Buckling-resistant blade tenon and assembly method for ceramic matrix composite turbine blades
By incorporating metal reinforcements and skeletons with a higher coefficient of thermal expansion within the tenon of a ceramic matrix composite turbine blade, an adaptive pre-tightening fit is formed, which solves the buckling problem of the tenon of the ceramic matrix composite turbine blade under high temperature and high centrifugal load, improves buckling resistance, prevents detachment, and keeps the cooling air passage unobstructed.
Patent Information
- Application Number
- CN202611539790.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-10
AI Technical Summary
Ceramic matrix composite turbine blade tenons are prone to buckling failure under high temperature and high centrifugal load conditions, leading to turbine failure. Existing metal cladding and indirect connection solutions have failed to effectively improve buckling resistance.
A metal reinforcement with a thermal expansion coefficient greater than that of the ceramic matrix composite blade tenon is used and set in the tenon cavity. The cooling air channel runs through it. The support is enhanced by adaptive pre-tightening fit. Combined with the metal reinforcement skeleton and auxiliary parts, they are arranged in the buckling-prone area to form an adaptive pre-tightening fit.
It effectively improves the buckling resistance of ceramic matrix composite blade tenons under high temperature and high centrifugal load, avoids detachment failure, keeps the cooling air passage unobstructed, and has good engineering compatibility.
Smart Images

Figure CN123064531A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of turbine technology, specifically relating to a buckling-resistant tenon for a ceramic matrix composite turbine blade and its assembly method. Background Technology
[0002] Ceramic matrix composites (CMCs) have become ideal candidate materials for hot-end components of next-generation aero-engines and gas turbines due to their low density (about one-third to one-quarter that of traditional nickel-based superalloys), high temperature resistance (capable of withstanding temperatures above 1200 ℃) and good oxidation resistance.
[0003] Currently, ceramic matrix composites have been successfully applied to components such as combustion chambers, turbine outer rings, and turbine guide vanes (i.e., turbine rotor blades), and have also been used in turbine rotor blades (i.e., turbine moving blades) in some advanced aero-engines. Compared to traditional nickel-based superalloys, using ceramic matrix composites to manufacture turbine moving blades can significantly reduce the weight of the aero-engine itself, reduce the cooling gas requirement, and allow for increased combustion chamber exit temperatures, thereby effectively improving the thrust-to-weight ratio and thermal efficiency of the aero-engine.
[0004] However, the further promotion of ceramic matrix composites in turbine blades still faces many technical challenges, among which the structural integrity of the ceramic matrix composite blade tenon is particularly prominent. To reduce the weight of the ceramic matrix composite turbine blade and provide a cooling air channel, hollow ceramic matrix composite blade tenons are considered a potential technical direction. However, the hollow structure further weakens the load-bearing capacity of the ceramic matrix composite blade tenon, making it prone to buckling failure under huge centrifugal loads. Once the ceramic matrix composite blade tenon buckles, it will cause the ceramic matrix composite turbine blade to fall off from the root, leading to serious turbine failure.
[0005] The solutions proposed by the industry to address the above problems currently have the following shortcomings:
[0006] (1) Metal cladding scheme
[0007] A common approach is to wrap a metal layer around the outside of the ceramic matrix composite (CMC) blade tenon. This metal layer bears the friction between the CMC blade tenon and the wheel mortise, aiming to improve the operating conditions of the CMC blade tenon. However, this approach primarily addresses the wear problem between the CMC blade tenon and the wheel mortise, offering limited improvement to the overall load-bearing capacity of the CMC blade tenon. Furthermore, due to the significant difference in thermal expansion coefficients between the metal layer and the CMC blade tenon, interface stress concentration can easily occur under high-temperature conditions, leading to interface peeling between the metal layer and the CMC blade tenon, further weakening the structural integrity of the CMC blade tenon.
[0008] (2) Indirect connection scheme
[0009] Another approach is to use a separate transition piece to indirectly connect the end of the ceramic matrix composite turbine blade to the wheel disk tenon through the transition piece. However, this approach has problems such as complex structure, large number of parts, and complicated assembly process. Moreover, the transition piece itself also faces challenges in strength and reliability under the coupled action of high temperature and high centrifugal load, and does not fundamentally solve the problem of insufficient buckling resistance of the ceramic matrix composite turbine blade tenon.
[0010] In summary, neither the existing metal cladding solution nor the indirect connection solution can fundamentally solve the technical problem of insufficient buckling resistance of ceramic matrix composite turbine blade tenons under high temperature and high centrifugal load conditions. Once the ceramic matrix composite turbine blade tenon fails to buckle, it will directly cause the ceramic matrix composite turbine blade to fall off from the root, thereby causing serious turbine failure.
[0011] Therefore, there is an urgent need to provide a solution that can effectively improve the buckling resistance of ceramic matrix composite blade tenons in order to meet the high reliability and long service life requirements of hot-end components in the new generation of aero engines and gas turbines. Summary of the Invention
[0012] In view of the above-mentioned deficiencies of the prior art, the present invention provides a buckling-resistant tenon for a ceramic matrix composite turbine blade and an assembly method thereof, which can effectively improve the buckling resistance of the ceramic matrix composite blade tenon body under high temperature and high centrifugal load conditions.
[0013] The technical solution adopted by this invention to solve its technical problem is:
[0014] A buckling-resistant blade tenon for a ceramic matrix composite turbine blade, wherein the ceramic matrix composite turbine blade includes a blade tenon and a ceramic matrix composite blade body;
[0015] The moving blade tenon includes a ceramic matrix composite moving blade tenon body and a metal reinforcing member. The coefficient of thermal expansion of the metal reinforcing member is greater than that of the ceramic matrix composite moving blade tenon body. One end of the ceramic matrix composite moving blade tenon body is used to connect with a corresponding end of the ceramic matrix composite moving blade body and is defined as the first end. The other end of the ceramic matrix composite moving blade tenon body is arranged opposite to the first end and is defined as the second end. The ceramic matrix composite moving blade tenon body is a hollow structure with both the first end and the second end open. The inner cavity of the ceramic matrix composite moving blade tenon body is defined as the tenon body cavity. The metal reinforcing member is disposed in the tenon body cavity, and the structure and size of the metal reinforcing member are adapted to the structure and size of the tenon body cavity. The metal reinforcing member is provided with a through cooling air channel, which extends along the line connecting the first end and the second end.
[0016] Furthermore, an isolation coating is provided on the surface of the metal reinforcement, the metal reinforcement is arranged in the entire area of the tenon body cavity, and is achieved by pre-embedding during the prefabrication layup stage of the ceramic matrix composite moving blade tenon body.
[0017] Furthermore, the isolation coating is disposed on the surface of the metal reinforcement at a position corresponding to the sidewall of the ceramic matrix composite moving blade tenon body.
[0018] Furthermore, the metal reinforcement is disposed in the buckling-prone area of the tenon body cavity and includes a metal reinforcing skeleton and multiple metal reinforcing auxiliary components. The metal reinforcing skeleton and multiple metal reinforcing auxiliary components are inserted into the tenon body cavity through the second end opening of the ceramic matrix composite moving blade tenon body. The multiple metal reinforcing auxiliary components are arranged around the outer side of the metal reinforcing skeleton in the tenon body cavity. The structure and size of each metal reinforcing auxiliary component are adapted to the structure and size of the corresponding position in the tenon body cavity.
[0019] Furthermore, the sidewall of the ceramic matrix composite moving blade tenon body includes a tenon body load-bearing wall and a tenon body non-load-bearing wall. The tenon body load-bearing wall is used to withstand the force applied by the wheel mortise during operation. Each of the metal reinforcing auxiliary members is located in the tenon body cavity between the tenon body load-bearing wall and the metal reinforcing skeleton member.
[0020] Furthermore, an assembly gap is reserved between each of the metal reinforcing auxiliary parts and the load-bearing wall of the tenon body at room temperature; an assembly gap is reserved between the metal reinforcing skeleton part and the non-load-bearing wall of the tenon body at room temperature.
[0021] Furthermore, the cooling air passage is arranged on the metal reinforcing frame.
[0022] Furthermore, the metal reinforcement is fixedly connected to the ceramic matrix composite moving blade tenon body by a pin.
[0023] A method for assembling a buckling-resistant tenon for a ceramic matrix composite turbine blade, specifically comprising: firstly, setting an isolation coating on the surface of the metal reinforcement; then, during the prefabrication layup stage of the ceramic matrix composite blade tenon body and the ceramic matrix composite blade body, embedding the metal reinforcement into the prefabrication of the ceramic matrix composite blade tenon body and fixing it; and finally completing the preparation of the ceramic matrix composite blade tenon body and the ceramic matrix composite blade body.
[0024] A method for assembling a buckling-resistant tenon for a ceramic matrix composite turbine blade is disclosed. Specifically, the method involves: first, based on the service condition analysis of the turbine blade composed of the tenon body and the blade body, combined with finite element simulation or centrifugal testing, determining the severely deformed areas of the tenon body under centrifugal load, corresponding to the buckling-prone areas of the tenon body cavity; then, inserting each of the metal reinforcing auxiliary components into the corresponding positions of the buckling-prone areas of the tenon body cavity from the second end opening of the tenon body and fixing them; then, inserting the metal reinforcing skeleton into the buckling-prone areas of the tenon body cavity from the second end opening of the tenon body and fixing it, so that multiple metal reinforcing auxiliary components are arranged around the outside of the metal reinforcing skeleton within the tenon body cavity, thus completing the assembly of the blade tenon.
[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0026] The buckling-resistant tenon of the ceramic matrix composite turbine blade in this invention includes a ceramic matrix composite blade tenon body and a metal reinforcement. The coefficient of thermal expansion of the metal reinforcement is greater than that of the ceramic matrix composite blade tenon body. One end of the ceramic matrix composite blade tenon body is used to connect with the corresponding end of the ceramic matrix composite blade body and is defined as the first end. The other end of the ceramic matrix composite blade tenon body is arranged opposite to the first end and is defined as the second end. The ceramic matrix composite blade tenon body is a hollow structure with both the first and second ends open. The inner cavity of the ceramic matrix composite blade tenon body is defined as the tenon body cavity. The metal reinforcement is disposed in the tenon body cavity, and the structure and size of the metal reinforcement are adapted to the structure and size of the tenon body cavity. The metal reinforcement is provided with a through cooling air channel, which extends along the line connecting the first and second ends. Because the coefficient of thermal expansion of the metal reinforcement is greater than that of the ceramic matrix composite moving blade tenon body, at operating temperature, the thermal expansion of the metal reinforcement is greater than that of the ceramic matrix composite moving blade tenon body. The metal reinforcement exerts an outward supporting force on the load-bearing wall of the ceramic matrix composite moving blade tenon body within the tenon body cavity. Simultaneously, the wheel mortise and tenon groove on the outside of the tenon body cavity constrains the load-bearing wall of the ceramic matrix composite moving blade tenon body. The combined effect of these two forces allows the metal reinforcement to apply pre-tightening pressure to the inner surface of the load-bearing wall of the ceramic matrix composite moving blade tenon body, thereby generating an automatic wedging effect and forming an adaptive pre-tightening fit, effectively... This invention ensures the support effect of the metal reinforcement on the load-bearing wall of the ceramic matrix composite blade tenon body under high-temperature conditions, and effectively improves the buckling resistance of the ceramic matrix composite blade tenon body under high-temperature and high-centrifugal load conditions. It effectively avoids the failure of the ceramic matrix composite turbine blade due to buckling failure of the ceramic matrix composite blade tenon body. Moreover, this invention does not change the contact interface between the ceramic matrix composite blade tenon body and the wheel disk tenon, does not require treatment of the outer surface of the ceramic matrix composite blade tenon body, and does not require modification of the existing wheel disk tenon. It can be directly applied to existing aero engines or gas turbines, and has good engineering compatibility. Attached Figure Description
[0027] Figure 1 This is a schematic diagram of the front cross-sectional structure of the anti-buckling blade tenon of the ceramic matrix composite turbine blade in this invention;
[0028] Figure 2 This is a partial side sectional view of the anti-buckling blade tenon of the ceramic matrix composite turbine blade in Embodiment 1 of the present invention;
[0029] Figure 3 for Figure 2 Enlarged structural diagram at point A in the middle circle;
[0030] Figure 4 This is a partial front view sectional view of the anti-buckling blade tenon of the ceramic matrix composite turbine blade in Embodiment 1 of the present invention;
[0031] Figure 5 This is a partial side sectional view of the anti-buckling blade tenon of the ceramic matrix composite turbine blade in Embodiment 2 of the present invention;
[0032] Figure 6 This is a top sectional view of the anti-buckling blade tenon of the ceramic matrix composite turbine blade in Embodiment 2 of the present invention.
[0033] The following are the annotations in the figure: 1. Ceramic matrix composite moving blade body; 2. Ceramic matrix composite moving blade tenon body; 201. First end; 202. Second end; 203. Tenon body cavity; 204. Tenon body load-bearing wall; 205. Tenon body non-load-bearing wall; 3. Metal reinforcement; 301. Metal reinforcement skeleton; 302. Metal reinforcement auxiliary component; 4. Cooling air channel; 5. Isolation coating; 6. Assembly gap; 7. Reserved gap; 8. Pin mounting hole; 9. Ceramic matrix composite moving blade blade holder. Detailed Implementation
[0034] The specific embodiments of the present invention will be further described in detail below with reference to the accompanying drawings. These embodiments are for illustrative purposes only and are not intended to limit the scope of the invention.
[0035] In the description of this invention, it should be noted that the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0036] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0037] Furthermore, in the description of this invention, unless otherwise stated, "a plurality of" means two or more.
[0038] like Figure 1 As shown, a buckling-resistant blade tenon for a ceramic matrix composite turbine blade is provided. The ceramic matrix composite turbine blade includes a blade tenon and a ceramic matrix composite blade body 1.
[0039] The moving blade tenon includes a ceramic matrix composite moving blade tenon body 2 and a metal reinforcing member 3. The coefficient of thermal expansion of the metal reinforcing member 3 is greater than that of the ceramic matrix composite moving blade tenon body 2. One end of the ceramic matrix composite moving blade tenon body 2 is used to connect with the corresponding end of the ceramic matrix composite moving blade body 1 and is defined as the first end 201. The other end of the ceramic matrix composite moving blade tenon body 2 is arranged opposite to the first end 201 and is defined as the second end 202. The ceramic matrix composite moving blade tenon body 2 is a hollow structure with both the first end 201 and the second end 202 open. The inner cavity of the ceramic matrix composite moving blade tenon body 2 is defined as the tenon body cavity 203. The metal reinforcing member 3 is disposed in the tenon body cavity 203, and the structure and size of the metal reinforcing member 3 are adapted to the structure and size of the tenon body cavity 203. The metal reinforcing member 3 is provided with a through cooling air channel 4, which extends along the line connecting the first end 201 and the second end 202. The first end 201 of the ceramic matrix composite moving blade tenon body 2 is connected to the corresponding end of the ceramic matrix composite moving blade body 1 through the ceramic matrix composite moving blade basin 9.
[0040] Because the coefficient of thermal expansion of the metal reinforcing member 3 is greater than that of the ceramic matrix composite moving blade tenon body 2, at the operating temperature, the amount of thermal expansion of the metal reinforcing member 3 is greater than that of the ceramic matrix composite moving blade tenon body 2. The metal reinforcing member 3 exerts an outward supporting force on the force-bearing wall of the ceramic matrix composite moving blade tenon body 2 within the tenon body cavity 203. Simultaneously, the wheel mortise groove constrains the force-bearing wall of the ceramic matrix composite moving blade tenon body 2 outside the tenon body cavity 203. The combined effect of these two forces causes the metal reinforcing member 3 to apply pre-tightening pressure to the inner surface of the force-bearing wall of the ceramic matrix composite moving blade tenon body 2, thereby generating an automatic wedging effect and forming an adaptive pre-tightening fit. This effectively ensures the support effect of the metal reinforcement 3 on the load-bearing wall of the ceramic matrix composite blade tenon body 2 under high temperature conditions, and effectively improves the buckling resistance of the ceramic matrix composite blade tenon body 2 under high temperature and high centrifugal load conditions, effectively avoiding the failure of the ceramic matrix composite turbine blade due to buckling failure of the ceramic matrix composite blade tenon body 2; moreover, the present invention does not change the contact interface between the ceramic matrix composite blade tenon body 2 and the wheel disk tenon groove, does not require treatment of the outer surface of the ceramic matrix composite blade tenon body 2, and does not require modification of the existing wheel disk tenon groove, and can be directly applied to existing aero engines or gas turbines, with good engineering compatibility.
[0041] By setting a cooling air channel 4 on the metal reinforcement 3, it is ensured that the cooling air can flow from the tenon side of the moving blade to the ceramic matrix composite moving blade body 1 side, or flow in the opposite direction, so as not to block the original cooling airflow path due to the setting of the metal reinforcement 3.
[0042] Example 1, as Figure 2-4 As shown, an isolation coating 5 is provided on the surface of the metal reinforcement 3. The metal reinforcement 3 is arranged throughout the entire area of the tenon body cavity 203 and is achieved by pre-embedding during the prefabrication layup stage of the ceramic matrix composite moving blade tenon body 2. The ceramic matrix composite moving blade tenon body 2 and the ceramic matrix composite moving blade body 1 are integrally laid using continuous fiber prefabrication.
[0043] Since the metal reinforcement 3 is arranged throughout the entire area of the tenon body cavity 203, and the structure and size of the metal reinforcement 3 are adapted to the structure and size of the tenon body cavity 203, the metal reinforcement 3 can support the side wall of the ceramic matrix composite moving blade tenon body 2 along the circumference of the tenon body cavity 203.
[0044] By setting the isolation coating 5, the metal reinforcement 3 is not affected by the high-temperature process during the preparation of the ceramic matrix composite moving blade tenon body 2, thereby reducing the risk of direct chemical reaction between the metal reinforcement 3 and the ceramic matrix composite moving blade tenon body 2.
[0045] During the preparation of the ceramic matrix composite moving blade tenon body 2 and the ceramic matrix composite moving blade blade body 1, due to the presence of a high-temperature stage, the metal reinforcement 3 undergoes thermal expansion. The size of the tenon body cavity 203 of the prepared ceramic matrix composite moving blade tenon body 2 matches the size of the metal reinforcement 3 in its high-temperature expansion state. After cooling to room temperature, the metal reinforcement 3 shrinks, forming a reserved gap 7 between itself and the side wall of the ceramic matrix composite moving blade tenon body 2. This can alleviate the excessive pressure on the side wall of the ceramic matrix composite moving blade tenon body 2 caused by the re-thermal expansion of the metal reinforcement 3 under high-temperature service conditions.
[0046] The isolation coating 5 is arranged on the surface of the metal reinforcement 3 at a position corresponding to the side wall of the ceramic matrix composite moving blade tenon body 2.
[0047] Among them, the isolation coating 5 is a niobium coating.
[0048] Example 2, as Figure 5 and Figure 6 As shown, the metal reinforcing member 3 is disposed in the buckling-prone area of the tenon body cavity 203, and includes a metal reinforcing skeleton member 301 and multiple metal reinforcing auxiliary members 302. Both the metal reinforcing skeleton member 301 and the multiple metal reinforcing auxiliary members 302 are inserted into the tenon body cavity 203 through the opening at the second end 202 of the ceramic matrix composite moving blade tenon body 2. The multiple metal reinforcing auxiliary members 302 are arranged around the outer side of the metal reinforcing skeleton member 301 within the tenon body cavity 203, and the structure and dimensions of each metal reinforcing auxiliary member 302 are adapted to the structure and dimensions of the corresponding position in the tenon body cavity 203. The buckling-prone area can be determined based on the stress distribution, deformation distribution, and stability analysis results of the ceramic matrix composite moving blade tenon body 2 under high-temperature service conditions.
[0049] In this way, the metal reinforcing skeleton 301 and multiple metal reinforcing auxiliary parts 302 work together to provide local support for the sidewalls of the ceramic matrix composite moving blade tenon body 2 at corresponding positions. In addition, since the metal reinforcing parts 3 are only placed in the buckling-prone areas, it is possible to improve the buckling resistance of critical areas while reducing the amount of metal material used, reducing additional weight, and retaining a large cooling airflow space.
[0050] The ceramic matrix composite moving blade tenon body 2 has a side wall including a tenon body load-bearing wall 204 and a tenon body non-load-bearing wall 205. The tenon body load-bearing wall 204 is used to bear the force applied by the wheel mortise during operation. Each metal reinforcing auxiliary member 302 is located in the tenon body cavity 203 between the tenon body load-bearing wall 204 and the metal reinforcing skeleton member 301.
[0051] In this way, when the tenon body load-bearing wall 204 is subjected to external pressure transmitted by the wheel mortise and groove and has an inward buckling tendency, the metal reinforcing auxiliary member 302 can be directly located on the load transmission path and transmit the local deformation of the tenon body load-bearing wall 204 to the metal reinforcing skeleton member 301. The metal reinforcing skeleton member 301 further provides overall support. This structure can provide targeted reinforcement to the load-bearing wall area most prone to buckling without significantly increasing the weight of the moving blade tenon.
[0052] Preferably, the metal reinforcing auxiliary member 302 located at the edge of the easily buckled area of the tenon body cavity 203 extends towards the non-severely deformed area to ensure a smooth stress transition. The shape and number of the metal reinforcing skeleton members 301 are selected according to the installation process.
[0053] Preferably, an assembly gap 6 is provided between each metal reinforcing auxiliary component 302 and the load-bearing wall 204 of the tenon body at room temperature; an assembly gap 6 is also provided between the metal reinforcing skeleton component 301 and the non-load-bearing wall 205 of the tenon body at room temperature. The size of the above-mentioned assembly gap 6 is determined comprehensively based on the room temperature installation requirements and the high temperature pre-tightening requirements, and is calculated and optimized in combination with the difference in the thermal expansion coefficients of the metal reinforcing skeleton component 301 and the metal reinforcing auxiliary component 302 and the ceramic matrix composite moving blade tenon body 2.
[0054] As the service temperature increases, the thermal expansion of the metal reinforced skeleton 301 and the metal reinforced auxiliary component 302 is greater than that of the ceramic matrix composite moving blade tenon body 2, causing the corresponding assembly gap 6 to gradually decrease. This results in more effective internal support under high-temperature service conditions, applying pre-tightening pressure to the inner surface of the tenon body stress wall 204 to form an adaptive pre-tightening fit. This setting can reduce the risk of interference during the normal temperature assembly stage and improve the buckling resistance under high-temperature service conditions.
[0055] The cooling air passage 4 is arranged on the metal reinforced frame 301.
[0056] In Embodiments 1 and 2, the metal reinforcing member 3 and the ceramic matrix composite moving blade tenon body 2 are fixedly connected by pins. The number, size, and placement of the pins are determined based on the load distribution of the ceramic matrix composite moving blade tenon body 2 and the installation process requirements of the metal reinforcing member 3. Figures 4-6 The reference numeral 8 in the attached figure indicates the pin mounting hole.
[0057] In both Embodiment 1 and Embodiment 2, the metal reinforcing member 3 is made of a nickel-based high-temperature alloy.
[0058] In Examples 1 and 2, the ceramic matrix composite leaf tenon body 2 is shaped like a fir tree, see... Figure 2 and Figure 5 .
[0059] A method for assembling a buckling-resistant tenon for a ceramic matrix composite turbine blade, used to assemble the buckling-resistant tenon of the ceramic matrix composite turbine blade in Example 1, specifically involves: firstly, setting an isolation coating 5 on the surface of a metal reinforcement 3; then, during the prefabrication layup stage of the ceramic matrix composite blade tenon body 2 and the ceramic matrix composite blade body 1, embedding the metal reinforcement 3 into the prefabrication of the ceramic matrix composite blade tenon body 2 and fixing it; and finally completing the preparation of the ceramic matrix composite blade tenon body 2 and the ceramic matrix composite blade body 1.
[0060] By adopting this assembly method, the metal reinforcement 3 is pre-embedded in the tenon body cavity 203 during the forming process of the ceramic matrix composite moving blade tenon body 2. Therefore, the positional relationship between the metal reinforcement 3 and the tenon body cavity 203 is stable, and it can provide continuous support for the ceramic matrix composite moving blade tenon body 2 within the entire tenon body cavity 203. It is especially suitable for ceramic matrix composite turbine moving blades where the need to improve the buckling resistance of the ceramic matrix composite moving blade tenon body 2 can be determined in the design stage.
[0061] A method for assembling a buckling-resistant tenon for a ceramic matrix composite turbine blade, used to assemble the buckling-resistant tenon of the ceramic matrix composite turbine blade in Example 2, specifically involves: firstly, based on the service condition analysis of the turbine blade composed of the ceramic matrix composite tenon body 2 and the ceramic matrix composite blade body 1, and combined with finite element simulation or centrifugal test methods, determining the severely deformed areas of the ceramic matrix composite tenon body 2 under centrifugal load, and corresponding to the buckling-prone areas of the tenon body cavity 203; then, based on the location and extent of the buckling-prone areas and the local shape of the tenon body cavity 203, designing a metal reinforcing skeleton 301 and various metal reinforcing auxiliary parts 3. The structural dimensions of 02 are determined by machining each metal reinforcing auxiliary component 302 into a shape that matches the corresponding position of the tenon body cavity 203. Then, each metal reinforcing auxiliary component 302 is inserted into the corresponding position of the easily buckled area of the tenon body cavity 203 from the second end 202 opening of the ceramic matrix composite moving blade tenon body 2 and fixed. After that, the metal reinforcing skeleton component 301 is inserted into the easily buckled area of the tenon body cavity 203 from the second end 202 opening of the ceramic matrix composite moving blade tenon body 2 and fixed. This allows multiple metal reinforcing auxiliary components 302 to be arranged around the outside of the metal reinforcing skeleton component 301 within the tenon body cavity 203, thus completing the assembly of the moving blade tenon.
[0062] By adopting this assembly method, the metal reinforcement 3 can be assembled after the ceramic matrix composite moving blade tenon body 2 is prepared. It is not necessary to pre-embed the metal reinforcement 3 during the prefabrication layup stage of the ceramic matrix composite moving blade tenon body 2 and the ceramic matrix composite moving blade body 1, which provides high process flexibility. At the same time, this method can target the buckling-prone areas based on the simulation or test results of the specific moving blade tenon, avoiding excessive reinforcement of non-critical areas, which is conducive to balancing structural reliability, weight reduction effect and cooling air flow capacity.
[0063] The metal reinforcing skeleton 301 can restrict the metal reinforcing auxiliary 302 from moving towards the center of the tenon body cavity 203. Preferably, the metal reinforcing auxiliary 302 is located between the tenon body force-bearing wall 204 and the metal reinforcing skeleton 301, thus forming a load transmission path composed of the tenon body force-bearing wall 204, the metal reinforcing auxiliary 302 and the metal reinforcing skeleton 301.
[0064] In summary, the moving blade tenon of the present invention has outstanding advantages such as compact structure, strong load-bearing capacity, good thermal adaptability, and feasible manufacturing process.
[0065] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and substitutions can be made without departing from the technical principles of the present invention, and these improvements and substitutions should also be considered within the scope of protection of the present invention.
Claims
1. A buckling-resistant tenon for a ceramic matrix composite turbine blade, the ceramic matrix composite turbine blade comprising a blade tenon and a ceramic matrix composite blade body (1); characterized in that: The moving blade tenon includes a ceramic matrix composite moving blade tenon body (2) and a metal reinforcing member (3). The coefficient of thermal expansion of the metal reinforcing member (3) is greater than that of the ceramic matrix composite moving blade tenon body (2). One end of the ceramic matrix composite moving blade tenon body (2) is used to connect with the corresponding end of the ceramic matrix composite moving blade body (1) and is defined as the first end (201). The other end of the ceramic matrix composite moving blade tenon body (2) is arranged opposite to the first end (201) and is defined as the second end (202). The body (2) is a hollow structure with openings at both the first end (201) and the second end (202). The inner cavity of the ceramic matrix composite moving blade tenon body (2) is defined as the tenon body cavity (203). The metal reinforcement (3) is disposed in the tenon body cavity (203), and the structure and size of the metal reinforcement (3) are adapted to the structure and size of the tenon body cavity (203). The metal reinforcement (3) is provided with a through cooling air channel (4), which extends along the line connecting the first end (201) and the second end (202).
2. The anti-buckling tenon for a ceramic matrix composite turbine blade according to claim 1, characterized in that: The surface of the metal reinforcement (3) is provided with an isolation coating (5). The metal reinforcement (3) is arranged in the entire area of the tenon body cavity (203) and is realized by pre-embedding in the prefabrication stage of the ceramic matrix composite moving blade tenon body (2).
3. The anti-buckling tenon for a ceramic matrix composite turbine blade according to claim 2, characterized in that: The isolation coating (5) is arranged on the surface of the metal reinforcement (3) at a position corresponding to the side wall of the ceramic matrix composite blade tenon body (2).
4. The anti-buckling tenon for a ceramic matrix composite turbine blade according to claim 1, characterized in that: The metal reinforcement (3) is disposed in the buckling area of the tenon body cavity (203) and includes a metal reinforcement skeleton (301) and multiple metal reinforcement auxiliary parts (302). The metal reinforcement skeleton (301) and multiple metal reinforcement auxiliary parts (302) are inserted into the tenon body cavity (203) through the opening of the second end (202) of the ceramic matrix composite moving blade tenon body (2). The multiple metal reinforcement auxiliary parts (302) are arranged around the outside of the metal reinforcement skeleton (301) in the tenon body cavity (203). The structure and size of each metal reinforcement auxiliary part (302) are adapted to the structure and size of the corresponding position of the tenon body cavity (203).
5. The anti-buckling tenon for a ceramic matrix composite turbine blade according to claim 4, characterized in that: The sidewall of the ceramic matrix composite moving blade tenon body (2) includes a tenon body load-bearing wall (204) and a tenon body non-load-bearing wall (205). The tenon body load-bearing wall (204) is used to bear the force applied by the wheel mortise during operation. Each of the metal reinforcing auxiliary members (302) is located in the tenon body cavity (203) between the tenon body load-bearing wall (204) and the metal reinforcing skeleton member (301).
6. The anti-buckling tenon for a ceramic matrix composite turbine blade according to claim 5, characterized in that: Each of the metal reinforcing auxiliary parts (302) and the tenon body load-bearing wall (204) has an assembly gap (6) reserved at room temperature; the metal reinforcing skeleton part (301) and the tenon body non-load-bearing wall (205) have an assembly gap (6) reserved at room temperature.
7. The anti-buckling tenon for a ceramic matrix composite turbine blade according to claim 4, characterized in that: The cooling air passage (4) is arranged on the metal reinforcing frame (301).
8. The anti-buckling tenon for a ceramic matrix composite turbine blade according to claim 2 or 4, characterized in that: The metal reinforcement (3) is fixedly connected to the ceramic matrix composite moving blade tenon body (2) by a pin.
9. A method for assembling a buckling-resistant tenon for a ceramic matrix composite turbine blade, used for assembling the buckling-resistant tenon for a ceramic matrix composite turbine blade as described in any one of claims 2, 3, and 8, characterized in that, Specifically, an isolation coating (5) is first applied to the surface of the metal reinforcement (3). Then, during the prefabrication layup stage of the ceramic matrix composite moving blade tenon body (2) and the ceramic matrix composite moving blade body (1), the metal reinforcement (3) is pre-embedded into the prefabrication of the ceramic matrix composite moving blade tenon body (2) and fixed. After that, the preparation of the ceramic matrix composite moving blade tenon body (2) and the ceramic matrix composite moving blade body (1) is completed.
10. A method for assembling a buckling-resistant tenon for a ceramic matrix composite turbine blade, used for assembling the buckling-resistant tenon for a ceramic matrix composite turbine blade as described in any one of claims 4-8, characterized in that, Specifically, based on the service condition analysis of the turbine blade composed of the ceramic matrix composite blade tenon body (2) and the ceramic matrix composite blade body (1), combined with finite element simulation or centrifugal test methods, the severely deformed area of the ceramic matrix composite blade tenon body (2) under centrifugal load is determined, and the buckling-prone area of the tenon body cavity (203) is correspondingly identified; then, each of the metal reinforcing auxiliary parts (302) is removed from the second... The end (202) opening is inserted into the corresponding position of the easily buckled area of the tenon body cavity (203) and fixed. Then, the metal reinforcing skeleton (301) is inserted into the easily buckled area of the tenon body cavity (203) from the second end (202) opening of the ceramic matrix composite moving blade tenon body (2) and fixed. Multiple metal reinforcing auxiliary parts (302) are arranged around the outside of the metal reinforcing skeleton (301) in the tenon body cavity (203) to complete the assembly of the moving blade tenon.