A method for preparing NbTi superconducting switching wires by braiding

The fabrication of NbTi superconducting switching wires by braiding method solves the processing difficulties in traditional processes, realizes efficient and stable fabrication of multi-core wires, and improves material utilization and thermal diffusion efficiency.

CN123072841APending Publication Date: 2026-11-10XIAN SUPERCONDUCTING WIRE TECHNOLOGIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611543143.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the traditional NbTi superconducting switch wire fabrication process, the hardness difference between NbTi and copper or copper-nickel substrates makes processing difficult, easily leading to wire breakage or core wire fracture, making it difficult to achieve stable fabrication of multi-core, kilometer-long wires.

Method used

NbTi superconducting switch wires are prepared by braiding. This involves assembling NbTi rods with copper-nickel alloy tubes and hot-processing them, followed by cold drawing and aging heat treatment. Then, multi-layer braiding and slotted wire embedding are performed, combined with soldering and plastic deformation, to form a continuous thermal network, thereby improving mechanical coupling and thermal diffusion efficiency.

Benefits of technology

It avoids high-temperature and high-pressure assembly and deformation, reduces the damage risk of NbTi superconducting phase, simplifies the process, improves material utilization, enhances mechanical coupling and thermal diffusion efficiency between composite wires, and adapts to different specifications and performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123072841A_ABST
    Figure CN123072841A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of superconducting technology and relates to a method for preparing NbTi superconducting switch wires using a braiding method. The invention involves assembling an NbTi rod and a copper-nickel alloy tube, followed by heat treatment to obtain a single-core rod. After removing the oxide film from the surface of the single-core rod, it is drawn and reassembled to obtain a composite rod. The composite rod undergoes aging heat treatment during the drawing interval to obtain a composite wire. The composite wire is wound onto a braiding machine spool, and after aligning the core wire center with the braiding center, the braiding machine is started layer by layer. After all layers are started, the core wire traction is simultaneously initiated, resulting in a braided superconducting wire. The braided superconducting wire and grooved wire are cleaned, coated with flux, and then molded. They are then welded through a molten solder bath and with the mold to obtain the NbTi superconducting switch wire precursor. The obtained NbTi superconducting switch wire precursor is drawn to obtain the NbTi superconducting switch wire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of superconducting technology and relates to a method for preparing NbTi superconducting switching wires by braiding. Background Technology

[0002] NbTi superconducting switching wires are a special type of superconducting wire that combines "zero resistance" and "controllable normal state." They are widely used in superconducting systems requiring magnetic field stability and energy control, such as MRI (Magnetic Resonance Imaging), NMR (Nuclear Magnetic Resonance) continuous current magnets, quench protection circuits in fusion devices, and bias coils for quantum computing. Common NbTi superconducting switching wires employ an NbTi / CuNi multi-core composite structure, and their manufacturing primarily utilizes an "assembly-hot deformation-drawing" process. This process first embeds NbTi rods into copper tubes and bundles them into a composite ingot; then, hot extrusion achieves overall material densification and preliminary shaping; finally, multiple cold drawing passes combined with intermediate heat treatment process the wire is processed to the target size, while simultaneously refining the superconducting core wire and optimizing its electromagnetic properties.

[0003] As magnet design demands increasingly higher performance from switching wires, NbTi switching wires are evolving towards higher core counts and more complex composite structures. However, in the traditional "assembly-heat deformation-drawing" process, the significant hardness difference between NbTi and copper or copper-nickel substrates leads to processing difficulties, wire breakage, or core wire fracture during drawing, resulting in wire performance below design expectations and hindering the stable fabrication of high-core, kilometer-long wires. Therefore, process optimization and material adaptation have become crucial for driving the development of this type of wire. Summary of the Invention

[0004] To address the problems and deficiencies in the existing technology, this invention provides a method for preparing NbTi superconducting switching wires using a braiding method.

[0005] In a first aspect, the present invention provides a method for preparing NbTi superconducting switch wires by braiding, comprising: assembling an NbTi rod with a copper-nickel alloy tube and hot-working it to form a single-core rod; assembling the single-core rod with the copper-nickel alloy tube to form a composite rod; drawing the composite rod into a composite wire after m cycles of cold drawing and aging heat treatment; winding the composite wire and braiding it into n layers with the center of the core wire as the braiding center to obtain a braided superconducting wire; cleaning and coating the braided superconducting wire and the grooved wire with flux, embedding the braided superconducting wire into the grooved wire, and drawing it through a circular die to obtain an assembly; plastically deforming the assembly while soldering to obtain an NbTi superconducting switch wire precursor; and cold-working the NbTi superconducting switch wire precursor to obtain the NbTi superconducting switch wire. The core wire is a composite wire or a copper-nickel alloy wire; Where m is an integer from 4 to 8, and n is an integer from 3 to 7.

[0006] Furthermore, in the method for preparing NbTi superconducting switch wires by braiding provided by the present invention, the nickel content of the copper-nickel alloy tube is 1wt%~45wt%; The diameter of the single core rod is 30~300mm, and the copper ratio is 0.3~1.5.

[0007] Furthermore, in the method for preparing NbTi superconducting switch wires by braiding provided by the present invention, the operations of cold drawing and aging heat treatment include: cold drawing the composite rod until the accumulated true strain reaches a preset threshold and then stopping the cold drawing, performing aging heat treatment on the composite rod and cooling it to room temperature; The preset threshold is 0.5~0.8.

[0008] Furthermore, in the method for preparing NbTi superconducting switch wires by braiding provided by the present invention, the aging heat treatment temperature is 280~520℃ and the time is 30h~60h.

[0009] Furthermore, in the method for preparing NbTi superconducting switch wires by braiding provided by the present invention, the diameter of the composite wire is 0.05~0.5mm; The diameter of the core wire is 0.05~0.5mm.

[0010] Furthermore, in the method for preparing NbTi superconducting switch wires by braiding provided by the present invention, the braiding operation includes: winding the composite wire onto the matching spool of the braiding machine; arranging the spools in an n-layer structure from the inside out; starting the braiding machine layer by layer; and after all layers have been started, simultaneously starting the core wire traction to perform braiding and obtain the braided superconducting wire.

[0011] Furthermore, in the method for preparing NbTi superconducting switch wires by braiding provided by the present invention, the braiding angle of the first layer of composite wire is not greater than 70°, the braiding angle of the nth layer of composite wire is not less than 40°, and the braiding angle of each intermediate layer of composite wire decreases uniformly from the first layer to the nth layer.

[0012] Furthermore, in the method for preparing NbTi superconducting switch wires by braiding provided by the present invention, the grooved wire is made of copper or a copper-nickel alloy; The nickel content of the copper-nickel alloy is 1wt% to 45wt%.

[0013] Furthermore, in the method for preparing NbTi superconducting switch wires by braiding provided by the present invention, the drawing strain of the cold working treatment is ≥15%.

[0014] Secondly, the present invention provides an NbTi superconducting switch wire, which is prepared by the above-described braiding method for preparing NbTi superconducting switch wire.

[0015] Compared with the prior art, the technical solution provided by the present invention has at least the following beneficial effects or advantages: (1) The present invention uses braiding to replace the “assembly-thermal deformation-drawing” process, so that the composite wires present an orderly cross and uniform distribution structure in three-dimensional space, which enhances the mechanical coupling and stress support between the composite wires, avoids the breakage and degradation of the composite wires under repeated electromagnetic force or thermal cycling, and the continuous thermal network formed by braiding greatly improves the thermal diffusion efficiency of NbTi superconducting switch wires in the switching working state (i.e. when changing from the superconducting state to the normal state).

[0016] (2) This invention avoids the repeated high-temperature and high-pressure assembly and deformation required by the "assembly-thermal deformation-drawing" process to achieve a high core count, reduces the risk of damage to the NbTi superconducting phase by high temperature, simplifies the process flow, and improves material utilization. At the same time, the braiding process itself has high flexibility and scalability, and it is easy to adjust the core count, layer count, and braiding angle, providing a universal manufacturing platform for NbTi superconducting switch wires with different specifications and performance requirements. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the structure after the braided superconducting wire is embedded in the slotted wire. In the diagram, 1 represents the braided superconducting wire, and 2 represents the slotted wire.

[0018] Figure 2 This is a schematic diagram of the structure of the NbTi superconducting switch wire prepared in Example 1. Detailed Implementation

[0019] The technical solution of the present invention will be described below with reference to embodiments. However, the present invention is not limited to the following embodiments. Unless otherwise specified, the experimental methods and detection methods described in each embodiment are conventional methods; unless otherwise specified, the reagents and materials can be purchased commercially.

[0020] Example 1 This embodiment provides a method for preparing NbTi superconducting switching wires.

[0021] The method for preparing the NbTi superconducting switching wire described in this embodiment is as follows: S1. Assemble a 50mm diameter NbTi rod and a 70mm outer diameter, 52mm inner diameter copper-nickel alloy tube (nickel content 25wt%), and then perform hot working (750℃, deformation amount 81.6%) to obtain a single-core rod with a diameter of 30mm and a copper ratio (the ratio of the cross-sectional area of ​​the copper-nickel alloy tube to the cross-sectional area of ​​the NbTi rod) of 0.88.

[0022] S2. After removing the oxide film on the surface of the single core rod using a high-hardness peeling die, it is drawn to H15 (a hexagonal rod with a height of 15mm), and then assembled and drawn again with a copper-nickel alloy tube (nickel content of 25wt%) to produce a composite rod.

[0023] S3. The composite rod is plastically processed using a cold drawing method, with real-time monitoring of its cumulative true strain. When the cumulative true strain reaches 0.7, the drawing process is immediately stopped, and the composite rod is treated at 300℃ for 50 hours (aging heat treatment). After the aging heat treatment, it is cooled to room temperature and cold-drawn again. When the cumulative true strain reaches 0.7 again, the aging heat treatment is repeated. The above operation of "drawing to a strain of 0.7 + aging heat treatment" is repeated 6 times. After the 6th aging heat treatment, the composite rod is drawn to a diameter of 0.08 mm to obtain the composite wire.

[0024] S4. The composite yarn is wound onto the spools of the braiding machine using a yarn separator. The spools are divided into 5 layers from the inside out, with the number of spools in each layer being 6 (first layer), 12 (second layer), 18 (third layer), 24 (fourth layer), and 24 (fifth layer). The composite yarn is then precision-braided in multiple layers. After aligning the center of the 0.08mm diameter core yarn (the core yarn is composite yarn) with the braiding center, the braiding machine is started layer by layer. After each layer is started, the braiding pattern must be observed to ensure there is no deviation or overlap before starting the next layer. After all layers are started, the core yarn traction is started simultaneously to obtain the braided superconducting wire. During the braiding process, the braiding angle of the first layer is 65°, and the braiding angle of the fifth layer is 45°. The braiding angles of the second, third, and fourth layers decrease uniformly from the inside out in a 5° gradient, i.e., the braiding angle of the second layer is 60°, the third layer is 55°, and the fourth layer is 50°.

[0025] S5. For example Figure 1 As shown, after ultrasonic cleaning (40kHz) and flux application (RMA-218) of the braided superconducting wire and the slotted wire (copper-nickel alloy, nickel content 25wt%), the braided superconducting wire is embedded in the slotted wire and then drawn through a circular die to obtain an assembly. The assembly is then welded in a molten solder bath, and a die is used simultaneously during the welding process to shape and deform the assembly, thereby obtaining a 1.4mm diameter NbTi superconducting switch wire precursor. The NbTi superconducting switch wire precursor is then cold-drawn (drawing strain greater than or equal to 15%) to a diameter of 1.2mm, causing the copper-nickel alloy of the slotted wire and the braided superconducting wire to undergo synergistic deformation, achieving a tight bond at the interface under radial pressure, thus obtaining the NbTi superconducting switch wire. Figure 2 ).

[0026] The NbTi superconducting switch wire prepared in this embodiment has no broken cores, the NbTi utilization rate reaches 95.7%, and the critical current reaches 1000A (5T).

[0027] Comparative Example 1 This comparative example provides a method for preparing NbTi superconducting switch wires using an "assembly-thermal deformation-drawing" process.

[0028] S1. Assemble a 50mm diameter NbTi rod and a 70mm outer diameter, 52mm inner diameter copper-nickel alloy tube (nickel content 5wt%), and then perform hot working (720℃, deformation amount 87.2%) to obtain a 25mm diameter single core rod with a copper ratio of 0.88.

[0029] S2. After removing the oxide film from the surface of the single-core rod using a high-hardness peeling die, it is drawn to H15 (a hexagonal rod with a height of 15mm). Then, it undergoes a second assembly with a copper-nickel alloy tube (nickel content of 5wt%), followed by hot deformation and cold drawing (hot deformation temperature 720℃, deformation amount 70%, then cold drawing to H15) to produce a 36-core composite rod. Five 36-core composite rods are then assembled with copper-nickel alloy tubes (nickel content of 5wt%) for a third time, followed by hot deformation and cold drawing (hot deformation temperature 720℃, deformation amount 70%, then cold drawing to H15) to produce an 180-core composite rod. Seventeen 180-core composite rods are then assembled with copper-nickel alloy tubes (nickel content of 5%) for a fourth time, followed by hot deformation and cold drawing (hot deformation temperature 720℃, deformation amount 70%, then cold drawing to H15) to produce a 3060-core composite rod.

[0030] S3. The 3060 core composite rod was plastically processed by cold drawing, and its cumulative true strain was monitored in real time during the process. When the cumulative true strain reached 0.7, the drawing process was immediately stopped, and the composite rod was treated at 300℃ for 50 hours (aging heat treatment). After the aging heat treatment, it was cooled to room temperature and cold drawn again. When the cumulative true strain reached 0.7 again, the aging heat treatment was repeated. The above operation of "drawing to strain of 0.7 + aging heat treatment" was repeated 6 times. After the 6th aging heat treatment, the composite rod was drawn to a diameter of 1.2 mm to obtain the NbTi superconducting switch wire. The NbTi superconducting switch wire prepared in this comparative example has a core breakage rate of <3%, an NbTi utilization rate of 80%, and a critical current of 890A (5T).

[0031] Compared with the three-stage "assembly-thermal deformation-drawing" forming method of Comparative Example 1, the preparation method of NbTi superconducting switch wire provided in Example 1 reduces the number of thermal deformation processes, saves preparation steps and time, significantly reduces the number of wire breakages and core breakages, greatly improves core wire deformation, and increases the utilization rate of NbTi from 80% to 95.7%.

[0032] Example 2 This embodiment provides a method for preparing NbTi superconducting switching wires.

[0033] The method for preparing the NbTi superconducting switching wire described in this embodiment is as follows: S1. Assemble a 60mm diameter NbTi rod and a 75mm outer diameter, 63mm inner diameter copper-nickel alloy tube (nickel content 30wt%), and then perform hot working (770℃, deformation 71.5%) to obtain a 40mm diameter single-core rod with a copper ratio of 0.45.

[0034] S2. After removing the oxide film on the surface of the single core rod using a high-hardness peeling die, it is drawn to H2O and then reassembled and drawn with a copper-nickel alloy tube (nickel content of 30wt%) to produce a composite rod.

[0035] S3. The composite rod is plastically processed using a cold drawing method, with real-time monitoring of its cumulative true strain. When the cumulative true strain reaches 0.6, the drawing process is immediately stopped, and the composite rod is treated at 300℃ for 50 hours (aging heat treatment). After the aging heat treatment, it is cooled to room temperature and cold-drawn again. When the cumulative true strain reaches 0.6 again, the aging heat treatment is repeated. The above operation of "drawing to a strain of 0.6 + aging heat treatment" is repeated 6 times. After the 6th aging heat treatment, the composite rod is drawn to a diameter of 0.10 mm to obtain the composite wire.

[0036] S4. The composite yarn is wound onto the spools of the braiding machine using a yarn separator. The spools are divided into three layers from the inside out, with 12 spools in each layer (first layer), 18 in the second layer, and 18 in the third layer. The composite yarn is then precision-braided in multiple layers. After aligning the center of the 0.3mm diameter core wire (made of Cu30Ni alloy) with the braiding center, the braiding machine is started layer by layer. After each layer is started, the braiding pattern must be observed to ensure there is no deviation or overlap before starting the next layer. Once all layers are started, the core wire traction is started simultaneously to obtain the braided superconducting wire. During the braiding process, the braiding angle of the first layer is 60°, the braiding angle of the third layer is 40°, and the braiding angle of the second layer decreases uniformly from the inside out in 10° increments, i.e., the braiding angle of the second layer is 50°.

[0037] S5. After ultrasonically cleaning (40kHz) and applying flux (OA-201) to the braided superconducting wire and the slotted wire (copper-nickel alloy, nickel content 30wt%), the braided superconducting wire is embedded in the slotted wire and drawn through a circular die to obtain an assembly. The assembly is welded through a molten solder bath, and during the welding process, a die is used simultaneously to shape and deform the assembly, thereby obtaining a 1.0mm diameter NbTi superconducting switch wire precursor. The NbTi superconducting switch wire precursor is then cold-drawn (drawing strain greater than or equal to 15%) to a diameter of 0.85mm, causing the copper-nickel alloy of the slotted wire and the braided superconducting wire to undergo synergistic deformation, achieving a tight bond at the interface under radial pressure, thus obtaining the NbTi superconducting switch wire.

[0038] The NbTi superconducting switch wire prepared in this embodiment has no broken cores, the NbTi utilization rate is 92%, and the critical current is 820A (5T).

[0039] Example 3 This embodiment provides a method for preparing NbTi superconducting switching wires.

[0040] The method for preparing the NbTi superconducting switching wire described in this embodiment is as follows: S1. Assemble a 242mm diameter NbTi rod and a 300mm outer diameter, 245mm inner diameter copper-nickel alloy tube (nickel content 1wt%), and then perform hot working (650℃, deformation amount 92.9%) to obtain a single core rod with a diameter of 80mm and a copper ratio of 0.50.

[0041] S2. After removing the oxide film on the surface of the single core rod using a high-hardness peeling die, it is drawn to H30 and then reassembled and drawn with a copper-nickel alloy tube (nickel content of 1wt%) to produce a composite rod.

[0042] S3. The composite rod is plastically processed using a cold drawing method, with real-time monitoring of its cumulative true strain. When the cumulative true strain reaches 0.5, the drawing process is immediately stopped, and the composite rod is treated at 280℃ for 60 hours (aging heat treatment). After the aging heat treatment, it is cooled to room temperature and cold-drawn again. When the cumulative true strain reaches 0.5 again, the aging heat treatment is repeated. The above operation of "drawing to a strain of 0.5 + aging heat treatment" is repeated 8 times. After the 8th aging heat treatment, the composite rod is drawn to a diameter of 0.05 mm to obtain the composite wire.

[0043] S4. The composite yarn is wound onto the spools of the braiding machine using a yarn separator. The spools are divided into 7 layers from the inside out, with the number of spools in each layer being 6 (first layer), 12 (second layer), 18 (third layer), 24 (fourth layer), 30 (fifth layer), 36 (sixth layer), and 36 (seventh layer). The composite yarn is then precision braided in multiple layers. After aligning the center of the 0.1mm diameter core wire (the core wire is a Cu1Ni alloy with a nickel content of 1wt%) with the braiding center, the braiding machine is started layer by layer. After each layer is started, the braiding pattern must be observed to ensure there is no deviation or overlap before starting the next layer. After all layers are started, the core wire traction is started simultaneously to obtain the braided superconducting wire. During the weaving process, the weaving angle of the first layer is 70° and the weaving angle of the seventh layer is 40°. The weaving angles of the second, third, fourth, fifth, sixth and seventh layers decrease evenly from the inside to the outside with a gradient of 5°, that is, the weaving angle of the second layer is 65°, the weaving angle of the third layer is 60°, the weaving angle of the fourth layer is 55°, the weaving angle of the fifth layer is 50° and the weaving angle of the sixth layer is 45°.

[0044] S5. After ultrasonically cleaning (32kHz) and applying flux (rosin RMA) to the braided superconducting wire and the slotted wire (copper-nickel alloy, nickel content 1wt%), the braided superconducting wire is embedded into the slotted wire and drawn through a circular die to obtain an assembly. The assembly is welded through a molten solder bath, and during the welding process, a die is used simultaneously to shape and deform the assembly, thereby obtaining a 1.10mm diameter NbTi superconducting switch wire precursor. The NbTi superconducting switch wire precursor is then cold-drawn (drawing strain greater than or equal to 15%) to a diameter of 1.0mm, causing the copper-nickel alloy of the slotted wire and the braided superconducting wire to undergo synergistic deformation, achieving a tight bond at the interface under radial pressure, thus obtaining the NbTi superconducting switch wire.

[0045] The NbTi superconducting switch wire prepared in this embodiment has no broken cores, the NbTi utilization rate is 96%, and the critical current is 1060A (5T).

[0046] Example 4 This embodiment provides a method for preparing NbTi superconducting switching wires.

[0047] The method for preparing the NbTi superconducting switching wire described in this embodiment is as follows: S1. Assemble a 36mm diameter NbTi rod and a 50mm outer diameter, 38mm inner diameter copper-nickel alloy tube (nickel content 45wt%), and then perform hot working (900℃, deformation 64%) to obtain a 30mm diameter single-core rod with a copper ratio of 0.81.

[0048] S2. After removing the oxide film on the surface of the single core rod using a high-hardness peeling die, it is drawn to H25 and then reassembled and drawn with a copper-nickel alloy tube (nickel content of 45wt%) to produce a composite rod.

[0049] S3. The composite rod is plastically processed using a cold drawing method, with real-time monitoring of its cumulative true strain during the process. When the cumulative true strain reaches 0.8, the drawing process is immediately stopped, and the composite rod is treated at 520℃ for 30 hours (aging heat treatment). After the aging heat treatment, it is cooled to room temperature and cold-drawn again. When the cumulative true strain reaches 0.8 again, the aging heat treatment is repeated. The above operation of "drawing to a strain of 0.8 + aging heat treatment" is repeated 4 times. After the 4th aging heat treatment, the composite rod is drawn to a diameter of 0.2 mm to obtain the composite wire.

[0050] S4. The composite yarn is wound onto the spools of the braiding machine using a yarn separator. The spools are divided into three layers from the inside out, with 6 spools in the first layer, 12 in the second layer, and 12 in the third layer. The composite yarn is then precision-braided in multiple layers. After aligning the center of the 0.5mm diameter core yarn (which is a composite yarn) with the braiding center, the braiding machine is started layer by layer. After each layer is started, the braiding pattern must be observed to ensure there is no deviation or overlap before starting the next layer. Once all layers are started, the core yarn traction is started simultaneously to obtain the braided superconducting wire. During the braiding process, the braiding angle for the first layer is 70°, the second layer is 60°, and the third layer is 50°.

[0051] S5. After ultrasonically cleaning (60kHz) and applying flux (EF-9000) to the braided superconducting wire and slotted wire (copper-nickel alloy, nickel content 45wt%), the braided superconducting wire is embedded into the slotted wire and drawn through a circular die to obtain an assembly. The assembly is then welded in a molten solder bath, with a die used simultaneously to shape and deform the assembly during the welding process, thereby obtaining a 2.0mm diameter NbTi superconducting switch wire precursor. The NbTi superconducting switch wire precursor is then cold-drawn (drawing strain greater than or equal to 15%) to a diameter of 1.6mm, causing the copper-nickel alloy of the slotted wire and the braided superconducting wire to deform synergistically, achieving a tight bond at the interface under radial pressure, thus obtaining the NbTi superconducting switch wire.

[0052] The NbTi superconducting switch wire prepared in this embodiment has no broken cores, the NbTi utilization rate is 89%, and the critical current is 560A (5T).

[0053] The embodiments described above are some, but not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art through related deductions and substitutions based on the inventive concept, without inventive effort, are within the scope of protection of the present invention.

Claims

1. A method for preparing NbTi superconducting switching wires by braiding, characterized in that, include: NbTi rods are assembled with copper-nickel alloy tubes and hot-processed to form single-core rods; single-core rods are then reassembled with copper-nickel alloy tubes to form composite rods; after m cycles of cold drawing and aging heat treatment, composite wires are drawn; after the composite wires are wound, n layers are braided with the center of the core wire as the braiding center to obtain braided superconducting wires; after cleaning and coating the braided superconducting wires and slotted wires with flux, the braided superconducting wires are embedded in the slotted wires and drawn through a circular die to obtain an assembly; the assembly undergoes plastic deformation while being soldered to obtain the NbTi superconducting switch wire precursor; the NbTi superconducting switch wire precursor is cold-processed to obtain the NbTi superconducting switch wire; The core wire is a composite wire or a copper-nickel alloy wire; Where m is an integer from 4 to 8, and n is an integer from 3 to 7.

2. The method for preparing NbTi superconducting switching wires by braiding according to claim 1, characterized in that, The nickel content of the copper-nickel alloy tube is 1wt%~45wt%; The diameter of the single core rod is 30~300mm, and the copper ratio is 0.3~1.

5.

3. The method for preparing NbTi superconducting switching wires by braiding according to claim 1, characterized in that, The cold drawing and aging heat treatment operations include: cold drawing the composite rod until the accumulated true strain reaches a preset threshold and then stopping the cold drawing; performing aging heat treatment on the composite rod and cooling it to room temperature. The preset threshold is 0.5~0.

8.

4. The method for preparing NbTi superconducting switching wires by braiding according to claim 1, characterized in that, The aging heat treatment is performed at a temperature of 280~520℃ for a time of 30h~60h.

5. The method for preparing NbTi superconducting switching wires by braiding according to claim 1, characterized in that, The diameter of the composite filament is 0.05~0.5mm; The diameter of the core wire is 0.05~0.5mm.

6. The method for preparing NbTi superconducting switching wires by braiding according to claim 1, characterized in that, The braiding operation includes: loading the composite yarn onto the matching spools of the braiding machine; arranging the spools into n layers from the inside out; starting the braiding machine layer by layer; and after all layers have been started, simultaneously starting the core wire traction to braid and obtain the braided superconducting wire.

7. The method for preparing NbTi superconducting switching wires by braiding according to claim 6, characterized in that, The weaving angle of the first layer of composite yarn is no greater than 70°, the weaving angle of the nth layer of composite yarn is no less than 40°, and the weaving angle of each intermediate layer of composite yarn decreases uniformly from the first layer to the nth layer.

8. The method for preparing NbTi superconducting switching wires by braiding according to claim 1, characterized in that, The groove line is made of copper or a copper-nickel alloy; The nickel content of the copper-nickel alloy is 1wt% to 45wt%.

9. The method for preparing NbTi superconducting switching wires by braiding according to claim 1, characterized in that, The pull-out strain of the cold working treatment is ≥15%.

10. An NbTi superconducting switching wire, characterized in that, The NbTi superconducting switching wire is prepared by the braiding method described in any one of claims 1 to 9.