, and a calcium silicate:calcium carbonate mass ratio of 1:1.

[0030] The above composite filler is used in acid-free corrugated base paper and acid-free linerboard for cultural relic protection (basis weight 70-120 g / m²). 2 Through pulping, mixing, screening, purification, forming, pressing, drying, calendering, and curling processes, high-performance acid-free corrugated base paper and acid-free linerboard with a composite filler content of 25-30% are prepared for the preservation of cultural relics. The acid-free corrugated base paper and acid-free linerboard are then corrugated and laminated to prepare acid-free corrugated cardboard for the preservation of cultural relics. This cardboard has advantages such as high whiteness, good bulkiness, good pH control, and strong compression and buffering capacity. It can be used to make cardboard boxes, cases, lining boards, and mounting materials for the preservation of cultural relics, effectively improving the preventive protection effect and extending the life of cultural relics.

[0031] The present invention provides a method for preparing a composite filler for acid-free paper for cultural relic protection. The main physical properties of the calcium silicate / calcium carbonate composite filler are shown in Table 1. It is a new type of composite functional filler with high whiteness, low abrasion, good pH control effect, and high papermaking retention rate, which meets the requirements for use in acid-free paper for cultural relic protection.

[0032] Table 1. Main physical properties of calcium silicate / calcium carbonate composite fillers

[0033]

[0034] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a composite filler for acid-free paper used in the preservation of cultural relics, characterized in that, Includes the following steps: a1. Preparation of porous calcium silicate suspension: The selected porous calcium silicate raw material is uniformly dispersed in water under stirring conditions to prepare a suspension with a mass concentration of 5-15% for later use. a2. Preparation of aqueous solutions of inorganic salts: (1) Preparation of calcium salt aqueous solution: using water-soluble calcium salts such as calcium chloride, calcium nitrate, and calcium gluconate as raw materials, dissolve them completely in water at a certain concentration under stirring, and set aside for later use; (2) Preparation of carbonate aqueous solution: Sodium carbonate, potassium carbonate, ammonium carbonate and other water-soluble carbonates are used as raw materials and completely dissolved in water at a certain concentration under stirring, and then set aside. a3. Preparation of calcium silicate / calcium carbonate composite filler suspension by in-situ generation method: Slowly add the calcium salt aqueous solution prepared in step a2 to the porous calcium silicate suspension prepared in step a1, stir thoroughly for 15-30 minutes, mix evenly, and while stirring, slowly add the carbonate aqueous solution prepared in step a2 to the above porous calcium silicate / calcium salt mixture, and after reacting thoroughly for 30-45 minutes, nano or micron calcium carbonate is generated in-situ in the pores and surface of the porous calcium silicate, thus obtaining a suspension of porous calcium silicate / calcium carbonate composite filler; a4. Filtration, washing, deflocculation, and drying: Filtration and washing are performed to fully remove residual soluble inorganic salt ions from the calcium silicate / calcium carbonate composite filler. Then, moderate grinding, deflocculation, and drying are carried out to obtain a composite filler for cultural relic preservation with high whiteness, low abrasion, high retention rate, and good pH control performance. The filler has a whiteness ≥90% ISO, an average particle size of 3-15 μm, a pH value (10% concentration) of 8.0-9.5, an abrasion value ≤5 mg / 2000 times, and a calcium silicate to calcium carbonate mass ratio of 10:1-1:

1.

2. The method for preparing a composite filler for acid-free paper used in cultural relic preservation according to claim 1, characterized in that: The main physical properties of the porous calcium silicate raw material selected in step a1 are as follows: whiteness ≥90% ISO, average particle size 5-35 μm, porosity ≥0.35 mL / g, sedimentation volume ≥5.0 mL / g, and abrasion value ≤5 mg / 2000 times.

3. The method for preparing a composite filler for acid-free paper used in cultural relic preservation according to claim 1, characterized in that: The molar ratio of calcium ions to calcium silicate in the water-soluble calcium salt added in step a3 is in the range of 0.116-1.

160.

4. The method for preparing a composite filler for acid-free paper used in cultural relic preservation according to claim 1, characterized in that: The molar ratio of calcium ions in the water-soluble calcium salt added in step a3 to carbonate ions in the water-soluble carbonate added is 1:

1.

5. The method for preparing a composite filler for acid-free paper used in cultural relic preservation as described in claim 1, characterized in that: The prepared calcium silicate / calcium carbonate composite filler can be used as a filler for acid-free lining paper, acid-free lining paperboard, and acid-free corrugated paper for cultural relic protection, replacing traditional buffers such as calcium carbonate and magnesium carbonate, and improving the performance of cultural relic protection.

6. The method for preparing a composite filler for acid-free paper used in cultural relic preservation as described in claim 1, characterized in that: The prepared calcium silicate / calcium carbonate composite filler is added at a weight of 5%-30% relative to the oven-dry acid-free paper.

Citation Information

Patent Citations

  • Method for making acid-free lining paper for historic preservation

    CN106436437A