A method for processing the positive plate grid of a lead-acid battery
By forming a dense lead monoxide and porous lead dioxide interface layer on the positive plate grid of a lead-acid battery, the problem of decreased conductivity during over-discharge of lead-acid batteries is solved, thus extending the battery's service life.
Patent Information
- Application Number
- CN202510581917.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-10
AI Technical Summary
When existing lead-acid batteries are over-discharged during user cycling, the conductivity of the lead dioxide interface layer decreases, leading to a shortened lifespan.
The positive electrode grid is treated in a persulfate solution to form a dense lead monoxide interface layer and a porous lead dioxide interface layer, thereby improving the conductivity of the interface layer.
It enhances the conductivity of the lead dioxide interface layer in lead-acid batteries under over-discharge conditions, thus extending the battery's lifespan.
Smart Images

Figure CN123073033A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lead-acid battery manufacturing, and in particular to a method for processing the positive grid of a lead-acid battery. Background Technology
[0002] In existing lead-acid batteries, the interface between the active material and the grid consists of a dense layer and a porous layer. The dense layer is a lead monoxide interface layer, which is formed during curing. The porous layer is a lead dioxide interface layer, which is formed during formation when the lead monoxide layer on the grid reacts with water in an electrochemical reaction to generate the lead dioxide interface layer. When users perform deep discharge during cycling, this leads to over-discharge of the lead dioxide interface layer in the lead-acid battery, resulting in the formation of lead sulfate at the lead dioxide interface layer. The lead sulfate formed at the interface layer is difficult to convert back to lead dioxide through charging, which in turn reduces the conductivity of the lead dioxide interface layer and affects the lifespan of the lead-acid battery. Summary of the Invention
[0003] To solve the above-mentioned technical problems, the present invention provides a method for processing the positive grid of a lead-acid battery, wherein the positive grid is placed in a persulfate solution for treatment to obtain the positive grid.
[0004] Further, the positive electrode grid is placed in a persulfate solution with a temperature of 20℃-90℃ and a concentration of 3%-20% for 0-170 minutes to obtain the positive electrode grid.
[0005] Further, the positive electrode grid is placed in a persulfate solution at a temperature of 50℃-70℃ and a concentration of 3%-20% for 2-80 minutes to obtain the positive electrode grid.
[0006] Furthermore, an oxide film is formed on the surface of the positive electrode grid, wherein the inner layer of the oxide film is a dense lead monoxide interface layer and the outer layer of the oxide film is a porous lead dioxide interface layer.
[0007] Furthermore, the positive electrode grid is placed in a persulfate solution with a temperature of 20℃-90℃ and a concentration of 3%-20% for treatment, and the treated positive electrode grid is obtained with an oxide film thickness of 1-3 μm.
[0008] Furthermore, the persulfate solution also includes at least one of the following: carbonates, bicarbonates, phosphates, monohydrogen phosphates, citrates, phthalates, and metaborates, with cations of sodium, potassium, rubidium, cesium, or ammonium ions.
[0009] Furthermore, the persulfate solution is a sodium persulfate solution.
[0010] Furthermore, the concentration of the persulfate solution is 3%-15%.
[0011] This invention also protects a method for preparing a positive electrode plate for a lead-acid battery.
[0012] This invention also protects a method for preparing a lead-acid battery.
[0013] The method for processing the positive grid of the lead-acid battery of the present invention improves the conductivity of the lead dioxide interface layer under the condition of over-discharge during cycling, thus ensuring the life of the lead-acid battery. Attached Figure Description
[0014] Figure 1 The positive electrode grid of the lead-acid battery of the present invention was treated in persulfate solutions of concentrations of 3%, 8%, 15%, and 20% to obtain an interface with a thickness of 2 μm. The relationship between the treatment time and the temperature of the persulfate solution is shown.
[0015] Figure 2 The present invention describes the process of treating the positive electrode grid of a lead-acid battery in a 3% persulfate solution to obtain interfaces with thicknesses of 1µm, 2µm, and 3µm, and the relationship between the treatment time and the temperature of the persulfate solution.
[0016] Figure 3 The present invention describes the process of treating the positive electrode grid of a lead-acid battery in an 8% persulfate solution to obtain interfaces with thicknesses of 1 μm, 2 μm, and 3 μm, and the relationship between the treatment time and the temperature of the persulfate solution.
[0017] Figure 4 A schematic diagram of the positive grid of the lead-acid battery of the present invention obtained by treating it in a persulfate solution. Detailed Implementation
[0018] The present invention will be further described below with reference to specific embodiments.
[0019] The present invention discloses a method for processing the positive electrode grid of a lead-acid battery, wherein the positive electrode grid is placed in a persulfate solution for treatment to obtain a positive electrode grid. An oxide film is formed on the surface of the positive electrode grid, the inner layer of the oxide film is a dense lead monoxide interface layer, and the outer layer of the oxide film is a porous lead dioxide interface layer, with an oxide film thickness of 1-3 μm. Preferably, the concentration of the persulfate solution is 3%-20%, the temperature is 20℃-90℃, and the treatment time is 0-170 minutes. More preferably, the concentration of the sulfate solution is 3%-15%, the temperature is 50℃-70℃, and the treatment time is 2-80 minutes.
[0020] The chemical reaction process of the lead-acid battery positive grid in this invention is as follows: When persulfate reacts with the positive grid, it first oxidizes the metallic lead I in the grid to lead monoxide, and then oxidizes the lead monoxide to lead dioxide. Taking sodium persulfate as an example, the reaction equation is Pb + H₂O + Na₂S₂O₈ = PbO + H₂SO₄ + Na₂SO₄ 4、PbO+H2O+Na2S2O8=PbO2+H2SO4+Na2SO 4。 The overall reaction is Pb + 2H₂O + 2Na₂S₂O₈ == PbO₂ + 2H₂SO₄ + 2Na₂SO₄ 4。 Finally, an oxide film is formed on the surface of the grid, which is the interface layer, such as... Figure 4 As shown, the inner layer of the oxide film is a dense lead monoxide interface layer 2, and the outer layer is a porous lead dioxide interface layer 3, wherein some lead sulfate remains in the pores of the outer porous lead dioxide layer. During the application of the paste, the lead paste is applied onto the porous lead dioxide interface layer 3.
[0021] Other persulfates have similar technical effects, such as potassium persulfate.
[0022] The lead-acid battery of this invention has a lead dioxide interface layer on the outer layer of the positive electrode grid interface, which is generated by a chemical method. Compared with the lead dioxide interface layer generated by an electrochemical method, the lead dioxide interface layer generated by the chemical method has low activity. During discharge, the lead dioxide is unlikely to generate lead sulfate, thus avoiding the decrease in interfacial conductivity caused by lead sulfate. The method for processing the positive electrode grid of the lead-acid battery of this invention also improves the production efficiency of lead-acid batteries.
[0023] Taking a 6-20AH lead-acid battery grid as an example
[0024] Example 1
[0025] Example 1-1
[0026] The grid was immersed in an 8% sodium persulfate solution at 20°C for 30 minutes to obtain an interface layer with a thickness of 1 μm.
[0027] Examples 1-2
[0028] The grid was immersed in an 8% sodium persulfate solution at 20°C for 70 minutes to obtain an interface layer with a thickness of 2 μm.
[0029] Examples 1-3
[0030] The grid was immersed in an 8% sodium persulfate solution at 20°C for 118 minutes to obtain an interface layer with a thickness of 3 μm.
[0031] Example 2
[0032] Example 2-1
[0033] The grid was immersed in an 8% sodium persulfate solution at 40°C for 12 minutes to obtain an interface layer with a thickness of 1 μm.
[0034] Example 2-2
[0035] The grid was immersed in an 8% sodium persulfate solution at 40°C for 31 minutes to obtain an interface layer with a thickness of 2 μm.
[0036] Example 2-3
[0037] The grid was immersed in an 8% sodium persulfate solution at 40°C for 52 minutes to obtain an interface layer with a thickness of 3 μm.
[0038] Example 3
[0039] Example 3-1
[0040] The grid was immersed in an 8% sodium persulfate solution at 50°C for 5 minutes to obtain an interface layer with a thickness of 1 μm.
[0041] Example 3-2
[0042] The grid was immersed in an 8% sodium persulfate solution at 50°C for 12 minutes to obtain an interface layer with a thickness of 2 μm.
[0043] Example 3-3
[0044] The grid was immersed in an 8% sodium persulfate solution at 50°C for 20 minutes to obtain an interface layer with a thickness of 3 μm.
[0045] Example 4
[0046] Example 4-1
[0047] The grid was immersed in an 8% sodium persulfate solution at 60°C for 2 minutes to obtain an interface layer with a thickness of 1 μm.
[0048] Example 4-2
[0049] The grid was immersed in an 8% sodium persulfate solution at 60°C for 7 minutes to obtain an interface layer with a thickness of 2 μm.
[0050] Example 4-3
[0051] The grid was immersed in an 8% sodium persulfate solution at 60°C for 13 minutes to obtain an interface layer with a thickness of 3 μm.
[0052] Example 5
[0053] Example 5-1
[0054] The grid was immersed in an 8% sodium persulfate solution at 70°C for 4 minutes to obtain an interface layer with a thickness of 1 μm.
[0055] Example 5-2
[0056] The grid was immersed in an 8% sodium persulfate solution at 70°C for 8 minutes to obtain an interface layer with a thickness of 2 μm.
[0057] Example 5-3
[0058] The grid was immersed in an 8% sodium persulfate solution at 70°C for 15 minutes to obtain an interface layer with a thickness of 3 μm.
[0059] Example 6
[0060] Example 6-1
[0061] The grid was immersed in an 8% sodium persulfate solution at 80°C for 6 minutes to obtain an interface layer with a thickness of 1 μm.
[0062] Example 6-2
[0063] The grid was immersed in an 8% sodium persulfate solution at 80°C for 20 minutes to obtain an interface layer with a thickness of 2 μm.
[0064] Example 6-3
[0065] The grid was immersed in an 8% sodium persulfate solution at 80°C for 38 minutes to obtain an interface layer with a thickness of 3 μm.
[0066] Example 7
[0067] Example 7-1
[0068] The grid was immersed in an 8% sodium persulfate solution at 90°C for 20 minutes to obtain an interface layer with a thickness of 1 μm.
[0069] Example 7-2
[0070] The grid was immersed in an 8% sodium persulfate solution at 80°C for 48 minutes to obtain an interface layer with a thickness of 2 μm.
[0071] Example 7-3
[0072] The grid was immersed in an 8% sodium persulfate solution at 80°C for 85 minutes to obtain an interface layer with a thickness of 3 μm.
[0073] Example 8
[0074] The grid was immersed in a 15% sodium persulfate solution at 20°C for 88 minutes to obtain an interface layer with a thickness of 2 μm.
[0075] Example 9
[0076] The grid was immersed in a 15% sodium persulfate solution at 40°C for 40 minutes to obtain an interface layer with a thickness of 2 μm.
[0077] Example 10
[0078] The grid was immersed in a 15% sodium persulfate solution at 50°C for 18 minutes to obtain an interface layer with a thickness of 2 μm.
[0079] Example 11
[0080] The grid was immersed in a 15% sodium persulfate solution at 60°C for 5 minutes to obtain an interface layer with a thickness of 2 μm.
[0081] Example 12
[0082] The grid was immersed in a 15% sodium persulfate solution at 70°C for 10 minutes to obtain an interface layer with a thickness of 2 μm.
[0083] Example 13
[0084] The grid was immersed in a 15% sodium persulfate solution at 80°C for 18 minutes to obtain an interface layer with a thickness of 2 μm.
[0085] Example 14
[0086] The grid was immersed in a 15% sodium persulfate solution at 90°C for 58 minutes to obtain an interface layer with a thickness of 2 μm.
[0087] Example 15
[0088] The grid was immersed in a 20% sodium persulfate solution at 20°C for 78 minutes to obtain an interface layer with a thickness of 2 μm.
[0089] Example 16
[0090] The grid was immersed in a 20% sodium persulfate solution at 40°C for 48 minutes to obtain an interface layer with a thickness of 2 μm.
[0091] Example 17
[0092] The grid was immersed in a 20% sodium persulfate solution at 50°C for 21 minutes to obtain an interface layer with a thickness of 2 μm.
[0093] Example 18
[0094] The grid was immersed in a 20% sodium persulfate solution at 60°C for 18 minutes to obtain an interface layer with a thickness of 2 μm.
[0095] Example 19
[0096] The grid was immersed in a 20% sodium persulfate solution at 70°C for 24 minutes to obtain an interface layer with a thickness of 2 μm.
[0097] Example 20
[0098] The grid was immersed in a 20% sodium persulfate solution at 80°C for 34 minutes to obtain an interface layer with a thickness of 2 μm.
[0099] Example 21
[0100] The grid was immersed in a 20% sodium persulfate solution at 90°C for 70 minutes to obtain an interface layer with a thickness of 2 μm.
[0101] Example 22
[0102] Example 22-1
[0103] The grid was immersed in a 3% sodium persulfate solution at 20°C for 40 minutes to obtain an interface layer with a thickness of 1 μm.
[0104] Example 22-2
[0105] The grid was immersed in a 3% sodium persulfate solution at 20°C for 90 minutes to obtain an interface layer with a thickness of 2 μm.
[0106] Example 22-3
[0107] The grid was immersed in a 3% sodium persulfate solution at 20°C for 160 minutes to obtain an interface layer with a thickness of 3 μm.
[0108] Example 23
[0109] Example 23-1
[0110] The grid was immersed in a 3% sodium persulfate solution at 40°C for 30 minutes to obtain an interface layer with a thickness of 1 μm.
[0111] Example 23-2
[0112] The grid was immersed in a 3% sodium persulfate solution at 40°C for 70 minutes to obtain an interface layer with a thickness of 2 μm.
[0113] Example 23-3
[0114] The grid was immersed in a 3% sodium persulfate solution at 40°C for 120 minutes to obtain an interface layer with a thickness of 3 μm.
[0115] Example 24
[0116] Example 24-1
[0117] The grid was immersed in a 3% sodium persulfate solution at 50°C for 20 minutes to obtain an interface layer with a thickness of 1 μm.
[0118] Example 24-2
[0119] The grid was immersed in a 3% sodium persulfate solution at 50°C for 45 minutes to obtain an interface layer with a thickness of 2 μm.
[0120] Example 24-3
[0121] The grid was immersed in a 3% sodium persulfate solution at 50°C for 80 minutes to obtain an interface layer with a thickness of 3 μm.
[0122] Example 25
[0123] Example 25-1
[0124] The grid was immersed in a 3% sodium persulfate solution at 60°C for 11 minutes to obtain an interface layer with a thickness of 1 μm.
[0125] Example 25-2
[0126] The grid was immersed in a 3% sodium persulfate solution at 60°C for 38 minutes to obtain an interface layer with a thickness of 2 μm.
[0127] Example 25-3
[0128] The grid was immersed in a 3% sodium persulfate solution at 60°C for 65 minutes to obtain an interface layer with a thickness of 3 μm.
[0129] Example 26
[0130] Example 26-1
[0131] The grid was immersed in a 3% sodium persulfate solution at 70°C for 10 minutes to obtain an interface layer with a thickness of 1 μm.
[0132] Example 26-2
[0133] The grid was immersed in a 3% sodium persulfate solution at 70°C for 33 minutes to obtain an interface layer with a thickness of 2 μm.
[0134] Example 26-3
[0135] The grid was immersed in a 3% sodium persulfate solution at 70°C for 66 minutes to obtain an interface layer with a thickness of 3 μm.
[0136] Example 27
[0137] Example 27-1
[0138] The grid was immersed in a 3% sodium persulfate solution at 80°C for 20 minutes to obtain an interface layer with a thickness of 1 μm.
[0139] Example 27-2
[0140] The grid was immersed in a 3% sodium persulfate solution at 80°C for 50 minutes to obtain an interface layer with a thickness of 2 μm.
[0141] Example 27-3
[0142] The grid was immersed in a 3% sodium persulfate solution at 80°C for 90 minutes to obtain an interface layer with a thickness of 3 μm.
[0143] Example 28
[0144] Example 28-1
[0145] The grid was immersed in a 3% sodium persulfate solution at 90°C for 40 minutes to obtain an interface layer with a thickness of 1 μm.
[0146] Example 28-2
[0147] The grid was immersed in a 3% sodium persulfate solution at 90°C for 90 minutes to obtain an interface layer with a thickness of 2 μm.
[0148] Example 28-3
[0149] The grid was immersed in a 3% sodium persulfate solution at 90°C for 170 minutes to obtain an interface layer with a thickness of 3 μm.
[0150] After processing the positive electrode grid according to the methods of Embodiments 3-1, 5-1, and 22-1 of this invention, and then preparing the finished batteries according to existing subsequent processes, the resulting batteries are No. 3 12V 20AH finished batteries, No. 5 12V 20AH finished batteries, and No. 22 12V 20AH finished batteries. Compared with the 12V 20AH finished batteries obtained by existing processes without the positive electrode grid processing method of this invention, which instead generate a lead dioxide interface through formation, under the same discharge and charge conditions (charge condition is the existing three-stage charging method, discharge is 10 consecutive over-discharges at 10A to 10V), the test results are as follows:
[0151] For a size 3 battery: First over-discharge to 10V at 10A, discharging 22AH; fully charged, then second over-discharge to 10V at 10A, discharging 21.99AH; fully charged...; fully charged, then tenth over-discharge to 10V at 10A, discharging 21.96AH.
[0152] For a size 9 battery: First over-discharge to 10V at 10A, discharging 22AH; fully charged, then second over-discharge to 10V at 10A, discharging 21.99AH; fully charged...; fully charged, then tenth over-discharge to 10V at 10A, discharging 21.96AH.
[0153] For a size 15 battery: First over-discharge to 10V at 10A, discharging 22AH; fully charged, then second over-discharge to 10V at 10A, discharging 21.98AH; fully charged...; fully charged, then tenth over-discharge to 10V at 10A, discharging 21.95AH.
[0154] The existing technology yields a 12V 20AH battery that, after a first over-discharge at 10A to 10V, releases 22AH; after being fully charged, is then over-discharged again at 10A to 10V, releasing 21.5AH; after being fully charged...; and finally over-discharged again at 10A to 10V, releasing 20AH.
[0155] Furthermore, the over-discharge of this invention refers to the discharge of lead dioxide at the interface, which causes lead sulfate to be generated at the interface during discharge.
[0156] The positive electrode grid of the lead-acid battery of the present invention is preferably a perforated grid.
[0157] In the method for processing the positive grid of the lead-acid battery of the present invention, in order to improve the processing efficiency of the positive grid interface, at least one of carbonates, bicarbonates, phosphates, monohydrogen phosphates, citrates, phthalates, and metaborates with sodium ions, potassium ions, rubidium ions, cesium ions, and ammonium ions can be added to the persulfate solution. The mass percentage of the added salt is preferably between 1% and 25%, so as to maintain a relatively stable pH value of the persulfate solution.
[0158] The present invention also protects a method for preparing a positive electrode plate of a lead-acid battery, which includes applying paste and curing the positive electrode grid obtained by the method for processing the positive electrode grid of the lead-acid battery of the present invention to obtain a positive electrode plate.
[0159] This invention also protects a method for preparing a lead-acid battery, comprising: applying paste and curing a positive electrode grid obtained by the positive electrode grid treatment method of this invention to obtain a positive electrode plate; soaking, coating, placing in a tank, and forming the positive electrode plate to prepare a lead-acid battery; and soaking the positive electrode plate in water or an aqueous solution. The lead-acid battery prepared using the positive electrode grid of this invention, by soaking the positive electrode plate, ensures formation efficiency while avoiding inconsistent α-PbO2 content at different locations at the interface formed during formation due to inconsistent water content inside the positive electrode plate, thus ensuring the lifespan of the lead-acid battery. (Positive electrode plate soaking)
[0160] The lead-acid battery prepared by this invention improves the conductivity of the lead dioxide interface layer under over-discharge conditions, thus ensuring the service life of the lead-acid battery under over-discharge conditions.
[0161] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the present invention in any way. Other variations and modifications are possible without departing from the technical solutions described in the claims.
Claims
1. A method for processing the positive electrode grid of a lead-acid battery, characterized in that, The positive electrode grid is treated in a persulfate solution to obtain the positive electrode grid.
2. The method for processing the positive electrode grid of a lead-acid battery as described in claim 1, characterized in that, include: The positive electrode grid is obtained by placing it in a persulfate solution with a temperature of 20℃-90℃ and a concentration of 3%-20% for 0-170 minutes.
3. The method for processing the positive electrode grid of a lead-acid battery as described in claim 2, characterized in that, The positive electrode grid is obtained by placing it in a persulfate solution with a temperature of 50℃-70℃ and a concentration of 3%-20% for 2-80 minutes.
4. The method for processing the positive electrode grid of a lead-acid battery as described in claim 1, characterized in that, An oxide film is formed on the surface of the positive electrode grid, the inner layer of the oxide film is a dense lead monoxide interface layer, and the outer layer of the oxide film is a porous lead dioxide interface layer.
5. The method for processing the positive electrode grid of a lead-acid battery as described in claim 4, characterized in that, include: The positive electrode grid is placed in a persulfate solution with a temperature of 20℃-90℃ and a concentration of 3%-20% for treatment. The treated positive electrode grid is then removed, and the oxide film thickness is 1-3 μm.
6. A method for processing the positive electrode grid of a lead-acid battery as described in any one of claims 1-5, characterized in that, The persulfate solution also includes at least one of the following: carbonates, bicarbonates, phosphates, monohydrogen phosphates, citrates, phthalates, and metaborates, with cations of sodium, potassium, rubidium, cesium, or ammonium ions.
7. A method for processing the positive electrode grid of a lead-acid battery as described in any one of claims 1-5, characterized in that, The persulfate solution is a sodium persulfate solution.
8. A method for processing the positive electrode grid of a lead-acid battery as described in any one of claims 1-5, characterized in that, The concentration of the persulfate solution is 3%-15%.
9. A method for preparing a positive electrode plate of a lead-acid battery, characterized in that, The positive electrode plate obtained by any one of claims 1-5 is coated with paste and cured to prepare a positive electrode plate.
10. A method for preparing a lead-acid battery, characterized in that, The positive electrode plate prepared according to claim 9 is soaked, coated, placed in a tank, and formed to prepare a lead-acid battery.