A conductor micro-compact twisting process for reducing the resistivity of copper conductors

By using a bundled, layered pre-twisting process and a multi-stage progressive micro-compacting process, combined with low-temperature stress relief, the problems of high resistivity and poor structural stability of copper conductors have been solved, achieving the production of copper conductors with low resistivity, high structural stability, and low cost.

CN123072848APending Publication Date: 2026-11-10HENGYANG HENGFEI CABLE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611406843.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The existing copper conductor strong compression stranding process results in high resistivity, large transmission loss, high raw material cost, and large production loss. In addition, the simple micro-compression process has poor structural stability, making it difficult to achieve low resistivity, high structural stability, and low cost for large-scale mass production.

Method used

By employing a process of pre-stranding in layers, multi-stage progressive micro-compression, and low-temperature stress relief, the compression rate and stress release during the stranding process are controlled through layered pre-stranding, multi-stage micro-compression, and low-temperature treatment. This optimizes the arrangement and stress state of the copper monofilaments and avoids lattice distortion and residual stress.

Benefits of technology

It significantly reduces the resistivity of copper conductors, improves conductivity, reduces raw material procurement costs, increases production efficiency and product qualification rate, and enables low-cost large-scale production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A conductor micro-compression stranding process for reducing the resistivity of copper conductors is characterized by the following steps: raw material pretreatment, bundled and layered pre-stretching, segmented micro-compression forming, low-temperature stress relief, and uniform-speed shaping and winding. Compared to the traditional 12% compression rate strong compression process, under the same raw materials, equipment, and production speed, the resistivity of the product of this invention is reduced by 2%-4%, cable transmission loss is significantly reduced, and conductivity is greatly improved; there is no excessive compression damage, the breakage and damage rate of copper single wires is greatly reduced, the amount of copper conductor material used is reduced by 2%, and the overall production loss cost is significantly reduced; it is suitable for various long-term service conditions of cables, the parameters of the whole process are controllable and the fault tolerance rate is high, and it can be adapted to the mass production of copper conductors of all specifications from 1.5-120mm²; no large-scale production equipment needs to be modified, it can be directly adapted to existing cable stranding production lines, and the conductor resistivity, structural dimensions, and mechanical properties of the mass-produced conductors are highly consistent, and the product qualification rate is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wire and cable conductor processing technology, and in particular to a conductor micro-compact stranding process for reducing the resistivity of copper conductors. Background Technology

[0002] Copper conductors are the core conductive substrate of wires and cables. Their resistivity directly determines the cable's conductivity, current carrying capacity, and transmission loss. The conductor stranding process is a key processing step that affects the resistivity of copper conductors.

[0003] Currently, the industry generally uses a high-compression-ratio, high-pressure stranding process for copper conductors, with a compression ratio typically between 10% and 15%. While this process can improve conductor roundness and reduce conductor outer diameter, it has significant technical drawbacks: under high-speed stranding and high-pressure conditions, the copper single wires undergo severe plastic deformation, causing distortion, misalignment, and deformation of the internal lattice of the copper material, resulting in a large number of dislocation defects and concentrated residual internal stress. These lattice defects and residual stress hinder the directional movement of free electrons, directly leading to a significant increase in the resistivity of the copper conductor, a decrease in conductivity, and an increase in the energy consumption of cable power transmission.

[0004] To compensate for the conductivity loss caused by the high-pressure compaction process, high-purity refined copper raw materials are usually used to produce conductors, which significantly increases the cost of raw material procurement. At the same time, the high-pressure compaction process can cause local excessive compression, breakage, and damage to copper monofilaments, resulting in a high scrap rate and low copper utilization rate, which further increases the cost of cable production.

[0005] In existing technologies, a small number of micro-pressure stranding processes simply reduce the pressure strength without systematically optimizing the stranding pitch, delamination gap, stress relief, and pretreatment processes. This results in problems such as loose conductor structure, poor roundness, and insufficient mechanical strength. It cannot meet the production requirements of low resistivity, high structural stability, and low cost, making it difficult to achieve large-scale mass production applications.

[0006] Therefore, developing a micro-compact stranding process that can reduce the resistivity of copper conductors, simplify raw material requirements, and reduce production costs is an urgent need in the current cable conductor processing field. Summary of the Invention

[0007] To address the problems of high resistivity, high transmission loss, high raw material cost, high production loss, and poor structural stability of the existing copper conductor strong compression stranding process, this invention provides a conductor micro compression stranding process that reduces the resistivity of copper conductors.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: A conductor micro-compact stranding process for reducing the resistivity of copper conductors, characterized by the following process steps: 1. Raw material pretreatment: Select conventional industrial copper monofilaments that conform to the national standard GB / T3956, remove the surface oxide layer, oil and impurities, and perform low-temperature softening pretreatment on the copper monofilaments. The pretreatment temperature is 80-120℃, the holding time is 15-30min, and the copper monofilaments are naturally cooled to room temperature to eliminate the original residual stress of the copper monofilaments. 2. Bundle and Layer Pre-twisting: Based on the cross-sectional area of ​​the target conductor, the pre-treated copper monofilaments are evenly divided into multiple bundles and arranged in layers using a concentric layer-twisting method. The inner layer monofilaments are arranged with zero gaps, while the outer layer monofilaments have a uniform micro-gap of 0.02-0.05mm. The twisting pitch of each layer is controlled to be 18-22 times the outer diameter of the layer, so as to achieve uniform arrangement of monofilaments, no overlapping of wires, and no dead corners of compression. 3. Segmented Micro-compression Molding: A multi-stage progressive micro-compression mold is used to compact the pre-stranded conductors, divided into three stages: initial compression, intermediate compression, and fine compression. The compression rate is controlled between 3% and 8% throughout the process. Initial compression ratio of 2%-3% eliminates loose gaps in the conductor; Medium-pressure compression ratio 1%-3%, correcting conductor roundness; The compression rate is 0%-2%, ensuring shape stability and preventing copper lattice distortion caused by instantaneous high pressure throughout the process; 4. Low-temperature stress relief: During the micro-compression molding process, constant temperature air duct insulation is used simultaneously to control the conductor molding temperature at 40-60℃. After molding, the conductor is kept at a constant temperature for 20-40 seconds to relieve the mechanical internal stress generated during stranding and compaction and to repair micro-lattice defects. 5. Uniform speed shaping and winding: Control the overall stranding speed to 80-120m / min, ensure that the tension difference between each layer is ≤5N, and keep the winding tension constant, so as to finally obtain stranded copper conductors with low resistivity, low residual stress and low cost.

[0009] A further aspect of this invention is that, in the raw material pretreatment step, the low-temperature softening pretreatment adopts a hot air constant temperature drying method, with the heating rate controlled at 3-5℃ / min, to avoid uneven local stress in the copper monofilament caused by rapid heating.

[0010] A further aspect of the present invention is that, in the pre-twisting step of the bundle splitting and layering, the inner layer twisting direction is opposite to the outer layer twisting direction, and the twisting pitch error between adjacent layers is ≤ ±0.5mm, ensuring that the conductor structure is symmetrical and the force is balanced.

[0011] A further aspect of this invention is that, in the segmented micro-compacting molding step, the multi-stage micro-compacting mold adopts an arc transition cavity with a surface roughness Ra≤0.8μm, to avoid scratching the surface of the copper single wire and causing structural defects during the compaction process.

[0012] A further aspect of this invention is that, in the low-temperature stress relief step, the constant-temperature air duct adopts a ring-shaped air supply, and the temperature difference around the conductor is ≤±2℃, thereby achieving uniform stress relief throughout the entire area.

[0013] A further aspect of this invention is that, in order to meet the molding requirements and conductivity optimization requirements of conductors with small cross-sections of 1.5-10mm², the total compression rate in the segmented micro-compression molding step is controlled at 3%-5%.

[0014] A further aspect of this invention is that, in order to meet the molding requirements and conductivity optimization requirements of medium-to-large cross-section conductors of 16-120mm², the total compression rate in the segmented micro-compression molding step is controlled at 5%-8%.

[0015] The beneficial effects of this invention are as follows: Using an ultra-low micro-compression ratio of 3%-8% and combined with a low-temperature stress relief process, the lattice defects and residual internal stress during the copper single wire stranding process are greatly reduced, the free electron transport path is optimized, and the resistivity of the finished conductor is stable at ≤0.0171Ω·mm² / m at 20℃, which is 2%-4% lower than that of conventional compacted conductors. The power transmission loss of the cable is significantly reduced and the conductivity is greatly improved. There is no need to use expensive and high-purity refined copper raw materials. Conventional industrial copper monofilaments that meet the standards can meet the production requirements, reducing raw material procurement costs by 8%-12%. At the same time, the micro-compression process avoids excessive extrusion damage, significantly reduces the breakage and damage rate of copper monofilaments, reduces the amount of copper conductor material used by 2%, and significantly reduces the overall production loss cost. By using layered differentiated gap arrangement and multi-level progressive micro-compression shaping, the problems of loose conductors, poor roundness, and unstable structure in traditional micro-compression processes are solved. The roundness error of the finished conductor is ≤0.02mm, and the tensile strength and bending performance meet the national standards. It is suitable for the long-term service conditions of various cables. The parameters of the whole process are controllable and the fault tolerance rate is high. It can be adapted to the mass production of copper conductors of all specifications from 1.5-120mm². The stranding speed is stable and controllable, and the production efficiency is on par with traditional processes. There is no need to modify large-scale production equipment, and it can be directly adapted to existing cable stranding production lines, resulting in low cost for large-scale implementation. With balanced tension in layered stranding, uniform circumferential temperature, and progressively stable compressive strength, the resistivity, structural dimensions, and mechanical properties of conductors produced in batches are highly consistent, resulting in a significant improvement in product qualification rate. Detailed Implementation Example

[0016] A conductor micro-compact stranding process for reducing the resistivity of copper conductors comprises the following steps: 1. Select conventional industrial copper monofilaments that conform to the national standard GB / T3956, remove the surface oxide layer, oil and impurities, and perform low-temperature softening pretreatment on the copper monofilaments. The pretreatment temperature is 80-120℃, the holding time is 15-30min, and the copper monofilaments are naturally cooled to room temperature to eliminate the original residual stress of the copper monofilaments. 2. Based on the target conductor cross-sectional area, the pre-treated copper monofilaments are evenly divided into multiple bundles and arranged in layers using a concentric stranding method. The inner layer monofilaments are arranged with zero gaps, while the outer layer monofilaments have a uniform micro-gap of 0.02-0.05mm. The stranding pitch of each layer is controlled to be 18-22 times the outer diameter of the layer, so as to achieve uniform arrangement of monofilaments, no overlapping of wires, and no squeezing dead corners. 3. A multi-stage progressive micro-compression die is used to compact the pre-stranded conductors, divided into three stages: initial compression, intermediate compression, and fine compression. The compression rate is controlled at 3%-8% throughout the process. Initial compression ratio of 2%-3% eliminates loose gaps in the conductor; Medium-pressure compression ratio 1%-3%, correcting conductor roundness; The compression rate is 0%-2%, ensuring shape stability and preventing copper lattice distortion caused by instantaneous high pressure throughout the process; 4. During the micro-compression molding process, constant temperature air duct insulation is used simultaneously to control the conductor molding temperature at 40-60℃. After molding, the conductor is kept at a constant temperature for 20-40 seconds to release the mechanical internal stress generated during stranding and compaction and to repair micro-lattice defects. 5. Control the overall stranding speed to 80-120m / min, ensure that the tension difference between each layer is ≤5N, and keep the winding tension constant, so as to finally obtain stranded copper conductors with low resistivity, low residual stress and low cost.

[0017] In the raw material pretreatment step, the low-temperature softening pretreatment adopts a hot air constant temperature drying method, and the heating rate is controlled at 3-5℃ / min to avoid uneven local stress in the copper monofilament caused by rapid heating.

[0018] In the aforementioned bundle splitting and layer pre-twisting step, during the layer pre-twisting process, the inner layer twisting direction is opposite to the outer layer twisting direction, and the twisting pitch error between adjacent layers is ≤ ±0.5mm, ensuring that the conductor structure is symmetrical and the force is balanced.

[0019] In the segmented micro-compacting molding process, the multi-stage micro-compacting mold adopts a rounded transition cavity with a surface roughness Ra≤0.8μm to avoid scratching the surface of the copper single wire and causing structural defects during the compaction process.

[0020] In the aforementioned low-temperature stress relief step, the constant temperature air duct adopts a ring-shaped air supply, and the temperature difference around the conductor is ≤±2℃, thereby achieving uniform stress relief throughout the entire area.

[0021] To meet the molding requirements and conductivity optimization requirements of conductors with small cross-sections of 1.5-10mm², the total compression ratio in the segmented micro-compression molding step is controlled at 3%-5%.

[0022] In order to meet the forming requirements and conductivity optimization requirements of medium and large cross-section conductors of 16-120mm², the total compression rate is controlled at 5%-8% in the segmented micro-compression forming step.

[0023] Compared to the traditional 12% compression rate high-pressure process, under the same raw materials, equipment, and production speed, the resistivity of the finished product at 20℃ is 0.0177Ω·mm² / m, which is higher than that of the embodiment of this invention. In addition, the copper wire loss during the production process is large, and high-purity copper materials are required to ensure the basic mechanical and electrical performance, resulting in higher overall production costs.

Claims

1. A conductor micro-compact stranding process for reducing the resistivity of copper conductors, characterized in that: The process involves the following steps: (1) Raw material pretreatment: Select conventional industrial copper monofilaments that conform to the national standard GB / T3956, remove the surface oxide layer, oil and impurities, and perform low-temperature softening pretreatment on the copper monofilaments. The pretreatment temperature is 80-120℃, the heat preservation time is 15-30min, and the copper monofilaments are naturally cooled to room temperature to eliminate the original residual stress of the copper monofilaments. (2) Bundle-by-bundle pre-twisting: According to the cross-sectional area of ​​the target conductor, the pre-treated copper single wires are divided into multiple bundles and arranged in layers using a concentric layer-twisting method. The inner layer of single wires is arranged with zero gaps, and the outer layer of single wires is reserved with a uniform micro gap of 0.02-0.05mm. The twisting pitch of each layer is controlled to be 18-22 times the outer diameter of the layer, so as to achieve uniform arrangement of single wires, no overlapping wires, and no squeezing dead corners. (3) Segmented micro-compression molding: Multi-stage progressive micro-compression molds are used to compact the pre-stranded conductors, which is divided into three stages: initial compression, intermediate compression, and fine compression. The compression rate is controlled at 3%-8% throughout the process. Initial compression ratio of 2%-3% eliminates loose gaps in the conductor; Medium-pressure compression ratio 1%-3%, correcting conductor roundness; The compression rate is 0%-2%, ensuring shape stability and preventing copper lattice distortion caused by instantaneous high pressure throughout the process; (4) Low temperature stress relief: During the micro-compression molding process, constant temperature air duct is used to keep the conductor forming temperature at 40-60℃. After forming, the conductor is kept at a constant temperature for 20-40s to relieve the mechanical internal stress generated during stranding and compaction and repair micro lattice defects. (5) Uniform speed shaping and winding: control the overall stranding speed to 80-120m / min, ensure that the stranding tension difference between each layer is ≤5N, and the winding tension is constant, so as to finally obtain stranded copper conductors with low resistivity, low residual stress and low cost.

2. The conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 1, characterized in that: In the aforementioned raw material pretreatment steps, the low-temperature softening pretreatment adopts a hot air constant temperature drying method, with the heating rate controlled at 3-5℃ / min.

3. A conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 1 or 2, characterized in that: In the aforementioned bundle splitting and layer pre-twisting step, during the layer pre-twisting process, the inner layer twisting direction is opposite to the outer layer twisting direction, and the twisting pitch error between adjacent layers is ≤ ±0.5mm.

4. A conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 1 or 2, characterized in that: In the segmented micro-compression molding step, the multi-stage micro-compression mold adopts a circular arc transition cavity with a surface roughness Ra≤0.8μm.

5. The conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 3, characterized in that... In the segmented micro-compression molding step, the multi-stage micro-compression mold adopts a circular arc transition cavity with a surface roughness Ra≤0.8μm.

6. A conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 1, 2, or 5, characterized in that: In the aforementioned low-temperature stress relief step, the constant temperature air duct adopts a ring-shaped air supply, and the temperature difference around the conductor is ≤±2℃.

7. The conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 3, characterized in that: In the aforementioned low-temperature stress relief step, the constant temperature air duct adopts a ring-shaped air supply, and the temperature difference around the conductor is ≤±2℃.

8. The conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 4, characterized in that... In the aforementioned low-temperature stress relief step, the constant temperature air duct adopts a ring-shaped air supply, and the temperature difference around the conductor is ≤±2℃.

9. A conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 1, 2, 5, 7, or 8, characterized in that: In the segmented micro-compression molding step, the total compression ratio is controlled at 3%-5%.

10. A conductor micro-compact stranding process for reducing the resistivity of copper conductors as described in claim 1, 2, 5, 7, or 8, characterized in that... In the segmented micro-compression molding step, the total compression ratio is controlled at 5%-8%.