A battery cell, a method for manufacturing a battery cell, a battery, and an electric device
By coating the positive electrode active material with organic coating materials, the problem of battery cell performance degradation caused by contact between the positive electrode active material and the electrolyte is solved, the storage and cycle performance of the battery cell is improved, and the cost and process complexity are reduced.
Patent Information
- Application Number
- CN202510584716.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-07
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, direct contact between the positive electrode active material and the electrolyte during the charging and discharging process of a battery cell can affect the cycle performance and storage life of the battery cell. Furthermore, inorganic coating materials are costly and have complex processes.
Organic coating materials are used to coat the positive electrode active material, including functional groups and highly electronegative elements. Through chelation and competitive binding of electronegative elements, side reactions are reduced and the bonding strength between transition metals and oxygen atoms is lowered, thus optimizing lithium ion insertion and extraction.
While minimizing the impact of electrolyte on the performance of positive electrode active materials, this approach reduces the influence of electrolyte on other properties of battery cells, improves storage and cycle performance, and simultaneously reduces costs and simplifies the process.
Smart Images

Figure CN123073035A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a battery cell, a method for preparing the battery cell, a battery, and an electrical device. Background Technology
[0002] During the charging and discharging process of a battery cell, the direct contact between the positive electrode active material and the electrolyte may affect the performance of the positive electrode active material, thereby affecting the cycle performance and storage life of the battery cell.
[0003] While existing solutions can mitigate the impact of contact between the positive electrode active material and the electrolyte on the cycle performance and storage life of battery cells, they may still affect other performance characteristics. Therefore, developing a battery cell that reduces the impact of the electrolyte on the performance of the positive electrode active material while also minimizing its influence on other battery cell performance is a pressing technical challenge. Summary of the Invention
[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide a battery cell, a method for preparing the battery cell, a battery, and an electrical device that can reduce the impact of electrolyte on the performance of positive electrode active material while also reducing the impact on other performance of the battery cell.
[0005] To achieve the above objectives, this application provides a battery cell, a method for preparing the battery cell, a battery, and an electrical device.
[0006] The first aspect of this application provides a battery cell, including a positive electrode sheet, the positive electrode sheet comprising: a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material and an organic coating material, the organic coating material coating at least a portion of the surface of the positive electrode active material; wherein, the organic coating material comprises functional groups and a highly electronegative element; the functional groups comprise at least one of the following: carboxyl group, phosphate group, and the Pauling scale P of the highly electronegative element satisfies: 2.5≤P≤4.0.
[0007] In this embodiment, the functional groups in the molecular structure of the organic coating material are used to chelate with the positive electrode active material. This allows the organic coating material to coordinate with the transition metal on the surface of the positive electrode active material, stabilizing the surface of the positive electrode sheet. This results in a continuous coating of the organic coating material on the surface of the positive electrode active material, reducing side reactions between the electrolyte and the positive electrode active material, and ultimately improving the storage and cycle performance of the battery cell under high temperature and high capacity conditions. Furthermore, the introduction of highly electronegative elements into the molecular structure of the organic coating material reduces the bonding strength between the transition metal and oxygen atoms on the surface of the positive electrode active material, further optimizing the reversible insertion and extraction of lithium ions in the positive electrode active material. Simultaneously, the highly electronegative elements undergo charge transfer during the delithiation process of the positive electrode active material, further improving the storage and cycle performance of the positive electrode sheet. Moreover, organic coating materials are less expensive than inorganic coating materials.
[0008] In any embodiment, the highly electronegative element includes at least one of the following: sulfur, nitrogen, and fluorine.
[0009] In any embodiment, the organic coating material includes thiocarboxylic acids.
[0010] In any embodiment, the organic coating material includes at least one of the following: thioalkylcarboxylic acid, dithioalkylcarboxylic acid, arylthiocarboxylic acid, and aryldithiocarboxylic acid.
[0011] In the embodiments of this application, the carboxyl group and sulfur element in the thiocarboxylic acid can simultaneously reduce the side reactions between the electrolyte and the positive electrode active material, as well as improve the storage performance and cycle performance of the battery cell.
[0012] In any embodiment, the organic coating material includes electron-withdrawing groups and / or electron-donating groups.
[0013] In any embodiment, the organic coating material further includes at least one of the following: ester group, acyl group, cyano group, sulfonic acid group, and amino group.
[0014] Alternatively, the organic coating material may include aminotrimethylenephosphonic acid.
[0015] In the embodiments of this application, electron-withdrawing groups and / or electron-donating groups with highly electronegative elements can also be introduced into the molecular structure of the organic coating material, thereby reducing the bonding strength between the transition metal and oxygen atoms on the surface of the positive electrode active material, thereby further optimizing the reversible insertion and extraction of lithium ions in the positive electrode active material, and improving the storage performance and cycle performance of the positive electrode sheet.
[0016] In any embodiment, the molecular weight M of the organic coating material satisfies: 266 g / mol ≤ M ≤ 660 g / mol.
[0017] In the embodiments of this application, the organic coating material can be a small molecule compound including functional groups and highly electronegative elements, or it can be a macromolecular multi-functional compound including highly electronegative elements and multiple and / or various functional groups. For example, a polycarboxylic acid organic coating material can form multi-site coupling with the transition metal on the surface of the positive electrode active material, resulting in stronger bonding, more robust coating, and greater stability of the organic coating material during the aging process of the battery cell.
[0018] In any embodiment, the mass ratio C of the organic coating material to the positive electrode active material satisfies: 0.5% ≤ C ≤ 1%.
[0019] In the embodiments of this application, the mass ratio of organic coating material to positive electrode active material allows the organic coating material to be better adsorbed onto the surface of the positive electrode active material.
[0020] In any embodiment, the average thickness L of the organic coating material on the positive electrode active material satisfies: 2nm≤L≤2.8nm.
[0021] In the embodiments of this application, the processing technology of organic coating materials is simpler under the same thickness conditions.
[0022] In any embodiment, the positive electrode active material includes at least one of the following: lithium-rich layered oxide, lithium-rich disordered rock salt, and lithium nickel cobalt manganese oxide.
[0023] The second aspect of this application provides a method for preparing a battery cell, comprising: providing an organic coating agent and a positive electrode active material, wherein the organic coating agent includes carboxyl groups and sulfur elements; mixing and stirring the organic coating agent, the positive electrode active material, and a dispersant to obtain a positive electrode active material slurry; subjecting the positive electrode active material slurry to post-processing to obtain a positive electrode active material containing the organic coating material, wherein the post-processing includes any one of the following: spray drying, in-situ coating, and physical precipitation; and using the positive electrode active material containing the organic coating material to prepare a battery cell.
[0024] In this embodiment, because the organic coating agent itself has better adsorption properties, the process for preparing the positive electrode active material containing the organic coating material does not require an additional high-temperature calcination process, thereby reducing the additional energy consumption caused by the high-temperature calcination process. Furthermore, it also reduces the impact of the high-temperature calcination process on the specific capacity of the positive electrode active material. In addition, after the organic coating material forms on the surface of the positive electrode active material, the carboxylic acid in the innermost molecular structure of the organic coating material will preemptively consume residual alkali and other impurities in the outer layer of the positive electrode active particles, ultimately remaining on the surface of the positive electrode active material in the form of lithium salt. This can reduce gelation and gas generation phenomena during the production of the positive electrode sheet, improving the reliability of the battery cell's life cycle.
[0025] A third aspect of this application provides a battery, including a battery cell according to the first aspect of this application and a battery cell prepared according to the preparation method of the second aspect of this application.
[0026] A fourth aspect of this application provides an electrical device, including a battery cell of the first aspect of this application, a battery cell prepared according to the preparation method of the second aspect of this application, and / or a battery of the third aspect of this application. Attached Figure Description
[0027] Figure 1 This is a schematic diagram of the positive electrode sheet according to one embodiment of this application.
[0028] Figure 2 This is a schematic diagram of a method for preparing a battery cell according to an embodiment of this application.
[0029] Figure 3 This is a schematic diagram of a battery cell according to one embodiment of this application.
[0030] Figure 4 This is a schematic diagram of a battery module according to one embodiment of this application.
[0031] Figure 5 This is a schematic diagram of a battery according to one embodiment of this application.
[0032] Figure 6 yes Figure 5 An exploded view of a battery according to one embodiment of this application is shown.
[0033] Figure 7 This is a schematic diagram of an electrical device in which a single battery cell is used as a power source according to one embodiment of this application.
[0034] Figure 8 This is a schematic diagram of the 25°C cycle performance test results in Embodiment 1 and Comparative Example 1 of this application.
[0035] Figure 9 This is a schematic diagram of the 60°C high-temperature storage performance test results in Embodiment 1 and Comparative Example 1 of this application.
[0036] Figure 10 This is a schematic diagram of the internal resistance growth rate test results during storage at 60°C in Embodiment 1 and Comparative Example 1 of this application.
[0037] Figure 11 This is a schematic diagram of the transmission electron microscope energy dispersive spectroscopy and scanning electron microscope energy dispersive spectroscopy test results in Embodiment 1 of this application.
[0038] Explanation of reference numerals in the attached figures:
[0039] 1 Battery; 2 Upper casing; 3 Lower casing; 4 Battery module; 5 Battery cell; 6 Positive electrode sheet; 61 Positive current collector; 62 Positive active material layer. Detailed Implementation
[0040] The following detailed description, with appropriate reference to the accompanying drawings, specifically discloses embodiments of the electrode plates, battery cells, battery modules, batteries, and power-consuming devices of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0041] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0042] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0043] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0044] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0045] During the research on the performance of battery cells, the applicant discovered that in battery cells containing high specific capacity positive electrode active materials (or lithium-rich positive electrode active materials), the layered phase of the positive electrode sheet may change due to direct contact with the electrolyte during charging and discharging. This may lead to material loss of the positive electrode sheet and voltage decay of the battery cell, and may also cause transition metal ions in the positive electrode sheet to escape, thereby damaging the SEI film of the negative electrode sheet, increasing lithium consumption of the battery cell, and thus affecting the cycle performance and storage life of the battery cell.
[0046] In related solutions, inorganic coating materials are typically used to coat the positive electrode active material, thereby avoiding direct contact between the positive electrode active material and the electrolyte, reducing side reactions and dissolution of transition metals by the electrolyte on the surface of the positive electrode active material. However, inorganic coating materials are expensive, and the coating process is complex, requiring a high-temperature calcination step. Furthermore, the high-temperature calcination step can also affect the capacity performance of the positive electrode active material.
[0047] In view of this, embodiments of this application provide a battery cell including a positive electrode sheet, the positive electrode sheet comprising: a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material and an organic coating material, the organic coating material covering at least a portion of the surface of the positive electrode active material; wherein, the organic coating material comprises functional groups and a highly electronegative element; the functional groups include at least one of the following: carboxyl groups, phosphate groups, and the Pauling scale P of the highly electronegative element satisfies: 2.5 ≤ P ≤ 4.0. Thus, while reducing the influence of the electrolyte on the performance of the positive electrode active material, it is also possible to reduce the impact on other performance characteristics of the battery cell.
[0048] [Battery cell]
[0049] In one embodiment of this application, a battery cell 5 is provided. The battery cell 5 includes a positive electrode 6.
[0050] Figure 1This is a schematic diagram of the structure of the positive electrode 6 according to this application. The positive electrode 6 includes a positive current collector 61 and a positive active material layer 62, the positive active material layer 62 being disposed on the surface of the positive current collector 61; the positive active material layer 62 includes a positive active material and an organic coating material, the organic coating material covering at least a portion of the surface of the positive active material; wherein, the organic coating material includes functional groups and highly electronegative elements; the functional groups include at least one of the following: carboxyl groups, phosphate groups, and the Pauling scale P of the highly electronegative elements satisfies: 2.5 ≤ P ≤ 4.0.
[0051] P can be 2.5, 2.58, 3.0, 3.5, 4.0, or any value within the above range.
[0052] For example, the organic coating material can be an organic compound containing carboxyl groups and sulfur, a polycarboxylic acid organic compound containing sulfur and multiple carboxyl groups, or a polymer containing sulfur and one or more carboxyl groups. Furthermore, the organic coating material can also be an isomer of an organic compound containing the same type and number of sulfur-containing groups and the same type and number of carboxyl groups.
[0053] Specifically, the organic coating material includes highly electronegative elements, which can be elements corresponding to one or more atoms in the molecular structure of the organic coating material, or elements contained in one or more groups in the molecular structure of the organic coating material.
[0054] Specifically, the positive electrode active material layer 62 is disposed on at least one side of the surface of the positive electrode current collector 61. As an example, the positive electrode current collector 61 may have two surfaces opposite each other in its own thickness direction, and the positive electrode active material layer 62 is disposed on either or both of the two opposite surfaces of the positive electrode current collector 61.
[0055] Specifically, the organic coating material coats at least a portion of the surface of the positive electrode active material. This can be either the organic coating material partially surrounding the surface of the positive electrode active material, or the organic coating material completely encapsulating all surfaces of the positive electrode active material. As an example, in the first positive electrode active material layer 62, there can be both a positive electrode active material partially surrounded by the organic coating material and a positive electrode active material completely encapsulated by the organic coating material, or only a positive electrode active material partially surrounded by the organic coating material, or only a positive electrode active material completely encapsulated by the organic coating material.
[0056] The functional groups (e.g., carboxyl groups) in the molecular structure of the organic coating material can chelate with the transition metals on the surface of the positive electrode active material, thereby further strengthening the anchoring effect between the positive electrode active material particles and the organic coating material. This allows the organic coating material to effectively isolate the positive electrode interface and the electrolyte. The highly electronegative elements (e.g., sulfur) in the molecular structure of the organic coating material have high electronegativity, allowing them to compete with oxygen atoms in the positive electrode active material for bonding with metal atoms. This inhibits the formation of metal oxides, reduces the bonding strength between the transition metal and oxygen atoms on the surface of the positive electrode active material, and consequently reduces the oxidation depth of lattice oxygen in the positive electrode active material during cell aging. This inhibits the migration of oxygen atoms or molecules within the positive electrode active material, ultimately reducing the mixing of metal ions in the positive electrode active material, improving its structural stability, and further optimizing the reversible insertion and extraction of lithium ions in the positive electrode active material.
[0057] In this embodiment, the functional groups in the molecular structure of the organic coating material are used to chelate with the positive electrode active material. This allows the organic coating material to coordinate with the transition metal on the surface of the positive electrode active material, stabilizing the surface of the positive electrode sheet. This results in a continuous coating of the organic coating material on the surface of the positive electrode active material, reducing side reactions between the electrolyte and the positive electrode active material, and ultimately improving the storage and cycle performance of the battery cell under high temperature and high capacity conditions. Furthermore, the introduction of highly electronegative elements into the molecular structure of the organic coating material reduces the bonding strength between the transition metal and oxygen atoms on the surface of the positive electrode active material, further optimizing the reversible insertion and extraction of lithium ions in the positive electrode active material. Simultaneously, the highly electronegative elements undergo charge transfer during the delithiation process of the positive electrode active material, further improving the storage and cycle performance of the positive electrode sheet. Moreover, organic coating materials are less expensive than inorganic coating materials.
[0058] Optionally, highly electronegative elements include at least one of the following: sulfur, nitrogen, and fluorine.
[0059] In some embodiments, the organic coating material includes thiocarboxylic acids.
[0060] It is understandable that thiocarboxylic acids include a carboxyl group and a sulfur element.
[0061] In one possible scenario, the organic coating material may include a thioalkyl carboxylic acid. As an example, the organic coating material may include at least one of the following: a thioalkyl carboxylic acid or a dithioalkyl carboxylic acid. Further, the thioalkyl carboxylic acid (such as acetic acid, propionic acid, or butyric acid) may be a monothioalkyl carboxylic acid, a dithioalkyl carboxylic acid, and / or a polythioalkyl carboxylic acid containing a coordinating group. For example, the organic coating material may be thiosuccinic acid.
[0062] In another possible scenario, the organic coating material may include aryl thiocarboxylic acids. As an example, the organic coating material may include at least one of the following: aryl thiocarboxylic acids, aryl dithiocarboxylic acids. Further, the aryl thiocarboxylic acids (such as acetic acid, propionic acid, butyric acid) may be monoaryl thiocarboxylic acids, diaryl thiocarboxylic acids, and / or polyaryl thiocarboxylic acids containing a coordinating group.
[0063] In the embodiments of this application, the carboxyl group and sulfur element in the thiocarboxylic acid can simultaneously reduce the side reactions between the electrolyte and the positive electrode active material, as well as improve the storage performance and cycle performance of the battery cell.
[0064] In some embodiments, the organic coating material includes electron-withdrawing groups and / or electron-donating groups.
[0065] It is understandable that both electron-withdrawing and electron-donating groups are groups of elements with high electronegativity.
[0066] Specifically, organic coating materials can be organic compounds that simultaneously include highly electronegative elements, one or more functional groups, and one or more electron-withdrawing and / or electron-donating groups, or organic compounds that simultaneously include one or more functional groups and one or more electron-withdrawing and / or electron-donating groups. Furthermore, organic coating materials can be polymers that simultaneously include highly electronegative elements, one or more functional groups, and one or more electron-withdrawing and / or electron-donating groups, or polymers that simultaneously include one or more functional groups and one or more electron-withdrawing and / or electron-donating groups.
[0067] In the embodiments of this application, electron-withdrawing groups and / or electron-donating groups with highly electronegative elements can also be introduced into the molecular structure of the organic coating material, thereby reducing the bonding strength between the transition metal and oxygen atoms on the surface of the positive electrode active material, thereby further optimizing the reversible insertion and extraction of lithium ions in the positive electrode active material, and improving the storage performance and cycle performance of the positive electrode sheet.
[0068] In some embodiments, the organic coating material further includes at least one of the following: ester group, acyl group, cyano group, sulfonic acid group, and amino group.
[0069] Specifically, the organic coating material can be an organic compound that simultaneously includes one or more functional groups and one or more electron-withdrawing and / or electron-donating groups (i.e., ester, acyl, cyano, sulfonic acid, amino groups), or an organic compound that simultaneously includes a highly electronegative element, one or more functional groups, and one or more electron-withdrawing and / or electron-donating groups (i.e., ester, acyl, cyano, sulfonic acid, amino groups). Furthermore, the organic coating material can be a polymer that simultaneously includes one or more functional groups and one or more electron-withdrawing and / or electron-donating groups (i.e., ester, acyl, cyano, sulfonic acid, amino groups), or a polymer that simultaneously includes a highly electronegative element, one or more functional groups, and one or more electron-withdrawing and / or electron-donating groups (i.e., ester, acyl, cyano, sulfonic acid, amino groups). For example, the organic coating material can be aminotrimethylenephosphonic acid.
[0070] In the embodiments of this application, electron-withdrawing groups and / or electron-donating groups with highly electronegative elements can also be introduced into the molecular structure of the organic coating material, thereby reducing the bonding strength between the transition metal and oxygen atoms on the surface of the positive electrode active material, thereby further optimizing the reversible insertion and extraction of lithium ions in the positive electrode active material, and improving the storage performance and cycle performance of the positive electrode sheet.
[0071] In some embodiments, the molecular weight M of the organic coating material satisfies: 266 g / mol ≤ M ≤ 660 g / mol.
[0072] M can be 266 g / mol, 299 g / mol, 300 g / mol, 350 g / mol, 400 g / mol, 450 g / mol, 500 g / mol, 550 g / mol, 600 g / mol, 650 g / mol, 660 g / mol or any value within the above range.
[0073] In the embodiments of this application, the organic coating material can be a small molecule compound including functional groups and highly electronegative elements, or it can be a macromolecular multi-functional compound including highly electronegative elements and multiple and / or various functional groups. For example, a polycarboxylic acid organic coating material can form multi-site coupling with the transition metal on the surface of the positive electrode active material, resulting in stronger bonding, more robust coating, and greater stability of the organic coating material during the aging process of the battery cell.
[0074] In some embodiments, the mass ratio C of the organic coating material to the positive electrode active material satisfies: 0.5% ≤ C ≤ 1%.
[0075] C can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, or any value within the above range.
[0076] In the embodiments of this application, the mass ratio of organic coating material to positive electrode active material allows the organic coating material to be better adsorbed onto the surface of the positive electrode active material.
[0077] In some implementations, the average thickness L of the organic coating material on the positive electrode active material satisfies: 2nm ≤ L ≤ 2.8nm.
[0078] L can be 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, or any value within the above range.
[0079] In the embodiments of this application, the processing technology of organic coating materials is simpler under the same thickness conditions.
[0080] In some embodiments, the positive electrode active material includes at least one of the following: lithium-rich layered oxide, lithium-rich disordered rock salt, and lithium nickel cobalt manganese oxide.
[0081] [Preparation methods for battery cells]
[0082] Figure 2 This is a schematic diagram of a method 200 for preparing a battery cell according to an embodiment of this application. (In conjunction with...) Figure 2 As shown, the method 200 for preparing a single battery cell may include the following steps.
[0083] S210 provides an organic coating agent and a positive electrode active material. The organic coating agent includes functional groups and highly electronegative elements. The functional groups include at least one of the following: carboxyl group, phosphate group, and the Pauling scale P of the highly electronegative elements satisfies: 2.5≤P≤4.0.
[0084] It should be noted that the composition of the organic coating agent is the same as that of the organic coating material in battery cell 5 in the above embodiments, and will not be repeated here.
[0085] S220 involves mixing and stirring an organic coating agent, a positive electrode active material, and a dispersant to obtain a positive electrode active material slurry.
[0086] Specifically, a dispersant is a substance used to optimize the viscosity of the positive electrode active material slurry, improve the dispersion uniformity of the organic coating agent and the positive electrode active material, and reduce particle agglomeration. For example, the dispersant may be N-methylpyrrolidone (NMP).
[0087] S230, post-processing the positive electrode active material slurry to obtain a positive electrode active material containing organic coating material, the post-processing including any one of the following: spray drying, in-situ coating, physical precipitation.
[0088] As an example, by spray drying, in-situ coating or physical precipitation of the positive electrode active material slurry, a positive electrode active material containing organic coating material can be directly obtained.
[0089] S240 uses a positive electrode active material containing an organic coating material to prepare a battery cell.
[0090] As an example, the positive electrode active material containing the organic coating material prepared above is used to prepare the positive electrode active material layer of the positive electrode sheet, and then the positive electrode sheet containing the positive electrode active material layer is used to prepare a battery cell.
[0091] In this embodiment, because the organic coating agent itself has better adsorption properties, the process for preparing the positive electrode active material containing the organic coating material does not require an additional high-temperature calcination process, thereby reducing the additional energy consumption caused by the high-temperature calcination process. Furthermore, it also reduces the impact of the high-temperature calcination process on the specific capacity of the positive electrode active material. In addition, after the organic coating material forms on the surface of the positive electrode active material, the carboxylic acid in the innermost molecular structure of the organic coating material will preemptively consume residual alkali and other impurities in the outer layer of the positive electrode active particles, ultimately remaining on the surface of the positive electrode active material in the form of lithium salt. This can reduce gelation and gas generation phenomena during the production of the positive electrode sheet, improving the reliability of the battery cell's life cycle.
[0092] In some embodiments, the battery cell preparation method 200 is used to prepare battery cell 5.
[0093] In addition, the battery cell, battery module, battery and power device of this application will be described below with appropriate reference to the accompanying drawings.
[0094] Typically, a battery cell includes a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor of ions between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.
[0095] [Positive electrode plate]
[0096] The positive electrode includes a positive current collector and a layer of positive active material disposed on the positive current collector. The positive electrode can be the positive electrode 6 described above.
[0097] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0098] In some embodiments, the positive electrode active material layer may employ positive electrode active materials known in the art for use in batteries. As an example, the positive electrode active material may include at least one of the following materials: lithium phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (such as LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi) 0.85 Co 0.15 Al 0.05 At least one of O2 and its modified compounds. Examples of lithium phosphates with an olivine structure include, but are not limited to, lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.
[0099] In some embodiments, the positive electrode active material layer may optionally include a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0100] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0101] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned positive electrode active material containing organic coating material, conductive agent, binder and any other components in a solvent (e.g. N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0102] [Negative electrode plate]
[0103] The negative electrode includes a negative current collector and a negative electrode film layer disposed on the negative current collector.
[0104] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. The negative electrode current collector may be copper foil. The composite negative electrode current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0105] In some embodiments, the negative electrode film layer includes a negative electrode active material. The negative electrode active material may be any negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include one or more of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material may be selected from one or more of elemental silicon, silicon-oxygen compounds, silicon-carbon compounds, silicon-nitrogen compounds, and silicon alloys. The tin-based material may be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0106] In some embodiments, the negative electrode film layer may optionally include a binder. As an example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.
[0107] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0108] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0109] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode film, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.
[0110] [Electrolytes]
[0111] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.
[0112] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0113] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.
[0114] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0115] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0116] [Isolation membrane]
[0117] In some embodiments, the battery cell also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0118] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0119] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0120] In some embodiments, the battery cell may include an outer packaging. This outer packaging can be used to encapsulate the electrode assembly and electrolyte described above.
[0121] In some embodiments, the outer packaging of the battery cell can be a rigid shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the battery cell can also be a flexible package, such as a pouch. The material of the flexible package can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0122] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 3 The battery cell 5 is used as an example. Battery cell 5 may include a housing. A positive electrode, a negative electrode, and a separator may be formed into an electrode assembly via a winding or stacking process. The electrode assembly is encapsulated within the housing. An electrolyte is immersed in the electrode assembly. The number of electrode assemblies contained in battery cell 5 may be one or more, which can be selected by those skilled in the art according to specific practical needs.
[0123] In some implementations, individual battery cells can be assembled into a battery module. The number of individual battery cells contained in a battery module can be one or more, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery module.
[0124] Figure 4 This is battery module 4, used as an example. (See reference...) Figure 4 In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.
[0125] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.
[0126] In some embodiments, the battery modules described above can also be assembled into a battery. The number of battery modules contained in the battery can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery.
[0127] Figure 5 and Figure 6 This is battery 1 as an example. (See reference...) Figure 5 and Figure 6 The battery 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0128] In addition, this application also provides an electrical device, which includes at least one of the battery cell, battery module, or battery provided in this application. The battery cell, battery module, or battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0129] As the electrical device, a single battery cell, a battery module, or a battery can be selected according to its usage requirements.
[0130] Figure 7 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of individual battery cells, batteries or battery modules can be used.
[0131] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a single battery cell as their power source.
[0132] [Example]
[0133] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0134] Example 1
[0135] (1) Preparation of positive electrode sheet
[0136] I. Preparation of positive electrode active materials containing organic coating materials
[0137] Provides thiosuccinic acid and positive electrode active material Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2 was used to disperse thiosuccinic acid at 1% of the mass of the positive electrode active material in N-methylpyrrolidone (NMP) solvent, followed by mixing and stirring to obtain a positive electrode active material slurry. The prepared positive electrode active material slurry was then spray-dried at an inlet air temperature of 160–220°C and a flow rate of 30 L / min. The powder obtained from the spray drying was further dried to completely evaporate any residual solvent, and then sieved through a 300–600 mesh screen to remove large particles or impurities, yielding a positive electrode active material containing an organic coating.
[0138] II. Preparation of Positive Electrode Slurry
[0139] The above-prepared positive electrode active material containing organic coating material, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) were dissolved in solvent N-methylpyrrolidone (NMP) at a weight ratio of 97:1.5:1.5. The mixture was stirred and mixed at a speed of 400 r / s-1000 r / s, and then wetted, kneaded and dispersed to obtain positive electrode slurry.
[0140] III. Preparation of Positive Electrode Sheet
[0141] The prepared positive electrode slurry was uniformly coated onto an aluminum foil current collector and dried at 80℃-150℃, with the water content controlled to be less than 150ppm. After cold pressing and slitting, the positive electrode sheet was obtained.
[0142] (2) Preparation of negative electrode sheet
[0143] The negative electrode active material graphite, conductive agent acetylene black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are dissolved in deionized water at a mass ratio of 96:1:1:2 and thoroughly mixed to prepare a negative electrode slurry. The negative electrode slurry is coated onto the negative electrode current collector copper foil, and then dried, cold-pressed, and slit to obtain the negative electrode sheet.
[0144] (3) Separating membrane
[0145] Polyethylene film was selected as the separator.
[0146] (4) Electrolyte
[0147] Ethyl carbonate (EC), methyl ethyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1, and then LiPF6 was uniformly dissolved in the above solution at a concentration of 1 mol / L to obtain the electrolyte.
[0148] (5) Preparation of battery cells
[0149] The positive electrode, separator, and negative electrode are arranged in the order of "separator—negative electrode—separator—positive electrode," so that the separator acts as a barrier between the positive and negative electrodes. One end of the positive electrode, negative electrode, and two separators is fixed to the discharge roller, and the other end is stacked together and fixed to the winding shaft. A motor is used to rotate the winding shaft to wind the positive electrode, negative electrode, and two separators. After baking, electrolyte injection, and formation, a single battery cell is obtained.
[0150] Example 2
[0151] The difference between Example 2 and Example 1 is that the mass ratio of the positive electrode active material coating material to the positive electrode active material is different, and the average thickness of the positive electrode active material coating material on the positive electrode active material is different.
[0152] Example 3
[0153] The difference between Example 3 and Example 1 is that the positive electrode active material is LiNi. 0.6 Co 0.2 Mn 0.2 O2.
[0154] Example 4
[0155] The difference between Example 4 and Example 1 is that the positive electrode active material coating material also includes amino groups.
[0156] Example 5
[0157] The difference between Example 4 and Example 1 is that the positive electrode active material coating material also includes phosphate groups.
[0158] Comparative Example 1
[0159] The difference between Comparative Example 1 and Example 1 is that the positive electrode active material coating material is an inorganic coating material.
[0160] The specific parameters of the battery cells in Examples 1-5 and Comparative Example 1 are shown in Table 1 below.
[0161] Table 1: Specific parameters of Examples 1-5 and Comparative Example 1
[0162] In addition, the battery cells in Examples 1-5 and Comparative Example 1 were subjected to performance tests. The test results are shown in Tables 2-3 below. Figure 8-11 As shown.
[0163] Table 2: Battery cell performance test results of Examples 1-5 and Comparative Example 1
[0164] Table 3: Trace element analysis results of the negative electrode sheets of Examples 1-2 and Comparative Example 1
[0165] Combined with Examples 1-3 and Comparative Example 1, as shown in Table 2 and Figure 8-10 As shown, compared to Comparative Example 1, in Examples 1-3, when the positive electrode active material coating material is thiosuccinic acid, an organic coating material containing sulfur (a highly electronegative element) and carboxyl groups, the cycle capacity retention and storage capacity retention of the battery cells are slightly higher than those of the battery cells with aluminum fluoride, an inorganic coating material, as the positive electrode active material coating material. As an example, compared to Comparative Example 1, Example 1 showed a 0.8% increase in cycle capacity retention at 250 cycles and a 5.9% increase in storage capacity retention at 60 days. This indicates that the cycle performance and storage performance of the positive electrode active material coated with an organic coating material including carboxyl groups and sulfur (a highly electronegative element) are improved. Furthermore, as... Figure 10 As shown, the DCR growth rate of Comparative Example 1 after 30 days of storage at 60°C was 23.4%, while the DCR growth rate of Example 1 was only 4.8%. This indicates that the coating of organic coating materials including carboxyl groups and sulfur elements (high electronegativity elements) greatly improves the stability of the positive electrode main material.
[0166] Combined with Examples 1-2 and Comparative Example 1, as shown in Table 3, the amounts of various transition metals on the negative electrode sheets of Examples 1-2 are all less than those of Comparative Example 1. For example, compared with Comparative Example 1, the Mn content in the negative electrode sheet of Example 1 is reduced from 340 ppm to 126 ppm. This indicates that the organic coating material including carboxyl groups and sulfur effectively binds the transition metals released from the positive electrode active material during the high-pressure and high-temperature storage of the battery cell, inhibits the migration of transition metals to the negative electrode sheet, reduces the damage of transition metals to the SEI film on the surface of the negative electrode sheet, and thus extends the long-term service life of the battery cell.
[0167] Combined with Example 1 and Figure 11 As shown, a battery cell made by coating the positive electrode active material with an organic coating material including carboxyl groups and sulfur elements, after undergoing 120 days of high-temperature and high-pressure storage at 60°C, exhibits the following transmission electron microscopy (TEM) energy dispersive spectroscopy (EDS) of the positive electrode sheet. Figure 11 a) and scanning electron microscopy energy dispersive spectroscopy ( Figure 11 b) Sulfur content of approximately 1600 ppm can be detected in both, thus proving that under high temperature and high pressure, the organic coating material including carboxyl groups and sulfur elements did not decompose or oxidize, but remained stable in the positive electrode structure.
[0168] [Testing methods for individual battery cell parameters]
[0169] The battery cells being tested can be either freshly assembled and unformed, or they can be battery cells removed from electrical devices (such as vehicles).
[0170] (1) Testing of the 25℃ cycle performance of individual battery cells
[0171] The prepared battery cells were charged at a constant current of 0.5C to the upper limit cutoff voltage of 4.4V, then charged at a constant voltage of 4.4V until the current ≤0.05C. After resting for 5 minutes, they were discharged at 0.5C to 2.5V. The resulting capacity was recorded as the initial capacity C0. The above steps were repeated for the prepared battery cells, and the discharge capacity C of the battery after the nth cycle was recorded. n Then, the battery cell capacity retention rate after each cycle = C n / C0×100%, with the battery cell capacity retention rate as the vertical axis and the corresponding cycle number as the horizontal axis, a curve of battery cell capacity retention rate versus cycle number is obtained.
[0172] (2) Testing of the storage capacity retention rate of individual battery cells at 60℃
[0173] ① Charge the prepared battery cells at a constant current of 1 / 3C to 4.4V, then charge them at a constant voltage of 4.4V until the current ≤0.05C, let them stand for 5 minutes, and then discharge them at 1 / 3C to 2.5V. Repeat this process twice and record the second discharge capacity D0. ② Charge the prepared battery cells at a constant current of 1 / 3C to 4.4V, then charge them at a constant voltage of 4.4V until the current ≤0.05C, and then store them in a constant temperature environment at 60℃ for a specified number of days. ③ Discharge them at 1 / 3C to 2.5V, let them stand for 5 minutes, then charge them at a constant voltage of 4.4V until the current ≤0.05C, let them rest for 5 minutes, and then discharge them at 1 / 3C to 2.5V. Record the capacity as D. n D n Divide by the value of D0 as the cell capacity retention rate on day n of high-temperature storage, to characterize the degree of capacity decay of the battery during high-temperature storage; ④ Repeat steps ② and ③.
[0174] (3) Test of the growth rate of internal resistance (DCR) of individual cells during storage at 60℃
[0175] After the initial capacity C0 test is completed, ① charge the battery at a constant current of 1 / 3C to 4.4V, then charge it at a constant voltage of 4.4V until the current ≤0.05C, let it stand for 30 minutes, and then discharge it at 0.33C to 0.5C0; ② let it rest for 60 minutes, then discharge it at 4.0C for 30 seconds, and extract the 30-second discharge DCR data. Record the impedance value before storage as DCR0. After storing for a specified number of days, repeat the above steps for the same battery, and simultaneously record the discharge impedance of the battery on the m-th day of storage as DCR. m Then the DCR growth rate after battery storage = (DCR) m -DCR0) / DCR0×100%.
[0176] (4) Trace element analysis of negative electrode sheet
[0177] Inductively coupled plasma atomic emission spectrometry (ICP) was used to determine trace elements in the negative electrode sheet. The negative electrode sheet to be tested was taken, ground, dissolved in concentrated nitric acid, and microwave-digested to form a clear solution. Particulate matter was removed by filtration or the solution was directly diluted to a suitable concentration before injection for testing. The trace element content (mass fraction w / w%) = element mass / (sample weight - current collector mass) * 100%.
[0178] (5) Scanning electron microscopy (SEM) / transmission electron microscopy (TEM) energy dispersive spectroscopy
[0179] The surface elemental analysis of the negative electrode sheet was performed using a Sigma 300 cryo-electron microscope and a Thermo Scientific-Talos F200S G2 transmission electron microscope in accordance with the GB / T17359-2012 standard.
[0180] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A battery cell, characterized in that, Includes a positive electrode plate, wherein the positive electrode plate comprises: A positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material and an organic coating material, wherein the organic coating material coats at least a portion of the surface of the positive electrode active material; The organic coating material includes functional groups and highly electronegative elements; The functional group includes at least one of the following: carboxyl group, phosphate group, and the Pauling scale P of the highly electronegative element satisfies: 2.5≤P≤4.
0.
2. The battery cell according to claim 1, characterized in that, The highly electronegative elements include at least one of the following: sulfur, nitrogen, and fluorine.
3. The battery cell according to claim 1 or 2, characterized in that, The organic coating material includes thiocarboxylic acids.
4. The battery cell according to any one of claims 1-3, characterized in that, The organic coating material includes at least one of the following: thioalkylcarboxylic acid, dithioalkylcarboxylic acid, arylthiocarboxylic acid, and aryldithiocarboxylic acid.
5. The battery cell according to any one of claims 1-4, characterized in that, The organic coating material includes electron-withdrawing groups and / or electron-donating groups.
6. The battery cell according to any one of claims 1-5, characterized in that, The organic coating material includes at least one of the following: ester group, acyl group, cyano group, sulfonic acid group, and amino group.
7. The battery cell according to any one of claims 1-6, characterized in that, The organic coating material includes aminotrimethylenephosphonic acid.
8. The battery cell according to any one of claims 1-7, characterized in that, The molecular weight M of the organic coating material satisfies: 266 g / mol ≤ M ≤ 660 g / mol.
9. The battery cell according to any one of claims 1-8, characterized in that, The mass ratio C of the organic coating material to the positive electrode active material satisfies: 0.5% ≤ C ≤ 1%.
10. The battery cell according to any one of claims 1-9, characterized in that, The average thickness L of the organic coating material on the positive electrode active material satisfies: 2nm≤L≤2.8nm.
11. The battery cell according to any one of claims 1-10, characterized in that, The positive electrode active material includes at least one of the following: lithium-rich layered oxide, lithium-rich disordered rock salt, and lithium nickel cobalt manganese oxide.
12. A method for preparing a single battery cell, characterized in that, The preparation method includes: An organic coating agent and a positive electrode active material are provided. The organic coating agent includes functional groups and a highly electronegative element. The functional groups include at least one of the following: carboxyl group and phosphate group. The Pauling scale P of the highly electronegative element satisfies: 2.5 ≤ P ≤ 4.
0. The organic coating agent, the positive electrode active material, and the dispersant are mixed and stirred to obtain a positive electrode active material slurry; The positive electrode active material slurry is post-processed to obtain the positive electrode active material containing organic coating material. The post-processing includes any one of the following: spray drying, in-situ coating, and physical precipitation. The battery cell is prepared using the positive electrode active material containing the organic coating material.
13. A battery, characterized in that, It includes at least one of the following: a battery cell according to any one of claims 1-11, or a battery cell prepared by the preparation method according to claim 12.
14. An electrical appliance, characterized in that, It includes at least one of the following: a battery cell according to any one of claims 1-11, a battery cell prepared by the preparation method according to claim 12, and a battery according to claim 13.