A cotton pulp and chemical fiber composite anti-counterfeiting paper for certificates and its preparation method

By using carboxylated cotton pulp fibers loaded with trivalent europium ions and polyethylene terephthalate chopped fibers to connect 1,10-phenanthroline-4-carboxylic acid residues in anti-counterfeiting paper, the problem of insufficient correlation between anti-counterfeiting features and paper fiber structure in existing technologies is solved, and the distinction and enhancement of the contact relationship between anti-counterfeiting features and internal paper fibers are realized.

CN123064055APending Publication Date: 2026-11-10LAIYANG YINTONG PAPERMAKING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611329686.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing anti-counterfeiting paper, the optical functional fibers are difficult to use during the paper forming process to establish a spatially distinguishable anti-counterfeiting state that is different from the non-contact area by utilizing the fiber contact relationship, resulting in a limited correlation between anti-counterfeiting features and the paper fiber structure.

Method used

Carboxylated cotton pulp fibers were loaded with trivalent europium ions, and 1,10-phenanthroline-4-carboxylic acid residues were attached to the surface of polyethylene terephthalate chopped fibers. The fiber contact area was determined by microscopic observation and Raman spatial localization, which showed the difference between the integrated emission intensity at 610–620 nm and the luminescence lifetime of trivalent europium ions.

Benefits of technology

It improves the correlation between anti-counterfeiting features and paper fiber structure, and enhances the distinguishability of anti-counterfeiting optical states.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123064055A_ABST
    Figure CN123064055A_ABST
Patent Text Reader

Abstract

This invention discloses a cotton pulp and chemical fiber composite anti-counterfeiting paper for certificates and its preparation method, relating to the field of special anti-counterfeiting paper technology. The paper sheet is composed of carboxylated cotton pulp fibers and polyethylene terephthalate (PET) chopped fibers interwoven together. The carboxylated cotton pulp fibers are loaded with trivalent europium ions, and the PET chopped fibers have 1,10-phenanthroline-4-carboxylic acid residues linked to their surfaces via amide bonds. The paper sheet contains direct contact and non-contact regions of the two types of fibers. Under 365 nm excitation, the integrated emission intensity at 610–620 nm of the direct contact region and the Eu... 3+ The luminescence lifetime is longer than that of the non-contact area. The two types of functional components are respectively set on different fiber sides and are formed together into paper, so that the anti-counterfeiting optical state corresponds to the actual fiber contact relationship inside the paper, thereby improving the correlation between the anti-counterfeiting features and the paper fiber structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of special anti-counterfeiting paper technology, and in particular to a cotton pulp and chemical fiber composite certificate anti-counterfeiting paper and its preparation method. Background Technology

[0002] Certificates, anti-counterfeiting tickets, and security documents typically require anti-counterfeiting features that can be identified through specific optical methods while maintaining the paper's forming and usability. In existing technologies, fluorescent materials, rare earth luminescent materials, or functional components with characteristic spectral responses are often pre-added to the anti-counterfeiting fiber or pulp system, and then distributed inside the paper during papermaking, thereby obtaining corresponding luminescent signals under ultraviolet excitation or special detection conditions.

[0003] The optical functions of existing anti-counterfeiting paper are usually determined before the anti-counterfeiting fibers are added to the pulp. During the paper forming process, the actual contact position between the cotton pulp fibers and chemical fibers only participates in the papermaking as part of the fiber network. It is difficult to use the local contact relationship formed by the two types of fibers inside the paper to establish a spatially distinguishable anti-counterfeiting state that is different from the non-contact area, resulting in a limited degree of correlation between the anti-counterfeiting features and the fiber structure of the paper itself. Summary of the Invention

[0004] In a first aspect, the present invention provides a cotton pulp and chemical fiber composite anti-counterfeiting paper for certificates, comprising: The paper sheet is composed of interwoven carboxylated cotton pulp fibers and polyethylene terephthalate chopped fibers. The carboxylated cotton pulp fibers are loaded with trivalent europium ions, and the surface of the polyethylene terephthalate chopped fibers is connected to 1,10-phenanthroline-4-carboxylic acid residues through amide bonds. The paper sheet contains areas where the two types of fibers are in direct contact and areas where the carboxylated cotton pulp fibers are not in contact with the polyethylene terephthalate chopped fibers. Under 365 nm excitation, the integrated emission intensity at 610–620 nm and the luminescence lifetime of trivalent europium ions in the direct contact region are both higher than those in the non-contact region.

[0005] Preferably, the carboxyl content of the carboxylated cotton pulp fiber is 0.20 to 0.70 mmol / g, and the carboxyl group is derived from the oxidation of the primary hydroxyl group at the C6 position of the cotton pulp cellulose.

[0006] Preferably, the length of the polyethylene terephthalate chopped fibers is 3 to 6 mm and the average diameter is 10 to 25 μm.

[0007] Preferably, the direct contact area is determined by microscopic observation and Raman spatial positioning, and the two types of fibers are continuously adjacent at their edges within this area, with no indistinguishable gaps within the spatial resolution range of the microscopic system.

[0008] Secondly, the present invention provides a method for preparing cotton pulp and chemical fiber composite anti-counterfeiting paper for certificates, characterized in that it includes: Bleached cotton pulp was treated in an oxidation system consisting of TEMPO, sodium bromide and sodium hypochlorite. After the reaction was completed, the pulp was washed to obtain carboxylated cotton pulp. The carboxylated cotton pulp was then contacted with an aqueous solution of europium chloride to complete the europium loading treatment. After washing, the pulp was obtained as europium-loaded carboxylated cotton pulp. Polyethylene terephthalate chopped fibers were placed in an aqueous solution of ethylenediamine for surface ammonolysis, and washed to obtain aminated PET chopped fibers. Then, 1,10-phenanthroline-4-carboxylic acid activated with 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide was reacted with the aminated PET chopped fibers, and washed to obtain phenanthroline-functionalized PET chopped fibers. Europium-carboxylated cotton pulp and phenanthrene-functionalized PET chopped fibers, which have been washed separately, are dispersed together in water and wet-formed to obtain wet paper sheets. The wet paper sheets are then pressed and dried to obtain cotton pulp and chemical fiber composite certificate anti-counterfeiting paper.

[0009] Preferably, the bleached cotton pulp is oxidized at 20–30°C and pH 10.0–10.5, and the resulting carboxylated cotton pulp has a carboxyl content of 0.20–0.70 mmol / g; the molar amount of trivalent europium ions is 0.15–0.20 times the molar amount of carboxyl ions, the pH of the europium-loaded treatment solution is 5.5–6.0, and the contact time is 30–120 min.

[0010] Preferably, polyethylene terephthalate short-cut fibers are treated in an aqueous solution of 5%–15% ethylenediamine at 40–60°C for 30–90 min; 1,10-phenanthroline-4-carboxylic acid was activated with 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide at pH 5.3–5.8, and then subjected to amidation reaction with aminated PET chopped fibers at pH 7.0–7.3.

[0011] Preferably, based on a total of 100 parts of the oven-dry weight of the two types of fibers, the europium-carboxylated cotton pulp is 92-97 parts and the phenanthrene-functionalized PET short fiber is 3-8 parts; The pulp consistency after co-blending is 0.3%–0.8%, the dryness of the wet paper after pressing is 40%–50%, the drying temperature is 95–110℃, and the moisture content of the dried paper is 4%–8%.

[0012] The beneficial effects of this invention are as follows: This invention sets trivalent europium ions on the carboxylated cotton pulp fiber side and fixes 1,10-phenanthroline-4-carboxylic acid residues on the PET chopped fiber side. After the two types of fibers are co-formed into paper, their directly contacting region and the non-contacting cotton pulp region form distinguishable 610–620 nm integrated emission intensities and Eu values. 3+ The difference in luminescence lifetime establishes a correspondence between the anti-counterfeiting optical state and the actual fiber contact relationship inside the paper, thereby improving the correlation between anti-counterfeiting features and the paper fiber structure. Attached Figure Description

[0013] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0014] Figure 1 This is a flowchart of the preparation method of cotton pulp and chemical fiber composite certificate anti-counterfeiting paper in Example 1; Figure 2 This is a schematic diagram of the direct contact area and non-contact area of ​​the paper in Example 1. Detailed Implementation

[0015] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0016] Bleached cotton pulp is used as a raw material for cellulose fibers, and the amount of cotton pulp used is based on oven-dry weight. The chemical fiber raw material is polyethylene terephthalate chopped fiber, hereinafter referred to as PET chopped fiber, with a length of 3-6 mm and an average diameter of 10-25 μm. The reagents used for cotton pulp oxidation include 2,2,6,6-tetramethylpiperidine-1-oxy free radical, sodium bromide, sodium hypochlorite, and sodium hydroxide. The effective chlorine content of sodium hypochlorite is determined by iodometric titration before use, and the amount of feed is calculated according to the effective molar amount of NaClO. The europium source is europium hexahydrate. Ethylenediamine is used for PET surface treatment. The ligands used for ligand linkage are 1,10-phenanthroline-4-carboxylic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, N-hydroxysuccinimide, and 2-(N-morpholine)ethanesulfonic acid. All other reagents are of analytical grade. Deionized water is used for solution preparation, fiber washing, pulping, and wet forming.

[0017] The oven-dry weights of cotton pulp, PET chopped fibers, and paper sheets were determined using the constant weight method at 105±2℃. Samples were dried at 105±2℃ and weighed every 30 minutes. The last weighing result was recorded when the difference between two consecutive weighings did not exceed 0.1% of the previous weighing. The dryness of the wet paper sheet was calculated as the ratio of the oven-dry weight to the total wet paper sheet weight. The moisture content of the dried paper sheet was calculated as the ratio of the difference between the initial weight and the oven-dry weight to the initial weight of the paper sheet.

[0018] The carboxyl content of carboxylated cotton pulp was determined by conductivity titration. 0.20 g of cotton pulp (octane-dry weight) was weighed, soaked in 0.01 mol / L hydrochloric acid for 30 min, filtered, and washed with deionized water until the pH of the final wash was 6.5–7.0. The washed cotton pulp was dispersed in 100 mL of 0.01 mol / L sodium chloride aqueous solution, titrated with 0.01 mol / L sodium hydroxide standard solution, and the conductivity was continuously recorded. The carboxyl content was calculated based on the molar amount of sodium hydroxide consumed corresponding to the carboxyl neutralization range and the oven-dry weight of the cotton pulp. Each sample was measured in triplicate, and the average value was calculated.

[0019] Raw cotton pulp and representative oxidized cotton pulp were subjected to solid-state processing. 13 C NMR detection; after drying, the sample is loaded into a solid-state NMR rotor, and samples are collected under consistent testing conditions within the same batch of samples. 13 C-chromatograms were used to record carboxyl carbon signals in the range of 174–176 ppm and the carbon signal associated with the C6 position of cellulose.

[0020] The Eu content in europium-loaded cotton pulp was determined by ICP-OES. A specified amount of oven-dry washed europium-loaded cotton pulp was weighed, digested with nitric acid, and then brought to a fixed volume and the Eu concentration was determined. The Eu fixation amount of europium-loaded cotton pulp was calculated based on the Eu concentration of the digestion solution, the fixed volume, and the oven-dry weight of the cotton pulp. The fiber Eu fixation ratio was calculated by dividing the total Eu in the washed cotton pulp by the total Eu input in this europium-loaded treatment. Three digestion solutions were prepared in parallel for each solid sample.

[0021] The volumes of each washing solution generated during europium loading treatment were collected and recorded. The total volumes of white water and press drain generated during wet forming were collected and recorded. A representative portion of each liquid sample was taken, acidified, and diluted as necessary before ICP-OES determination. The total amount of Eu in each liquid phase was calculated based on the Eu concentration and the corresponding total liquid volume.

[0022] After the co-mixing was completed, a representative mixed slurry was taken and centrifuged at 5000×g for 10 min. The supernatant was filtered through a 0.45 μm aqueous filter membrane and then subjected to ICP-OES analysis. The amount of Eu in the aqueous phase of the co-mixing was calculated based on the Eu concentration of the filtrate and the total volume of the aqueous phase of the mixed slurry, and its proportion of the total Eu carried in by the europium-loaded cotton slurry was calculated.

[0023] After the same batch of paper sheets is formed and pressed, the pulp mixing container, pulp transfer container and paper forming device components in contact with the pulp are rinsed sequentially with pre-measured deionized water. The rinsing liquids from each rinse are combined and the total volume is recorded. The Eu concentration of the rinsing liquid is determined by ICP-OES. The Eu content of the final paper sheet is determined after nitric acid digestion. The Eu material balance result of the batch of paper sheets is calculated based on the Eu content measured in the final paper sheet, forming white water, press drain water and equipment rinsing liquid.

[0024] PET short-cut fibers were subjected to ninhydrin color development, elemental analysis, and X-ray photoelectron spectroscopy before and after ethylenediamine treatment. The PET short-cut fibers after ethylenediamine treatment were designated as aminated PET. The total nitrogen mass fraction of the sample was recorded by elemental analysis, and the surface N atom fraction and N 1s spectrum were recorded by X-ray photoelectron spectroscopy. Samples in the same batch were treated under the same sample preparation, energy calibration, and peak fitting conditions.

[0025] Representative fibers from PET treated with ethylenediamine were taken for microscopic morphology observation. After the fibers were spread on a glass slide, surface and edge images were collected to record the continuity of the fibers, surface morphology, and damage to the fiber cross-section before and after treatment.

[0026] PET samples before and after treatment with 1,10-phenanthroline-4-carboxylic acid were subjected to elemental analysis, Fourier transform infrared spectroscopy, and X-ray photoelectron spectroscopy. The total nitrogen mass fraction of the aminated PET was defined as w0, and the total nitrogen mass fraction of the coupled and washed PET was defined as w1. Both w0 and w1 were expressed as decimal mass fractions. The apparent grafting amount of the 1,10-phenanthroline structural unit was calculated as (w1-w0)×1000 / 28.02, with the unit being mmol / g PET. The amide-related absorption signal in the Fourier transform infrared spectrum and the N 1s and C 1s lines in the X-ray photoelectron spectroscopy were recorded.

[0027] The concentration of free ligands in the final wash solution after coupling treatment with 1,10-phenanthroline-4-carboxylic acid was determined by high performance liquid chromatography. The wash solution was filtered through a 0.22 μm filter membrane before injection. The same chromatographic column, mobile phase composition, flow rate, column temperature, and detection wavelength were used for samples in the same batch. The concentration of ligands in the final wash solution was calculated based on the external standard curve established using 1,10-phenanthroline-4-carboxylic acid standard solution.

[0028] Before luminescence detection, the paper sheets were conditioned for 24 h at 23±1℃ and 50±2% relative humidity. An excitation wavelength of 365 nm was used, and emission spectra were collected in the range of 570–700 nm. The excitation power, spot area, slit width, integration time, and detector parameters were kept consistent for samples from the same batch. Five non-overlapping locations were selected for detection on each paper sheet, and the Eu values ​​were recorded. 3+The location of the main emission peak and the integrated emission intensity in the range of 610–620 nm.

[0029] PET chopped fibers and cotton pulp fibers in the paper were spatially located using microscopic observation combined with confocal Raman spectroscopy. Reference Raman spectra of PET chopped fibers and cotton pulp fibers were collected separately, and the characteristic wavenumbers that could distinguish the two types of fibers were determined. The target micro-area of ​​the paper was scanned using the same spectral acquisition parameters. The fiber positions were determined based on the characteristic Raman signals corresponding to the two types of fibers. The positions where the edges of the two types of fibers were continuously adjacent and within the spatial resolution range of the microscopic system used, and where no resolvable gaps were observed, were recorded as the direct contact area.

[0030] Spatial-resolved fluorescence detection was performed on the direct contact area and the carboxylated cotton pulp fiber area that was not in direct contact with the PET chopped fibers in the same microscopic field of view on the same sheet of paper. Ten locations on each sheet of paper were selected where the fiber contact relationship could be determined. The integrated emission intensity in the range of 610–620 nm was measured using the same excitation and acquisition parameters. The ratio, mean, and standard deviation of the integrated emission intensity of the direct contact area to the corresponding non-contact cotton pulp area at each location were calculated.

[0031] Eu 3+ The luminescence lifetime was obtained by time-resolved fluorescence detection; the excitation wavelength was set to 365 nm, the emission detection center was set to 615 nm, the emission acquisition range was 610–620 nm, and the time acquisition range was 0–3.0 ms after the excitation pulse ended; time decay curves were collected in the direct contact area determined by the aforementioned microscopic positioning and the corresponding non-contact pulp area in the same field of view. After subtracting the average background signal within 0.2 ms at the end of the time acquisition range, the decay curves were fitted with a least-squares model according to the double exponential decay model. The fitting parameters included the lifetime and corresponding amplitude of the two decay components. The average luminescence lifetime was calculated using the integral contribution of the two decay components as the weight; 10 sets of corresponding positions were measured for each sheet of paper, the average luminescence lifetime of each position was recorded, and the average value and standard deviation of the direct contact area and the non-contact pulp area were calculated.

[0032] The reduced χ² of the fitting results was controlled between 0.8 and 1.2, and the fitting residuals were randomly distributed on both sides of the time axis; if the above conditions were not met, the time decay curves at the corresponding positions were re-acquired.

[0033] Micro-regions containing the direct contact boundary between cotton pulp fibers and PET chopped strands were detected using micro-region X-ray photoelectron spectroscopy. The analysis location was determined based on microscopic observation and Raman spatial localization results. Monochromatic Al Kα rays were used as the excitation source, with a photon energy of 1486.6 eV. The analysis area was controlled within a diameter of 50 μm, and low-energy electron charge neutralization was enabled during the test. The pass energy for the full spectrum scan was set to 100 eV, and the energy step size was set to 1.0 eV. The pass energy for the N 1s and C 1s high-resolution spectra was set to 20 eV, and the energy step size was set to 0.05 eV. The binding energy of the C-C / C-H component in C 1s was 284.8 eV as the calibration position. The N 1s high-resolution spectrum was fitted using Shirley background subtraction and a Gaussian-Lorentzian mixed peak shape with least squares fitting. Samples from the same batch maintained the same background, peak shape, and full width at half maximum (FWHM) constraints. Three independent contact micro-regions were selected from each sheet of paper, and the N 1s high-resolution spectrum was recorded. The peak positions and peak areas of each fitted component in 1s were determined, and the corresponding nitrogen-containing components were identified by combining the N 1s spectra of phenanthroline-functionalized PET that had not been co-printed.

[0034] Representative paper sheets were subjected to Eu L3 edge XANES / EXAFS analysis. X-ray absorption spectra were collected near the Eu L3 absorption edge, and energy calibration was performed using Eu standard samples. The obtained spectra were then subjected to pre-edge background subtraction, absorption edge normalization, and EXAFS oscillation extraction. χ(k) was weighted by k², and the values ​​were calculated in the range of k = 30–100 nm. -1 Perform Hanning window Fourier transform within the range, with a window width parameter corresponding to 5 nm. -1 The first coordination shell was selected within the range of R = 0.12–0.28 nm for fitting; the Eu-O single scattering path in the Eu₂O₃ standard sample was used as the reference path for the first coordination shell, and the amplitude attenuation factor S₀ was used. 2 After being fitted from Eu2O3 standard samples and fixed, the average coordination number N, average coordination distance R, Debye-Waller factor σ², and absorption edge energy offset ΔE0 were used as fitting variables. The average coordination distance, average coordination number, and corresponding uncertainty of the first coordination shell obtained by fitting were recorded.

[0035] Example 1 refer to Figure 1 Bleached cotton pulp is oxidized and treated with europium to obtain europium-carboxylated cotton pulp. PET chopped fibers are treated with ethylenediamine and coupled with 1,10-phenanthroline-4-carboxylic acid to obtain phenanthroline-functionalized PET chopped fibers. The two types of fibers are processed and washed separately and then mixed into pulp. The pulp is then wet-formed, pressed and dried to obtain cotton pulp and chemical fiber composite certificate anti-counterfeiting paper.

[0036] Take 38.0 g of bleached cotton pulp (octane-dry weight), soak and loosen it with deionized water, and adjust the pulp concentration to 1.0%. Add 0.59 g of TEMPO and 3.91 g of sodium bromide to the pulp, stir at 25°C for 10 min, then add sodium hypochlorite solution (based on available NaClO, 2.60 mmol / g of oven-dry cotton pulp). Maintain the pH of the reaction solution at 10.0–10.4 with 0.5 mol / L sodium hydroxide solution, continue the reaction at 25°C for 55 min, and then add 20 mL of anhydrous ethanol to terminate the reaction. Filter the resulting cotton pulp and wash it with 760 mL of deionized water each time, for a total of 4 washes. The carboxyl content of the three parallel samples was determined by the aforementioned conductivity titration method to be 0.45 mmol / g, 0.47 mmol / g, and 0.46 mmol / g, with an average of 0.46 mmol / g. 13 C14 NMR detection recorded carboxyl carbon signals in the range of 174–176 ppm, and simultaneously recorded the carbon signal associated with the C6 position of cellulose.

[0037] Based on a carboxyl content of 0.46 mmol / g, 38.0 g of carboxylated cotton pulp contains 17.48 mmol of carboxyl groups; 1.10 g of europium chloride hexahydrate was weighed, equivalent to Eu... 3+ It was 3.00 mmol, Eu 3+ The ratio of the molar amount of feedstock to the measured molar amount of carboxyl groups was 0.172:1. The carboxylated cotton pulp was dispersed in 1.50 L of deionized water. Europium chloride hexahydrate was dissolved in 150 mL of deionized water, and the pH was adjusted to 5.7 with 0.1 mol / L hydrochloric acid or 0.1 mol / L sodium hydroxide solution. The cotton pulp dispersion was added over 10 min and stirred at 25 °C for 60 min. After treatment, the mixture was filtered and washed four times with 760 mL of deionized water. The Eu concentration of the final wash was 0.042 mg / L. The Eu content of the three parallel samples of the washed cotton pulp was 0.056 mmol / g, 0.059 mmol / g, and 0.058 mmol / g, respectively. The average Eu fixation was 0.058 mmol / g of oven-dry cotton pulp, and the fiber Eu fixation ratio based on the feedstock Eu was 73.5%.

[0038] 2.0 g of PET short-cut fibers with a length of 4.5 mm and an average diameter of 18 μm were taken and added to 100 mL of 10% ethylenediamine aqueous solution. The mixture was treated at 50 °C and 150 r / min for 60 min. After filtration, the fibers were washed five times with 100 mL of deionized water, once with 100 mL of anhydrous ethanol, and once with 100 mL of deionized water. The fibers were then vacuum dried at 40 °C. The total nitrogen mass fraction of the obtained aminated PET was 0.64%, and the surface N atom fraction was 2.3% as measured by XPS. Microscopic observation showed that the fibers maintained a continuous morphology and no damage was recorded that penetrated the cross-section of the fibers.

[0039] 0.45 g of 1,10-phenanthroline-4-carboxylic acid was dissolved in 10 mL of dimethyl sulfoxide. The resulting solution was added to 190 mL of MES solution with a pH of 5.5, followed by the addition of 0.46 g of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and 0.28 g of N-hydroxysuccinimide. After stirring at 25 °C for 20 min, the above-mentioned aminated PET was added. The pH of the system was adjusted to 7.1 with 0.1 mol / L sodium hydroxide solution. The reaction was carried out at 25 °C and 120 r / min for 4 h. After filtration, the solution was washed three times with 100 mL of 1:1 (v / v) ethanol-water solution and three times with 100 mL of deionized water, and then dried under vacuum at 40 °C. The concentration of 1,10-phenanthroline-4-carboxylic acid in the final washing solution was 0.068 g. The total nitrogen mass fraction of PET after coupling treatment was 0.95%, and the apparent grafting amount of 1,10-phenanthroline structural units was 0.111 mmol / g PET according to the aforementioned calculation method. The Fourier transform infrared spectra, N 1s and C 1s spectra of the samples before and after coupling treatment were recorded.

[0040] Based on oven-dry weight, 38.0 g of europium-carboxylated cotton pulp and 2.0 g of phenanthrene-functionalized PET chopped fibers were taken. The europium-carboxylated cotton pulp was adjusted to a pulp consistency of 0.50% and dispersed at 300 r / min for 5 min. The PET chopped fibers were pre-dispersed in 500 mL of deionized water and stirred at 250 r / min for 3 min. The PET dispersion was then added to the cotton pulp and stirred together at 250 r / min for 8 min. After the co-mixing, the aqueous phase Eu accounted for 5.8% of the total Eu carried in by the europium-carboxylated cotton pulp.

[0041] The mixed pulp was slowly stirred, and the pulp was divided according to the amount of oven-dry fiber per sheet of paper. The pulp was wet-formed in an experimental paper sheet forming device with an effective forming area of ​​0.040 m² to obtain a wet paper sheet with a target basis weight of 90 g / m². The wet paper sheet was pressed at 0.35 MPa for 60 s, and the dryness after pressing was 45.3%. It was then dried at 102℃ hot air to a moisture content of 6.2%, and conditioned at 23℃ and 50% relative humidity for 24 h.

[0042] Eu in the final paper sheet accounts for 88.9% of the total Eu brought in by europium carboxylated cotton pulp, Eu in forming white water and press drainage accounts for 7.1% in total, Eu in equipment rinsing fluid accounts for 2.4%, and the total Eu material balance is 98.4%. In this embodiment, the proportion of PET oven-dry mass in the final paper sheet is no longer converted based on the microfiber cross-point.

[0043] In the resulting paper sheet, europium-carboxylated cotton pulp fibers and phenanthrene-functionalized PET chopped fibers are interwoven. Locations where the edges of the two types of fibers are continuously adjacent and have no indistinguishable gaps within the spatial resolution range of the microscopic system are designated as directly contact areas. Locations of carboxylated cotton pulp fibers in the same paper sheet that are not in direct contact with the PET chopped fibers are designated as non-contact areas. The positional relationship between the two types of areas is as follows: Figure 2 As shown.

[0044] The PET chopped fibers, cotton pulp fibers, and the direct contact area between the two types of fibers in the paper were determined using the aforementioned microscopic observation and confocal Raman spatial localization method; Eu at five detection locations under 365 nm excitation conditions was used. 3+ The main emission peaks are located at 614.8 nm, 615.3 nm, 615.5 nm, 615.0 nm, and 615.2 nm, with an average of 615.2 nm. The average ratio of the integrated emission intensity of the 610–620 nm region between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions in the same field of view is 1.56, with a standard deviation of 0.10. The Eu emission intensity of the non-contact cotton pulp region is... 3+ The average luminescence lifetime was 0.329 ms with a standard deviation of 0.024 ms, while the average luminescence lifetime in the direct contact area was 0.482 ms with a standard deviation of 0.031 ms.

[0045] In the same batch of phenanthroline-functionalized PET that were not co-formed into paper, the N 1s component center associated with the 1,10-phenanthroline structural unit was located at 398.90 eV. The corresponding component centers in the three analytical micro-regions containing the direct fiber contact boundary were located at 399.20 eV, 399.27 eV, and 399.23 eV, respectively. After Eu L3 edge XANES / EXAFS analysis of two independent paper sheets, the average coordination distances of the first coordination shell were 2.42 nm and 2.44 nm, respectively, with an average of 2.43 ± 0.02 nm. The corresponding average coordination numbers were 8.2 and 8.6, respectively, with an average of 8.4 ± 0.8.

[0046] Example 2 The PET functionalization, co-mixing, wet forming, pressing, and drying operations in Example 2 were the same as in Example 1. The conditions for cotton pulp oxidation and europium loading were adjusted according to the parameters of this example. 38.0 g of oven-dried bleached cotton pulp was taken, and 0.59 g of TEMPO and 3.91 g of sodium bromide were added. Sodium hypochlorite solution with an effective NaClO content of 1.35 mmol / g of oven-dried cotton pulp was added. The reaction was carried out at 22°C and pH 10.0–10.3 for 45 min. After the reaction was terminated, the mixture was filtered and washed four times with 760 mL of deionized water. The carboxyl content of the three parallel samples was 0.23 mmol / g, 0.24 mmol / g, and 0.25 mmol / g, respectively, with an average value of 0.24 mmol / g.

[0047] Based on a carboxyl content of 0.24 mmol / g, 38.0 g of cotton pulp contains 9.12 mmol of carboxyl groups; adding the equivalent of Eu... 3+ The concentration of europium chloride hexahydrate was 1.414 mmol, Eu 3+ The ratio of the molar amount of feedstock to the measured molar amount of carboxyl groups was 0.155:1. The pH of the europium-loaded system was adjusted to 5.6, and the mixture was stirred at 25°C for 35 min before filtration and washing. The Eu concentration of the final wash solution was 0.039 mg / L. The average Eu fixation of the three parallel samples of cotton pulp after washing was 0.024 mmol / g oven-dry cotton pulp, and the fiber Eu fixation ratio based on the feedstock Eu was 64.5%.

[0048] The PET short-cut fibers had a length of 4.5 mm and an average diameter of 18 μm. The ammonolysis and 1,10-phenanthroline-4-carboxylic acid coupling treatment followed the conditions of Example 1. After coupling treatment, the total nitrogen mass fraction of PET was 0.94%, and the apparent grafting amount of 1,10-phenanthroline structural units was 0.104 mmol / g PET.

[0049] Europium-carboxylated cotton pulp and phenanthrene-functionalized PET were mixed together at an oven-dry feed ratio of 95:5 and paper was prepared according to the conditions of Example 1. The Eu in the mixed pulp accounted for 7.8% of the total Eu carried in, and the Eu in the final paper accounted for 84.9% of the total Eu carried in, with a total Eu material balance of 97.5%.

[0050] Eu at 5 detection sites under 365 nm excitation conditions 3+ The main emission peak is located at 614.7–615.4 nm, with an average of 615.1 nm. The average ratio of the integrated emission intensity of the 610–620 nm region between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions is 1.32, with a standard deviation of 0.07. The Eu values ​​of the non-contact cotton pulp regions and the directly contacted regions are also relatively high. 3+ The average luminescence lifetimes were 0.319 ms and 0.396 ms, respectively.

[0051] In three analytical micro-regions containing the direct fiber contact boundary, the N 1s component associated with the 1,10-phenanthroline structural unit recorded peak position changes of 0.19 eV, 0.25 eV, and 0.22 eV relative to the functionalized PET of the same batch that was not co-printed; the average coordination distance of the Eu first coordination shell was 2.42 ± 0.02 nm, and the average coordination number was 8.1 ± 0.8.

[0052] Example 3 The PET functionalization, co-mixing, and papermaking operations of Example 3 followed those of Example 2, with the cotton pulp oxidation and europium loading parameters adjusted to the conditions of this example. 38.0 g of oven-dry bleached cotton pulp was taken, and 0.59 g of TEMPO and 3.91 g of sodium bromide were added. Then, a sodium hypochlorite solution with an effective NaClO concentration of 3.80 mmol / g oven-dry cotton pulp was added. The reaction was carried out at 28°C and pH 10.1–10.5 for 65 min. After terminating the reaction with anhydrous ethanol, the mixture was filtered and washed five times with 760 mL of deionized water. The carboxyl content of the three parallel samples was 0.62 mmol / g, 0.64 mmol / g, and 0.63 mmol / g, respectively, with an average of 0.63 mmol / g.

[0053] Based on a carboxyl content of 0.63 mmol / g, 38.0 g of cotton pulp contains 23.94 mmol of carboxyl groups; adding the equivalent of Eu... 3+ The concentration of europium chloride hexahydrate was 4.56 mmol. 3+ The ratio of the molar amount of feed to the measured molar amount of carboxyl groups was 0.190:1. The pH of the system was adjusted to 5.8, and the mixture was stirred at 25°C for 110 min, then filtered and washed. The Eu concentration of the final wash was 0.045 mg / L, and the average Eu fixation of the cotton pulp after washing was 0.081 mmol / g oven-dry cotton pulp. The Eu fixation ratio of the fiber, calculated based on the feed Eu, was 67.5%.

[0054] The PET short-cut fibers had a length of 4.5 mm and an average diameter of 18 μm. The ammonolysis and coupling conditions were the same as in Example 1. After coupling treatment, the total nitrogen mass fraction of PET was 0.96%, and the apparent grafting amount of 1,10-phenanthroline structural units was 0.107 mmol / g PET.

[0055] Europium-carboxylated cotton pulp and phenanthrene-functionalized PET were mixed together at an oven-dry feed ratio of 95:5 and then formed into paper. The aqueous phase of the mixed pulp accounted for 6.3% of the total Eu carried over, and the Eu of the final paper accounted for 87.7% of the total Eu carried over, with a total Eu material balance of 98.1%.

[0056] Under 365 nm excitation conditions, Eu 3+ The main emission peak is located at 614.9–615.6 nm, with an average of 615.2 nm. The average ratio of the integrated emission intensity of the 610–620 nm region between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions is 1.50, with a standard deviation of 0.06. The Eu values ​​of the non-contact cotton pulp regions and the directly contacted regions are also relatively high. 3+ The average luminescence lifetimes were 0.348 ms and 0.496 ms, respectively.

[0057] In three analytical micro-regions containing the direct fiber contact boundary, the N 1s component associated with the 1,10-phenanthroline structural unit recorded peak position changes of 0.28 eV, 0.34 eV, and 0.31 eV relative to the same batch of functionalized PET, respectively; the average coordination distance of the Eu first coordination shell was 2.43 ± 0.02 nm, and the average coordination number was 8.3 ± 0.8.

[0058] Example 4 The conditions for cotton pulp oxidation, Eu loading, PET surface ammonolysis, and 1,10-phenanthroline-4-carboxylic acid coupling in Example 4 were the same as in Example 1. The length of the PET chopped fibers was adjusted to 3.2 mm and the average diameter was adjusted to 12 μm. The oven-dry feed weights of europium-loaded carboxylated cotton pulp and phenanthroline-functionalized PET were 38.72 g and 1.28 g, respectively, with an oven-dry feed weight ratio of 96.8:3.2. The resulting europium-loaded carboxylated cotton pulp had an average carboxyl content of 0.46 mmol / g and an average Eu fixation amount of 0.058 mmol / g. The apparent grafting amount of 1,10-phenanthroline structural units in the phenanthroline-functionalized PET was 0.108 mmol / g PET.

[0059] After the two types of fibers were treated and washed separately, they were dispersed together in water and mixed together to adjust the pulp concentration to 0.35%. After mixing for 8 minutes, the Eu in the aqueous phase of the pulp accounted for 5.7% of the total Eu brought in by the europium carboxylated cotton pulp. The pulp was divided according to the amount of oven-dry fiber per sheet and wet-formed. The wet paper sheets were pressed at 0.25 MPa for 45 seconds, and the dryness after pressing was 41.4%. Then, it was dried at 96℃ with hot air to a moisture content of 7.6%. After the paper sheets were dried, they were conditioned for 24 hours under the aforementioned conditions.

[0060] The final paper sheet contains 88.4% Eu of the total Eu brought in by the europium carboxylated cotton pulp, and the total Eu material balance is 98.0%. In this embodiment, the proportion of the two types of fibers is recorded according to the oven-dry feeding mass, and the final paper sheet PET mass ratio is no longer converted by microscopic cross-point.

[0061] Under 365 nm excitation conditions, Eu 3+ The main emission peak is located at 614.8–615.5 nm, with an average of 615.1 nm. The average ratio of the integrated emission intensity of the 610–620 nm region between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions is 1.39, with a standard deviation of 0.07. The Eu values ​​of the non-contact cotton pulp regions and the directly contacted regions are also relatively high. 3+ The average luminescence lifetimes were 0.325 ms and 0.443 ms, respectively.

[0062] Example 5 The conditions for cotton pulp oxidation, Eu loading, and PET surface functionalization in Example 5 were the same as in Example 1. The length of the PET chopped fibers was adjusted to 5.8 mm and the average diameter was adjusted to 23 μm. The oven-dry feed weights of europium-loaded carboxylated cotton pulp and phenanthroline-functionalized PET were 36.88 g and 3.12 g, respectively, with an oven-dry feed weight ratio of 92.2:7.8. The resulting europium-loaded carboxylated cotton pulp had an average carboxyl content of 0.45 mmol / g and an average Eu fixation amount of 0.057 mmol / g. The apparent grafting amount of 1,10-phenanthroline structural units in the phenanthroline-functionalized PET was 0.112 mmol / g PET.

[0063] The two types of fibers were treated and washed separately and then mixed together to form pulp. The pulp consistency was adjusted to 0.75%. After mixing, the Eu phase of the pulp accounted for 6.5% of the total Eu brought in by the europium carboxylated cotton pulp. The pulp was divided according to the amount of oven-dry fiber per sheet and wet-formed. The wet paper sheets were pressed at 0.45 MPa for 75 s, and the dryness after pressing was 49.1%. The paper sheets were dried at 109℃ hot air to a moisture content of 4.6% and then conditioned for 24 h after drying.

[0064] The final paper sheet accounted for 87.2% of the total Eu carried by the europium carboxylated cotton pulp, and the total Eu material balance was 97.8%.

[0065] Under 365 nm excitation conditions, Eu 3+ The main emission peak is located at 614.9–615.6 nm, with an average of 615.2 nm. The average ratio of the integrated emission intensity of the 610–620 nm region between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions is 1.48, with a standard deviation of 0.08. The Eu values ​​of the non-contact cotton pulp regions and the directly contacted regions are also shown. 3+ The average luminescence lifetimes were 0.333 ms and 0.469 ms, respectively.

[0066] Example 6 The cotton pulp oxidation, Eu loading, the oven-dry feed ratio of the two types of fibers, and the paper-making conditions in Example 6 were the same as in Example 1. The PET chopped fiber length was 4.5 mm and the average diameter was 18 μm. 2.0 g of PET chopped fiber was added to 100 mL of 6% ethylenediamine aqueous solution and treated at 42°C and 150 r / min for 35 min. The washing and drying operations after filtration were the same as in Example 1. The total nitrogen mass fraction of the obtained aminated PET was 0.35%, and the surface N atom fraction measured by XPS was 1.4%. The fiber maintained a continuous morphology during microscopic observation.

[0067] The activation, coupling, washing, and drying procedures for 1,10-phenanthroline-4-carboxylic acid were the same as in Example 1; the total nitrogen mass fraction of the PET after coupling treatment was 0.52%, and the apparent grafting amount of 1,10-phenanthroline structural units was 0.061 mmol / g PET.

[0068] 38.0 g of europium-carboxylated cotton pulp and 2.0 g of the above-mentioned phenanthroline-functionalized PET were mixed together and formed into paper. The Eu in the aqueous phase of the mixed pulp accounted for 6.1% of the total Eu carried in. The dryness of the paper after pressing was 45.0%, and the moisture content of the paper after drying was 6.4%. The Eu in the final paper accounted for 87.5% of the total Eu carried in, and the total Eu material balance was 97.6%.

[0069] Under 365 nm excitation conditions, Eu 3+ The main emission peak is located at 614.8–615.4 nm, with an average of 615.1 nm. The average ratio of the integrated emission intensity of the 610–620 nm region between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions is 1.30, with a standard deviation of 0.06. The Eu values ​​of the non-contact cotton pulp regions and the directly contacted regions are also shown. 3+ The average luminescence lifetimes were 0.324 ms and 0.404 ms, respectively.

[0070] In three analytical micro-regions containing the direct fiber contact boundary, the N 1s component associated with the 1,10-phenanthroline structural unit recorded peak position changes of 0.13 eV, 0.19 eV, and 0.16 eV relative to the same batch of functionalized PET, respectively; the average coordination distance of the Eu first coordination shell was 2.42 ± 0.02 nm, and the average coordination number was 8.2 ± 0.8.

[0071] Example 7 Example 7 follows the same cotton pulp side treatment, fiber feeding ratio, and common pulp preparation and papermaking conditions as Example 6, with the PET ethylenediamine treatment parameters adjusted to the conditions of this example. 2.0 g of PET short-cut fibers with a length of 4.5 mm and an average diameter of 18 μm were taken and added to 100 mL of 14% ethylenediamine aqueous solution. The mixture was treated at 58°C and 150 r / min for 85 min. After filtration, it was treated according to the washing and drying method of Example 1. The total nitrogen mass fraction of the obtained aminated PET was 0.94%, and the surface N atom fraction measured by XPS was 3.5%. Microscopic observation showed that the PET short-cut fibers maintained a continuous morphology, and the surface roughness of some fibers increased. No damage penetrating the cross-section of the fibers was recorded.

[0072] The activation, coupling, washing, and drying procedures for 1,10-phenanthroline-4-carboxylic acid were the same as in Example 1; the total nitrogen mass fraction of the PET after coupling treatment was 1.32%, and the apparent grafting amount of 1,10-phenanthroline structural units was 0.136 mmol / g PET.

[0073] 38.0 g of europium carboxylated cotton pulp and 2.0 g of the above-mentioned phenanthroline functionalized PET were mixed together and formed into paper. The Eu in the aqueous phase of the mixed pulp accounted for 6.6% of the total Eu carried in. The dryness of the paper after pressing was 45.5%, and the moisture content of the paper after drying was 6.1%. The Eu in the final paper accounted for 86.8% of the total Eu carried in, and the total Eu material balance was 97.7%.

[0074] Under 365 nm excitation conditions, Eu 3+ The main emission peak is located at 614.9–615.6 nm, with an average of 615.2 nm. The average ratio of the integrated emission intensity of the 610–620 nm region between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions is 1.55, with a standard deviation of 0.08. The Eu values ​​of the non-contact cotton pulp regions and the directly contacted regions are also shown. 3+ The average luminescence lifetimes were 0.336 ms and 0.491 ms, respectively.

[0075] In three analytical micro-regions containing the direct fiber contact boundary, the N 1s component associated with the 1,10-phenanthroline structural unit recorded peak position changes of 0.27 eV, 0.35 eV, and 0.31 eV relative to the same batch of functionalized PET, respectively; the average coordination distance of the Eu first coordination shell was 2.43 ± 0.02 nm, and the average coordination number was 8.4 ± 0.8.

[0076] Comparative Example 1 This comparative example uses low-carboxyl-content bleached cotton pulp without TEMPO oxidation treatment to replace the carboxylated cotton pulp in Example 1. The ammonolysis of PET chopped fibers, coupling of 1,10-phenanthroline-4-carboxylic acid, the oven-dry feed ratio of the two types of fibers, the co-blending of pulp, and the paper forming conditions are the same as in Example 1. The carboxyl content of the three parallel samples of bleached cotton pulp without TEMPO oxidation treatment is 0.041 mmol / g, 0.046 mmol / g, and 0.043 mmol / g, respectively, with an average of 0.043 mmol / g. This cotton pulp is contacted with europium chloride aqueous solution and washed according to the europium loading conditions of Example 1. The Eu concentration of the final wash is 0.31 mg / L. The Eu fixation of the three parallel samples of the washed cotton pulp is 0.010 mmol / g, 0.012 mmol / g, and 0.011 mmol / g, respectively, with an average of 0.011 mmol / g oven-dry cotton pulp. The fiber Eu fixation ratio based on the feed Eu is 13.9%.

[0077] 38.0 g of the Eu-loaded cotton pulp and 2.0 g of the phenanthrene-functionalized PET short fibers prepared under the conditions of Example 1 were mixed together and formed into paper. After the mixed pulping, the aqueous phase Eu accounted for 17.2% of the total Eu carried in by the Eu-loaded cotton pulp, and the Eu in the final paper sheet accounted for 74.6% of the total Eu carried in. The Eu in the forming white water and press wastewater accounted for 17.9% in total, and the Eu in the equipment rinsing fluid accounted for 5.1%. The total Eu material balance was 97.6%.

[0078] Eu at 5 detection sites under 365 nm excitation conditions 3+ The main emission peak is located at 614.6–615.3 nm, with an average of 615.0 nm. The average ratio of the integrated emission intensity of the 610–620 nm region between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions is 1.17, with a standard deviation of 0.07. The Eu emission intensity of the non-contact cotton pulp regions is... 3+ The average luminescence lifetime was 0.286 ms with a standard deviation of 0.026 ms, while the average luminescence lifetime in the direct contact area was 0.331 ms with a standard deviation of 0.030 ms.

[0079] In the same batch of phenanthroline-functionalized PET that was not co-printed, the N 1s component center associated with the 1,10-phenanthroline structural unit was located at 398.90 eV. The corresponding component centers in the three analytical micro-regions containing the two types of fiber contact boundaries were located at 398.98 eV, 399.03 eV, and 399.00 eV, respectively. The average coordination distance of the Eu first coordination shell was 2.40 ± 0.02 nm, and the average coordination number was 8.0 ± 0.8.

[0080] Comparative Example 2 In this comparative example, carboxylated cotton pulp was prepared under the oxidation conditions of Example 1. The washed carboxylated cotton pulp was not treated with europium chloride. The PET functionalization, the oven-dry feeding ratio of the two types of fibers, the co-mixing of pulp, and the paper forming conditions were the same as in Example 1. The average carboxyl content of the three parallel samples of the obtained carboxylated cotton pulp was 0.46 mmol / g, and the apparent grafting amount of 1,10-phenanthroline structural units of phenanthroline-functionalized PET was 0.108 mmol / g PET.

[0081] The resulting carboxylated cotton pulp and phenanthrene-functionalized PET were mixed together at an oven-dry mass ratio of 95:5 and then made into paper. This sample was not subjected to Eu loading, so the Eu fixation amount was not recorded. The Eu in the final paper was detected by ICP-OES and found to be below the limit of quantitation.

[0082] Stable Eu was not obtained in the 570–700 nm range under 365 nm excitation conditions. 3+Characteristic emission peaks; the average ratio of background integrated emission intensity between the 10 directly contacted regions and the corresponding non-contact cotton pulp regions in the 610–620 nm range was 1.05 with a standard deviation of 0.04, which is significant in Eu. 3+ No time decay curve satisfying the fitting conditions was obtained for the main transmission band.

[0083] In the three analytical micro-regions containing two types of fiber contact boundaries, the N 1s component centers associated with the 1,10-phenanthroline structural unit were located at 398.94 eV, 398.99 eV, and 398.96 eV, respectively; no absorption signal satisfying the first coordination shell fitting condition was obtained at the Eu L3 edge.

[0084] Comparative Example 3 The cotton pulp oxidation and Eu loading conditions in this comparative example were the same as in Example 1. The EDC / NHS coupling step of 1,10-phenanthroline-4-carboxylic acid was omitted after the PET chopped fibers were treated with ethylenediamine in Example 1. The resulting aminated PET was washed three times with 100 mL of ethanol aqueous solution (1:1 v / v) and three times with 100 mL of deionized water, and then vacuum dried at 40 °C. The total nitrogen mass fraction of the aminated PET was 0.63%, and the surface N atom fraction was 2.2% as determined by XPS.

[0085] The obtained europium-loaded carboxylated cotton pulp had an average carboxyl content of 0.46 mmol / g and an average Eu fixation of 0.058 mmol / g oven-dry cotton pulp. 38.0 g of europium-loaded carboxylated cotton pulp and 2.0 g of the above-mentioned aminated PET were mixed together and formed into paper. The Eu in the aqueous phase of the mixed pulp accounted for 6.4% of the total Eu carried in, and the Eu in the final paper accounted for 88.1% of the total Eu carried in. The Eu in the forming white water, press wastewater and equipment flushing liquid and the Eu in the final paper accounted for 97.8% of the Eu in the feed.

[0086] Eu at 5 detection sites under 365 nm excitation conditions 3+ The main emission peak is located at 614.7–615.4 nm, with an average of 615.0 nm. The average ratio of the integrated emission intensity at 610–620 nm between the direct contact region and the corresponding non-contact pulp region of the two types of fibers is 1.14, with a standard deviation of 0.06. The Eu values ​​of the non-contact pulp region and the direct contact region are also relatively high. 3+ The average luminescence lifetimes were 0.328 ms and 0.356 ms, respectively, with corresponding standard deviations of 0.024 ms and 0.027 ms.

[0087] The main nitrogen-containing N 1s component center in the unco-formed aminated PET is located at 399.42 eV. The corresponding component centers in the three analytical micro-regions containing the contact boundary between europium-loaded cotton pulp fibers and aminated PET are located at 399.48 eV, 399.53 eV, and 399.50 eV, respectively. The average coordination distance of the first coordination shell of Eu is 2.41 ± 0.02 nm, and the average coordination number is 8.1 ± 0.8.

[0088] Comparative Example 4 The conditions for cotton pulp oxidation, Eu loading, and PET ethylenediamine treatment in this comparative example were the same as in Example 1. During the contact between PET and 1,10-phenanthroline-4-carboxylic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide were not added. 2.0 g of aminated PET was taken, and 0.45 g of 1,10-phenanthroline-4-carboxylic acid was dissolved in 10 mL of dimethyl sulfoxide and 190 mL of MES solution was added. After adjusting the pH of the system to 7.1, the aminated PET was added, and the mixture was treated at 25°C and 120 r / min for 4 h. After filtration, the mixture was washed three times with 100 mL of 1:1 ethanol aqueous solution and three times with 100 mL of deionized water, and then vacuum dried at 40°C.

[0089] The total nitrogen mass fraction of the PET before amination treatment was 0.64%, and the total nitrogen mass fraction of the PET after treatment and washing was 0.68%. According to the aforementioned nitrogen mass fraction difference conversion method, the apparent residual amount of nitrogen-containing substances related to 1,10-phenanthroline-4-carboxylic acid was 0.014 mmol / g PET, and the concentration of 1,10-phenanthroline-4-carboxylic acid in the final washing solution was 0.094 mg / L.

[0090] 38.0 g of europium carboxylated cotton pulp and 2.0 g of the above-mentioned PET were mixed together and made into paper. The Eu in the aqueous phase of the mixed pulp accounted for 6.3% of the total Eu brought in by the europium carboxylated cotton pulp, and the Eu in the final paper accounted for 88.0% of the total Eu brought in. The total Eu material balance was 97.7%.

[0091] Under 365 nm excitation conditions, Eu 3+ The main emission peak is located at 614.7–615.4 nm, with an average of 615.0 nm. The average ratio of the integrated emission intensity at 610–620 nm between the direct contact region and the corresponding non-contact pulp region of the two types of fibers is 1.21, with a standard deviation of 0.06. The Eu values ​​of the non-contact pulp region and the direct contact region are also relatively high. 3+ The average luminescence lifetimes were 0.330 ms and 0.372 ms, respectively, with corresponding standard deviations of 0.025 ms and 0.029 ms.

[0092] N 1s signals corresponding to nitrogen-containing structures associated with 1,10-phenanthroline-4-carboxylic acid were recorded in the processed and washed PET. The centers of the associated N 1s components in three analytical micro-regions containing the contact boundaries of the two types of fibers were located at 398.97 eV, 399.02 eV, and 398.99 eV, respectively. The average coordination distance of the first coordination shell of Eu was 2.41 ± 0.02 nm, and the average coordination number was 8.1 ± 0.8.

[0093] Comparative Example 5 In this comparative example, carboxylated cotton pulp and phenanthroline-functionalized PET were prepared according to the conditions of Example 1. After oxidation and washing, the carboxylated cotton pulp was not loaded with Eu. Eu was added to the phenanthroline-functionalized PET side before co-mixing. 2.0 g of functionalized PET with an apparent grafting amount of 0.110 mmol / g PET of 1,10-phenanthroline structural units was taken. 95.3 mg of europium chloride hexahydrate was dissolved in 100 mL of deionized water, which was equivalent to 0.260 mmol of Eu³⁺. The pH of the solution was adjusted to 5.7 and then PET was added. The mixture was contacted at 25 °C and 120 r / min for 60 min. After filtration, the mixture was washed four times with 100 mL of deionized water and dried under vacuum at 40 °C.

[0094] The Eu content of the three parallel samples of washed PET was 0.102 mmol / g, 0.108 mmol / g, and 0.105 mmol / g, respectively, with an average of 0.105 mmol / g PET. The Eu fixation ratio on the PET side, based on the Eu added, was 80.8%. 38.0 g of unloaded carboxylated cotton pulp and 2.0 g of the above-mentioned Eu-loaded functionalized PET were mixed together to form a pulp. The Eu in the aqueous phase of the mixed pulp accounted for 14.6% of the total Eu introduced by Eu-loaded PET. The remaining pulp was used to prepare paper sheets according to the forming, pressing, and drying conditions of Example 1. The Eu in the final paper sheet accounted for 80.9% of the total Eu introduced by Eu-loaded PET. The Eu in the forming white water and press drainage accounted for 12.1% in total, and the Eu in the equipment rinsing fluid accounted for 4.4%. The total Eu material balance was 97.4%.

[0095] Under 365 nm excitation conditions, Eu 3+ The main emission peak is located at 615.0–615.7 nm, with an average of 615.3 nm. The average ratio of the integrated emission intensity at 610–620 nm between the direct contact region and the corresponding non-contact pulp region of the two types of fibers is 1.18, with a standard deviation of 0.08. The Eu values ​​of the non-contact pulp region and the direct contact region are also relatively high. 3+ The average luminescence lifetimes were 0.374 ms and 0.409 ms, respectively, with corresponding standard deviations of 0.031 ms and 0.034 ms.

[0096] In Eu-treated phenanthroline-functionalized PET, the N 1s component center associated with the 1,10-phenanthroline structural unit is located at 399.21 eV, and the corresponding component centers in the three analytical micro-regions containing the two types of fiber contact boundaries are located at 399.19 eV, 399.25 eV, and 399.22 eV, respectively. The average coordination distance of the Eu first coordination shell is 2.44 ± 0.02 nm, and the average coordination number is 8.5 ± 0.8.

[0097] Table 1. Results of raw material functionalization degree and Eu distribution sample Carboxyl content of cotton pulp (mmol / g) PET-side functionalization status Eu introduction method Eu fixation level / (mmol / g carrier) Eu percentage of mixed slurry aqueous phase (in terms of Eu carryover) / % Final paper Eu percentage of total Eu carried over / Eu Material Balance / % Example 1 0.46 The apparent grafting amount of 1,10-phenanthroline structural units was 0.111 mmol / g. Carboxylated cotton pulp loaded with Eu 0.058 5.8 88.9 98.4 Comparative Example 1 0.043 Apparent grafting amount of 1,10-phenanthroline structural units: 0.110 mmol / g Low-carboxyl content cotton pulp loaded with Eu without TEMPO oxidation 0.011 17.2 74.6 97.6 Comparative Example 2 0.46 Apparent grafting amount of 1,10-phenanthroline structural units: 0.108 mmol / g Eu load not performed — — Below the limit of quantitation — Comparative Example 3 0.46 Aminated PET, without 1,10-phenanthroline-4-carboxylic acid coupling. Carboxylated cotton pulp loaded with Eu 0.058 6.4 88.1 97.8 Comparative Example 4 0.46 Apparent residue of nitrogenous compounds related to 1,10-phenanthroline-4-carboxylic acid: 0.014 mmol / g Carboxylated cotton pulp loaded with Eu 0.058 6.3 88.0 97.7 Comparative Example 5 0.46 Apparent grafting amount of 1,10-phenanthroline structural units: 0.110 mmol / g Phenanthroline-functionalized PET preloaded with Eu 0.105 14.6 80.9 97.4 Table 2. Results of spatially resolved luminescence detection of paper sheets sample <![CDATA[Eu 3+ Average position of main emission peak (nm) Integral emission intensity ratio at 610–620 nm between direct contact region and non-contact pulp region <![CDATA[Non-contact cotton pulp area Eu 3+ Luminescence lifetime / ms]]> <![CDATA[Direct contact area Eu 3+ Luminescence lifetime / ms]]> Example 1 615.2 1.56±0.10 0.329±0.024 0.482±0.031 Comparative Example 1 615.0 1.17±0.07 0.286±0.026 0.331±0.030 Comparative Example 2 Stable Eu³⁺ characteristic peaks were not obtained. 1.05±0.04 No decay curves satisfying the fitting conditions were obtained. No decay curves satisfying the fitting conditions were obtained. Comparative Example 3 615.0 1.14±0.06 0.328±0.024 0.356±0.027 Comparative Example 4 615.0 1.21±0.06 0.330±0.025 0.372±0.029 Comparative Example 5 615.3 1.18±0.08 0.374±0.031 0.409±0.034 Table 3. Detection results of N 1s and Eu first coordination shell in microregions sample PET side reference N 1s component center / eV Three direct contact analysis micro-regions related N 1s component centers / eV Average distance of Eu first coordination shell / nm Average coordination number of Eu's first coordination shell Example 1 398.90 399.20、399.27、399.23 2.43±0.02 8.4±0.8 Comparative Example 1 398.90 398.98、399.03、399.00 2.40±0.02 8.0±0.8 Comparative Example 2 398.90 398.94、398.99、398.96 No fitting results were obtained for the first coordination shell. No fitting results were obtained for the first coordination shell. Comparative Example 3 399.42¹ 399.48、399.53、399.50¹ 2.41±0.02 8.1±0.8 Comparative Example 4 Approximately 398.90² 398.97、399.02、398.99² 2.41±0.02 8.1±0.8 Comparative Example 5 399.21 399.19、399.25、399.22 2.44±0.02 8.5±0.8 The N 1s data listed in Comparative Example 3 correspond to the main nitrogen-containing components in aminated PET, and the N 1s data listed in Comparative Example 4 correspond to the detected components with nitrogen-containing structures related to 1,10-phenanthroline-4-carboxylic acid.

[0098] In Example 1, europium-carboxylated cotton pulp and phenanthrene-functionalized PET chopped fibers were processed and washed separately before being co-formed into paper. The ratio of the integrated emission intensity at 610–620 nm between the directly contacted region and the non-contact cotton pulp region was 1.56 ± 0.10. The Eu values ​​in both regions... 3+ The average emission lifetimes were 0.482±0.031 ms and 0.329±0.024 ms, respectively. For Comparative Examples 1, 3, 4, and 5, after retaining the introduction of Eu, the integrated emission intensity ratios of the direct contact region and the non-contact region were 1.17±0.07, 1.14±0.06, 1.21±0.06, and 1.18±0.08, respectively. Comparative Example 2 did not obtain stable Eu. 3+ Characteristic emission peaks; combined with the Eu distribution, spatially resolved luminescence and micro-area detection results in Tables 1 to 3, under the conditions of loading Eu on the cotton pulp side, fixing 1,10-phenanthroline structural units on the PET side, and processing the two types of fibers separately before wet forming, the resulting paper sheet forms a spatially resolved Eu luminescence state in the area where the two types of fibers are in direct contact, which is different from the area of ​​the same paper sheet that is not in contact with the cotton pulp.

[0099] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A cotton pulp and chemical fiber composite anti-counterfeiting paper for certificates, characterized in that, The paper sheet is composed of interwoven carboxylated cotton pulp fibers and polyethylene terephthalate chopped fibers. The carboxylated cotton pulp fibers are loaded with trivalent europium ions, and the surface of the polyethylene terephthalate chopped fibers is connected to 1,10-phenanthroline-4-carboxylic acid residues through amide bonds. The paper sheet contains areas where the two types of fibers are in direct contact and areas where the carboxylated cotton pulp fibers are not in contact with the polyethylene terephthalate chopped fibers. Under 365 nm excitation, the integrated emission intensity at 610–620 nm and the luminescence lifetime of trivalent europium ions in the direct contact region are both higher than those in the non-contact region.

2. The cotton pulp and chemical fiber composite certificate anti-counterfeiting paper according to claim 1, characterized in that, The carboxyl content of the carboxylated cotton pulp fiber is 0.20–0.70 mmol / g, and the carboxyl group is derived from the oxidation of the primary hydroxyl group at the C6 position of the cotton pulp cellulose.

3. The cotton pulp and chemical fiber composite certificate anti-counterfeiting paper according to claim 1, characterized in that, The length of polyethylene terephthalate chopped fibers is 3–6 mm, and the average diameter is 10–25 μm.

4. The cotton pulp and chemical fiber composite certificate anti-counterfeiting paper according to claim 1, characterized in that, The direct contact area was determined by microscopic observation and Raman spatial positioning. The two types of fibers were continuously adjacent at their edges within this area, and there was no indistinguishable gap within the spatial resolution range of the microscopic system.

5. A method for preparing a cotton pulp and chemical fiber composite certificate anti-counterfeiting paper, characterized in that, include: Bleached cotton pulp was treated in an oxidation system consisting of TEMPO, sodium bromide and sodium hypochlorite. After the reaction was completed, the pulp was washed to obtain carboxylated cotton pulp. The carboxylated cotton pulp was then contacted with an aqueous solution of europium chloride to complete the europium loading treatment. After washing, the pulp was obtained as europium-loaded carboxylated cotton pulp. Polyethylene terephthalate chopped fibers were placed in an aqueous solution of ethylenediamine for surface ammonolysis, and washed to obtain aminated PET chopped fibers. Then, 1,10-phenanthroline-4-carboxylic acid activated with 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide was reacted with the aminated PET chopped fibers, and washed to obtain phenanthroline-functionalized PET chopped fibers. Europium-carboxylated cotton pulp and phenanthrene-functionalized PET chopped fibers, which have been washed separately, are dispersed together in water and wet-formed to obtain wet paper sheets. The wet paper sheets are then pressed and dried to obtain cotton pulp and chemical fiber composite certificate anti-counterfeiting paper.

6. The method for preparing the cotton pulp and chemical fiber composite certificate anti-counterfeiting paper according to claim 5, characterized in that, Bleached cotton pulp was oxidized at 20–30°C and pH 10.0–10.5 to obtain carboxylated cotton pulp with a carboxyl content of 0.20–0.70 mmol / g. The molar amount of trivalent europium ions added was 0.15–0.20 times the molar amount of carboxyl ions. The pH of the europium-loaded treatment solution was 5.5–6.0, and the contact time was 30–120 min.

7. The method for preparing the cotton pulp and chemical fiber composite certificate anti-counterfeiting paper according to claim 5, characterized in that, Short-cut polyethylene terephthalate fibers were treated in an aqueous solution of 5%–15% ethylenediamine at 40–60°C for 30–90 min. 1,10-phenanthroline-4-carboxylic acid was activated with 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide at pH 5.3–5.8, and then subjected to amidation reaction with aminated PET chopped fibers at pH 7.0–7.

3.

8. The method for preparing the cotton pulp and chemical fiber composite certificate anti-counterfeiting paper according to claim 5, characterized in that, Based on a total of 100 parts of the oven-dry weight of the two types of fibers, europium-carboxylated cotton pulp is 92-97 parts, and phenanthrene-functionalized PET short-cut fiber is 3-8 parts; The pulp consistency after co-blending is 0.3%–0.8%, the dryness of the wet paper after pressing is 40%–50%, the drying temperature is 95–110℃, and the moisture content of the dried paper is 4%–8%.