Nickel-manganese bimetallic sulfides and their preparation methods, as well as positive electrode plates and capacitors

By preparing hollow tubular nickel-manganese bimetallic sulfides and utilizing a composite shell design of NiMn-LDH nanosheets and Ni3S2, the problems of nanoparticle aggregation and poor cycling stability in the preparation process of nickel-manganese bimetallic sulfides were solved, achieving high specific capacitance and excellent cycling stability.

CN123072935APending Publication Date: 2026-11-10GREE ALTAIRNANO NEW ENERGY INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610899469.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-22
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing nickel-manganese-based bimetallic sulfide materials are prone to nanoparticle aggregation during preparation, resulting in reduced specific surface area and poor cycle stability, making it difficult to meet the requirements of high energy density supercapacitors.

Method used

A hollow tubular nickel-manganese bimetallic sulfide was prepared by using a rod-shaped sacrificial template combined with hydrothermal reaction and high-temperature calcination technology. Through the composite shell design of NiMn-LDH nanosheets and Ni3S2, a continuous charge transport path and volume buffer space were formed, which enhanced the structural stability and electrolyte accessibility of the material.

Benefits of technology

This improved the specific surface area and charge transport efficiency of the material, enhanced the specific capacitance and cycle stability of the capacitor, and solved the structural instability problem caused by volume deformation during charging and discharging of traditional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123072935A_ABST
    Figure CN123072935A_ABST
Patent Text Reader

Abstract

This application relates to the field of capacitors, disclosing a nickel-manganese bimetallic sulfide, its preparation method, a positive electrode plate, and a capacitor. This application utilizes a rod-shaped sacrificial template to prepare a self-supporting nickel-manganese bimetallic sulfide electrode material with a hollow tubular structure through high-temperature calcination and selective etching processes. This nickel-manganese bimetallic sulfide electrode material possesses hollow channels left after removing the rod-shaped sacrificial template, providing a continuous charge transport path and volume buffer space, effectively mitigating volume deformation during charge and discharge. Furthermore, the NiMn-LDH nanosheets grown on the outer layer expose abundant electrochemical active sites and have a high specific surface area, improving electrolyte accessibility, thereby achieving high specific capacitance and excellent cycle stability in the capacitor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of capacitors, and more particularly to a nickel-manganese bimetallic sulfide, its preparation method, a positive electrode plate, and a capacitor. Background Technology

[0002] With the accelerated transformation of the global energy structure and the continuous evolution of electronic devices towards lightweight and highly integrated designs, building high-performance, long-life energy storage systems has become a core issue in current energy technology development. Supercapacitors, with their advantages in instantaneous power output, excellent cycle durability, and energy storage characteristics resulting from the synergistic effect of the double layer and Faraday reaction, have effectively bridged the performance gap between traditional capacitors and secondary batteries in the energy storage device spectrum. However, their application in high-end scenarios such as electric vehicles and smart grids is significantly limited by their relatively low energy density. This is based on the fundamental energy density equation E=1 / 2CV. 2 Analysis shows that improving the specific capacitance of electrode materials is the key to breaking through the energy density bottleneck.

[0003] In electrode material research, transition metal sulfides have attracted much attention due to their superior electron transport capabilities and abundant redox activity compared to oxide systems. Nickel-manganese-based bimetallic sulfides, with their synergistic effect of multivalent manganese and nickel ions, structural tunability, and high theoretical capacity potential, have become promising candidate materials. However, nickel-manganese sulfides prepared by existing synthesis processes generally suffer from microstructural defects: nanoparticles are prone to irreversible aggregation during preparation, leading to a reduction in the specific surface area of ​​the material and burying effective electrochemical active sites; simultaneously, during repeated charge-discharge cycles, the lattice stress induced by ion insertion and extraction causes severe volume deformation, resulting in particle breakage and conductive network fracture, ultimately manifesting as accelerated capacity decay and deterioration of cycle stability. These structural defects severely hinder the intrinsic electrochemical performance of the materials, making it difficult to meet the stringent requirements of high-energy-density supercapacitors for electrode materials. Summary of the Invention

[0004] In view of this, the purpose of this application is to provide a nickel-manganese bimetallic sulfide and a method for preparing the same, such that the nickel-manganese bimetallic sulfide has a high specific surface area, improves electrolyte accessibility, charge transport efficiency and structural stability, thereby achieving high specific capacitance and excellent cycle stability of the capacitor. Another objective of this application is to provide a positive electrode plate and a capacitor based on the aforementioned nickel-manganese bimetallic sulfide.

[0005] To solve the aforementioned technical problems / achieve the aforementioned objectives, or at least partially solve the aforementioned technical problems / achieve the aforementioned objectives, as a first aspect of this application, a nickel-manganese bimetallic sulfide is provided, comprising a composite shell continuously surrounding the hollow tubular structure; the composite shell comprises NiMn-LDH nanosheets and Ni3S2, the NiMn-LDH nanosheets constituting the main continuous framework of the composite shell, and the Ni3S2 dispersed on the surface and / or inside the main continuous framework of the NiMn-LDH nanosheets.

[0006] As a second aspect of this application, a method for preparing nickel-manganese bimetallic sulfides as described in this application is provided, comprising: S1. Prepare rod-shaped sacrificial templates; S2. After mixing nickel source, manganese source and hexamethylenetetramine, a hydrothermal reaction is carried out in full contact with the rod-shaped sacrificial template to obtain a rod-shaped intermediate material with a core of rod-shaped sacrificial template and a shell of NiMn-LDH nanosheets. S3. The sulfur source and the rod-shaped intermediate material are calcined at high temperature to perform incomplete sulfidation, and Ni3S2 is generated in situ on the surface and / or inside of the NiMn-LDH nanosheets. The product after high-temperature calcination is aged using an etching solution to remove the rod-shaped sacrificial template and obtain the nickel-manganese bimetallic sulfide NiMn-LDH / Ni3S2.

[0007] Optionally, S1 includes: The precursor of the rod-shaped sacrificial template is dissolved in an organic solution and subjected to a hydrothermal reaction to obtain the rod-shaped sacrificial template.

[0008] Optionally, the rod-shaped sacrificial template comprises ZnO nanorods, and the precursor of the rod-shaped sacrificial template comprises a zinc salt or its hydrate, wherein the zinc salt comprises one or more of zinc nitrate, zinc chloride, zinc acetate, and zinc sulfate.

[0009] Optionally, the temperatures of the hydrothermal reactions described in S1 and S2 are each independently 60-120°C.

[0010] Optionally, the nickel source includes one or more of nickel chloride, nickel sulfate, nickel nitrate, nickel acetate, or their hydrates; the manganese source includes one or more of manganese chloride, manganese nitrate, manganese sulfate, or their hydrates; and the sulfur source includes one or more of sulfur, thiourea, and thioacetamide.

[0011] Optionally, the high-temperature calcination temperature is 200-400℃.

[0012] Optionally, the etching solution includes one or more of tannic acid solution, gallic acid solution, and ammonia solution.

[0013] As a third aspect of this application, a positive electrode plate is provided, including a current collector and a positive electrode active material disposed on the surface of the current collector, the positive electrode active material including the nickel-manganese bimetallic sulfide described in this application.

[0014] As a fourth aspect of this application, a capacitor is provided, including the positive electrode plate described in this application.

[0015] This application utilizes a rod-shaped sacrificial template to fabricate a self-supporting nickel-manganese bimetallic sulfide electrode material with a hollow tubular structure through high-temperature calcination and selective etching. This nickel-manganese bimetallic sulfide electrode material possesses hollow channels left after removing the rod-shaped sacrificial template, providing a continuous charge transport path and volume buffer space, effectively mitigating volume deformation during charge and discharge. Furthermore, the NiMn-LDH nanosheets grown on the outer layer expose abundant electrochemical active sites and possess a high specific surface area, improving electrolyte accessibility and thus achieving high specific capacitance and excellent cycle stability of the capacitor. Attached Figure Description

[0016] Figure 1 The diagram shows the preparation process of the nickel-manganese bimetallic sulfide NiMn-LDH / Ni3S2 of this application; NS: nickel foam current collector; NiMn-LDH: nickel-manganese bimetallic hydroxide nanosheets. Detailed Implementation

[0017] This application discloses a nickel-manganese bimetallic sulfide, its preparation method, a positive electrode plate, and a capacitor. Those skilled in the art can refer to this document and appropriately modify the process parameters to achieve the desired result. It is particularly important to note that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in this application. The products, processes, and applications described in this application have been described through preferred embodiments. Those skilled in the art can obviously modify or appropriately change and combine the preparation methods described herein without departing from the content, spirit, and scope of this application to realize and apply the technology of this application. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.

[0018] It should be noted that, in this document, relational terms such as "first" and "second," "step 1" and "step 2," and "(1)" and "(2)" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element. Moreover, the embodiments and features described in this application can be combined with each other without conflict.

[0019] For ease of understanding, the following explains some key terms in this embodiment: Nickel-manganese bimetallic sulfides are compounds composed of nickel, manganese, and sulfur. They typically exhibit a wide range of redox valence states and high electrochemical activity, making them suitable for energy storage applications.

[0020] A composite shell is an external covering layer composed of two or more different material components. Its function is to provide specific structural support and functional synergy.

[0021] Hollow tubular structures refer to materials with interconnected cavities inside and a tubular shape on the outside. These structures typically feature increased specific surface area and an increased number of ion transport channels.

[0022] NiMn-LDH nanosheets refer to nickel-manganese layered bimetallic hydroxides existing in a nanoscale sheet-like morphology. Their layered structure facilitates ion insertion and extraction and can serve as a carrier for active substances.

[0023] Ni3S2 is a nickel sulfide that typically has high electrical conductivity. In composite materials, it can act as a bridge for electron transport and participate in electrochemical reactions.

[0024] The main continuous skeleton refers to the part of the composite material that constitutes the main supporting structure and maintains continuity. It is formed by NiMn-LDH nanosheets, which provide a platform for the attachment and dispersion of other components such as Ni3S2.

[0025] Traditional nickel-manganese-based bimetallic sulfide electrode materials suffer from several drawbacks in energy storage applications, including a tendency for nanoparticles to aggregate, insufficient exposure of active sites, and low cycle stability due to volume expansion during charge and discharge. These limitations restrict the full realization of their electrochemical performance, thereby affecting the improvement of supercapacitor energy density.

[0026] Based on this, in the first aspect of this application, a nickel-manganese bimetallic sulfide is provided, characterized by comprising a composite shell that continuously surrounds a hollow tubular structure. Specifically, the nickel-manganese bimetallic sulfide can be formed into a hollow tubular structure in various ways. Furthermore, the composite shell comprises NiMn-LDH nanosheets and Ni3S2. The NiMn-LDH nanosheets constitute the main continuous framework of the composite shell. The formation of the NiMn-LDH nanosheets as the main continuous framework can be achieved by controlling the growth conditions of NiMn-LDH. For example, the precipitation reaction of NiMn-LDH can be directly carried out in solution, allowing it to grow and interconnect on a specific substrate, forming a continuous sheet-like network structure.

[0027] Furthermore, Ni3S2 is dispersed on the surface and / or inside the continuous framework of the NiMn-LDH nanosheets. The dispersion of Ni3S2 on the continuous framework of the NiMn-LDH nanosheets can take many forms. For example, Ni3S2 particles can adhere to the surface of the NiMn-LDH nanosheets through simple physical adsorption or electrostatic interactions. Alternatively, Ni3S2 can be formed inside or on the surface of the nanosheets through a sulfidation reaction in the presence of the NiMn-LDH nanosheets. Furthermore, Ni3S2 can also be induced to form on the framework by mixing a Ni3S2 precursor with NiMn-LDH nanosheets followed by heat treatment.

[0028] This application constructs a hollow tubular nickel-manganese bimetallic sulfide, in which NiMn-LDH nanosheets form the main continuous framework, with Ni3S2 dispersed on its surface and / or inside, thereby increasing the specific surface area and active sites of the material. Simultaneously, the hollow structure provides ion transport channels and volume buffer space. This design synergistically improves the charge transport efficiency and structural stability of the material, overcoming the problems of traditional nanoparticles such as agglomeration tendency, insufficient exposure of active sites, and low cycle stability due to volume expansion during charge and discharge, thus improving the electrochemical energy storage performance of the electrode material. In a second aspect of this application, a method for preparing a nickel-manganese bimetallic sulfide is provided, the method comprising the following steps: S1. Prepare rod-shaped sacrificial templates; S2. After mixing nickel source, manganese source and hexamethylenetetramine, a hydrothermal reaction is carried out with full contact with rod-shaped sacrificial template to obtain a rod-shaped intermediate material with a core of rod-shaped sacrificial template and a shell of NiMn-LDH nanosheets. S3. The sulfur source and rod-shaped intermediate material are calcined at high temperature to perform incomplete sulfidation, and Ni3S2 is generated in situ on the surface and / or inside of NiMn-LDH nanosheets. The product after high-temperature calcination is aged using an etching solution to remove the rod-shaped sacrificial template and obtain the nickel-manganese bimetallic sulfide NiMn-LDH / Ni3S2.

[0029] In step S1, the preparation of the rod-shaped sacrificial template is a temporary structure used to guide the growth of the target material and form a specific morphology (such as a hollow tubular structure). Its function is to provide a framework that can be subsequently removed, enabling precise control over the morphology of the final product, preventing disordered aggregation of nanoparticles, and providing a substrate for the uniform deposition of active materials. This rod-shaped sacrificial template can be prepared in various ways. For example, it can be prepared in situ using hydrothermal or solvothermal methods, utilizing the reaction of metal salts (such as zinc salts) with a precipitant (such as hexamethylenetetramine) at specific temperatures and times to grow metal oxide nanostructures with rod-shaped morphologies. Alternatively, electrochemical deposition or chemical vapor deposition can be used to prepare rod-shaped polymers or carbon materials with the desired size and morphology on a suitable substrate as sacrificial templates.

[0030] In step S2, the nickel source, manganese source, and hexamethylenetetramine are mixed and then subjected to a hydrothermal reaction in full contact with the rod-shaped sacrificial template to obtain a rod-shaped intermediate material with a rod-shaped sacrificial template core and NiMn-LDH nanosheets as the shell. This step aims to utilize a hydrothermal reaction to uniformly grow NiMn-LDH nanosheets on the surface of the rod-shaped sacrificial template, forming a rod-shaped intermediate material with a core-shell structure. The nickel and manganese sources provide Ni and Mn ions; hexamethylenetetramine acts as a precipitant and pH adjuster, promoting the nucleation and growth of NiMn-LDH nanosheets on the template surface. Under hydrothermal conditions, it slowly releases OH-. - Ni 2+ and Mn 2+ With slowly released OH -The metal hydroxide monomers are formed through bonding. Furthermore, under hydrothermal conditions, LDH nuclei preferentially grow along the ab plane, ultimately forming two-dimensional nanosheet structures with a thickness of only a few nanometers and a lateral dimension of tens to hundreds of nanometers. This core-shell structure design utilizes the morphology-guiding effect of the sacrificial template to ensure that NiMn-LDH nanosheets can be continuously coated on the template's outer layer, laying the foundation for the subsequent formation of a hollow structure and effectively suppressing the disordered aggregation of NiMn-LDH nanosheets. For example, soluble salts of nickel and manganese sources can be used. These salts are dissolved with hexamethylenetetramine in deionized water or a mixed solvent in a certain proportion. Then, the rod-shaped sacrificial template is immersed in this mixed solution, and a hydrothermal reaction is carried out in a reactor at a temperature of 60-120°C for several hours.

[0031] In step S3, through high-temperature calcination, the sulfur source undergoes an incomplete sulfidation reaction with the NiMn-LDH nanosheets, allowing Ni3S2 to be generated in situ on the surface and / or inside the NiMn-LDH nanosheets, forming a tightly bonded composite structure. This incomplete sulfidation strategy aims to retain part of the NiMn-LDH structure to leverage its unique electrochemical properties. Subsequently, the internal rod-shaped sacrificial template is selectively removed using an etching solution, thereby obtaining a nickel-manganese bimetallic sulfide NiMn-LDH / Ni3S2 with a hollow tubular structure. This in-situ generation and etching strategy not only enhances the interfacial bonding between the two active components and improves ion transport efficiency, but also increases the specific surface area and active site exposure of the material by forming a hollow structure, while mitigating volume changes during charge and discharge. For example, sulfur powder, thiourea, thioacetamide, etc., can be used as the sulfur source. The rod-shaped intermediate material and a sulfur source are calcined at high temperatures ranging from 200-400°C under an inert atmosphere (e.g., using argon or nitrogen as carrier gases to carry the sulfur source to the rod-shaped intermediate material for reaction). The calcination time can be adjusted according to the required degree of sulfidation, including the amount of sulfur source, the sulfidation reaction time, and the reaction temperature. After calcination, the product is immersed in a suitable etching solution for aging treatment to dissolve and remove the internal sacrificial template. Alternatively, the sulfur source can be introduced via gas-phase sulfidation, for example, by introducing H2S gas or CS2 vapor and reacting it with the rod-shaped intermediate material at high temperatures. The choice of etching solution depends on the material of the sacrificial template. For example, if the sacrificial template is ZnO, a weakly acidic solution or ammonia can be used for etching.

[0032] In some embodiments of this application, S1 includes: The rod-shaped sacrificial template precursor is obtained by hydrothermal reaction with hexamethylenetetramine dissolved in an organic solution. Hexamethylenetetramine provides a uniform and mild alkaline environment for the hydrolysis and precipitation of the precursor, and also acts as a morphology control agent, guiding anisotropic crystal growth along specific directions through selective adsorption onto specific crystal faces. The organic solution (e.g., ammonia solution) effectively regulates the solubility and diffusion rate of the precursor, suppressing disordered nucleation and resulting in a more uniform template size distribution.

[0033] This template, which is induced to grow through a specific chemical environment, provides an ideal substrate for the uniform deposition of nickel-manganese bimetallic sulfide nanosheets. It ensures that the composite shell can be tightly and continuously coated on the template surface, so that after removing the template, hollow tubular materials with complete structure, large specific surface area and sufficient exposure of active sites can be obtained. This effectively avoids problems such as irregular template morphology, uneven distribution of surface active sites and structural collapse or weak loading of active materials in the final product.

[0034] In some embodiments of this application, the precursor of the rod-shaped sacrificial template is a starting material used to form the rod-shaped sacrificial template. These precursors are diverse, and can be zinc salts or their hydrates, such as zinc nitrate, zinc chloride, zinc acetate, zinc sulfate, and one or more of their hydrates. The hydrates include, but are not limited to, zinc acetate dihydrate, zinc chloride hexahydrate, and zinc sulfate heptahydrate. The corresponding rod-shaped sacrificial template is ZnO nanorods. Choosing zinc salts or their hydrates as precursors for ZnO nanorods aims to precisely control the growth kinetics and final morphology of the ZnO nanorods. Zinc salts can hydrolyze and crystallize to form ZnO nanorods under hydrothermal conditions. By controlling the reaction conditions and the type of zinc salt, rod-shaped templates with uniform size and suitable surface activity can be obtained. ZnO nanorods, as a common semiconductor material, are easy to prepare, have controllable morphology, moderate chemical stability, and are easy to remove via subsequent etching. Their rod-shaped structure provides a regular physical support framework for the subsequent growth of NiMn-LDH nanosheets, thereby guiding the composite shell to continuously and uniformly form a hollow tubular structure. Furthermore, the introduction of ZnO nanorods effectively suppressed the disordered aggregation of nickel-manganese bimetallic sulfides during the synthesis process through their template effect, which helps to maintain the high specific surface area and full exposure of active sites of the material.

[0035] In some embodiments of this application, the mass ratio of the precursor to hexamethylenetetramine in the rod-shaped sacrificial template is in the range of 1:2 to 1:4. For example, 1:2, 1:3, 1:4, or any ratio between the two. By optimizing the mass ratio of the precursor to hexamethylenetetramine, this application effectively controls the formation rate of crystal nuclei and the growth direction of crystals during the hydrothermal reaction. This precise ratio avoids runaway crystal growth or agglomeration caused by improper reactant concentration, thereby ensuring that the prepared rod-shaped sacrificial template has a highly regular morphology and excellent size uniformity, providing an ideal substrate for the uniform growth of NiMn-LDH nanosheets on its surface by nickel and manganese sources, and ensuring the integrity and uniformity of the continuous framework of the NiMn-LDH nanosheet main body.

[0036] In some embodiments of this application, the temperatures of the hydrothermal reactions in S1 and S2 are each independently between 60-120°C, for example, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, or any value between the two; wherein, the hydrothermal reaction in S1 is preferably between 60-110°C. Optimizing the hydrothermal reaction temperature within the range of 60 to 120°C provides a suitable kinetic and thermodynamic environment for the growth of rod-shaped sacrificial templates and NiMn-LDH nanosheets.

[0037] In some other embodiments of this application, the hydrothermal reaction time in S1 can be selected as 22-26h, such as 22h, 23h, 24h, 25h, 26h or any value between the two; the hydrothermal reaction time in S2 can be selected as 0.5-5h, such as 0.5h, 1h, 2h, 3h, 4h, 5h or any value between the two.

[0038] In some embodiments of this application, the nickel source includes one or more of nickel chloride, nickel sulfate, nickel nitrate, nickel acetate, or their hydrates; the manganese source includes one or more of manganese chloride, manganese nitrate, manganese sulfate, or their hydrates; and the sulfur source includes one or more of sulfur, thiourea, and thioacetamide. In some embodiments of this application, the hydrates of the nickel and manganese sources include, but are not limited to, nickel chloride hexahydrate and manganese chloride tetrahydrate. In other embodiments of this application, the molar ratio of the nickel source to the manganese source is optimized to 1:(2-4), for example, 1:2, 1:3, 1:4, or any ratio between the two. By optimizing the ratio and type of the nickel and manganese sources, nickel and manganese elements coexist in a specific ratio within the NiMn-LDH nanosheet framework. This specific ratio helps to form a structurally stable NiMn-LDH and Ni3S2 composite phase during subsequent sulfidation, thereby enhancing the pseudocapacitive properties of the material. Meanwhile, by selecting various nickel sources such as nickel chloride, nickel sulfate, nickel nitrate, and nickel acetate, as well as various manganese sources such as manganese chloride, manganese nitrate, and manganese sulfate, the ion concentration and anion environment in the reaction system can be flexibly adjusted to ensure that nickel-manganese precursors can be uniformly formed during the hydrothermal reaction stage, providing a material basis for the subsequent generation of continuous nanosheet frameworks.

[0039] In some embodiments of this application, the amount of sulfur source added is 20-60 mg / 2cm². 2 Rod-shaped intermediate material (i.e., every 2cm) 2 The amount of sulfur source added to the rod-shaped intermediate material can be specified, for example, 20 mg, 30 mg, 40 mg, 50 mg, 60 mg, or any value between two options. Within this optimized range, it is possible to effectively avoid insufficient sulfur source leading to low sulfidation, or excessive sulfur source leading to over-sulfidation, which would damage the continuous framework of the NiMn-LDH nanosheets. This allows for precise control of Ni3S2 formation without disrupting the hollow tubular structure of the nickel-manganese bimetallic sulfide. This ensures good structural stability and efficient exposure of active sites in the electrochemical reaction, significantly improving the electrochemical performance of the nickel-manganese bimetallic sulfide.

[0040] In some embodiments of this application, the high-temperature calcination temperature is 200-400°C, and the time is 1-3 hours, for example, 200°C, 250°C, 300°C, 350°C, 400°C, or any value between two of these. The high-temperature calcination refers to the heat treatment of a sulfur source and a rod-shaped intermediate material during the preparation of the nickel-manganese bimetallic sulfide NiMn-LDH / Ni3S2 to achieve incomplete sulfidation, thereby generating Ni3S2 in situ on the surface and / or inside the NiMn-LDH nanosheets. Limiting the calcination temperature to the range of 200-400°C aims to provide a precise and controllable thermodynamic environment for the sulfidation reaction. This temperature range effectively regulates the reaction rate between the sulfur source and the rod-shaped intermediate material, ensuring that the sulfidation reaction remains in an incomplete sulfidation state. For example, calcination can be carried out using a tube furnace with precise temperature control. The furnace temperature can be set at 200°C, 300°C, or 400°C and maintained for a certain period of time. The sulfur source can be placed in the upstream region of the tube furnace, and the rod-shaped intermediate material can be placed in the downstream reaction region of the tube furnace. An inert atmosphere (such as argon or nitrogen) can be used as a carrier gas to carry the sulfur source to the downstream reaction region, and an incomplete sulfidation reaction can occur in situ on the surface and / or inside of the rod-shaped intermediate material to generate discontinuous Ni3S2.

[0041] In some embodiments of this application, the etching solution includes one or more of tannic acid solution, gallic acid solution, and ammonia solution. The mass percentage concentration of the etching solution is typically 1-5%, for example, 1%, 2%, 3%, 4%, 5%, or any value between the two. The outer NiMn-LDH / Ni3S2 layer is porous and permeable, which is the basis for the etching solution to penetrate into the interior to etch the rod-shaped sacrificial template (such as ZnO nanorods). Taking ZnO nanorods as an example, they are typical amphoteric oxides and can undergo complexation reactions with etching solutions such as ammonia solution at room temperature to generate soluble tetraammine zinc complex ions. Moreover, NiMn-LDH and Ni3S2 hardly react in etching solutions such as ammonia solution. In other embodiments of this application, the aging time can be selected as 3-5 hours.

[0042] In a third aspect of this application, a positive electrode plate is provided, comprising a current collector and a positive electrode active material disposed on the surface of the current collector, wherein the positive electrode active material comprises the nickel-manganese bimetallic sulfide described in this application or the nickel-manganese bimetallic sulfide prepared by the preparation method described in this application.

[0043] A current collector is the conductive substrate of an electrode material. Its main function is to collect electrons generated by the active material during the electrochemical reaction and effectively transfer them to the external circuit. Simultaneously, it provides necessary mechanical support to the active material to maintain the structural integrity of the electrode. Specifically, current collectors can be made from various conductive materials. For example, they can be porous nickel foam to provide a larger specific surface area and better electrolyte permeability; nickel mesh to balance conductivity and mechanical strength; or carbon cloth or carbon paper to provide good flexibility and chemical stability. In addition, stainless steel mesh, nickel foil, and copper foil are also commonly used as current collectors.

[0044] In some embodiments of this application, when preparing the nickel-manganese bimetallic sulfide, a current collector can be directly used as a substrate. The scale of the rod-shaped sacrificial template / rod-shaped intermediate material / nickel-manganese bimetallic sulfide is limited by selecting the size of the current collector (e.g., 1cm × 2cm). For example, an array of ZnO nanorods can be generated on a nickel foam substrate through a hydrothermal reaction of zinc salt and hexamethylenetetramine. Then, a rod-shaped intermediate material can be prepared through a hydrothermal reaction of a nickel source, a manganese source, and hexamethylenetetramine. Finally, the nickel-manganese bimetallic sulfide is prepared through incomplete sulfidation and aging in an etching solution. This structural design can effectively solve key problems such as interface compatibility, charge transport efficiency, and structural stability faced by active materials in electrode preparation and use. Specifically, the current collector, as a highly efficient electron collection and transport channel, forms a tight electrical contact with the nickel-manganese bimetallic sulfide loaded on its surface, significantly reducing the charge transport impedance. The hollow tubular structure of nickel-manganese bimetallic sulfides provides a huge specific surface area, which greatly increases the contact area between the active material and the electrolyte, thereby promoting the rapid transport of ions inside the active material.

[0045] In a fourth aspect of this application, a capacitor is provided, including the positive electrode plate described in this application. A capacitor is an electronic component capable of storing charge and electrical energy, and its working principle utilizes the polarization of the dielectric between electrode plates to store charge. In practical applications, capacitors can be classified into various types according to their energy storage mechanism. For example, it can be a double-layer capacitor that mainly relies on the double-layer effect at the electrode / electrolyte interface, a pseudocapacitor that utilizes rapid reversible redox reactions (pseudocapacitance) on or near the surface of the electrode material for energy storage, or a hybrid capacitor that combines the advantages of both. This capacitor, as the final energy storage device, aims to transform the excellent electrochemical performance of the electrode material into practically usable device performance. The positive electrode plate is one of the core components of the capacitor, and its main function is to serve as the site of electrochemical reactions and provide a channel for charge transport. Typically, the positive electrode plate is prepared by coating a mixture of active material, conductive agent, and binder onto a current collector, while the positive electrode plate provided in this application is formed by directly growing the active material in situ on the surface of the current collector. For example, the nickel-manganese bimetallic sulfide of this application is directly grown on the surface of the nickel foam current collector to form a self-supporting electrode.

[0046] In this application, the specific conventional conductive agents, binders, and other materials used in the negative electrode plate can be selected with reference to existing records in the field, and the capacitor can also be prepared with reference to existing processes. This application does not impose any restrictions on these aspects.

[0047] In the comparative experiments provided in this application, unless otherwise specified, all experimental conditions and materials are kept consistent to ensure comparability. Unless otherwise specified, all experimental materials and reagents used in the examples are commercially available.

[0048] The following provides a further description of the nickel-manganese bimetallic sulfide, its preparation method, positive electrode plate, and capacitor provided in this application.

[0049] Example 1: Reference Figure 1 The schematic diagram shown illustrates the preparation of NiMn-LDH / Ni3S2, including: S1: Preparation of ZnO Take 338.4 mg of zinc nitrate hexahydrate, 147.2 mg of hexamethylenetetramine, and 4 mL of ammonia water and disperse them in 70 mL of deionized water. Stir magnetically for 1 h to form a homogeneous solution. Immerse 1 cm × 2 cm nickel foam in the above solution and transfer it to a stainless steel reactor. React at 60 °C for 24 h. Wash and dry the resulting product to obtain ZnO nanoarrays.

[0050] S2: Preparation of ZnO / NiMn-LDH Disperse 700.1 mg of hexamethylenetetramine in 30 mL of deionized water and stir for 30 min to form solution A. Disperse 713 mg of nickel chloride hexahydrate and 198 mg of manganese chloride tetrahydrate in 30 mL of deionized water and stir for 30 min to form solution B. Mix solution B and solution A and stir for 1 h to form a mixture. Immerse the ZnO-loaded nickel foam at the bottom of the mixture and then transfer it to a stainless steel reactor. React at 60 °C for 1 h. Wash and dry the resulting product to obtain ZnO / NiMn-LDH.

[0051] S3: Preparation of NiMn-LDH / Ni3S2 20 mg of sulfur powder was placed upstream of a tubular furnace, and nickel foam loaded with ZnO / NiMn-LDH was placed downstream. Argon was used as the protective gas, the heating rate was 2 °C / min, the calcination temperature was 200 °C, and the calcination time was 2 h. After the temperature dropped to room temperature, the calcined sulfurized product was immersed in a 3% ammonia solution and allowed to stand for 3 h for aging. After the reaction was completed, it was washed several times with deionized water and anhydrous ethanol to obtain a hollow core-shell structure NiMn-LDH / Ni3S2.

[0052] Example 2: S1: Preparation of ZnO Take 338.4 mg of zinc nitrate hexahydrate, 147.2 mg of hexamethylenetetramine, and 4 mL of ammonia water and disperse them in 70 mL of deionized water. Stir magnetically for 1 h to form a homogeneous solution. Immerse 1 cm × 2 cm nickel foam in the above solution and transfer it to a stainless steel reactor. React at 90 °C for 24 h. Wash and dry the resulting product to obtain ZnO nanoarrays.

[0053] S2: Preparation of ZnO / NiMn-LDH Disperse 700.1 mg of hexamethylenetetramine in 30 mL of deionized water and stir for 30 min to form solution A. Disperse 713 mg of nickel chloride hexahydrate and 198 mg of manganese chloride tetrahydrate in 30 mL of deionized water and stir for 30 min to form solution B. Mix solution B and solution A and stir for 1 h to form a mixture. Immerse the ZnO-loaded nickel foam at the bottom of the mixture and then transfer it to a stainless steel reactor. React at 90 °C for 1 h. Wash and dry the resulting product to obtain ZnO / NiMn-LDH.

[0054] S3: Preparation of NiMn-LDH / Ni3S2 20 mg of thioacetamide was placed upstream of a tube furnace, and nickel foam loaded with ZnO / NiMn-LDH was placed downstream. Argon was used as the protective gas, the heating rate was 2 °C / min, the calcination temperature was 200 °C, and the calcination time was 2 h. After the temperature dropped to room temperature, the calcined and sulfided product was immersed in a 3% ammonia solution and allowed to stand for 3 h for aging. After the reaction was completed, the product was washed several times with deionized water and anhydrous ethanol to obtain a hollow core-shell structure NiMn-LDH / Ni3S2.

[0055] Example 3: S1: Preparation of ZnO Take 338.4 mg of zinc nitrate hexahydrate, 147.2 mg of hexamethylenetetramine, and 4 mL of ammonia water and disperse them in 70 mL of deionized water. Stir magnetically for 1 h to form a homogeneous solution. Immerse 1 cm × 2 cm nickel foam in the above solution and transfer it to a stainless steel reactor. React at 90 °C for 24 h. Wash and dry the resulting product to obtain ZnO nanoarrays.

[0056] S2: Preparation of ZnO / NiMn-LDH Disperse 700.1 mg of hexamethylenetetramine in 30 mL of deionized water and stir for 30 min to form solution A. Disperse 713 mg of nickel chloride hexahydrate and 198 mg of manganese chloride tetrahydrate in 30 mL of deionized water and stir for 30 min to form solution B. Mix solution B with solution A and stir for 1 h to form a mixture. Immerse the ZnO-loaded nickel foam at the bottom of the mixture and then transfer it to a stainless steel reactor. React at 90 °C for 1 h. Wash and dry the resulting product to obtain ZnO / NiMn-LDH.

[0057] S3: Preparation of NiMn-LDH / Ni3S2 20 mg of thioacetamide was placed upstream of a tube furnace, and nickel foam loaded with ZnO / NiMn-LDH was placed downstream. Argon was used as the protective gas, the heating rate was 2 °C / min, the calcination temperature was 300 °C, and the calcination time was 2 h. After the temperature dropped to room temperature, the calcined and sulfided product was immersed in a 3% ammonia solution and allowed to stand for 3 h for aging. After the reaction was completed, the product was washed several times with deionized water and anhydrous ethanol to obtain a hollow core-shell structure NiMn-LDH / Ni3S2.

[0058] Example 4: The difference between Example 4 and Example 3 is that the hydrothermal temperature in step S2 is 120°C.

[0059] Example 5: The difference between Example 5 and Example 3 is that the etching solution in step S3 is a 3% tannic acid solution.

[0060] Example 6: The difference between Example 6 and Example 3 is that the etching solution in step S3 is a 3% gallic acid solution.

[0061] Example 7: The difference between Example 6 and Example 3 is that the sulfur source in step S3 is thiourea.

[0062] Example 8: The difference between Example 8 and Example 3 is that the calcination temperature in step S3 is 400℃.

[0063] Comparative Example 1: S1: Preparation of NiMn-LDH Disperse 700.1 mg of hexamethylenetetramine in 30 mL of deionized water and stir for 30 min to form solution A. Disperse 713 mg of nickel chloride hexahydrate and 198 mg of manganese chloride tetrahydrate in 30 mL of deionized water and stir for 30 min to form solution B. Mix solution B and solution A and stir for 1 h to form a mixture. Immerse the nickel foam at the bottom of the mixture and then transfer it to a stainless steel reactor. React at 90 °C for 1 h. Wash and dry the resulting product to obtain NiMn-LDH.

[0064] S2: Preparation of NiMn-LDH / Ni3S2 20 mg of thioacetamide was placed upstream of a tube furnace, and nickel foam loaded with NiMn-LDH was placed downstream. Argon was used as the protective gas, the heating rate was 2 °C / min, the calcination temperature was 300 °C, the calcination time was 2 h, and after cooling to room temperature, nano-flower-like NiMn-LDH / Ni3S2 was obtained.

[0065] Experimental example: The nickel-manganese bimetallic sulfide electrode materials prepared in each embodiment and comparative example were used as positive electrodes, and their electrochemical performance was tested in a three-electrode system. The voltage range was 0-0.5V. The performance of each embodiment was tested and compared at 1-10 A·g. -1 The specific capacitance at current density, and at 10 A·g -1 The capacity retention rate after 1000 cycles is shown in Table 1. Table 1 Comparison of electrochemical performance of nickel-manganese bimetallic sulfide electrode materials

[0066] As shown in Table 1, the specific capacitance of the capacitors prepared from the hollow tubular NiMn-LDH / Ni3S2 cathode materials in each embodiment is significantly improved compared to the capacitors prepared from the nanoflower-shaped NiMn-LDH / Ni3S2 cathode materials in Comparative Example 1, while the specific capacitance at 10 A·g -1The capacity retention rate after 1000 cycles was also significantly improved. Among the various embodiments, the electrical performance of Embodiment 3 was the best.

[0067] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A nickel-manganese bimetallic sulfide, characterized in that, The composite shell is continuously formed into a hollow tubular structure. The composite shell includes NiMn-LDH nanosheets and Ni3S2. The NiMn-LDH nanosheets constitute the main continuous framework of the composite shell, and the Ni3S2 is dispersed on the surface and / or inside the main continuous framework of the NiMn-LDH nanosheets.

2. A method for preparing the nickel-manganese bimetallic sulfide as described in claim 1, characterized in that, include: S1. Prepare rod-shaped sacrificial templates; S2. After mixing nickel source, manganese source and hexamethylenetetramine, a hydrothermal reaction is carried out in full contact with the rod-shaped sacrificial template to obtain a rod-shaped intermediate material with a core of rod-shaped sacrificial template and a shell of NiMn-LDH nanosheets. S3. The sulfur source and the rod-shaped intermediate material are calcined at high temperature to perform incomplete sulfidation, and Ni3S2 is generated in situ on the surface and / or inside of the NiMn-LDH nanosheets. The product after high-temperature calcination is aged using an etching solution to remove the rod-shaped sacrificial template and obtain the nickel-manganese bimetallic sulfide NiMn-LDH / Ni3S2.

3. The preparation method according to claim 2, characterized in that, S1 includes: The precursor of the rod-shaped sacrificial template is dissolved in an organic solution and subjected to a hydrothermal reaction to obtain the rod-shaped sacrificial template.

4. The preparation method according to claim 3, characterized in that, The rod-shaped sacrificial template includes ZnO nanorods, and the precursor of the rod-shaped sacrificial template includes a zinc salt or its hydrate, wherein the zinc salt includes one or more of zinc nitrate, zinc chloride, zinc acetate, and zinc sulfate.

5. The preparation method according to claim 3, characterized in that, The temperatures of the hydrothermal reactions described in S1 and S2 are each independently 60-120℃.

6. The preparation method according to claim 2, characterized in that, The nickel source includes one or more of nickel chloride, nickel sulfate, nickel nitrate, nickel acetate, or their hydrates; the manganese source includes one or more of manganese chloride, manganese nitrate, manganese sulfate, or their hydrates; and the sulfur source includes one or more of sulfur, thiourea, and thioacetamide.

7. The preparation method according to claim 2, characterized in that, The high-temperature calcination temperature is 200-400℃.

8. The preparation method according to claim 2, characterized in that, The etching solution includes one or more of tannic acid solution, gallic acid solution, and ammonia solution.

9. A positive electrode plate, characterized in that, It includes a current collector and a positive electrode active material disposed on the surface of the current collector, wherein the positive electrode active material includes the nickel-manganese bimetallic sulfide as described in claim 1.

10. A capacitor, characterized in that, Includes the positive electrode plate as described in claim 9.