A hydrophilic oxide microstructured copper-based capillary wick and its preparation method, and a phase change heat dissipation device.

By forming an oxide transition layer and a micro-rough structure on the surface of a copper-based capillary core, the problem of hydrophilic coating peeling off under high temperature and high humidity was solved, achieving good wettability and reflow stability in high temperature environments and improving the heat dissipation performance of phase change heat transfer devices.

CN123065281APending Publication Date: 2026-11-10SHANGHAI MORUAN COMM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611578778.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Under high temperature, high humidity and frequent phase change erosion of the working fluid, the hydrophilic coating of the existing copper-based capillary core is prone to peeling, powdering or flaking, resulting in a decrease in wetting and reflow performance.

Method used

An oxide transition layer and a micro-rough structure are formed on the surface of a copper-based capillary core. Through oxidation treatment with chlorite and persulfate, an oxide microstructure layer is grown in situ, including a micro-rough structure with alternating protrusions and depressions, which enhances the surface hydrophilicity and bonding strength.

Benefits of technology

It maintains good hydrophilicity in high-temperature environments, improves wettability and reflux stability, and enhances the heat dissipation performance of phase change heat transfer devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123065281A_ABST
    Figure CN123065281A_ABST
Patent Text Reader

Abstract

This application relates to the field of thermal management, and more particularly to a hydrophilic oxide microstructured copper-based capillary wick, its preparation method, and a phase change heat dissipation device. The hydrophilic oxide microstructured copper-based capillary wick includes a copper-based capillary wick substrate and a hydrophilic oxide microstructure layer located on the surface of the copper-based capillary wick substrate. The hydrophilic oxide microstructure layer includes an oxide transition layer and a micro-rough structure. The micro-rough structure is located on the side of the oxide transition layer away from the copper-based capillary wick substrate, and includes protrusions and depressions, which are alternately distributed. The hydrophilic oxide microstructured copper-based capillary wick provided by this application maintains good hydrophilicity even after being subjected to high-temperature environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of thermal management, and in particular to a hydrophilic oxide microstructure copper-based capillary wick, its preparation method, and a phase change heat dissipation device. Background Technology

[0002] The copper-based capillary wicks widely used in heat pipes and vapor chambers mainly include braided copper mesh, sintered copper powder, mechanically grooved, and composite types of the above structures. To improve the wetting and reflux performance of the working fluid, existing technologies mainly involve coating the surface of the capillary wick with hydrophilic polymer materials or inorganic particulate layers to promote the initial spreading of water-based working fluids by improving the surface energy of the materials. However, traditional surface coatings mostly rely on physical adhesion or weak chemical bonding, which are prone to peeling, powdering, or detachment under the long-term high temperature and humidity of the heat pipe and the frequent phase change erosion of the working fluid.

[0003] Therefore, improving the hydrophilicity of copper-based capillary wicks after exposure to high-temperature environments has become an urgent technical problem to be solved. Summary of the Invention

[0004] This application provides a hydrophilic oxide microstructured copper-based capillary core that maintains good hydrophilicity even after being subjected to high-temperature environments.

[0005] This application provides a method for preparing a hydrophilic oxidized microstructured copper-based capillary core. The hydrophilic oxidized microstructured copper-based capillary core prepared by this method can still maintain good hydrophilicity after being subjected to high temperature environment.

[0006] This application provides a phase change heat transfer device, which includes the above-mentioned hydrophilic oxide microstructured copper-based capillary core or the hydrophilic oxide microstructured copper-based capillary core prepared by the above-mentioned method, and has good reflux and heat dissipation performance.

[0007] The hydrophilic oxide microstructured copper-based capillary core provided in this application includes a copper-based capillary core substrate and a hydrophilic oxide microstructure layer located on at least a portion of the surface of the copper-based capillary core substrate. The hydrophilic oxide microstructure layer includes an oxide transition layer and a micro-rough structure. The micro-rough structure is located on the side of the oxide transition layer away from the copper-based capillary core substrate. The micro-rough structure includes protrusions and depressions, which are alternately distributed.

[0008] The above-described hydrophilic oxidized microstructured copper-based capillary core has an oxidized transition layer and / or a micro-rough structure grown in situ on the surface of the copper-based capillary core substrate.

[0009] The hydrophilic oxidized microstructure copper-based capillary core described above includes at least one of the following micro-rough structures: sheet-like, needle-like, linear, rod-like, flower-like, or coral-like.

[0010] The hydrophilic oxidative microstructured copper-based capillary core described above, wherein the oxidative transition layer and / or micro-rough structure includes one or more of copper oxide, cuprous oxide, and copper hydroxide.

[0011] The hydrophilic oxidized microstructured copper-based capillary core described above includes at least one of copper mesh capillary cores, copper powder sintered capillary cores, copper groove capillary cores, or copper-based composite capillary cores.

[0012] This application also provides a method for preparing the above-mentioned hydrophilic oxide microstructured copper-based capillary core, comprising the following steps:

[0013] The cleaned copper-based capillary core substrate was oxidized using chlorite and persulfate ions, and then shaped and sintered to obtain the hydrophilic oxidized microstructured copper-based capillary core.

[0014] The preparation method described above includes sequential oxidation with chlorite and persulfate or sequential oxidation with persulfate and chlorite.

[0015] According to the preparation method described above, the chlorite ion comprises a hydroxide and a chlorite, wherein the concentration of the hydroxide is 5-50 g / L and the concentration of the chlorite is 5-80 g / L; the oxidation treatment temperature is 50-100℃ and the oxidation treatment time is 2-60 min; the chlorite ion also includes a buffer, wherein the concentration of the buffer is 5-50 g / L.

[0016] According to the preparation method described above, the persulfate ion comprises an aqueous solution of hydroxide and persulfate, wherein the concentration of hydroxide is 1-8 mol / L and the concentration of persulfate is 0.02-0.5 mol / L; the oxidation treatment temperature is 20-80℃ and the oxidation treatment time is 2-90 min.

[0017] The hydroxide prepared by the above method includes at least one of sodium hydroxide and potassium hydroxide.

[0018] According to the preparation method described above, the persulfate includes at least one of sodium persulfate, potassium persulfate, and ammonium persulfate.

[0019] The chlorite prepared by the above method includes at least one of sodium chlorite and potassium chlorite.

[0020] The preparation method described above further includes heat treatment after oxidation treatment, which includes holding at 80-250℃ for 10-120 min.

[0021] This application also provides a phase change heat dissipation device, which includes a hydrophilic oxide microstructured copper-based capillary core prepared by the above-mentioned method for preparing the hydrophilic oxide microstructured copper-based capillary core.

[0022] By forming a hydrophilic oxide microstructure layer on the surface of a copper-based capillary substrate, and making this microstructure layer both an oxide transition layer and alternating protrusions and depressions, the hydrophilic oxide microstructure copper-based capillary can enhance surface hydrophilicity and provide a microscopic interface that is conducive to liquid spreading and transport. This allows it to maintain high hydrophilicity under thermal cycling and working fluid scouring conditions, enabling stable wetting and reflux while maintaining structural integrity, thereby improving the reflux and heat dissipation performance in phase change heat transfer devices. Attached Figure Description

[0023] Figure 1 A schematic diagram of the heat pipe cross-section and the capillary hydrophilic layer provided in this application;

[0024] Figure 2 A schematic diagram of the heat pipe provided in this application.

[0025] Among them, 1. Copper-based capillary core substrate; 2. Hydrophilic oxide microstructure layer. Detailed Implementation

[0026] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0027] Copper-based capillary wicks are widely used in phase change heat dissipation devices such as heat pipes and vapor chambers, commonly found in thermal management modules of laptops, servers, communication terminals, and new energy vehicle electronic control systems. Existing copper-based capillary wicks mostly employ surface coatings or conventional oxidation treatments to improve hydrophilicity. The working fluid spreads upon contact with the substrate due to the reduction in surface energy, and then returns through capillary action. While this approach can improve initial wetting in short-term use, under long-term thermal cycling and working fluid erosion conditions, the surface layer is prone to decreased adhesion, structural loosening, and localized detachment. Furthermore, uneven modification within the pores can easily lead to wetting dead zones.

[0028] Based on the above-mentioned technical problems, this application provides a hydrophilic oxide microstructured copper-based capillary core, including a copper-based capillary core substrate 1 and a hydrophilic oxide microstructure layer 2 located on the surface of the copper-based capillary core substrate 1. The hydrophilic oxide microstructure layer 2 includes an oxide transition layer and a micro-rough structure. The micro-rough structure is located on the side of the oxide transition layer away from the copper-based capillary core substrate 1. The micro-rough structure includes protrusions and depressions, which are alternately distributed (e.g., ...). Figure 1 (As shown).

[0029] The copper-based capillary core substrate 1 refers to the porous copper support structure that constitutes the main body of capillary liquid absorption. It provides a liquid return channel, evaporation heat exchange interface and capillary suction skeleton in phase change heat dissipation devices, and together with the working fluid, forms an evaporation, condensation and liquid return circulation path.

[0030] The hydrophilic oxide microstructure layer 2 refers to a hydrophilic functional layer formed on the surface of the copper-based capillary core substrate 1, consisting of an oxide transition layer and a micro-rough structure. The oxide transition layer is an interfacial transition structure formed closely against the surface of the copper-based capillary core substrate 1. It provides bonding support, stress relief, and chemical transition between the copper framework and the outer micro-rough structure, and serves as the inner bearing layer of the hydrophilic oxide microstructure layer 2. The micro-rough structure refers to a microscale hydrophilic morphology layer located on the side of the oxide transition layer away from the copper-based capillary core substrate 1. The micro-rough structure includes protrusions and depressions, which can directly contact the working fluid and form multi-level wetting paths, capillary channels, and liquid retention units.

[0031] A protrusion is a microstructural unit in a micro-rough structure that has a localized outward convexity relative to the surrounding surface. It serves to preferentially form liquid attachment points and spreading guide points upon contact with the working fluid, and to increase the interfacial capillary pressure differential through localized curvature changes. A depression is a microstructural unit in a micro-rough structure that has a localized concavity or porous cavity relative to the surrounding surface. It serves to store small amounts of working fluid, form liquid retention zones, and connect migration channels between adjacent protrusions. These depressions and protrusions are alternately distributed, forming a surface network with hierarchical porosity, allowing the liquid to quickly enter the micropores along the depressions and expand circumferentially upon contact.

[0032] The hydrophilic oxide microstructured copper-based capillary wick provided in this application, during operation, allows the working fluid to first contact the hydrophilic oxide microstructured layer 2 disposed on the surface of the copper-based capillary wick substrate 1. This oxide transition layer serves as the interface between the substrate and the outer rough structure, enabling the outer hydrophilic morphology to stably adhere to the copper skeleton surface. The micro-rough structure, through its alternating distribution of protrusions and depressions, forms multiple continuous liquid contact boundaries and capillary migration channels. This structure allows the hydrophilic oxide microstructured copper-based capillary wick to establish a stable hydrophilic interface without significantly occupying the main flow channel, and maintains consistency in the initial spreading, continuous reflux, and high-heat-fluidity liquid supply process, thereby maintaining long-term wettability and reflux stability.

[0033] In-situ growth refers to the direct generation of an oxide transition layer on the surface of a copper substrate through processes such as chemical reaction, oxide deposition, nucleus epitaxy, or thermal treatment transformation, forming an integrated interface with the copper substrate. In-situ growth can improve the bonding strength between the oxide layer and the copper substrate, enhance its anti-peeling ability under thermal cycling, working fluid erosion, and long-term service conditions, and thus improve the continuous liquid supply capability of the hydrophilic oxide microstructure copper-based capillary wick.

[0034] In some embodiments, the micro-rough structure is grown in situ on the surface of the copper-based capillary core substrate 1.

[0035] The micro-rough structure can grow in situ on the surface of the copper-based capillary core substrate 1, so that it can be firmly bonded to the copper substrate during the generation stage. This reduces the loosening, peeling and local failure of traditional adhesive coatings during service due to thermal expansion and contraction, media erosion or interface aging. At the same time, the rough structure can directly participate in the wetting, spreading and capillary migration process of liquid, thereby improving the continuous liquid supply capacity and stable liquid return capacity of the hydrophilic oxide microstructure copper-based capillary core under high heat flux density.

[0036] In some embodiments, the micro-rough structure includes at least one of sheet-like, needle-like, thread-like, rod-like, flower-like, or coral-like structures.

[0037] The high specific surface area of ​​these micro-rough structures—such as sheet-like, needle-like, thread-like, rod-like, flower-like, or coral-like structures—allows for multi-point wetting and multi-channel permeation of liquids within and on the surface of the microstructure. Through capillary action, the liquid is continuously drawn into the depths of the pores and, upon heating at the evaporation end, the interface is constantly renewed along the microstructural network, thus reducing the probability of localized liquid film rupture and drying. This allows the liquid to maintain good wetting response and capillary transport capacity under long-term thermal cycling and working fluid scouring conditions, thereby contributing to improved long-term wettability and reflux stability of the hydrophilic oxide microstructured copper-based capillary wick.

[0038] In some embodiments, the oxide transition layer includes one or more of copper oxide, cuprous oxide, and copper hydroxide.

[0039] The oxide transition layer is a continuous transition interface located on the surface of the copper-based capillary core substrate 1. Copper oxide, cuprous oxide, and copper hydroxide can be formed on the surface of the copper-based capillary core substrate 1 through in-situ oxidation, surface deposition, heat treatment dehydration, or phase transformation. At least one phase of copper oxide, cuprous oxide, and copper hydroxide is in direct contact with the copper substrate surface and forms a chemical bond or mechanical interlocking effect to enhance the adhesion of the oxide transition layer, thereby improving structural stability, reducing the risk of drying at the evaporation end, and improving the continuous heat dissipation performance of the phase change heat dissipation device.

[0040] In some embodiments, the micro-rough structure includes one or more of copper oxide, cuprous oxide, and copper hydroxide.

[0041] The micro-rough structure is a micro-nano undulating structure formed on the outside of the transition interface. Using copper oxide, cuprous oxide and copper hydroxide can improve the surface free energy while maintaining good bonding with the copper matrix, thereby reducing the contact angle of the liquid on the pore wall and accelerating the wetting speed, thus improving the reflux stability.

[0042] In some embodiments, the copper-based capillary core substrate 1 includes at least one of copper mesh capillary core, copper powder sintered capillary core, copper groove capillary core, or copper-based composite capillary core.

[0043] In this embodiment, the copper mesh capillary core is a porous mesh structure formed by weaving, stacking, or sintering copper wires. Its pores are formed by the interlacing of the wires, making it suitable as a carrier for a large-area spreading interface. The copper powder sintered capillary core is a three-dimensional interconnected hole structure formed by molding and high-temperature sintering of copper powder particles. Its internal channels are relatively uniformly distributed, making it suitable for providing stable capillary suction capacity. The copper trench capillary core is a regular array of trenches formed on the surface of a copper substrate through machining or forming processes. Its trench walls can be directly used as liquid migration channels. The copper-based composite capillary core is formed by stacking or embedding the aforementioned structures to form a composite transport skeleton that has both high liquid supply capacity and strong structural support capacity.

[0044] Under conditions of high heat flux density and repeated thermal cycling, the copper-based capillary core substrate 1 serves as a supporting framework to provide a stable adhesion interface for the oxide microstructure layer, enabling the hydrophilic modified layer to participate in the wetting and reflow process along with the pore walls and surface, thereby improving the initial spreading speed, long-term liquid supply stability and overall heat transfer uniformity, thus achieving better long-term wettability and reflow stability.

[0045] This application provides a method for preparing the above-mentioned hydrophilic oxide microstructured copper-based capillary core, comprising the following steps:

[0046] The cleaned copper-based capillary core substrate 1 was oxidized using chlorite and persulfate ions, and then shaped and sintered to obtain a hydrophilic oxidized microstructure copper-based capillary core.

[0047] This preparation method uses chlorite and persulfate ions for oxidation reaction to form a hydrophilic oxide microstructure layer 2 on at least a portion of the surface of the copper-based capillary core substrate 1. This hydrophilic oxide microstructure layer 2 grows directly on the surface of the copper skeleton without the need for an additional independent coating layer, thus forming a stable bond with the copper skeleton and meeting the application requirements of high heat flux density heat dissipation devices for long-term liquid return and continuous liquid supply. The hydrophilic oxide microstructure copper-based capillary core is then obtained through shaping and sintering.

[0048] In some embodiments, the preparation method includes sequential oxidation with chlorite and persulfate or sequential oxidation with persulfate and chlorite.

[0049] In this application, the oxidation order of chlorite and persulfate is not limited. Chlorite can be used to oxidize the capillary wick first to generate a continuous or semi-continuous oxidized transition layer, and then persulfate can be used to oxidize it to generate a micro-rough structure; or persulfate can be used to oxidize the capillary wick first, and then chlorite can be used for oxidation.

[0050] In some embodiments, chlorite ions include hydroxide and chlorite, wherein the concentration of hydroxide is 5-50 g / L and the concentration of chlorite is 5-80 g / L; the oxidation treatment temperature is 50-100°C and the oxidation treatment time is 2-60 min; chlorite ions also include a buffer, wherein the concentration of the buffer is 5-50 g / L.

[0051] Specifically, the concentration of hydroxide is 5 g / L, 10 g / L, 15 g / L, 20 g / L, 25 g / L, 30 g / L, 35 g / L, 40 g / L, 45 g / L, 50 g / L, or any range between any two of the above values. Specifically, the concentration of chlorite is 5 g / L, 10 g / L, 20 g / L, 30 g / L, 40 g / L, 50 g / L, 60 g / L, 70 g / L, 80 g / L, or any range between any two of the above values. Specifically, the oxidation treatment temperature is 50℃, 60℃, 70℃, 80℃, 90℃, 100℃, or any range between any two of the above values. Specifically, the oxidation treatment time is 2 min, 4 min, 6 min, 8 min, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, or any range between any two of the above values. Specifically, the concentration of the buffer is 5 g / L, 10 g / L, 15 g / L, 20 g / L, 25 g / L, 30 g / L, 35 g / L, 40 g / L, 45 g / L, 50 g / L, or any range between any two of the above values.

[0052] An oxidation solution was prepared by reacting hydroxide, chlorite, and a buffer, with the hydroxide concentration being 5-50 g / L, the chlorite concentration 5-80 g / L, and the buffer concentration 5-50 g / L. The reaction temperature was controlled at 50-100℃, and the reaction time was controlled at 2-60 min. This ensured a relatively stable reaction environment under the synergistic effect of the buffer, allowing for uniform oxidation. Through the coordinated control of the oxidation solution components, concentrations, and temperature and time windows, the hydrophilic oxidation microstructure layer 2 could be tightly bonded to the copper framework, thus meeting the long-term reflux requirements of the hydrophilic oxidation microstructure copper-based capillary core under thermal cycling and working fluid scouring conditions.

[0053] In some embodiments, persulfate ions comprise an aqueous solution of hydroxide and persulfate, wherein the concentration of hydroxide is 1-8 mol / L and the concentration of persulfate is 0.02-0.5 mol / L; the oxidation treatment temperature is 20-80°C and the oxidation treatment time is 2-90 min.

[0054] Specifically, the concentration of hydroxide is 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, or any range between any two of the above values. Specifically, the concentration of persulfate is 0.02 mol / L, 0.04 mol / L, 0.06 mol / L, 0.08 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, or any range between any two of the above values. Specifically, the oxidation treatment temperature is 20℃, 30℃, 40℃, 50℃, 60℃, 70℃, 80℃, or any range between any two of the above values. Specifically, the oxidation treatment time is 2 min, 4 min, 6 min, 8 min, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, or any range between any two of the above values.

[0055] An oxidation solution is prepared by mixing hydroxide and persulfate at a set concentration, wherein the hydroxide concentration is controlled at 1-8 mol / L and the persulfate concentration is controlled at 0.02-0.5 mol / L. The treatment temperature is controlled at 20-80℃ and the time is controlled at 2-90 min to carry out an oxidation reaction with a controllable reaction rate, generating a hydrophilic oxide microstructure layer 2 suitable for subsequent liquid spreading, thereby meeting the long-term reflux requirements of the hydrophilic oxide microstructure copper-based capillary core under thermal cycling and working fluid scouring conditions.

[0056] In some embodiments, the hydroxide includes at least one of sodium hydroxide and potassium hydroxide.

[0057] Using strong alkalis such as sodium hydroxide and potassium hydroxide to provide an alkaline environment for the oxidation reaction allows copper to be corroded and dissolved first to form intermediate products including copper hydroxide. Subsequently, the oxide layer formed by the decomposition of these intermediate products allows water to spread and penetrate rapidly, thereby meeting the long-term reflux requirements of the hydrophilic oxidation microstructure copper-based capillary core under thermal cycling and working fluid scouring conditions.

[0058] In some embodiments, persulfate includes at least one of sodium persulfate, potassium persulfate, and ammonium persulfate.

[0059] Oxidation treatment with persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate can generate a hydrophilic oxide microstructure layer 2 in situ on the copper-based capillary wick substrate 1. This significantly increases the surface roughness without altering the macroscopic framework of the capillary wick, thereby achieving high thermal stability and good hydrophilicity. Furthermore, persulfates are chemically stable, reusable, and can still be used after a week of storage. In some embodiments, the chlorite includes at least one of sodium chlorite and potassium chlorite.

[0060] Oxidation treatment with chlorite such as sodium chlorite and potassium chlorite can generate a hydrophilic oxidized microstructure layer 2 in situ on the copper-based capillary wick substrate 1. This layer can also serve as a roughening substrate for subsequent persulfate oxidation, improving the thermal stability and hydrophilicity of the capillary wick. Furthermore, chlorite is chemically stable, can be reused, and can still be used after a week of long-term storage.

[0061] In some embodiments, the oxidation treatment further includes a heat treatment, which comprises holding at 80-250°C for 10-120 minutes. Specifically, the heat treatment holding temperature can be 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, 240°C, 250°C, or any range between any two of these values. Specifically, the holding time can be 10 minutes, 20 minutes, 40 minutes, 60 minutes, 80 minutes, 100 minutes, 120 minutes, or any range between any two of these values.

[0062] Heat treatment of the oxidized copper-based capillary core can induce a controlled dehydration phase transformation of some copper hydroxide into copper oxide, eliminating the unstable hydroxyl phase in the structure, enhancing the compactness and thermomechanical stability of the oxide layer, and simultaneously solidifying the micro-nano morphology.

[0063] For example, a hydrophilic oxide microstructured copper-based capillary core can be prepared using the following method:

[0064] The copper mesh capillary core substrate was ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities. Then, it was briefly acid-washed with 5%-15% dilute hydrochloric acid to remove the surface oxide scale. Finally, it was rinsed with deionized water until neutral and dried to obtain the pretreated substrate.

[0065] A chlorite-based alkaline oxidation solution was prepared by dissolving sodium hydroxide, sodium chlorite, and trisodium phosphate at concentrations of 5-50 g / L, 5-80 g / L, and 5-50 g / L, respectively. The pretreated substrate was then placed in the chlorite-based alkaline oxidation solution at 50-100℃ and reacted for 2-60 minutes. After the reaction, the substrate was thoroughly washed with deionized water to obtain a hydrophilic copper mesh.

[0066] Sodium hydroxide and sodium persulfate were used to prepare a persulfate alkaline oxidation solution, wherein the concentration of sodium hydroxide was 1-8 mol / L and the concentration of sodium persulfate was 0.02-0.5 mol / L. A hydrophilic copper mesh was placed in the persulfate alkaline oxidation solution at 20-80℃ and reacted for 2-90 min. After the reaction, the mesh was thoroughly washed with deionized water to remove residual alkali and salts. Subsequently, it was heat-treated at 80-250℃ for 10-120 min to obtain a hydrophilic oxidized microstructured copper-based capillary core.

[0067] This application provides a phase change heat dissipation device, comprising the hydrophilic oxide microstructured copper-based capillary core described above or prepared by the above-described method for preparing the hydrophilic oxide microstructured copper-based capillary core.

[0068] The type of phase change heat dissipation device is not limited in this application, including heat pipes and vapor chambers. Among them, heat pipes, such as... Figure 2 As shown, the heat pipe includes an evaporator, an adiabatic section, and a condenser. The fabrication method of the heat pipe is not limited; exemplarily, the hydrophilic oxide microstructured copper-based capillary core prepared above is bonded, pressed, or sintered onto the inner wall of the heat pipe shell, followed by vacuuming, injection of working fluid, and sealing. The working fluid is preferably deionized water, but alcohols, ketones, or other suitable working fluids can also be selected depending on the heat pipe's operating temperature range.

[0069] The hydrophilic oxide microstructured copper-based capillary wick in this phase change heat transfer device can serve as a reflux framework inside a heat pipe or vapor chamber, forming evaporation, condensation, and capillary return channels together with the working fluid. For the same reasons mentioned above, this phase change heat transfer device can improve the liquid replenishment capacity at the evaporation end and the overall heat transfer efficiency in high heat flux density scenarios, and enhance the durability of the wetted state.

[0070] The technical solution of this application will be further explained below with reference to specific embodiments. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions or as recommended by the manufacturer. Unless otherwise specified, all reagents used are commercially available or obtained through public channels.

[0071] Example 1

[0072] This embodiment provides a hydrophilic oxide microstructured copper-based capillary core, which is prepared by the following method:

[0073] Step 1: The copper mesh capillary core precursor is ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities; then it is pickled for a short time with 5% dilute hydrochloric acid to remove the surface oxide scale, and then rinsed with deionized water until neutral and dried to obtain the pretreated copper mesh.

[0074] Step 2: Prepare an alkaline chlorite oxidation solution by mixing sodium hydroxide, sodium chlorite, and trisodium phosphate, wherein the concentration of sodium hydroxide is 50 g / L, the concentration of sodium chlorite is 37.5 g / L, and the concentration of trisodium phosphate is 30 g / L. Place the pretreated copper mesh in the alkaline chlorite oxidation solution at 90℃ and react for 30 min. After the reaction, thoroughly wash with deionized water to obtain the copper oxide mesh.

[0075] Step 3: Prepare a persulfate alkaline oxidation solution using sodium hydroxide and sodium persulfate, with a sodium hydroxide concentration of 2.5 mol / L and a sodium persulfate concentration of 0.08 mol / L. Place the copper oxide mesh in the persulfate alkaline oxidation solution at 70℃ for 30 min. After the reaction, thoroughly wash with deionized water to remove residual alkali and salts. Then dry at 60℃ for 30 min to obtain a hydrophilic copper oxide mesh.

[0076] Step 4: Place the hydrophilic copper oxide mesh into the mold and fix it. Sinter it in an atmosphere of 5% H2 and 95% N2 (hold at 850℃ for 1 hour) to obtain a hydrophilic oxide microstructured copper-based capillary core.

[0077] Example 2

[0078] This embodiment provides a hydrophilic oxide microstructured copper-based capillary core, which is prepared by the following method:

[0079] Step 1: The copper mesh capillary core precursor is ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities; then it is pickled for a short time with 5% dilute hydrochloric acid to remove the surface oxide scale, and then rinsed with deionized water until neutral and dried to obtain the pretreated copper mesh.

[0080] Step 2: Prepare an alkaline chlorite oxidation solution by mixing sodium hydroxide, sodium chlorite, and trisodium phosphate, wherein the concentration of sodium hydroxide is 5 g / L, the concentration of sodium chlorite is 20 g / L, and the concentration of trisodium phosphate is 5 g / L. Place the pretreated copper mesh in the alkaline chlorite oxidation solution at 100℃ for 60 min. After the reaction, thoroughly wash with deionized water to obtain the copper oxide mesh.

[0081] Step 3: Prepare a persulfate alkaline oxidation solution by mixing sodium hydroxide and sodium persulfate, wherein the concentration of sodium hydroxide is 8 mol / L and the concentration of sodium persulfate is 0.2 mol / L. Place the copper oxide mesh in the persulfate alkaline oxidation solution at 80℃ and react for 2 min. After the reaction, wash thoroughly with deionized water to remove residual alkali and salts; then dry at 60℃ for 30 min to obtain a hydrophilic copper oxide mesh.

[0082] Step 4: Place the hydrophilic copper oxide mesh into the mold and fix it. Sinter it in an atmosphere of 5% H2 and 95% N2 (hold at 850℃ for 1 hour) to obtain a hydrophilic oxide microstructured copper-based capillary core.

[0083] Example 3

[0084] This embodiment provides a hydrophilic oxide microstructured copper-based capillary core, which is prepared by the following method:

[0085] Step 1: The copper mesh capillary core precursor is ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities; then it is pickled for a short time with 5% dilute hydrochloric acid to remove the surface oxide scale, and then rinsed with deionized water until neutral and dried to obtain the pretreated copper mesh.

[0086] Step 2: Prepare an alkaline chlorite oxidation solution by mixing sodium hydroxide, sodium chlorite, and trisodium phosphate, wherein the concentration of sodium hydroxide is 15 g / L, the concentration of sodium chlorite is 80 g / L, and the concentration of trisodium phosphate is 20 g / L. Place the pretreated copper mesh in the alkaline chlorite oxidation solution at 50℃ and react for 2 minutes. After the reaction, thoroughly wash with deionized water to obtain copper oxide mesh.

[0087] Step 3: Prepare a persulfate alkaline oxidation solution using sodium hydroxide and sodium persulfate, with a sodium hydroxide concentration of 6 mol / L and a sodium persulfate concentration of 0.02 mol / L. Place the copper oxide mesh in the persulfate alkaline oxidation solution at 20℃ and react for 90 min. After the reaction, thoroughly wash with deionized water to remove residual alkali and salts; then dry at 60℃ for 30 min to obtain a hydrophilic copper oxide mesh.

[0088] Step 4: Place the hydrophilic copper oxide mesh into the mold and fix it. Sinter it in an atmosphere of 5% H2 and 95% N2 (hold at 850℃ for 1 hour) to obtain a hydrophilic oxide microstructured copper-based capillary core.

[0089] Example 4

[0090] This embodiment provides a hydrophilic oxide microstructured copper-based capillary core, which is prepared by the following method:

[0091] Step 1: The copper mesh capillary core precursor is ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities; then it is pickled for a short time with 5% dilute hydrochloric acid to remove the surface oxide scale, and then rinsed with deionized water until neutral and dried to obtain the pretreated copper mesh.

[0092] Step 2: Prepare an alkaline chlorite oxidation solution by mixing sodium hydroxide, sodium chlorite, and trisodium phosphate, wherein the concentration of sodium hydroxide is 35 g / L, the concentration of sodium chlorite is 5 g / L, and the concentration of trisodium phosphate is 50 g / L. Place the pretreated copper mesh in the alkaline chlorite oxidation solution at 75℃ for 60 min. After the reaction, thoroughly wash with deionized water to obtain the copper oxide mesh.

[0093] Step 3: Prepare a persulfate alkaline oxidation solution using sodium hydroxide and sodium persulfate, with a sodium hydroxide concentration of 1 mol / L and a sodium persulfate concentration of 0.5 mol / L. Place the copper oxide mesh in the persulfate alkaline oxidation solution at 55℃ for 60 min. After the reaction, thoroughly wash with deionized water to remove residual alkali and salts. Then dry at 60℃ for 30 min to obtain a hydrophilic copper oxide mesh.

[0094] Step 4: Place the hydrophilic copper oxide mesh into the mold and fix it. Sinter it in an atmosphere of 5% H2 and 95% N2 (hold at 850℃ for 1 hour) to obtain a hydrophilic oxide microstructured copper-based capillary core.

[0095] Example 5

[0096] This embodiment provides a hydrophilic oxidized microstructure copper-based capillary core. The difference between this embodiment and Embodiment 1 is that this embodiment first uses persulfate oxidation and then uses chlorite oxidation.

[0097] Specifically, step 1: The copper mesh capillary core precursor is ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities; then it is acid-washed for a short time with 5% dilute hydrochloric acid to remove the surface oxide scale, and then rinsed with deionized water until neutral and dried to obtain the pretreated copper mesh.

[0098] Step 2: Prepare a persulfate alkaline oxidation solution using sodium hydroxide and sodium persulfate, with a sodium hydroxide concentration of 2.5 mol / L and a sodium persulfate concentration of 0.08 mol / L. Place the pretreated copper mesh in the persulfate alkaline oxidation solution at 70℃ for 30 min. After the reaction, thoroughly wash with deionized water, and then keep it at 180℃ for 120 min to obtain copper oxide mesh.

[0099] Step 3: Prepare an alkaline chlorite oxidation solution by mixing sodium hydroxide, sodium chlorite, and trisodium phosphate, wherein the concentration of sodium hydroxide is 50 g / L, the concentration of sodium chlorite is 37.5 g / L, and the concentration of trisodium phosphate is 30 g / L. Place the copper oxide mesh in the alkaline chlorite oxidation solution at 90℃ and react for 30 min. After the reaction, thoroughly wash with deionized water to remove residual alkali and salts; then dry at 60℃ for 30 min to obtain a hydrophilic copper oxide mesh.

[0100] Step 4: Place the hydrophilic copper oxide mesh into the mold and fix it. Sinter it in an atmosphere of 5% H2 and 95% N2 (hold at 850℃ for 1 hour) to obtain a hydrophilic oxide microstructured copper-based capillary core.

[0101] Example 6

[0102] This embodiment provides a hydrophilic oxide microstructured copper-based capillary core, which is prepared by the following method:

[0103] Step 1: The copper mesh capillary core precursor is ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities; then it is pickled for a short time with 5% dilute hydrochloric acid to remove the surface oxide scale, and then rinsed with deionized water until neutral and dried to obtain the pretreated copper mesh.

[0104] Step 2: Prepare an alkaline chlorite oxidation solution by mixing sodium hydroxide, sodium chlorite, and trisodium phosphate, wherein the concentration of sodium hydroxide is 50 g / L, the concentration of sodium chlorite is 37.5 g / L, and the concentration of trisodium phosphate is 30 g / L. Place the pretreated copper mesh in the alkaline chlorite oxidation solution at 90℃ and react for 30 min. After the reaction, thoroughly wash with deionized water to obtain the copper oxide mesh.

[0105] Step 3: Prepare a persulfate alkaline oxidation solution using sodium hydroxide and sodium persulfate, with a sodium hydroxide concentration of 2.5 mol / L and a sodium persulfate concentration of 0.08 mol / L. Place the copper oxide mesh in the persulfate alkaline oxidation solution at 70℃ for 30 min. After the reaction, thoroughly wash with deionized water to remove residual alkali and salts. Then, keep it at 180℃ for 120 min to obtain a hydrophilic copper oxide mesh.

[0106] Step 4: Place the hydrophilic copper oxide mesh into the mold and fix it. Sinter it in an atmosphere of 5% H2 and 95% N2 (hold at 850℃ for 1 hour) to obtain a hydrophilic oxide microstructured copper-based capillary core.

[0107] Comparative Example 1

[0108] This comparative example provides a copper-based capillary core, which is prepared by the following method:

[0109] Step 1: The copper mesh capillary core precursor is ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities; then it is pickled for a short time with 5% dilute hydrochloric acid to remove the surface oxide scale, and then rinsed with deionized water until neutral and dried to obtain the pretreated copper mesh.

[0110] Step 2: Prepare a persulfate alkaline oxidation solution using sodium hydroxide and sodium persulfate, with a sodium hydroxide concentration of 2.5 mol / L and a sodium persulfate concentration of 0.08 mol / L. Place the pretreated copper mesh in the persulfate alkaline oxidation solution at 70℃ for 30 min. After the reaction, thoroughly wash with deionized water, then dry at 60℃ and hold at 180℃ for 120 min to obtain copper oxide mesh.

[0111] Step 3: Place the copper oxide mesh into the mold and fix it, then sinter it in an atmosphere of 5% H2 and 95% N2 (hold at 850℃ for 1 hour) to obtain a copper-based capillary core.

[0112] Comparative Example 2

[0113] This comparative example provides a copper-based capillary core, which is prepared by the following method:

[0114] Step 1: Place the copper powder sintered capillary core precursor into a mold and fix it. Sinter it in an atmosphere of 5% H2 and 95% N2 (hold at 850℃ for 1h) to obtain the copper powder capillary core matrix.

[0115] Step 2: The copper powder capillary core substrate is ultrasonically cleaned in acetone, ethanol and deionized water in sequence to remove oil and particulate impurities; then it is acid-washed for a short time with 5% dilute hydrochloric acid to remove the surface oxide scale, and then rinsed with deionized water until neutral and dried to obtain the pretreated copper powder capillary core substrate.

[0116] Step 3: Prepare an alkaline chlorite oxidation solution by mixing sodium hydroxide, sodium chlorite, and trisodium phosphate, wherein the concentration of sodium hydroxide is 50 g / L, the concentration of sodium chlorite is 37.5 g / L, and the concentration of trisodium phosphate is 30 g / L. Place the pretreated copper powder capillary core matrix in the alkaline chlorite oxidation solution at 90℃ and react for 30 min. After the reaction, thoroughly wash with deionized water, and then dry at 60℃ for 30 min to obtain a copper-based capillary core.

[0117] The hydrophilic oxidized microstructured copper-based capillary cores or copper-based capillary cores prepared in the above embodiments and comparative examples were subjected to water contact angle and capillary force measurements. The water contact angle was measured using a high-speed camera. Specifically, the hydrophilic oxidized microstructured copper-based capillary core or copper-based capillary core was horizontally fixed on a test stage. A microsyringe was used to control the volume of pure water to 2 μL, which was dripped onto the sample surface from a height of 1 cm. An image was taken immediately after the droplet made contact, and the water contact angle θ was obtained. The capillary force was measured using a microscope to measure the pore size r of the capillary core. eff Then, combining the contact angle test results above, according to the capillary force calculation formula:

[0118]

[0119] The capillary force is calculated, where σ1 is the surface tension of pure water.

[0120] The hydrophilic oxide microstructured copper-based capillary cores or copper-based capillary cores prepared in the examples and comparative examples were then placed in a heat pipe shell for fixation, annealed at 650°C for 1 hour, injected with pure water, and degassed under vacuum. The heat pipe was then clamped and welded to obtain the heat pipe. The heat pipe was tested at the power point where the heat source temperature stabilized, with the critical power P as the threshold, to obtain ΔT and ΔP. ΔT represents the decrease in heat source temperature compared to other examples or comparative examples in Comparative Example 1, and ΔP represents the increase in critical power compared to other examples or comparative examples in Comparative Example 1. The specific testing method is as follows: The heating block was placed tightly against the heat pipe, and a fan was used for heat dissipation at an airflow of 12 CFM. A constant power of 150 W was applied to the heat pipe and maintained for 5 minutes. After the temperature reading stabilized, this temperature was recorded as the heat source temperature T, where ΔT = T0 - T, and T0 is the heat source temperature of Comparative Example 1. Next, increase the heating power by 3W. After the temperature stabilizes, repeat the above steps until the heat source temperature suddenly accelerates and continues to rise even after the power is stopped. Record the power point at which the heat source temperature stabilizes as the critical power P, where ΔP = P - P0, and P0 is the critical power of Comparative Example 1.

[0121] Based on the above testing and analysis, the water contact angle of the hydrophilic oxide microstructured copper-based capillary cores in Examples 1-6 is no greater than 5°, and the capillary force is no less than 3.15 kPa. Furthermore, the water contact angle of Example 6 is smaller than that of Example 1, while the capillary force is greater than that of Example 1. In contrast, the water contact angle of the copper-based capillary cores in Comparative Examples 1-2 is no less than 30°, and the capillary force is no greater than 2.74 kPa. Therefore, it can be concluded that after high-temperature sintering, the hydrophilic oxide microstructured copper-based capillary core provided in this application exhibits higher hydrophilicity.

[0122] Compared to Comparative Example 1, the heat source temperature of Examples 1-6 is reduced by more than 3.9°C, and the critical power is increased by more than 3W. Furthermore, the heat source temperature of Example 6 is lower than that of Example 1, and the critical power is higher than that of Example 6. Therefore, it can be seen that the phase change heat transfer device, including the hydrophilic oxide microstructure copper-based capillary wick provided in this application, has better reflux properties and heat dissipation capabilities, and the capillary wick after heat treatment has even better performance.

[0123] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A hydrophilic oxide microstructured copper-based capillary wick, characterized in that, The invention includes a copper-based capillary core substrate (1) and a hydrophilic oxide microstructure layer (2) located on at least a portion of the surface of the copper-based capillary core substrate (1). The hydrophilic oxide microstructure layer (2) includes an oxide transition layer and a micro-rough structure. The micro-rough structure is located on the side of the oxide transition layer away from the copper-based capillary core substrate (1). The micro-rough structure includes protrusions and depressions, which are alternately distributed.

2. The hydrophilic oxide microstructured copper-based capillary wick according to claim 1, characterized in that, The oxide transition layer and / or the micro-rough structure are grown in situ on the surface of the copper-based capillary core substrate (1).

3. The hydrophilic oxide microstructured copper-based capillary wick according to claim 1 or 2, characterized in that, The micro-rough structure includes at least one of the following: plate-like, needle-like, linear, rod-like, flower-like, or coral-like structures.

4. The hydrophilic oxide microstructured copper-based capillary wick according to claim 1 or 2, characterized in that, The oxide transition layer and / or micro-rough structure includes one or more of copper oxide, cuprous oxide, and copper hydroxide.

5. The hydrophilic oxide microstructured copper-based capillary wick according to claim 1 or 2, characterized in that, The copper-based capillary matrix (1) includes at least one of copper mesh capillary, copper powder sintered capillary, copper groove capillary, or copper-based composite capillary.

6. A method for preparing a hydrophilic oxide microstructured copper-based capillary wick according to any one of claims 1-5, characterized in that, Includes the following steps: The cleaned copper-based capillary core substrate (1) was oxidized by chlorite and persulfate, and then shaped and sintered to obtain the hydrophilic oxidized microstructure copper-based capillary core.

7. The preparation method according to claim 6, characterized in that, The preparation method satisfies at least one of the following conditions: (1) The preparation method includes sequential oxidation with chlorite and persulfate or sequential oxidation with persulfate and chlorite; (2) The chlorite ion includes hydroxide and chlorite, wherein the concentration of hydroxide is 5-50 g / L and the concentration of chlorite is 5-80 g / L; the oxidation treatment temperature is 50-100℃ and the oxidation treatment time is 2-60 min; the chlorite ion also includes a buffer, wherein the concentration of the buffer is 5-50 g / L. (3) The persulfate ion includes an aqueous solution of hydroxide and persulfate, wherein the concentration of hydroxide is 1-8 mol / L and the concentration of persulfate is 0.02-0.5 mol / L; the temperature of the oxidation treatment is 20-80℃ and the time of the oxidation treatment is 2-90 min.

8. The preparation method according to claim 7, characterized in that, The preparation method satisfies at least one of the following conditions: (1) The hydroxide includes at least one of sodium hydroxide and potassium hydroxide; (2) The persulfate includes at least one of sodium persulfate, potassium persulfate, and ammonium persulfate; (3) The chlorite includes at least one of sodium chlorite and potassium chlorite.

9. The preparation method according to claim 6, characterized in that, The oxidation treatment is followed by a heat treatment, which includes holding at 80-250°C for 10-120 minutes.

10. A phase-change heat dissipation device, characterized in that, The hydrophilic oxidized microstructured copper-based capillary core is prepared by the method described in any one of claims 1-5 or any one of claims 6-9.