Brown fused alumina pouring type electric arc furnace inner insulation process

By employing a three-layer composite structure consisting of a nanoporous insulation layer, a high-alumina refractory brick support layer, and a high-performance refractory castable in a brown fused alumina tilting electric arc furnace, the problem of poor thermal insulation performance was solved, achieving the effects of reducing energy consumption, stabilizing furnace temperature, extending service life, and improving product quality.

CN123065221APending Publication Date: 2026-11-10GUIZHOU GUXIN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611037134.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-13
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The traditional brown fused alumina tilting electric arc furnace has poor insulation performance, resulting in high energy consumption, unstable furnace temperature, affecting product quality, short service life, high maintenance costs, and poor overall structural integrity.

Method used

The system employs a three-layer composite internal insulation structure consisting of a nanoporous insulation layer, a high-alumina refractory brick support layer, and a high-performance refractory castable. The insulation performance is enhanced through gradient design and a special adhesive, and key components are treated with differentiated sealing to optimize the overall insulation process.

Benefits of technology

It significantly reduces smelting power consumption, stabilizes furnace temperature, improves product quality and service life, reduces downtime for maintenance, eliminates safety hazards, and enhances production safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Brown corundum pouring type electric arc furnace inner heat insulation process, brown corundum pouring type electric arc furnace interior includes nano microporous heat insulation layer, high alumina refractory brick support layer and high performance refractory castable working layer, nano microporous heat insulation layer, high alumina refractory brick support layer and high performance refractory castable working layer constitute three layer composite inner heat insulation structure, the present application adopts nano microporous heat insulation layer + high alumina refractory brick support layer + high performance refractory castable three layer composite inner heat insulation process, the core application scene focuses on brown corundum smelting field, significantly reduce smelting comprehensive power consumption, compress production operation cost;Stable hearth temperature, improve the overall quality of brown corundum and high-end product proportion;Prolong the service life of furnace wall, reduce the production capacity waste caused by shutdown maintenance;Eliminate the safety hidden danger such as equipment heat leakage and structure damage, comprehensively improve the workshop safety production level, completely adapt to the production modification needs of various brown corundum production enterprises.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the internal insulation technology of a brown fused alumina tilting electric arc furnace, belonging to the field of brown fused alumina technology. Background Technology

[0002] Brown fused alumina is a synthetic corundum made primarily from bauxite through high-temperature electric arc melting. It possesses excellent properties such as high hardness, good toughness, strong self-sharpening ability, and good chemical stability, making it an indispensable core material in many key sectors of the national economy, including abrasives, refractories, precision casting, military equipment, and electronic semiconductors. The abrasives industry accounts for over 60% of total brown fused alumina consumption, the refractories industry accounts for approximately 25%, and the remainder is used in sandblasting, polishing, and filtration.

[0003] Tilting electric arc furnaces have become the mainstream equipment for brown fused alumina smelting in China due to their advantages such as high production efficiency, good product density, excellent self-sharpening properties, and ability to achieve continuous production, accounting for more than 70% of the total number of existing smelting furnaces. In recent years, with the rapid development of downstream high-end manufacturing industries, higher requirements have been placed on the quality indicators of brown fused alumina products, such as purity, density, and particle size uniformity. The market demand for high-quality brown fused alumina has maintained an average annual growth rate of over 8%.

[0004] Brown fused alumina smelting is a typical high-energy-consuming industry, with electricity consumption accounting for 50%-60% of production costs. The temperature inside the electric arc furnace during the smelting process can reach as high as 2300℃. The insulation system of traditional tilting electric arc furnaces generally suffers from poor heat preservation performance.

[0005] Currently, the furnace wall insulation structure of brown fused alumina tilting electric arc furnaces in China generally adopts a three-layer structure: "refractory castable working layer + high alumina brick support layer + ordinary insulation layer". Working layer: Made of high-alumina refractory castable, it comes into direct contact with the high-temperature molten metal and furnace gas, and is subjected to high-temperature erosion and chemical corrosion. Support layer: Constructed with grade III or II high-alumina bricks, providing structural support and some thermal insulation. Insulation layer: Made of ordinary aluminum silicate fiberboard or lightweight insulating bricks, mainly serving the function of heat insulation. This traditional structure has revealed the following prominent problems during long-term use: Poor heat insulation and high energy consumption: Ordinary heat insulation materials have a high thermal conductivity (the thermal conductivity of aluminum silicate fiber is about 0.15W / (m・K) at 1000℃), which causes the surface temperature of the furnace body to generally be above 150℃. A large amount of heat is lost through the furnace wall, resulting in serious energy waste.

[0006] Poor furnace temperature stability affects product quality: Heat loss leads to uneven temperature field inside the furnace, with furnace temperature fluctuations reaching ±100℃ or more. This affects the crystallization process of brown fused alumina, resulting in quality problems such as uneven product density, large fluctuations in Al2O3 content, and decreased self-sharpening properties.

[0007] Short service life and high maintenance costs: Traditional structures have poor thermal shock stability and are prone to cracking and peeling during frequent temperature rises and falls. The average stable operating cycle is only about 3 months. The furnace needs to be shut down for repairs every 3 months, and each maintenance takes 7-10 days. This not only consumes a lot of refractory materials and manpower, but also causes production interruptions and affects the company's capacity.

[0008] Poor structural integrity: The support layer built with high-alumina bricks has a large number of splicing gaps. At high temperatures, thermal bridging effects can easily occur at these gaps, further increasing heat loss and reducing the structural strength of the furnace wall. There is an urgent need for a brown corundum tilting electric arc furnace internal insulation technology to solve the above problems. Summary of the Invention

[0009] To address the shortcomings of existing technologies, the purpose of this invention is to provide an internal insulation process for a tilting electric arc furnace of brown fused alumina, thereby solving the problems mentioned in the background. This invention employs a three-layer composite internal insulation process consisting of a nanoporous insulation layer, a high-alumina refractory brick support layer, and a high-performance refractory castable. Its core application focuses on the brown fused alumina smelting field, significantly reducing overall smelting power consumption and compressing production and operating costs; stabilizing furnace temperature and improving the overall quality of brown fused alumina and the proportion of high-end products; extending the service life of the furnace wall and reducing production capacity waste caused by downtime maintenance; eliminating safety hazards such as equipment heat leakage and structural damage; comprehensively improving the level of safe production in the workshop; and fully adapting to the production transformation needs of large, medium, and small brown fused alumina production enterprises.

[0010] To achieve the above objectives, the present invention is implemented through the following technical solution: an internal insulation process for a brown fused alumina tilting electric arc furnace. The interior of the brown fused alumina tilting electric arc furnace includes a nanoporous insulation layer, a high-alumina refractory brick support layer, and a high-performance refractory castable working layer. These three layers constitute a three-layer composite internal insulation structure. The internal insulation process for the brown fused alumina tilting electric arc furnace includes the following steps: Step 1: Pre-treatment of the furnace body foundation. First, thoroughly remove rust, oil stains and residual old furnace lining material from the inner wall of the furnace shell. Grind with a wire brush until the metal color is exposed. Check the flatness and verticality of the furnace shell, and control the deviation within ±5mm / m. Repair and reinforce any cracks or deformed parts on the furnace shell to ensure the stability of the furnace structure. Then, apply a layer of high-temperature resistant anti-corrosion coating to the inner wall of the furnace shell. After drying, paste a 5mm thick aluminum silicate fiber elastic buffer layer. The buffer layer is pasted in a staggered manner, and the joints are sealed with high-temperature resistant tape. Step 2: Installation Process of Nano Insulation Layer The nano insulation layer uses a 30mm thick modified nano-microporous insulation board, installed layer by layer from the bottom of the furnace body upwards. The insulation board is spliced ​​in a staggered manner, with the upper and lower layer seams staggered by 1 / 2 board length, and the splicing gap controlled within 1mm. The gaps are filled with nano insulation powder and coated with high-temperature resistant sealant. After each layer is installed, it is temporarily fixed with a special clamp to prevent the insulation board from shifting. The insulation board is tightly fitted to the furnace shell without any gaps. For curved parts, the insulation board is pre-cut into suitable curved blocks to ensure flatness during installation. Step 3: Construction of the High-Alumina Refractory Brick Support Layer. The support layer uses high-strength high-alumina bricks with a thickness of 230mm, an Al2O3 content of ≥75%, and a refractoriness of ≥1790℃. The construction adopts a combination of dry and wet construction methods, with the brick joint thickness controlled at 1-2mm and the mortar fullness ≥95%. During the construction process, the verticality and flatness of the wall are strictly controlled, and calibration is performed every 3 layers. At stress concentration areas such as furnace corners and joints, special-shaped refractory bricks are used to avoid through joints. After the construction is completed, the brick joints are grouted to enhance the integrity and sealing of the wall. Step 4: Construction process of high-performance refractory castable working layer. The working layer thickness is 200mm. The whole one-time casting process is adopted. First, install steel formwork according to the design dimensions. The formwork support is firm and the joints are tight to prevent grout leakage. Then, add corundum refractory castable and a certain amount of water to a forced mixer and mix for 3-5 minutes until uniform. The amount of water added is strictly controlled between 5.5% and 6.5%. The mixed castable is poured within 30 minutes. Use an immersion vibrator to vibrate in layers with a vibration interval of 300mm. Vibrate until the surface is covered with slurry and no air bubbles overflow. Avoid over-vibration or under-vibration. After the pouring is completed, cover the surface with plastic film for moisture retention and curing. Step 5: Curing and Furnace Drying. After the cast body has naturally cured for 72 hours, remove the formwork and continue curing for another 7 days. During the curing period, maintain the ambient temperature between 5-30℃ and avoid direct sunlight and wind. After curing, proceed with furnace drying, strictly following the established furnace drying curve: from room temperature to 150℃, heating rate 5℃ / h, hold for 24 hours to remove free water; from 150℃ to 350℃, heating rate 10℃ / h, hold for 24 hours to remove crystal water; from 350℃ to 800℃, heating rate 15℃ / h, hold for 16 hours to complete sintering and solidification; from 800℃ to 1200℃, heating rate 20℃ / h, hold for 8 hours, then allow to cool naturally to room temperature. During the furnace drying process, continuously monitor the furnace surface temperature to ensure uniform heating and prevent furnace wall cracking.

[0011] Furthermore, the high-temperature modification of nanoporous thermal insulation materials and ordinary nano-thermal insulation materials are prone to agglomeration and sintering under smelting conditions of 2500℃. By introducing 15% mullite short fibers and 5% high-temperature silica micropowder as reinforcing phases into the silica aerogel matrix, a three-dimensional network skeleton structure is constructed, which increases the long-term service temperature of the material from 1200℃ to 1400℃, and the thermal conductivity is stably controlled below 0.035W / (m·K) at 1000℃.

[0012] Furthermore, the coefficient of thermal expansion of the nano-insulation layer is controlled at 2×10⁻⁶. -6 / ℃, the high-alumina refractory brick support layer is adjusted to 5×10 -6 / ℃, the working layer of the refractory castable is optimized to 7×10 -6 / ℃, forming a thermal expansion gradient that gradually increases from the inside to the outside. A special high-temperature resistant gradient adhesive is used at the interface of each layer. The thermal expansion coefficient of the adhesive is between that of the two adjacent layers. At the same time, ceramic fibers are added to enhance the interface bonding strength, so that the interface bonding strength remains above 0.8MPa at 1000℃. In addition, a 5mm thick elastic buffer layer is set between the nano-insulation layer and the furnace shell.

[0013] Furthermore, the integral casting and erosion-resistant strengthening technology for the working layer abandons the traditional segmented casting process and adopts a one-time integral casting technology for the furnace wall, eliminating transverse construction joints. The formula of corundum refractory castable is optimized by introducing 8% fused white corundum fine powder and 3% calcium aluminate cement binder, adding 0.2% water-reducing agent and 0.1% explosion-proof fiber, so that the fluidity of the castable reaches more than 180mm, which is convenient for construction and vibration. At the same time, it improves the density and thermal shock resistance of the castable. After heat treatment at 1500℃, the room temperature compressive strength is ≥60MPa, the high temperature flexural strength is ≥12MPa, and the number of thermal shock cycles (1100℃ water cooling) is ≥30, which is more than 50% higher than that of traditional high alumina castable.

[0014] Furthermore, for critical areas with traditionally severe heat leakage, such as the furnace door, tap hole, and electrode holes, differentiated heat insulation designs are adopted. The furnace door uses a composite structure of double-layer nano-insulation board and refractory fiber felt, with high-temperature resistant silicone rubber sealing strips around it. After closing, the heat loss from the gaps is reduced by more than 80%. The tap hole uses a combination structure of prefabricated corundum sleeve and nano-insulation ring to prevent the high-temperature molten metal from directly eroding the insulation layer during tapping. The electrode holes use an adjustable sealing device, combined with high-temperature resistant ceramic fiber packing, to effectively prevent the leakage of hot gas from the furnace. Through the enhanced sealing of key areas, the overall heat loss of the furnace body is further reduced by 5%-8%.

[0015] Further, the furnace foundation treatment involves cleaning up any remaining materials from the original furnace wall, checking the flatness and firmness of the steel structure support to ensure it meets construction requirements, then installing the furnace wall template, using wooden boards to fix the template to ensure it is flat and firm, and reserving necessary pouring and vibration ports. Next, the composite castable is prepared by pouring corundum powder, corundum aggregate, high-alumina cement, and an appropriate amount of water into a mixer and mixing until it reaches a slurry state, ensuring that all components are fully mixed. The pouring operation is then carried out, injecting the slurry into the template through the pouring port while simultaneously using a vibrator to ensure the slurry is dense, free of air bubbles and pores. Finally, an infrared thermometer, vernier calipers, and other tools are used to conduct a comprehensive inspection and acceptance of the furnace wall construction quality.

[0016] The beneficial effects of this invention: The internal insulation process of the brown fused alumina tilting electric arc furnace of this invention adopts a three-layer composite structure as its core technical route: a nanoporous insulation layer, a high-alumina refractory brick support layer, and a high-performance refractory castable working layer. It focuses on four major goals: improving safety, stabilizing furnace temperature, extending lifespan, and reducing energy consumption, and establishes an integrated technical system encompassing materials, structure, construction, and quality control. The outer layer uses nanoporous insulation material with excellent high-temperature stability, relying on the microporous structure to block heat conduction and reduce heat loss from the furnace wall; the middle layer uses high-strength high-alumina refractory bricks, balancing structural support and thermal buffering; the inner layer uses modified corundum refractory castable, enhancing resistance to high-temperature erosion, chemical corrosion, and thermal shock. Through formula adjustment and particle size distribution optimization, the properties of the three materials are made complementary. Structurally, a layered gradient design is adopted to match the thermal expansion coefficients of each layer, and a dedicated high-temperature resistant bonding layer and elastic buffer structure are set up to solve the problems of interface cracking and thermal bridging. This invention employs a three-layer composite internal insulation process consisting of a nanoporous insulation layer, a high-alumina refractory brick support layer, and a high-performance refractory castable. Its core application focuses on the smelting of brown fused alumina, significantly reducing overall smelting power consumption and compressing production and operating costs; stabilizing furnace temperature, improving the overall quality of brown fused alumina and increasing the proportion of high-end products; extending the service life of the furnace wall, reducing production capacity waste caused by downtime for maintenance; eliminating safety hazards such as equipment heat leakage and structural damage, comprehensively improving workshop safety, and fully adapting to the production transformation needs of large, medium, and small brown fused alumina production enterprises. Detailed Implementation

[0017] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.

[0018] Example: Insulation process for a brown fused alumina tilting electric arc furnace. The interior of the brown fused alumina tilting electric arc furnace includes a nanoporous insulation layer, a high-alumina refractory brick support layer, and a high-performance refractory castable working layer. These three layers constitute a three-layer composite internal insulation structure. The insulation process for the brown fused alumina tilting electric arc furnace includes the following steps: Step 1: Pre-treatment of the furnace body foundation. First, thoroughly remove rust, oil stains and residual old furnace lining material from the inner wall of the furnace shell. Grind with a wire brush until the metal color is exposed. Check the flatness and verticality of the furnace shell, and control the deviation within ±5mm / m. Repair and reinforce any cracks or deformed parts on the furnace shell to ensure the stability of the furnace structure. Then, apply a layer of high-temperature resistant anti-corrosion coating to the inner wall of the furnace shell. After drying, paste a 5mm thick aluminum silicate fiber elastic buffer layer. The buffer layer is pasted in a staggered manner, and the joints are sealed with high-temperature resistant tape. Step 2: Installation Process of Nano Insulation Layer The nano insulation layer uses a 30mm thick modified nano-microporous insulation board, installed layer by layer from the bottom of the furnace body upwards. The insulation board is spliced ​​in a staggered manner, with the upper and lower layer seams staggered by 1 / 2 board length, and the splicing gap controlled within 1mm. The gaps are filled with nano insulation powder and coated with high-temperature resistant sealant. After each layer is installed, it is temporarily fixed with a special clamp to prevent the insulation board from shifting. The insulation board is tightly fitted to the furnace shell without any gaps. For curved parts, the insulation board is pre-cut into suitable curved blocks to ensure flatness during installation. Step 3: Construction of the High-Alumina Refractory Brick Support Layer. The support layer uses high-strength high-alumina bricks with a thickness of 230mm, an Al2O3 content of ≥75%, and a refractoriness of ≥1790℃. The construction adopts a combination of dry and wet construction methods, with the brick joint thickness controlled at 1-2mm and the mortar fullness ≥95%. During the construction process, the verticality and flatness of the wall are strictly controlled, and calibration is performed every 3 layers. At stress concentration areas such as furnace corners and joints, special-shaped refractory bricks are used to avoid through joints. After the construction is completed, the brick joints are grouted to enhance the integrity and sealing of the wall. Step 4: Construction process of high-performance refractory castable working layer. The working layer thickness is 200mm. The whole one-time casting process is adopted. First, install steel formwork according to the design dimensions. The formwork support is firm and the joints are tight to prevent grout leakage. Then, add corundum refractory castable and a certain amount of water to a forced mixer and mix for 3-5 minutes until uniform. The amount of water added is strictly controlled between 5.5% and 6.5%. The mixed castable is poured within 30 minutes. Use an immersion vibrator to vibrate in layers with a vibration interval of 300mm. Vibrate until the surface is covered with slurry and no air bubbles overflow. Avoid over-vibration or under-vibration. After the pouring is completed, cover the surface with plastic film for moisture retention and curing. Step 5: Curing and Furnace Drying. After the cast body has naturally cured for 72 hours, remove the formwork and continue curing for another 7 days. During the curing period, maintain the ambient temperature between 5-30℃ and avoid direct sunlight and wind. After curing, proceed with furnace drying, strictly following the established furnace drying curve: from room temperature to 150℃, heating rate 5℃ / h, hold for 24 hours to remove free water; from 150℃ to 350℃, heating rate 10℃ / h, hold for 24 hours to remove crystal water; from 350℃ to 800℃, heating rate 15℃ / h, hold for 16 hours to complete sintering and solidification; from 800℃ to 1200℃, heating rate 20℃ / h, hold for 8 hours, then allow to cool naturally to room temperature. During the furnace drying process, continuously monitor the furnace surface temperature to ensure uniform heating and prevent furnace wall cracking.

[0019] To comprehensively verify the practical application effect of the optimized process, the project team selected two identical 10000KVA brown fused alumina tilting electric arc furnaces for concurrent comparative testing. The two furnaces employed a traditional bricklaying process (control group) and a three-layer composite insulation optimized process (experimental group), respectively. The testing period was from April 1st to June 30th, 2026. Throughout the process, raw material ratios, smelting current, daily operating time (24-hour continuous production), and operating procedures were kept completely consistent to eliminate external variable interference. The tests covered five core dimensions: service life, furnace surface temperature, furnace temperature uniformity, overall energy consumption, and product quality. All data were measured on-site and verified three times in parallel, ensuring the results are authentic and traceable.

[0020] Lifespan test Test Method: The furnace was shut down three times on April 30, May 31, and June 30 for a full-section manual inspection of the furnace wall working surface. Inspection indicators included the width and distribution of surface cracks, the depth of refractory material erosion, the number of loose / fallen bricks, and the area of ​​grout detachment. The development trend of furnace wall defects was recorded simultaneously to assess structural durability. Measurement Point Layout: Three inspection sections were selected along the furnace axis: the front, middle, and rear ends. Eight inspection points were evenly selected on each section, for a total of 24 inspection points.

[0021] Actual measurement data: ; Test results: The traditional process furnace wall reaches the maintenance threshold after 3 months of operation, requiring furnace shutdown, brick replacement, and grouting redoing. The stable operation cycle is only 90 days. The optimized process has excellent thermal shock resistance and erosion resistance of the overall cast structure. After 90 days of continuous operation, the structure is intact and the defect development is extremely slow. Based on the decay rate, the overall service life can reach more than 18 months, which is 5 times that of the traditional process.

[0022] Furnace surface temperature test Test Method: The test period was the entire month of April 2026. A TES-135 infrared thermometer (accuracy ±0.5℃) and a PT100 contact thermocouple (accuracy ±0.2℃) were used for cross-calibration to ensure data accuracy. Temperature measurements were taken simultaneously during three shifts: morning, afternoon, and night. Three consecutive readings were taken at each measuring point, and the average value was recorded. Furnace surface temperature changes during different smelting stages—melting, holding, and tapping—were recorded simultaneously. Measuring Point Layout: The main furnace wall was divided into three sections along the axial direction: front, middle, and rear. Three measuring points (upper, middle, and lower) were set along the circumference of each section, for a total of nine fixed basic measuring points. Additional measuring points were added at three key heat leakage points: the furnace door frame, the tapping flange, and the electrode hole sealing ring, achieving full coverage.

[0023] The measured temperature data are as follows for the three areas with the most severe heat leakage in traditional processes: furnace door, tap hole, and electrode holes: ; In traditional processes, key components have poor sealing and weak insulation, resulting in temperatures far exceeding those of the furnace wall, making them major heat leakage channels. The optimized process employs differentiated sealing and double-layer insulation design, significantly reducing the temperature of key components and fundamentally solving the heat leakage problem.

[0024] Measured data of furnace wall heat flux density The heat flux density on the outer surface of the furnace wall was measured using a JR-3 heat flux meter (accuracy ±3%) to directly quantify the heat dissipation per unit area. The data are as follows: ; Actual test results show that the heat dissipation per unit area of ​​the furnace wall with the optimized process is only 35.9% of that with the traditional process, the overall thermal resistance is increased by nearly 1.8 times, and the thermal insulation performance is significantly improved. This verifies the energy-saving effect of the three-layer composite structure from the perspective of heat conduction.

[0025] Thermal insulation stability under different ambient temperatures By selecting typical days with significant ambient temperature differences within the test period and comparing the rate of change of furnace surface temperature, the thermal insulation stability under extreme operating conditions is verified. ; Within an ambient temperature fluctuation range of ±10℃, the furnace surface temperature fluctuation of the control group was close to 8%, while that of the experimental group was only about 6%. This indicates that the optimized nano-insulation layer is less affected by the external ambient temperature and can maintain a stable insulation effect under different seasons and weather conditions. Its energy-saving performance is not significantly affected by the external environment.

[0026] Test results: The average surface temperature of the furnace body using the optimized process was only 62.9℃, which is 91℃ lower than that of the traditional process. The highest temperature throughout the process did not exceed 69℃, which is far lower than the highest temperature of 162℃ in the traditional process. The temperature of key heat leakage parts decreased by more than 60%, the heat dissipation per unit area decreased by 64%, the overall thermal resistance of the furnace wall increased by 1.8 times, and it was less affected by the fluctuation of ambient temperature. The uniformity and stability of heat insulation were greatly improved, which fully met the design expectations.

[0027] Furnace temperature uniformity test Test Method: The test period is the entire month of May 2026. Twelve Type B precious metal thermocouples (temperature range 0-1800℃, accuracy ±2℃) are pre-embedded in the furnace. Temperature data is continuously collected for 24 hours, recorded once per second. The daily average temperature, maximum temperature difference, and temperature fluctuation amplitude are statistically analyzed to evaluate the uniformity of the temperature field inside the furnace. Measurement Point Arrangement: The furnace is divided into three layers along its height: upper layer (500mm above the molten pool), middle layer (center of the molten pool), and lower layer (300mm above the furnace bottom). Four thermocouples are evenly arranged radially in each layer, for a total of 12 temperature measurement points.

[0028] Actual measurement data: ; Test results: Traditional process furnace has large temperature difference between upper and lower layers and violent temperature fluctuation, with temperature fluctuation in the center of the molten pool exceeding 100℃, which is not conducive to uniform crystallization of brown fused alumina; Optimized process furnace has a maximum temperature difference of only 50℃ across the entire cross section, temperature fluctuation is controlled within ±28℃, temperature is in a stable range for 94% of the operating time, temperature field uniformity is greatly improved, and a stable thermodynamic environment is provided for crystal growth.

[0029] Product quality testing Testing Method: The testing period spans from April to June 2026. Every Monday, three parallel samples are randomly selected from the discharge ports of two furnaces, for a total of 13 batches of samples. The Al2O3 content, bulk density, particle size distribution, and appearance defects are tested according to GB / T2478 "Brown Fused Alumina". The first-grade product rate (Al2O3 ≥ 95%, bulk density ≥ 3.9 g / cm³) is calculated monthly. 3 ) and the proportion of high-end products (Al2O3≥96%).

[0030] Actual measurement data: ; Test results: After the furnace temperature stabilized, the brown fused alumina crystals became more uniform, and defects such as pores and black cores were significantly reduced, resulting in a comprehensive improvement in product purity and density. The first-grade product rate increased from 72% to 91%, the proportion of high-end products doubled, and the batch stability of products was significantly enhanced, fully meeting the quality requirements of high-end abrasives, precision casting and other fields.

[0031] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. The internal insulation process of a brown corundum tilting electric arc furnace, characterized in that: The interior of the brown fused alumina tilting electric arc furnace includes a nanoporous insulation layer, a high-alumina refractory brick support layer, and a high-performance refractory castable working layer. These three layers constitute a three-layer composite internal insulation structure. The internal insulation process of the brown fused alumina tilting electric arc furnace includes the following steps: Step 1: Pre-treatment of the furnace body foundation. First, thoroughly remove rust, oil stains and residual old furnace lining material from the inner wall of the furnace shell. Grind with a wire brush until the metal color is exposed. Check the flatness and verticality of the furnace shell, and control the deviation within ±5mm / m. Repair and reinforce any cracks or deformed parts on the furnace shell to ensure the stability of the furnace structure. Then, apply a layer of high-temperature resistant anti-corrosion coating to the inner wall of the furnace shell. After drying, paste a 5mm thick aluminum silicate fiber elastic buffer layer. The buffer layer is pasted in a staggered manner, and the joints are sealed with high-temperature resistant tape. Step 2: Installation Process of Nano Insulation Layer The nano insulation layer uses a 30mm thick modified nano-microporous insulation board, installed layer by layer from the bottom of the furnace body upwards. The insulation board is spliced ​​in a staggered manner, with the upper and lower layer seams staggered by 1 / 2 board length, and the splicing gap controlled within 1mm. The gaps are filled with nano insulation powder and coated with high-temperature resistant sealant. After each layer is installed, it is temporarily fixed with a special clamp to prevent the insulation board from shifting. The insulation board is tightly fitted to the furnace shell without any gaps. For curved parts, the insulation board is pre-cut into suitable curved blocks to ensure flatness during installation. Step 3: Construction of the High-Alumina Refractory Brick Support Layer. The support layer uses high-strength high-alumina bricks with a thickness of 230mm, an Al2O3 content of ≥75%, and a refractoriness of ≥1790℃. The construction adopts a combination of dry and wet construction methods, with the brick joint thickness controlled at 1-2mm and the mortar fullness ≥95%. During the construction process, the verticality and flatness of the wall are strictly controlled, and calibration is performed every 3 layers. At stress concentration areas such as furnace corners and joints, special-shaped refractory bricks are used to avoid through joints. After the construction is completed, the brick joints are grouted to enhance the integrity and sealing of the wall. Step 4: Construction process of high-performance refractory castable working layer. The working layer thickness is 200mm. The whole one-time casting process is adopted. First, install steel formwork according to the design dimensions. The formwork support is firm and the joints are tight to prevent grout leakage. Then, add corundum refractory castable and a certain amount of water to a forced mixer and mix for 3-5 minutes until uniform. The amount of water added is strictly controlled between 5.5% and 6.5%. The mixed castable is poured within 30 minutes. Use an immersion vibrator to vibrate in layers with a vibration interval of 300mm. Vibrate until the surface is covered with slurry and no air bubbles overflow. Avoid over-vibration or under-vibration. After the pouring is completed, cover the surface with plastic film for moisture retention and curing. Step 5: Curing and Furnace Drying. After the cast body has naturally cured for 72 hours, remove the formwork and continue curing for another 7 days. During the curing period, maintain the ambient temperature between 5-30℃ and avoid direct sunlight and wind. After curing, proceed with furnace drying, strictly following the established furnace drying curve: from room temperature to 150℃, heating rate 5℃ / h, hold for 24 hours to remove free water; from 150℃ to 350℃, heating rate 10℃ / h, hold for 24 hours to remove crystal water; from 350℃ to 800℃, heating rate 15℃ / h, hold for 16 hours to complete sintering and solidification; from 800℃ to 1200℃, heating rate 20℃ / h, hold for 8 hours, then allow to cool naturally to room temperature. During the furnace drying process, continuously monitor the furnace surface temperature to ensure uniform heating and prevent furnace wall cracking.

2. The heat insulation process inside the brown fused alumina tilting electric arc furnace according to claim 1, characterized in that: High-temperature modification of nanoporous thermal insulation materials differs from that of ordinary nano-thermal insulation materials, which tend to agglomerate and sinter under 2500℃ smelting conditions. By introducing 15% mullite short fibers and 5% high-temperature silica micropowder as reinforcing phases into the silica aerogel matrix, a three-dimensional network skeleton structure is constructed, which increases the long-term service temperature of the material from 1200℃ to 1400℃, and the thermal conductivity is stably controlled below 0.035W / (m·K) at 1000℃.

3. The heat insulation process inside the brown fused alumina tilting electric arc furnace according to claim 1, characterized in that: The coefficient of thermal expansion of the nano-insulation layer is controlled at 2×10. -6 / ℃, the high-alumina refractory brick support layer is adjusted to 5×10 -6 / ℃, the working layer of the refractory castable is optimized to 7×10 -6 / ℃, forming a thermal expansion gradient that gradually increases from the inside to the outside. A special high-temperature resistant gradient adhesive is used at the interface of each layer. The thermal expansion coefficient of the adhesive is between that of the two adjacent layers. At the same time, ceramic fibers are added to enhance the interface bonding strength, so that the interface bonding strength remains above 0.8MPa at 1000℃. In addition, a 5mm thick elastic buffer layer is set between the nano-insulation layer and the furnace shell.

4. The heat insulation process inside the brown corundum tilting electric arc furnace according to claim 1, characterized in that: The integral casting and erosion-resistant strengthening technology for the working layer abandons the traditional segmented casting process and adopts a one-time integral casting technology for the furnace wall, eliminating transverse construction joints. The formula of corundum refractory castable is optimized by introducing 8% fused white corundum fine powder and 3% calcium aluminate cement binder, adding 0.2% water-reducing agent and 0.1% explosion-proof fiber, so that the fluidity of the castable reaches more than 180mm, which is convenient for construction and vibration. At the same time, it improves the density and thermal shock resistance of the castable. After heat treatment at 1500℃, the room temperature compressive strength is ≥60MPa, the high temperature flexural strength is ≥12MPa, and the number of thermal shock cycles (1100℃ water cooling) is ≥30, which is more than 50% higher than that of traditional high alumina castable.

5. The heat insulation process inside the brown fused alumina tilting electric arc furnace according to claim 1, characterized in that: For critical areas with traditionally severe heat leakage, such as furnace doors, tapholes, and electrode holes, a differentiated heat insulation design is adopted. The furnace door adopts a composite structure of double-layer nano-insulation board and refractory fiber felt, and high-temperature resistant silicone rubber sealing strips are set around the perimeter. After closing, the heat loss from the gaps is reduced by more than 80%. The taphole adopts a combination structure of prefabricated corundum sleeve and nano-insulation ring to prevent the high-temperature molten metal from directly eroding the insulation layer during the tapping process. The electrode holes adopt an adjustable sealing device, combined with high-temperature resistant ceramic fiber packing, to effectively prevent the leakage of hot gas inside the furnace. Through the enhanced sealing of key parts, the overall heat loss of the furnace body is reduced by 5%-8%.

6. The heat insulation process inside the brown fused alumina tilting electric arc furnace according to claim 1, characterized in that: Furnace foundation treatment: Clean up the residual materials on the original furnace wall, check the flatness and firmness of the steel structure support to ensure that it meets the construction requirements, and then install the furnace wall panel template. Use wooden boards to fix the template to ensure that the template is flat and firm, and reserve the necessary pouring port and vibration port. Then prepare the composite castable. Pour corundum powder, corundum aggregate, high alumina cement and appropriate amount of water into the mixer and stir until it reaches the slurry state. Ensure that the components are fully mixed, and carry out the pouring operation. Pour the slurry into the template through the pouring port, and use a vibrator to vibrate it to ensure that the slurry is dense and free of air bubbles and pores. Finally, use infrared thermometer, vernier caliper and other tools to conduct a comprehensive inspection and acceptance of the furnace wall construction quality.