Composite current collector, secondary battery, and electric device
By introducing a first polymer layer containing composite particles and a binder, and a second polymer layer with silicon-oxygen bonds connected to a metal layer in the composite current collector, the problems of easy delamination of the current collector under stress and migration of flame-retardant materials are solved, and the high conductivity, stability and safety are improved.
Patent Information
- Application Number
- CN202611342768.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-10
AI Technical Summary
Existing composite current collectors are prone to delamination and detachment under mechanical, thermal, and electrical stress, leading to internal short circuits and thermal runaway. Furthermore, flame-retardant materials migrate and precipitate within the polymer material layer, affecting the safety and performance of the secondary battery.
The composite current collector structure includes a first polymer layer, a metal layer, and a second polymer layer. The first polymer layer contains composite particles and a binder, and the second polymer layer has silicon-oxygen bonds and is connected to the metal layer through Si-OM chemical bonds. The metal-organic framework material serves as a carrier for the flame retardant material, which disintegrates at high temperatures to release the flame retardant material and form a solid-phase heat insulation layer.
The composite current collector improves conductivity, interfacial bonding stability, and safety. Through the synergistic fire suppression of flame spread and heat transfer via flame-retardant barriers and solid-phase insulation layers, it enhances the safety performance of the secondary battery.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application relates to the field of electrochemical energy storage technology, specifically to a composite current collector, a secondary battery, and an electrical device. Background Technology
[0002] With the continuous development and large-scale application of the battery industry, people have increasingly higher requirements for the mass density, lightweight, and safety of rechargeable batteries. This necessitates battery manufacturers to optimize and improve various components of rechargeable batteries to enhance their performance. As one of the core components of a rechargeable battery, the performance of the current collector directly affects the overall battery performance. Traditionally, rechargeable batteries use metal current collectors. Metal current collector batteries are prone to internal short circuits when subjected to mechanical stress (especially extrusion, puncture, and impact), thermal stress, or electrical stress, leading to thermal runaway and safety accidents. Therefore, improving the mechanical properties of the current collector and endowing it with flame-retardant properties are effective means to reduce internal short circuits and prevent thermal runaway.
[0003] In the prior art, composite current collectors with a "sandwich" structure (metal layer + polymer material layer + metal layer) have been invented to improve the mechanical properties of current collectors and impart flame retardant properties. However, commonly used polymer materials are insulating materials, which leads to poor electron conduction paths and significantly higher sheet resistance than traditional metal foils, affecting the rate performance of secondary batteries. Secondly, the polymer material layer and the metal layer are mainly bonded by physical adsorption, which makes them prone to delamination and detachment under volume changes and thermal stress during the charging and discharging process of secondary batteries. Thirdly, flame retardant materials added to improve safety are prone to migrate and precipitate in the polymer material layer, resulting in a decrease in flame retardant effect after long-term storage or repeated use.
[0004] Therefore, there is an urgent need to develop a composite current collector with high conductivity, interfacial bonding stability, and safety to improve the overall performance of secondary batteries. Summary of the Invention
[0005] The purpose of this application is to address the shortcomings of the prior art and provide a composite current collector, a secondary battery, and an electrical device.
[0006] To achieve the above objectives, the technical solution adopted in this application is as follows: In a first aspect, a composite current collector is provided, comprising a first polymer layer, a metal layer, and a second polymer layer located between the first polymer layer and the metal layer; The first polymer layer comprises composite particles; The composite particles include flame-retardant materials and metal-organic framework materials, wherein the metal-organic framework materials have a porous structure, and the flame-retardant materials are located on the surface and / or within the pores of the metal-organic framework materials.
[0007] In some embodiments, the first polymer layer comprises an adhesive that contains disulfide bonds.
[0008] In some embodiments, the adhesive content in the first polymer layer is 3-10% by mass.
[0009] In some embodiments, the adhesive comprises at least one of carboxylated chitosan-modified disulfide-containing aqueous polyurethane, disulfide dichloride (S2Cl2), 2,2'-dithiobenzoic acid, bis(4-hydroxyphenyl) disulfide, bis(2-hydroxyethyl) disulfide, epoxy resin, sulfur, polyethylene glycol containing dithiodipropionic acid blocks, and zinc salt of 1-vinyl-3-ethylimidazolium dithiocarboxylate.
[0010] In some embodiments, the second polymer layer has silicon-oxygen bonds; and there is a Si-OM chemical bond between the second polymer layer and the metal layer, wherein M is a metal element in the metal layer.
[0011] In some embodiments, the thickness of the second polymer layer is 0.2 to 1.0 μm.
[0012] In some embodiments, the second polymer layer comprises the following components in weight percentage: 70-80% second polymer, 20-30% aerogel, and 1-2% silane coupling agent.
[0013] In some embodiments, the composite current collector satisfies at least one of the following: (1) The glass transition temperature of the second polymer is greater than 300°C; (2) The second polymer includes at least one of polyimide, siloxane-modified polyimide, silsesquioxane polymer, aryl-substituted polysiloxane, geopolymer, organometallic polymer-siloxane hybrid, and silane-polyethylene glycol-acrylate polymer; (3) The silane coupling agent includes at least one of aminosilane coupling agents, vinylsilane coupling agents, and epoxysilane coupling agents; (4) The aerogel includes at least one of inorganic aerogel and organic aerogel.
[0014] In some embodiments, the composite current collector satisfies at least one of the following: (1) The aminosilane coupling agent includes at least one of aminopropyl-triethoxysilane, aminopropyl-trimethoxysilane, di-(trimethoxysilylpropyl)amine, N-(β-aminoethyl)-γ-aminopropyl-trimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyl-methyl-trimethoxysilane; (2) The vinyl silane coupling agent includes at least one of vinyltrichlorosilane, vinyltriethoxysilane, vinyl-tri-(2-methoxyethoxy)silane, and vinyltrimethoxysilane; (3) The epoxy silane coupling agent includes at least one of γ-glycidylpropyltrimethoxysilane and 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane; (4) The inorganic aerogel includes at least one of silica aerogel, titanium dioxide aerogel, zirconium dioxide aerogel, alumina aerogel, magnesium oxide aerogel, vanadium oxide aerogel, boron nitride aerogel or titanium nitride aerogel. (5) The organic aerogel includes at least one of polymethyl methacrylate aerogel, polystyrene aerogel or polyimide aerogel.
[0015] In some embodiments, the first polymer layer further includes a first conductive agent, which comprises a carbon material.
[0016] In some embodiments, the mass percentage of the first conductive agent in the first polymer layer is 10-18%.
[0017] In some embodiments, the carbon material includes at least one of carbon nanotubes, graphene, carbon nanofibers, and carbon nanotube / graphene hybrid materials.
[0018] In some embodiments, the mass percentage of the composite particles in the first polymer layer is 20-30%.
[0019] In some embodiments, the metal layer comprises the following components by weight percentage: 90-95% second conductive agent, 3-5% thermally conductive fiber, and 2-5% dispersant; the second conductive agent comprises metal particles.
[0020] In some embodiments, the composite current collector satisfies at least one of the following: (a) The average particle size of the metal particles is 50-100 nm; (b) The aspect ratio of the thermally conductive fiber is greater than 30; (c) The thermally conductive fiber includes at least one of SiC fiber, Si3N4 fiber, Mg3N2 fiber, GaN fiber, AlN fiber, and BN fiber; (d) The dispersant includes at least one of polyvinylpyrrolidone, polyacrylic acid (PAA), polyacrylamide, lignin sulfonate, sodium carboxymethyl cellulose (CMC-Na), hydroxyethyl cellulose, urea, citric acid, and sodium dodecylbenzene sulfonate.
[0021] In some embodiments, the composite current collector satisfies at least one of the following: (A) The flame retardant material includes at least one of inorganic flame retardant materials and organic flame retardant materials; (B) The metal-organic framework material includes at least one of zeolite imidazole framework, cobalt dimethylimidazolium, iron-containing organometallic framework material, zinc-containing organometallic framework material or chromium-containing organometallic framework material. (C) The thickness of the first polymer layer is 8~10 μm; (D) The thickness of the metal layer is 1~3μm.
[0022] In a second aspect, a secondary battery is provided, comprising a positive electrode, a negative electrode, and a separator, wherein the separator is located between the positive electrode and the negative electrode, and the positive electrode and / or the negative electrode comprises the composite current collector.
[0023] Thirdly, an electrical device is provided, including the aforementioned secondary battery.
[0024] Compared with the prior art, the beneficial effects of this application are as follows: In the first polymer layer of this application, metal-organic framework material is used as the carrier of flame retardant material. When the temperature of the secondary battery containing the composite current collector exceeds the disintegration temperature of the metal-organic framework material, the metal coordination bonds of the metal-organic framework material break, the pore structure disintegrates, and the flame retardant material located on the surface and / or in the pores of the metal-organic framework material is released. The heat absorption and flame retardant effect of the flame retardant material is used to form an effective flame retardant barrier, inhibiting the spread of flame and heat transfer. At the same time, some metal ions in the metal-organic framework material can react with oxygen to form metal oxides, forming a solid-phase heat insulation layer, achieving a synergistic fire extinguishing effect, thereby improving the safety performance of the secondary battery containing the composite current collector. Detailed Implementation
[0025] To facilitate understanding of this application, a more complete description will be provided below. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this application.
[0026] As used in this article: "Prepared from" is synonymous with "comprising". The terms "comprising", "including", "having", "containing", or any other variations thereof as used herein are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.
[0027] The conjunction "composed of..." excludes any unspecified elements, steps, or components. If used in a claim, this phrase makes the claim closed, excluding materials other than those described, except for associated conventional impurities. When the phrase "composed of..." appears in a clause of the body of a claim rather than immediately following it, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0028] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1-5” is disclosed, the described range should be interpreted as including ranges “1-4”, “1-3”, “1-2”, “1-2 and 4-5”, “1-3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.
[0029] In these embodiments, unless otherwise specified, the portions and percentages are all by weight.
[0030] "Parts by mass" refers to the basic unit of measurement that expresses the mass ratio of multiple components. One part can represent any unit mass, such as 1g or 2.689g. If we say that component A has 'a' parts by mass and component B has 'b' parts by mass, it means that the mass ratio of component A to component B is a:b. It is important to understand that, unlike mass percentage content, the sum of the mass parts of all components is not limited to 100 parts.
[0031] "And / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0032] To further illustrate this application, the composite current collector, secondary battery, and electrical device provided in this application are described in detail below with reference to embodiments, but they should not be construed as limiting the scope of protection of this application.
[0033] I. Composite Current Collector This application provides a composite current collector, comprising a first polymer layer, a metal layer, and a second polymer layer located between the first polymer layer and the metal layer; The first polymer layer comprises composite particles; The composite particles include flame-retardant materials and metal-organic framework materials, wherein the metal-organic framework materials have a porous structure, and the flame-retardant materials are located on the surface and / or within the pores of the metal-organic framework materials.
[0034] In the first polymer layer of this application, a metal-organic framework material is used as a carrier for the flame-retardant material. When the temperature of the secondary battery containing the composite current collector exceeds the disintegration temperature of the metal-organic framework material, the metal coordination bonds of the metal-organic framework material break, the pore structure disintegrates, and the flame-retardant material located on the surface and / or in the pores of the metal-organic framework material is released. The heat absorption and flame-retardant effect of the flame-retardant material is utilized to form an effective flame-retardant barrier, inhibiting the spread of flames and heat transfer. At the same time, some metal ions in the metal-organic framework material can react with oxygen to form metal oxides, forming a solid-phase heat insulation layer, achieving a synergistic fire extinguishing effect, thereby improving the safety performance of the secondary battery containing the composite current collector.
[0035] <First Polymer Layer> In some embodiments, the first polymer layer comprises an adhesive that contains disulfide bonds.
[0036] Adding a binder containing disulfide bonds to the first polymer layer can not only improve the self-healing ability of the first polymer layer, but also improve the bonding strength of the first polymer layer.
[0037] In some embodiments, the adhesive content in the first polymer layer is 3-10% by mass; for example, it can be a range of one or any two of 3%, 3.2%, 3.5%, 3.7%, 4%, 4.5%, 5%, 5.2%, 5.5%, 5.7%, 6%, 6.5%, 7%, 7.3%, 7.5%, 7.8%, 8%, 8.5%, 9%, 9.5%, and 10%; preferably 3-8%.
[0038] In the first polymer layer, an appropriate amount of adhesive can enhance the interfacial adhesion between the polymer layer and the metal layer, and improve the interlayer peel strength. Limiting the mass percentage of adhesive to 3-10% can ensure sufficient bond strength while also taking into account interfacial stability.
[0039] In some embodiments, the adhesive comprises at least one of carboxylated chitosan-modified disulfide-containing aqueous polyurethane, disulfide dichloride (S2Cl2), 2,2'-dithiobenzoic acid, bis(4-hydroxyphenyl) disulfide, bis(2-hydroxyethyl) disulfide, epoxy resin, sulfur, polyethylene glycol containing dithiodipropionic acid blocks, and zinc salt of 1-vinyl-3-ethylimidazolium dithiocarboxylate.
[0040] In some embodiments, the preparation method of the carboxylated chitosan-modified disulfide-containing aqueous polyurethane includes the following steps: Preparation of polyurethane prepolymer: Polyether diol, diisocyanate, first chain extender and bis(2-hydroxyethyl) disulfide are reacted at 70-80℃ for 2-3h under nitrogen protection to obtain polyurethane prepolymer with terminal -NCO groups containing disulfide bonds. Preparation of carboxylated chitosan solution: Dissolve carboxylated chitosan (CMCS) in deionized water to form a carboxylated chitosan solution; Preparation of waterborne polyurethane emulsion containing disulfide bonds: Neutralizing agent and carboxylated chitosan solution are added to polyurethane prepolymer and stirred to ionize polyurethane prepolymer; then deionized water is added at 3000-5000 rpm for emulsification to obtain waterborne polyurethane emulsion containing disulfide bonds. Preparation of carboxylated chitosan-modified waterborne polyurethane containing disulfide bonds: The waterborne polyurethane emulsion was post-treated, dried and pulverized to obtain carboxylated chitosan-modified waterborne polyurethane containing disulfide bonds.
[0041] In some embodiments, the molar ratio of polyether diol to diisocyanate is 1:1.5 to 1:2.5, for example, it can be 1:1.5, 1:1.8, 1:2.0, 1:2.2, or 1:2.5.
[0042] In some embodiments, based on the mass of the polyurethane prepolymer, the mass percentage of the first chain extender is 3 to 6%, for example, it can be a range of 3%, 4%, 5%, 6%, or any combination of both.
[0043] In some embodiments, based on the mass of the polyurethane prepolymer, the mass percentage of the carboxylated chitosan is 0.5% to 1.5%, for example, it can be a range of one or any two of 0.5%, 0.8%, 1%, 1.2%, 1.5%.
[0044] In some embodiments, based on the mass of the polyurethane prepolymer, the mass percentage of the neutralizing agent is 2 to 4%, for example, it can be a range of one or any combination of 2%, 2.5%, 3%, 3.5%, 4%.
[0045] In some embodiments, the polyether diol includes at least one of polyethylene glycol (PEG), polypropylene glycol (PPG), polytetramethylene ether glycol (PTMEG), and polycaprolactone polyol (PCL).
[0046] In some embodiments, the diisocyanate includes at least one of isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), and diphenylmethane diisocyanate (MDI).
[0047] In some embodiments, the first chain extender includes at least one of dimethylolpropionic acid (DMPA) and dimethylolbutyric acid (DMBA).
[0048] In some embodiments, the neutralizing agent includes at least one of triethylamine (TEA), N-methyldiethanolamine, and ammonia.
[0049] In some implementations, the post-processing step includes: After adding the second chain extender to an aqueous polyurethane emulsion containing disulfide bonds to carry out the chain extension reaction, the organic solvent is removed.
[0050] In some embodiments, based on the mass of the polyurethane prepolymer, the mass percentage of the second chain extender is 1 to 2%, for example, it can be a range of one or any combination of 1%, 1.5%, 2%.
[0051] In some embodiments, the second chain extender includes at least one of ethylenediamine, hexamethylenediamine, and diethylenetriamine.
[0052] In some embodiments, the method for removing organic solvents includes vacuum distillation.
[0053] In some embodiments, the first polymer layer further includes a first conductive agent, which comprises a carbon material.
[0054] Metal-organic framework materials provide abundant conductive sites, and their porous structure can buffer the volume expansion of the composite current collector. The metal-organic framework materials and conductive agents form a "point-line-surface" conductive network, reducing the surface resistance of the composite current collector and thus improving the conductivity retention rate of the composite current collector.
[0055] In some embodiments, the mass percentage of the first conductive agent in the first polymer layer is 10-18%; for example, it can be a range of one or any two of 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 16%, 17%, and 18%.
[0056] In the first polymer layer, the mass percentage of the first conductive agent is within the above-mentioned range, which is beneficial to further reduce the surface resistance of the composite current collector.
[0057] In some embodiments, the carbon material includes at least one of carbon nanotubes, graphene, carbon nanofibers, and carbon nanotube / graphene hybrid materials.
[0058] Specifically, carbon nanotube / graphene hybrid materials refer to carbon nanotube / graphene hybrid materials with a three-dimensional structure formed by physical and / or chemical grafting of one-dimensional multi-walled carbon nanotubes and two-dimensional graphene microsheets.
[0059] Specifically, the physical method refers to the organic combination of one-dimensional multi-walled carbon nanotubes and two-dimensional graphene microsheets through physical ultrasonic blending, using the effects of π-π bonds and van der Waals forces to form a three-dimensional carbon nanotube / graphene hybrid material.
[0060] Specifically, the chemical grafting method refers to the preparation of three-dimensional carbon nanotube / graphene hybrid materials by chemically grafting one-dimensional multi-walled carbon nanotubes and two-dimensional graphene microsheets using the "grafting-to" technique; the chemical grafting method includes one-step and multi-step methods.
[0061] Specifically, the one-step method involves the direct reaction of polyacrylamide chloride with a mixture of hydroxylated carbon nanotubes / hydroxylated graphene to prepare covalently bonded carbon nanotube / graphene hybrid materials.
[0062] Specifically, the multi-step method involves first grafting carbon nanotubes with polyacrylamide chloride to introduce active functional groups onto the surface of the carbon nanotubes, and then using the acrylamide chloride groups on the surface of the carbon nanotubes to react with the hydroxyl groups on the surface of the hydroxylated graphene microsheets to prepare carbon nanotube / graphene hybrid materials.
[0063] In some embodiments, the mass percentage of the composite particles in the first polymer layer is 20-30%; for example, it can be a range of one or any two of 20%, 20.5%, 21%, 21.5%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 28.5%, 29%, 29.5%, and 30%.
[0064] In some embodiments, the first polymer layer comprises a plurality of intersecting first polymer fibers; fibers generally refer to slender filaments, and multiple first polymer fibers are connected to form a three-dimensional nanofiber membrane with pores. That is, in the first polymer layer, each first polymer fiber is closely connected to form a three-dimensional nanofiber membrane, which serves as the supporting framework of the first polymer layer and improves the overall strength of the first polymer layer; the three-dimensional nanofiber membrane forms a "maze-like" thermal conductivity barrier, improving the thermal insulation effect of the composite current collector; at the same time, the three-dimensional nanofiber membrane can improve the flexibility of the composite current collector and reduce the conductivity attenuation rate after multiple bends of the composite current collector.
[0065] Specifically, the porosity of the nanofiber membrane is 55-65%, for example, it can be a range of values consisting of one or any combination of 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, and 65%.
[0066] Specifically, along the direction from the first polymer layer to the second polymer layer, the porosity of the first polymer layer tends to decrease. This porosity trend in the first polymer layer is beneficial for thermal and ion conduction.
[0067] In some embodiments, the flame-retardant material includes at least one of inorganic flame-retardant materials and organic flame-retardant materials.
[0068] Specifically, the inorganic flame retardant material includes at least one of aluminum hydroxide, magnesium hydroxide, zinc borate, antimony oxide, aluminum oxide, magnesium oxide, ammonium phosphate ((NH4)3PO4), sodium ammonium phosphate (NaNH4HPO4), ammonium sulfate ((NH4)2SO4), and ammonium polyphosphate (APP).
[0069] Specifically, the organic flame retardant material includes at least one of organophosphorus flame retardant materials, organonitrogen flame retardant materials, halogen flame retardant materials, and silicon flame retardant materials.
[0070] Specifically, organophosphorus flame retardant materials include one of the following: triphenyl phosphate (TPP), trimethyl phosphate (TMP), triethyl phosphate (TEP), tributyl phosphate (TBP), trimethyl phosphite (TMPI), trifluoroethyl phosphate (TFFP), dimethyl methyl phosphate (TMMP), 4-isopropylphenyl diphenyl phosphate (IPPP), hexamethoxyphosphazene (HMPN), di-(2,2,2-trifluoroethyl)-methyl phosphate (BMP), (2,2,2-trifluoroethyl)-diethyl phosphate (TDP), tri-(2,2,2-trifluoroethyl) phosphite (TTFP), hexamethylphosphoric acid triamine (HMPA), diethyl(cyanomethyl)phosphonate (DECP), and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO).
[0071] Specifically, organic nitrogen-based flame retardant materials include one of trimethylacetamide (TMAC), triallyl cyanurate (TAC), triallyl isocyanate (TAIC), and ethylenedionitrile (AND).
[0072] Halogenated flame retardant materials include one of the following: fluorocarbonate, brominated carbonate, brominated epoxy resin, and chlorinated paraffin.
[0073] Silicon-based flame retardant materials include one of polysiloxane, organosilicon epoxy resin, vinyl-3-(methylethyl ketone oxime)silane (VTMS), and methylphenyl dimethyl diethoxysilane (MPBMDS).
[0074] In some embodiments, the disintegration temperature of the metal-organic framework is 350~500°C, for example, it can be a range of one or any combination of 350°C, 370°C, 390°C, 410°C, 430°C, 450°C, 470°C, 490°C, and 500°C.
[0075] Within the aforementioned range, the disintegration temperature of the metal-organic framework ensures the structural stability of the metal-organic framework material in the composite current collector under normal operating conditions of the secondary battery. When thermal runaway occurs in the secondary battery and the local internal temperature exceeds the disintegration temperature of the metal-organic framework, the metal-organic framework disintegrates in time and releases flame-retardant materials. During the high-temperature propagation stage, the exothermic chain reaction is cut off through the synergistic effect of gas-phase free radical quenching and condensation into carbon, thereby delaying the thermal runaway time and inhibiting the propagation of thermal runaway.
[0076] In some embodiments, the metal-organic framework material includes at least one of zeolite imidazole framework, cobalt dimethylimidazolium, iron-containing organometallic framework, zinc-containing organometallic framework, or chromium-containing organometallic framework.
[0077] In some embodiments, the organometallic framework may include at least one of ZIF-8 (zeolite imidazole framework-8), ZIF-67 (dimethylimidazolium cobalt), MIL-100 (ferric 1,3,5-pyromellitic tricarboxylate), MIL-101 (chromium, terephthalic acid), or MOF-5 (zinc, terephthalic acid).
[0078] In some embodiments, the thickness of the first polymer layer is 8 to 10 μm; for example, it can be a range of one or any combination of 8 μm, 8.2 μm, 8.5 μm, 8.7 μm, 9 μm, 9.3 μm, 9.5 μm, 9.8 μm, and 10 μm.
[0079] In this application, the thickness of the first polymer layer is within the above-mentioned range, which can take into account both the flame retardant performance and energy density of the composite current collector.
[0080] In some embodiments, the first polymer may be at least one of polyarylamide, polyetheretherketone (PEEK), polybenzimidazole (PBI), polyethylene terephthalate (PET), polypropylene (PP), polyamide (PA), polyphenylene sulfide (PPS), polyurethane (PU), and polyimide-siloxane copolymer.
[0081] <Second Polymer Layer> In some embodiments, the second polymer layer has silicon-oxygen bonds; and there is a Si-OM chemical bond between the second polymer layer and the metal layer, wherein M is a metal element in the metal layer.
[0082] In this application, there are Si-OM chemical bonds between the second polymer layer and the metal layer, which can improve the interfacial stability between the second polymer layer and the metal layer, thereby improving the interlayer peel strength between the second polymer layer and the metal layer and reducing the risk of the metal layer falling off during the winding process.
[0083] In some embodiments, the thickness of the second polymer layer is 0.2 to 1.0 μm; for example, it can be a range of one or any combination of 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm, and 1.0 μm.
[0084] In this application, the thickness of the second polymer layer is within the above-mentioned range, which can balance the flame retardant performance of the composite current collector and the energy density of the battery.
[0085] In some embodiments, the second polymer layer comprises the following components in weight percentage: 70-80% second polymer, 20-30% aerogel, and 1-2% silane coupling agent.
[0086] Adding aerogel and silane coupling agent to the second polymer layer allows the nanoporous network structure of the aerogel to effectively block the transfer of heat and gas, forming a thermal barrier, while reducing the dielectric constant of the second polymer layer and suppressing interfacial polarization. The silane coupling agent can improve the compatibility between the second polymer and the aerogel.
[0087] Specifically, the mass percentage of the second polymer can be a range of one or any two of the following: 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, and 80%.
[0088] Specifically, the mass percentage of aerogel can be a range of one or any combination of 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, and 30%.
[0089] Specifically, the mass percentage of the silane coupling agent can be a range of one or any combination of 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, and 2%.
[0090] In some embodiments, the glass transition temperature of the second polymer is greater than 300°C; for example, it can be 305~370°C, specifically a range of one or any two of 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, 350°C, 355°C, 360°C, 365°C, and 370°C.
[0091] Having the glass transition temperature of the second polymer within the above-mentioned range is beneficial for improving the high-temperature stability of the second polymer layer.
[0092] In some embodiments, the second polymer includes at least one of polyimide, siloxane-modified polyimide, silsesquioxane polymer, aryl-substituted polysiloxane, geopolymer, organometallic polymer-siloxane hybrid, and silane-polyethylene glycol-acrylate polymer.
[0093] In some embodiments, the silane coupling agent includes at least one of aminosilane coupling agents, vinylsilane coupling agents, and epoxysilane coupling agents.
[0094] In some embodiments, the aminosilane coupling agent includes at least one of aminopropyl-triethoxysilane, aminopropyl-trimethoxysilane, di-(trimethoxysilylpropyl)amine, N-(β-aminoethyl)-γ-aminopropyl-trimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyl-methyl-trimethoxysilane.
[0095] In some embodiments, the vinyl silane coupling agent includes at least one of vinyltrichlorosilane, vinyltriethoxysilane, vinyl-tri-(2-methoxyethoxy)silane, and vinyltrimethoxysilane.
[0096] In some embodiments, the epoxy silane coupling agent includes at least one of γ-glycidylpropyltrimethoxysilane and 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane.
[0097] In some embodiments, the aerogel includes at least one of inorganic aerogels and organic aerogels.
[0098] In some embodiments, the inorganic aerogel includes at least one of silica aerogel, titanium dioxide aerogel, zirconium dioxide aerogel, alumina aerogel, magnesium oxide aerogel, vanadium oxide aerogel, boron nitride aerogel, or titanium nitride aerogel. In some embodiments, the organic aerogel includes at least one of polymethyl methacrylate aerogel, polystyrene aerogel, or polyimide aerogel.
[0099] <Metallic Layer> In some embodiments, the metal layer comprises the following components by weight percentage: 90-95% second conductive agent, 3-5% thermally conductive fiber, and 2-5% dispersant; the second conductive agent comprises metal particles.
[0100] This application incorporates thermally conductive fibers into the metal layer, which together with the second conductive agent form an effective thermally conductive network within the metal layer, thereby improving the thermal conductivity of the metal layer and thus enhancing the safety performance of the composite current collector.
[0101] Specifically, the mass percentage content of the second conductive agent can be a range of one or any two of the following: 90%, 90.2%, 90.5%, 90.7%, 91%, 91.5%, 92%, 92.5%, 93%, 93.5%, 94%, 94.3%, 94.5%, 94.8%, and 95%.
[0102] Specifically, the mass percentage of the thermally conductive fiber can be a range of one or any two of the following: 3%, 3.2%, 3.5%, 3.7%, 4%, 4.3%, 4.5%, 4.8%, and 5%.
[0103] Specifically, the mass percentage of the dispersant can be a range of one or any two of the following: 2%, 2.3%, 2.5%, 2.8%, 3%, 3.5%, 4%, 4.2%, 4.5%, 4.7%, and 5%.
[0104] In some embodiments, the average particle size of the metal particles is 50-100 nm; for example, it can be a range of one or any combination of two of the following: 50 nm, 52 nm, 55 nm, 57 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 93 nm, 95 nm, 98 nm, and 100 nm.
[0105] In some embodiments, the aspect ratio of the thermally conductive fiber is greater than 30; for example, it can be 32-100, specifically a range of one or any two of the following values: 32, 37, 40, 45, 50, 55, 57, 60, 63, 65, 68, 70, 75, 80, 85, 90, 93, 95, 98, 100.
[0106] In this application, the average particle size of the metal particles and the aspect ratio of the thermally conductive fibers are within the above-mentioned range, which can further improve the thermal conductivity of the metal layer, thereby improving the safety performance of the composite current collector.
[0107] In some embodiments, the thermally conductive fiber includes at least one of SiC fiber, Si3N4 fiber, Mg3N2 fiber, GaN fiber, AlN fiber, and BN fiber.
[0108] In some embodiments, the dispersant includes at least one of polyacrylic acid (PAA), polyvinylpyrrolidone (PVP), polyacrylamide, lignin sulfonate, sodium carboxymethyl cellulose (CMC-Na), hydroxyethyl cellulose, urea, citric acid, and sodium dodecylbenzene sulfonate.
[0109] In some embodiments, the metal particles may be a single element, alloy, compound, or mixture formed from at least one of the elements selected from aluminum, copper, nickel, titanium, and silver.
[0110] In some embodiments, the thickness of the metal layer is 1 to 3 μm; for example, it can be a range of one or any combination of two of the following: 1 μm, 1.2 μm, 1.5 μm, 1.7 μm, 2 μm, 2.3 μm, 2.5 μm, 2.8 μm, and 3 μm.
[0111] <Preparation of Composite Current Collectors> The preparation method of the composite current collector may include the following steps: First, the first polymer layer is prepared; Next, a second polymer layer slurry is coated onto at least one side of the first polymer layer, and after drying, a second polymer layer is formed. Then, a metal layer slurry is applied to the surface of the second polymer layer away from the first polymer layer and dried to form a metal layer.
[0112] In some embodiments, the second polymer layer slurry or metal layer slurry can be applied by any of the following methods: gravure coating, extrusion coating, dip coating, spray coating, dot coating, or wire rod coating.
[0113] In some embodiments, the drying temperature can be from 40°C to 60°C.
[0114] Secondary batteries This application provides a secondary battery, including a positive electrode, a negative electrode, and a separator, wherein the separator is located between the positive electrode and the negative electrode, and the positive electrode and / or the negative electrode includes the composite current collector.
[0115] This application does not impose any particular limitation on the type of secondary battery; any secondary battery known in the prior art can be used. In some embodiments, the secondary battery may include, but is not limited to, lithium-ion batteries, sodium-ion batteries, nickel-metal hydride batteries, lithium polymer batteries, lithium-sulfur batteries, sodium-sulfur batteries, and lithium metal sulfide batteries.
[0116] <Positive Electrode> In some embodiments, the positive electrode includes a positive current collector and a layer of positive active material located on at least one side of the positive current collector.
[0117] In some embodiments, the positive electrode active material layer may include a positive electrode active material, a positive electrode binder, and a positive electrode conductive agent.
[0118] In some embodiments, the positive electrode active material is selected from LiCoO2, LiNiO2, and LiNi x Mn y O2, Li 1+ z Ni x Mn y Co 1-x-y O2, LiNi x Co y Al zAt least one of O2, LiV2O5, LiTiS2, LiMoS2, LiMnO2, LiCrO2, LiMn2O4, Li2MnO3, LiFeO2, LiFePO4, and LiMnPO4, wherein each x is independently from 0.2 to 0.9; each y is independently from 0.1 to 0.45; and each z is independently from 0 to 0.2. The positive electrode active material of this application is not limited to the above-mentioned materials, but also includes other materials that can be used as positive electrode active materials.
[0119] In some embodiments, the positive electrode active material is selected from LiCoO2, LiNiO2, and LiNi x Mn y O2, Li 1+ z Ni x Mn y Co 1-x-y O2, LiNi x Co y Al z At least one of O2, LiV2O5, LiTiS2, LiMoS2, LiMnO2, LiCrO2, LiMn2O4, LiFeO2, and LiFePO4, wherein each x is independently 0.4 to 0.6; each y is independently 0.2 to 0.4; and each z is independently 0 to 0.1.
[0120] In some embodiments, the positive electrode active material includes Li 1+x Ni a Mn b Co c Al (1-a-b-c) Compounds of O2; wherein -0.2≤x≤0.2, 0≤a<1, 0≤b<1, 0≤c<1 and a+b+c≤1.
[0121] In some embodiments, the positive electrode active material has the general formula Li 1+x Ni a Mn b Co c Al (1-a-b-c)O2, where 0.33≤a≤0.92, 0.33≤a≤0.9, 0.33≤a≤0.8, 0.5≤a≤0.92, 0.5≤a≤0.9, 0.5≤a≤0.8, 0.6≤a≤0.92 or 0.6≤a≤0.9; 0≤b≤0.5, 0≤b≤0.3, 0.1≤b≤0.5, 0.1≤b≤0.4, 0.1≤b≤0.3, 0.1≤b≤0.2 or 0.2≤b≤0.5; 0≤c≤0.5, 0≤c≤0.3, 0.1≤c≤0.5, 0.1≤c≤0.4, 0.1≤c≤0.3, 0.1≤c≤0.2 or 0.2≤c≤0.5.
[0122] In some embodiments, the positive electrode active material is doped with a dopant, which is selected from at least one of Fe, Ni, Mn, Al, Mg, Zn, Ti, La, Ce, Sn, Zr, Ru, Si, and Ge.
[0123] In some embodiments, the positive electrode active material may include LiNi. 0.33 Mn 0.33 Co 0.33 O2, LiNiO2, LiNi 0.4 Mn 0.4 Co 0.2 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2, LiNi 0.6 Mn 0.2 Co 0.2 O2, LiNi 0.7 Mn 0.15 Co 0.15 O2, LiNi 0.8 Mn 0.1 Co 0.1 O2, LiNi 0.92 Mn 0.04 Co 0.04 O2, LiNi 0.8 Co 0.15 Al 0.05 At least one of O2.
[0124] In some embodiments, the positive electrode binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0125] In some embodiments, the positive electrode conductive agent includes at least one of conductive carbon black (SuperP), carbon nanotubes (CNTs), carbon fibers, flake graphite, graphene, metallic materials, or conductive polymers.
[0126] In some embodiments, the metallic material may include, but is not limited to, metal powder and / or metal fibers. Specifically, the metal may include, but is not limited to, at least one of copper, nickel, aluminum or silver.
[0127] In some embodiments, the conductive polymer may include, but is not limited to, at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene, or polypyrrole. The positive electrode binder may include, but is not limited to, at least one of polyacrylic acid, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyvinyl alcohol, carboxymethyl cellulose, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, polyamide-imide, styrene-butadiene rubber, or polyvinylidene fluoride.
[0128] This application does not impose any particular restrictions on the mass ratio of positive electrode active material, positive electrode conductive agent, and positive electrode binder in the positive electrode active material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of this application can be achieved.
[0129] This application does not impose any particular limitation on the thickness of the positive electrode active material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of this application can be achieved.
[0130] This application does not impose any particular restrictions on the positive electrode current collector, as long as it can achieve the purpose of this application. For example, it may include aluminum foil, aluminum alloy foil, or aluminum-carbon composite current collector.
[0131] In this application, positive current collectors of different thicknesses can be purchased and selected by measuring with a micrometer.
[0132] <Negative electrode sheet> In some embodiments, the negative electrode sheet includes a negative current collector and a layer of negative active material located on at least one side of the negative current collector.
[0133] In some embodiments, the negative electrode active material layer may include a negative electrode active material, a negative electrode binder, and a negative electrode conductive agent.
[0134] The negative electrode active material layer includes a negative electrode active material. This application does not impose any particular limitation on the negative electrode active material, as long as it can achieve the purpose of this application. For example, the negative electrode active material may include, but is not limited to, natural graphite, artificial graphite, mesophase microcarbon spheres, hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-SnO alloys, Sn, SnO, SnO2, and spinel-structured lithiated TiO2-Li4Ti5O.12 Or at least one of Li-Al alloys.
[0135] This application does not impose any particular restrictions on the types of negative electrode conductive agent and negative electrode binder, as long as they can achieve the purpose of this application. For example, they can be at least one of the above-mentioned positive electrode conductive agent and positive electrode binder. This application does not impose any particular restrictions on the mass ratio of negative electrode active material, negative electrode conductive agent, and negative electrode binder in the negative electrode material layer. Those skilled in the art can select them according to actual needs, as long as they can achieve the purpose of this application.
[0136] This application does not impose any particular restrictions on the negative electrode current collector, as long as it can achieve the purpose of this application. For example, it may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or composite current collector. For example, the composite current collector may be lithium copper composite current collector, carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector, etc.
[0137] <Septum> This application does not impose any particular restrictions on the diaphragm, as long as it can achieve the purpose of this application.
[0138] In some embodiments, the diaphragm includes a substrate layer. The substrate layer may include, but is not limited to, at least one of a nonwoven fabric, membrane, or composite membrane having a porous structure. The material of the substrate layer may include, but is not limited to, at least one of polyethylene, polypropylene, polyethylene terephthalate, and polyimide. In some embodiments, the substrate layer may include, but is not limited to, at least one of a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane.
[0139] In some embodiments, the separator further includes a surface treatment layer disposed on at least one surface of the substrate layer. The surface treatment layer may include, but is not limited to, at least one of a polymer layer, an inorganic layer, and a layer formed by a mixture of polymers and inorganic substances. The polymer layer includes polymers. This application does not particularly limit the polymer, as long as it achieves the purpose of this application. For example, the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymers, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene). The inorganic layer includes inorganic particles and a binder. This application does not particularly limit the inorganic particles and binder, as long as it achieves the purpose of this application. For example, the inorganic particles may include, but are not limited to, at least one of alumina, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate. As another example, the binder may include, but is not limited to, at least one of the binders used in the above-mentioned positive electrode material layer or negative electrode material layer.
[0140] In some embodiments, the present application does not have a particular limitation on the thickness of the diaphragm, as long as the purpose of the present application can be achieved. For example, the thickness of the diaphragm is 3 μm to 20 μm.
[0141] Electrolyte In some embodiments, the electrolyte includes a non-aqueous solvent and a lithium salt.
[0142] In some embodiments, the lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB, and lithium difluoroborate.
[0143] In some embodiments, the non-aqueous solvent may be at least one of carbonate compounds, carboxylic acid ester compounds, and ether compounds.
[0144] In some embodiments, the carbonate compound may include at least one of chain carbonate compounds, cyclic carbonate compounds, and fluorocarbonate compounds.
[0145] In some embodiments, the chain carbonate compound may include diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), and combinations thereof.
[0146] In some embodiments, the cyclic carbonate compound may include ethylene carbonate (EC), propylene carbonate (PC), butyl carbonate (BC), vinyl ethylene carbonate (VEC), and combinations thereof.
[0147] In some embodiments, the fluorocarbonate compound may include at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, and trifluoromethylethylene carbonate.
[0148] In some embodiments, the carboxylic acid ester compound may include at least one of methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid lactone, valerate lactone, mevalonate lactone, caprolactone, and methyl formate.
[0149] In some embodiments, the ether compound may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, and combinations thereof.
[0150] In some embodiments, the non-aqueous solvent may also include at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolium ketone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, and phosphate esters.
[0151] The secondary battery also includes a casing for housing the positive electrode, separator, negative electrode, and electrolyte, as well as other components known in the field of secondary batteries. This application does not limit the scope of these other components. This application does not impose any particular limitation on the casing; it can be a casing known in the art, as long as it achieves the purpose of this application. For example, the casing can be a rigid casing or a flexible casing. The material of the rigid casing can be metal; this application does not limit the type of metal and can use known metal rigid casings, as long as they achieve the purpose of this application. The flexible casing can be a metal plastic film, such as aluminum-plastic film, steel-plastic film, etc.
[0152] The fabrication process of the secondary battery described in this application is well known to those skilled in the art, and this application does not impose any particular limitations. For example, the fabrication process of the secondary battery may include, but is not limited to, the following steps: stacking the positive electrode, separator, and negative electrode in sequence, and performing operations such as winding and folding as needed to obtain a wound electrode assembly; placing the electrode assembly into a housing; injecting electrolyte into the housing and sealing it to obtain the secondary battery. Alternatively, stacking the positive electrode, separator, and negative electrode in sequence, and then fixing the four corners of the entire stacked structure with tape to obtain a stacked electrode assembly; placing the electrode assembly into a housing; injecting electrolyte into the housing and sealing it to obtain the secondary battery. In addition, overcurrent protection elements, conductive plates, etc., may be placed in the housing as needed to prevent pressure rise and overcharging / discharging inside the secondary battery.
[0153] III. Electrical Appliances This application provides an electrical device that includes any of the secondary batteries described herein.
[0154] The electrical device used in this application is not particularly limited and can be any electrical device known in the prior art.
[0155] The application of the secondary battery in this application is not particularly limited, and it can be used in any electrical device known in the prior art. According to some embodiments of this application, the electrical device includes, but is not limited to, mobile phones, smartphones, laptops, tablets, wearable devices, smartwatches, smart bracelets, smart glasses, power banks, televisions, game consoles, game controllers, digital cameras, smart speakers, headphones, keyboards, mice, monitors, drones, audio equipment, home appliances, toys, power tools, automobiles, motorcycles, electric bicycles, bicycles, robots, robot dogs, industrial robots, and android robots.
[0156] The raw materials used in the embodiments and comparative examples are described below, but are not limited to these materials: Polyarylamide: Dongguan Yingxiang Plastic Raw Materials Co., Ltd., TW271F8; The carboxylated chitosan-modified waterborne polyurethane containing disulfide bonds was prepared in-house, and the preparation method is as follows: the carboxylated chitosan was purchased from Zhejiang Zhoushan Mingri New Materials Co., Ltd., model NDPU-201. (1) Synthesis of polyurethane prepolymer: 100g of polytetramethylene ether glycol (PTMEG, molecular weight 2000) was added to the reactor and dehydrated for 1h under vacuum conditions of 110℃ and -0.095MPa; the temperature was lowered to 60℃, and 22.2g of isophorone diisocyanate (IPDI, molar ratio of PTMEG to IPDI is 1:2.0), 6g of hydrophilic chain extender dimethylolbutyric acid (DMBA, accounting for about 5% of the total mass of the prepolymer) and 2g of bis(2-hydroxyethyl) disulfide were added. The reaction was carried out at 75℃ for 3h under nitrogen protection. The NCO content was titrated to the theoretical value by di-n-butylamine method to obtain 130g of polyurethane prepolymer with terminal-NCO groups containing disulfide bonds.
[0157] (2) Introduction of carboxylated chitosan: 1.8g of carboxylated chitosan (CMCS, accounting for 1.4% of the total mass of polyurethane prepolymer) was dissolved in 20mL of deionized water and stirred until completely dissolved to obtain an aqueous solution of CMCS; before emulsification of polyurethane prepolymer, the aqueous solution of CMCS was slowly added dropwise to 130g of polyurethane prepolymer under stirring at 500rpm, and stirred at 50℃ for 30min to ensure that CMCS and polyurethane prepolymer were fully mixed and homogeneous.
[0158] (3) Neutralization and emulsification: Add 4.0g of triethylamine (TEA, neutralizing agent, accounting for 3% of the total mass of polyurethane prepolymer) to the above system to neutralize the carboxyl groups in DMBA and ionize the prepolymer; then, under high-speed shearing conditions of 4000rpm, slowly add 130g of deionized water for emulsification, and shear dispersion for 15min to form a stable waterborne polyurethane emulsion containing disulfide bonds with a solid content of about 50%.
[0159] (4) Post-treatment and film formation: 1.5g of ethylenediamine (diamine chain extender, accounting for 1.2% of the total mass of polyurethane prepolymer) was added to the emulsion to carry out the chain extension reaction and stirred at 40℃ for 30min; then the organic solvent and excess water were removed under reduced pressure of 60℃ and -0.095MPa, the emulsion was coated on a polytetrafluoroethylene template, dried at 60℃ for 24h to form a film, and powdered after cooling to obtain carboxylated chitosan modified waterborne polyurethane containing disulfide bonds.
[0160] The carbon nanotube / graphene hybrid material was prepared in-house, and its preparation method is as follows: (1) Preparation of graphite dispersion: 0.5g sodium dodecyl sulfate (SDS) was dissolved in 100mL deionized water and stirred at room temperature until completely dissolved; 5.0g expanded graphite was added and magnetically stirred at 500rpm for 1h at room temperature to obtain a uniform graphite dispersion; the graphite dispersion was vacuum dried at 60℃ for 12h to remove water and obtain 5.4g modified graphite.
[0161] (2) Preparation of iron-supported graphite catalyst: 1.8 g of ferric nitrate nonahydrate (Fe(NO3)3·9H2O) and 0.9 g of ammonium carbonate ((NH4)2CO3) were dissolved in 50 mL of deionized water and stirred until completely dissolved; 5.0 g of modified graphite obtained in step (1) was added and ultrasonically dispersed for 30 min to obtain a metal salt-graphite dispersion; after removing water from the metal salt-graphite dispersion, the obtained solid product was placed in a tube furnace and heated to 450 °C at a heating rate of 5 °C / min under nitrogen (N2) protection, and calcined at low temperature for 2 h to obtain an iron-supported graphite catalyst.
[0162] (3) In-situ growth of carbon nanotubes by chemical vapor deposition (CVD): The iron-supported graphite catalyst obtained in step (2) was placed in a tube furnace and heated to 750°C at a heating rate of 10°C / min under argon (Ar) protection; acetylene (C2H2) gas was introduced as carbon source (flow rate 100 mL / min) and argon gas was introduced as carrier gas (flow rate 300 mL / min), and chemical vapor deposition was carried out at 750°C for 30 min to grow carbon nanotubes in situ on the graphite surface; after the reaction was completed, the acetylene was stopped and the mixture was naturally cooled to room temperature under argon protection to obtain about 6.1 g of carbon nanotube / graphene hybrid material.
[0163] The Ni / Cu alloy powder was prepared in-house, with a mass ratio of nickel to copper (Ni:Cu) of 3:1. The preparation method is as follows: (1) Preparation of metal salt complexing solution: Dissolve 3.9g copper sulfate pentahydrate (CuSO4·5H2O) and 13.4g nickel sulfate hexahydrate (NiSO4·6H2O) in 150mL of deionized water, add 2.0g ammonium tartrate ((NH4)2C4H4O6) as a complexing agent, and stir at room temperature until completely dissolved to obtain the first metal salt complexing solution.
[0164] (2) Alkali adjustment and heating: The pH of the first metal salt complex solution was slowly adjusted to 9.5 with 1.0 mol / L sodium hydroxide (NaOH) solution and heated to 50°C to obtain the second metal salt complex solution; (3) Reduction reaction: Under stirring at 500 rpm, 80 mL of 0.5 mol / L hydrazine hydrate (N2H4·H2O) reducing agent solution was slowly added dropwise to the second metal salt complex solution at a rate of 2 mL / min. After the addition was completed, the solution was kept at 50 °C for 30 min to continue the reaction. During the reaction, copper ions (Cu) 2+ ) are preferentially reduced to form copper nuclei, while nickel ions (Ni) are preferentially reduced to form copper nuclei. 2+ Subsequently, it is reduced and coated on the surface of the copper core, forming a core-shell structured Ni / Cu composite powder.
[0165] (4) Post-processing: After the reaction is completed, cool to room temperature, centrifuge (8000 rpm, 10 min), wash three times each with deionized water and anhydrous ethanol, and vacuum dry at 50-60℃ for 12 h to obtain core-shell structured nanoscale Ni / Cu alloy powder with an average particle size of 50 nm.
[0166] Example 1 <Preparation of Composite Current Collectors> Preparation of the first polymer layer: Polyarylamide was dissolved in a DMAC / acetone mixed solvent (DMAC to acetone volume ratio of 7:3), and lithium chloride was added and stirred until homogeneous to obtain a spinning solution. Based on the mass of the spinning solution, the mass percentage of polyarylamide was 12%, and the mass percentage of lithium chloride was 0.5%. Under the conditions of 18kV voltage, 15cm receiving distance, 0.8mL / h propulsion speed, 25℃ ambient temperature, and 28% ambient humidity, the spinning solution was electrospun to obtain a first nanofiber membrane with a thickness of 12µm. The fiber diameter in the first nanofiber membrane was 500nm, and the porosity was 62%. The first nanofiber membrane was immersed in a 0.1M Zn(NO3)2·6H2O methanol solution, and then transferred to a 0.4M 2-methylimidazole solution. The membrane was hydrothermally reacted at 60℃ for 2 h to form a ZIF-8 coating (based on the mass of the first nanofiber membrane, the loading of the ZIF-8 coating was 42 wt%), thus obtaining the second nanofiber membrane. DOPO solid powder was vacuum dried at 80°C for 4 hours to remove adsorbed moisture; then it was heated and melted at 100°C to obtain liquid DOPO. The second nanofiber membrane was placed in a vacuum drying oven and degassed for 60 min at 80°C and a vacuum degree ≤133 Pa to fully remove air from the pores of the second nanofiber membrane. Open the valve of the DOPO storage tank of the vacuum impregnation device to allow liquid DOPO to flow in under atmospheric pressure and completely immerse the second nanofiber membrane; the liquid DOPO spontaneously permeates into the pores of the second nanofiber membrane under capillary action and fills the gaps between the ZIF-8 crystals; maintain the vacuum degree ≤133 Pa and continue impregnation for 20 min to ensure that DOPO fully fills all the interconnected pores; after impregnation, slowly depressurize to atmospheric pressure to obtain the third nanofiber membrane; The third nanofiber membrane was dried at 80℃ and under a vacuum of ≤133 Pa for 4 hours to solidify DOPO. DOPO solidified in the nanofiber pores, firmly bonding ZIF-8 crystals and polyamide nanofibers together to form composite particles, thus obtaining a nanofiber membrane containing composite particles. The mass ratio of ZIF-8 to DOPO was 2:1. The nanofiber membrane containing composite particles was placed in a mold and held at 100°C and 10 MPa for 5 minutes. After cooling, a first polymer layer with a thickness of 10 μm was obtained. Based on the mass of the first polymer layer, the mass percentage of polyarylamide was 75% and the mass percentage of composite particles was 25%.
[0167] Preparation of the second polymer layer: A thermosetting polyimide prepolymer (glass transition temperature 320℃) of 75% by mass, silica aerogel (average particle size 200nm) of 23% by mass, and KH-550 silane coupling agent of 2% by mass were added to a ball mill and ball-milled at 300 rpm for 2 hours. Then, ethyl acetate was added and stirred evenly to obtain a second polymer layer slurry with a viscosity of 320 mPa·s. Under the conditions of a coating speed of 8 m / min and a bar spacing of 10 μm, the second polymer layer slurry was coated on one side surface of the first polymer layer and pre-cured at 120°C for 2 min; then it was treated for 30 s under Ar / O2 mixed gas (Ar:O2 volume ratio of 4:1) and power of 300 W to obtain a second polymer layer with silicon-oxygen bonds and a thickness of 0.5 μm. Preparation of the metal layer: Ni / Cu alloy powder (Ni powder to Cu powder mass ratio of 3:1, average particle size of 50 nm), titanium carbide nanowires (aspect ratio of 60), and polyvinylpyrrolidone (polyvinylpyrrolidone) with a mass percentage of 94% were added to ethanol and ultrasonicated at 600 W for 30 min to obtain a metal layer slurry with a solid content of 40%. Under conditions of 50kV voltage, 15cm spray gun distance, 80℃ substrate temperature, and 0.3MPa carrier gas pressure, the metal layer slurry was sprayed onto the surface of the second polymer layer to obtain a metal layer with a thickness of 2μm.
[0168] <Preparation of the positive electrode> The positive electrode active material (lithium nickel cobalt manganese oxide NCM811), conductive agent (Super P), and binder (polyvinylidene fluoride) were thoroughly mixed in N-methylpyrrolidone solvent at a mass ratio of 96:2:2 to obtain a positive electrode slurry. The positive electrode slurry was coated onto a composite current collector, dried at 85°C, and then cold-pressed. After trimming and slitting, it was dried under vacuum at 85°C for 6 hours and then the tabs were welded to obtain the positive electrode sheet. The thickness of the double-sided positive electrode active layer was 80 μm.
[0169] <Preparation of Negative Electrode Sheets> Artificial graphite, super P, CMC, and SBR were added to a deionized water solvent in a mass ratio of 96.5:0.5:1.2:1.8 and stirred thoroughly to form a negative electrode active material slurry with a solid content of 53% and a viscosity of 3000 mPa·s. The negative electrode active material slurry was then coated on both sides of a copper foil, dried, rolled, and cut into sheets. Negative electrode tabs were cut from the corresponding positions of the empty foil areas of the copper foil to obtain negative electrode sheets. The thickness of the double-sided negative electrode active layer was 50 μm.
[0170] <Preparation of Electrolyte> Lithium hexafluorophosphate was dissolved in a mixed solvent of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a volume ratio of 1:1.5:1 to obtain an electrolyte, wherein the molar concentration of lithium hexafluorophosphate was 1 mol / L.
[0171] <Preparation of the diaphragm> A porous polyethylene film with a thickness of 7μm (supplied by Celgard) is used.
[0172] <Preparation of Secondary Batteries> The positive electrode, separator, and negative electrode prepared above are stacked in sequence, with the separator acting as a separator between the positive and negative electrode. Then, the four corners of the entire stacked structure are fixed with tape to obtain the electrode assembly of the stacked structure. The electrode assembly is placed in an aluminum-plastic film outer packaging foil and dehydrated at 80°C. The prepared electrolyte is then injected. After vacuum sealing, standing, formation, shaping, and capacity testing, a secondary battery is obtained. The formation temperature is 80°C, and the formation standing time is 2 hours.
[0173] Example 2 Except for the preparation of the metal layer in <Preparation of Composite Current Collector>, which differs from Example 1, the rest is the same as Example 1.
[0174] The method for preparing the metal layer in this embodiment includes the following steps: Ni / Cu alloy powder (Ni powder to Cu powder mass ratio of 3:1, average particle size of 50 nm), titanium carbide nanowires (aspect ratio of 60), and polyvinylpyrrolidone (polyvinylpyrrolidone) with a mass percentage of 94% were added to ethanol and ultrasonicated at 600 W for 30 min to obtain a metal layer slurry with a solid content of 40%. Under the conditions of 50kV voltage, 15cm spray gun distance, 80℃ substrate temperature and 0.3MPa carrier gas pressure, the metal layer slurry was sprayed onto the surface of the second polymer layer to obtain a metal layer with a thickness of 2μm. Next, at a wavelength of 365 nm and an intensity of 80 mW / cm 2 Irradiation under ultraviolet light for 10 seconds causes the formation of Si-OM chemical bonds between the second polymer layer and the metal layer, where M is a metal element in the metal layer.
[0175] Example 3 Except for the preparation of the first polymer layer in <Preparation of Composite Current Collector>, which differs from Example 2, the rest is the same as Example 2.
[0176] In this embodiment, the preparation method of the first polymer layer is carried out in the following steps: Step 1, Preparation of spinning solution: Dissolve polyarylamide in a DMAC / acetone mixed solvent (DMAC and acetone volume ratio of 7:3), add lithium chloride and stir until homogeneous to obtain the first spinning solution; wherein, based on the mass of the first spinning solution, the mass percentage of polyarylamide is 12% and the mass percentage of lithium chloride is 0.5%; Step 2, Preparation of adhesive solution: Add carboxylated chitosan-modified waterborne polyurethane containing disulfide bonds to a suitable amount of DMAC / acetone mixed solvent (volume ratio 7:3), and stir until completely dissolved to obtain the adhesive solution; wherein, the mass of carboxylated chitosan-modified waterborne polyurethane containing disulfide bonds is 3% of the mass of the first polymer layer; Step 3, Preparation of the second spinning solution: The binder solution from step 2 is slowly added to the first spinning solution and stirred at room temperature for 2 hours to ensure that the binder and polyarylamide are fully mixed and homogeneous, thus obtaining the second spinning solution; Step 4, electrospinning: Under the conditions of 18kV voltage, 15cm receiving distance, 0.8mL / h feed speed, 25℃ ambient temperature and 28% ambient humidity, the second spinning solution in step 3 is electrospinned to obtain a nanofiber membrane with a thickness of 12um. The fiber diameter in the nanofiber membrane is 500nm and the porosity is 62%, which is referred to as the first nanofiber membrane. Step 5, ZIF-8 in situ growth: The first nanofiber membrane was immersed in a 0.1M Zn(NO3)2·6H2O methanol solution, and then transferred to a 0.4M 2-methylimidazole solution. The membrane was hydrothermally reacted at 60℃ for 2 hours to form a ZIF-8 coating (based on the mass of the first nanofiber membrane, the loading of the ZIF-8 coating was 42wt%), thus obtaining the second nanofiber membrane. Step 6, melting of DOPO: Dry the DOPO solid powder under vacuum at 80°C for 4 hours to remove adsorbed moisture; then heat it at 100°C to melt it and obtain liquid DOPO. Step 7, Vacuum Degassing and DOPO Impregnation: The second nanofiber membrane is placed in a vacuum drying oven and degassed for 60 minutes at 80°C and a vacuum degree ≤133Pa to fully remove air from the pores of the second nanofiber membrane; then, the valve of the DOPO storage tank of the vacuum impregnation device is opened, allowing liquid DOPO to flow in under atmospheric pressure and completely impregnate the second nanofiber membrane; the liquid DOPO spontaneously permeates into the pores of the second nanofiber membrane under capillary action and fills the gaps between the ZIF-8 crystals; maintaining a vacuum degree ≤133Pa, impregnation continues for 20 minutes to ensure that DOPO fully fills all interconnected pores; after impregnation, the pressure is slowly released to atmospheric pressure to obtain the third nanofiber membrane; Step 8, Drying and curing: The third nanofiber membrane is dried at 80°C and vacuum degree ≤133Pa for 4 hours to cure DOPO; DOPO solidifies in the nanofiber pores, firmly bonding ZIF-8 crystals and polyamide nanofibers together to form composite particles, thus obtaining a nanofiber membrane containing composite particles; wherein, the mass ratio of ZIF-8 to DOPO is 2:1. Step 9, hot pressing: The nanofiber membrane containing composite particles is placed in a mold and held at 100°C and 10MPa for 5 minutes. After cooling, a first polymer layer with a thickness of 10μm is obtained.
[0177] Example 4 Except for the difference in the mass percentage of binder in the first polymer layer of <Preparation of Composite Current Collector> compared to Example 3, the rest is the same as in Example 3.
[0178] In this embodiment, the adhesive content in the first polymer layer is 5% by mass.
[0179] Example 5 Except for the difference in the mass percentage of binder in the first polymer layer of <Preparation of Composite Current Collector> compared to Example 3, the rest is the same as in Example 3.
[0180] In this embodiment, the adhesive content in the first polymer layer is 8% by mass.
[0181] Example 6 Except for the difference in the mass percentage of binder in the first polymer layer of <Preparation of Composite Current Collector> compared to Example 3, the rest is the same as in Example 3.
[0182] In this embodiment, the adhesive content in the first polymer layer is 10% by mass.
[0183] Example 7 Except for the preparation of the second spinning solution in the first polymer layer in the <Preparation of Composite Current Collector>, which is different from Example 3, the rest is the same as Example 3.
[0184] The first polymer layer in this embodiment was prepared according to the following experimental steps: Step 1, preparing the spinning solution: Dissolve polyarylamide in a DMAC / acetone mixed solvent (the volume ratio of DMAC to acetone is 7:3), add lithium chloride and stir evenly to obtain the first spinning solution; based on the mass of the first spinning solution, the mass percentage of polyarylamide is 12% and the mass percentage of lithium chloride is 0.5%.
[0185] Step 2: Prepare the first conductive agent (carbon nanotube / graphene hybrid material) as described above.
[0186] Step 3: Prepare a disulfide-bonded binder (carboxylated chitosan-modified disulfide-bonded aqueous polyurethane) as described above. Step 4: Prepare the binder solution and the conductive agent solution. Carboxylated chitosan-modified waterborne polyurethane containing disulfide bonds was added to a suitable amount of DMAC / acetone mixed solvent (volume ratio 7:3) and stirred until completely dissolved to obtain an adhesive solution. Carbon nanotube / graphene hybrid material was added to deionized water and dispersed under ultrasonic power of 400W for 2 hours to obtain a conductive agent dispersion.
[0187] Step 5, preparation of the second spinning solution: The binder solution and conductive agent dispersion obtained in step 4 are added sequentially to the first spinning solution obtained in step 1, and stirred and mixed evenly to obtain the second spinning solution; wherein, based on the mass of the first polymer layer, the mass percentage of carboxylated chitosan-modified waterborne polyurethane containing disulfide bonds is 5%, and the mass percentage of carbon nanotube / graphene hybrid material is 5%.
[0188] Example 8 Except for the mass percentage of the first conductive agent in the first polymer layer of <Preparation of Composite Current Collector>, which differs from that in Example 7, the rest is the same as in Example 7.
[0189] In this embodiment, the mass percentage of the first conductive agent in the first polymer layer is 10%.
[0190] Example 9 Except for the mass percentage of the first conductive agent in the first polymer layer of <Preparation of Composite Current Collector>, which differs from that in Example 7, the rest is the same as in Example 7.
[0191] In this embodiment, the mass percentage of the first conductive agent in the first polymer layer is 15%.
[0192] Example 10 Except for the mass percentage of the first conductive agent in the first polymer layer of <Preparation of Composite Current Collector>, which differs from that in Example 7, the rest is the same as in Example 7.
[0193] In this embodiment, the mass percentage of the first conductive agent in the first polymer layer is 18%.
[0194] Example 11 Except for the thickness of the second polymer layer in the <Preparation of Composite Current Collector>, which differs from that in Example 8, the rest is the same as in Example 8.
[0195] The thickness of the second polymer layer in this embodiment is 0.1 μm.
[0196] Example 12 Except for the thickness of the second polymer layer in the <Preparation of Composite Current Collector>, which differs from that in Example 8, the rest is the same as in Example 8.
[0197] The thickness of the second polymer layer in this embodiment is 0.2 μm.
[0198] Example 13 Except for the thickness of the second polymer layer in the <Preparation of Composite Current Collector>, which differs from that in Example 8, the rest is the same as in Example 8.
[0199] The thickness of the second polymer layer in this embodiment is 0.8 μm.
[0200] Example 14 Except for the thickness of the second polymer layer in the <Preparation of Composite Current Collector>, which differs from that in Example 8, the rest is the same as in Example 8.
[0201] The thickness of the second polymer layer in this embodiment is 1 μm.
[0202] Example 15 Except for the aspect ratio of the titanium carbide nanowires in the metal layer of <Preparation of Composite Current Collector>, which is different from that in Example 8, the rest is the same as in Example 8.
[0203] In this embodiment, the aspect ratio of the titanium carbide nanowires in the metal layer is 80.
[0204] Example 16 Except for the aspect ratio of the titanium carbide nanowires in the metal layer of <Preparation of Composite Current Collector>, which is different from that in Example 8, the rest is the same as in Example 8.
[0205] In this embodiment, the aspect ratio of the titanium carbide nanowires in the metal layer is 100.
[0206] Example 17 Except for the aspect ratio of the titanium carbide nanowires in the metal layer of <Preparation of Composite Current Collector>, which is different from that in Example 8, the rest is the same as in Example 8.
[0207] In this embodiment, the aspect ratio of the titanium carbide nanowires in the metal layer is 45.
[0208] Example 18 Except for the type of thermally conductive fiber in the metal layer of <Preparation of Composite Current Collector>, which is different from that in Example 8, the rest is the same as in Example 8.
[0209] In this embodiment, the thermally conductive fibers in the metal layer are GaN fibers with an aspect ratio of 60.
[0210] Example 19 Except for the type of thermally conductive fiber in the metal layer of <Preparation of Composite Current Collector>, which is different from that in Example 8, the rest is the same as in Example 8.
[0211] In this embodiment, the thermally conductive fiber in the metal layer is BN fiber, and the aspect ratio of the BN fiber is 60.
[0212] Example 20 Except for the mass percentage of Ni / Cu alloy powder and titanium carbide nanowires in the metal layer of <Preparation of Composite Current Collector>, which differs from Example 8, the rest is the same as Example 8.
[0213] In this embodiment, the mass percentage of Ni / Cu alloy powder in the metal layer is 98%, and the mass percentage of titanium carbide nanowires is 0%.
[0214] Example 21 Except for the preparation of the composite current collector, which differs from Example 2, everything else is the same as in Example 2.
[0215] This embodiment of <Preparation of Composite Current Collector> includes the following steps: <Preparation of Composite Current Collectors> Preparation of the first polymer layer: Polyetheretherketone (PEEK) was dissolved in a mixed solvent of concentrated sulfuric acid and trifluoroacetic acid (volume ratio of concentrated sulfuric acid to trifluoroacetic acid was 1:1), and lithium chloride was added and stirred until homogeneous to obtain a spinning solution. Based on the mass of the spinning solution, the mass percentage of PEEK was 10%, and the mass percentage of lithium chloride was 0.5%. Under the conditions of 18kV voltage, 15cm receiving distance, 0.8mL / h propulsion speed, 25℃ ambient temperature, and 28% ambient humidity, the spinning solution was electrospun to obtain a first nanofiber membrane with a thickness of 12µm. The fiber diameter in the first nanofiber membrane was 500nm, and the porosity was 62%. The first nanofiber membrane was immersed in a 0.1M Cr(NO3)3·9H2O methanol solution, and then transferred to a 0.4M terephthalic acid solution. The membrane was hydrothermally reacted at 120℃ for 4 h to form a MIL-101 coating (based on the mass of the first nanofiber membrane, the loading of the MIL-101 coating was 35 wt%), thus obtaining the second nanofiber membrane. Hexaphenoxycyclotriphosphazene (HPCP) solid powder was dried in a vacuum drying oven at 80°C for 4 hours to remove adsorbed moisture and residual organic solvents; then it was heated and melted at 130°C to obtain liquid HPCP. The second nanofiber membrane was placed in a vacuum drying oven and degassed for 60 min at 120℃ and a vacuum degree ≤133 Pa to fully remove air from the pores of the second nanofiber membrane. Open the valve of the HPCP storage tank of the vacuum impregnation device to allow liquid HPCP to flow in under atmospheric pressure and completely immerse the second nanofiber membrane; the liquid HPCP spontaneously seeps into the pores of the second nanofiber membrane under capillary action and fills the gaps between the MIL-101 crystals; maintain the vacuum degree ≤133 Pa and continue impregnation for 20 min to ensure that HPCP fully fills all the interconnected pores; after impregnation, slowly depressurize to atmospheric pressure to obtain the third nanofiber membrane; The third nanofiber membrane was dried at 80℃ and under a vacuum of ≤133 Pa for 4 hours to solidify HPCP; HPCP solidified in the nanofiber pores, firmly bonding MIL-101 crystals and PEEK nanofibers together to form composite particles, thus obtaining a nanofiber membrane containing composite particles; wherein, the mass ratio of MIL-101 to HPCP was 2:1. The nanofiber membrane containing composite particles was placed in a mold and held at 100°C and 10 MPa for 5 minutes. After cooling, a first polymer layer with a thickness of 10 μm was obtained. Based on the mass of the first polymer layer, the mass percentage of polyether ether ketone (PEEK) was 66% and the mass percentage of composite particles was 34%.
[0216] Preparation of the second polymer layer: A thermosetting polyimide prepolymer (glass transition temperature 320℃) of 75% by mass, silica aerogel (average particle size 200nm) of 23% by mass, and KH-550 silane coupling agent of 2% by mass were added to a ball mill and ball-milled at 300 rpm for 2 hours. Then, ethyl acetate was added and stirred evenly to obtain a second polymer layer slurry with a viscosity of 320 mPa·s. Under the conditions of a coating speed of 8 m / min and a bar spacing of 10 μm, the second polymer layer slurry was coated on one side surface of the first polymer layer and pre-cured at 120°C for 2 min; then it was treated for 30 s under Ar / O2 mixed gas (Ar:O2 volume ratio of 4:1) and power of 300 W to obtain a second polymer layer with silicon-oxygen bonds and a thickness of 0.5 μm. Preparation of the metal layer: Ni / Cu alloy powder (Ni powder to Cu powder mass ratio of 3:1, average particle size of 80 nm), titanium carbide nanowires (aspect ratio of 60) with a mass percentage of 94%, and polyvinylpyrrolidone with a mass percentage of 2% were added to ethanol and ultrasonicated at 600 W for 30 min to obtain a metal layer slurry with a solid content of 40%. Under the conditions of 50kV voltage, 15cm spray gun distance, 80℃ substrate temperature and 0.3MPa carrier gas pressure, the metal layer slurry was sprayed onto the surface of the second polymer layer to obtain a metal layer with a thickness of 2μm. Next, at a wavelength of 365 nm and an intensity of 80 mW / cm 2 Irradiation under ultraviolet light for 10 seconds causes the formation of Si-OM chemical bonds between the second polymer layer and the metal layer, where M is a metal element in the metal layer.
[0217] Comparative Example 1 Except for the preparation of the first polymer layer in <Preparation of Composite Current Collector>, which differs from Example 2, the rest is the same as Example 2.
[0218] The preparation of the first polymer layer in this embodiment includes the following steps: Polyarylamide was dissolved in a DMAC / acetone mixed solvent (DMAC to acetone volume ratio of 7:3), and lithium chloride was added and stirred until homogeneous to obtain a spinning solution. Based on the mass of the spinning solution, the mass percentage of polyarylamide was 12%, and the mass percentage of lithium chloride was 0.5%. Under the conditions of 18kV voltage, 15cm receiving distance, 0.8mL / h propulsion speed, 25℃ ambient temperature, and 28% ambient humidity, the spinning solution was electrospun to obtain a first nanofiber membrane with a thickness of 12µm. The fiber diameter in the first nanofiber membrane was 500nm, and the porosity was 62%. DOPO solid powder was heated and melted at 100°C to obtain liquid DOPO; The first nanofiber membrane was placed in a vacuum drying oven and degassed for 60 min at 80°C and a vacuum degree ≤133 Pa to fully remove air from the pores of the first nanofiber membrane. Open the valve of the DOPO storage tank of the vacuum impregnation device to allow liquid DOPO to flow in and completely immerse the first nanofiber membrane under atmospheric pressure; the liquid DOPO spontaneously permeates into the pores of the first nanofiber membrane under capillary action, maintaining a vacuum of ≤133 Pa, and continue impregnation for 20 min to ensure that DOPO fully fills all interconnected pores; after impregnation, slowly depressurize to atmospheric pressure to obtain the second nanofiber membrane; The second nanofiber membrane was dried at 80°C and under a vacuum of ≤133 Pa for 4 hours to solidify DOPO; DOPO solidified in the pores of the nanofibers to form composite particles, thus obtaining a nanofiber membrane containing DOPO. A nanofiber membrane containing DOPO was placed in a mold and held at 100°C and 10 MPa for 5 minutes. After cooling, a first polymer layer with a thickness of 10 μm was obtained. Based on the mass of the first polymer layer, the mass percentage of polyarylamide was 75% and the mass percentage of DOPO was 25%.
[0219] Comparative Example 2 Except for the preparation of the first polymer layer in <Preparation of Composite Current Collector>, which differs from Example 2, the rest is the same as Example 2.
[0220] The preparation of the first polymer layer in this embodiment includes the following steps: DOPO solid powder was vacuum dried at 80℃ for 4 hours to remove adsorbed moisture. Then, the dried DOPO solid powder was added to a mixer at a mass ratio of 1:3 with low-density polyethylene (using Sinopec Yanshan Petrochemical LDPE 1F7B, melt index 7.0 g / 10 min) and mixed at 150℃ and 80 rpm for 8 minutes. After cooling, the mixture was pelletized and pulverized to obtain DOPO@PE composite particles with a particle size Dv50=5μm. DOPO@PE composite particles were immersed in a 0.5 wt% methyltrimethoxysilane ethanol solution for 30 min, and then cured in an oven at 120 °C for 1 h to obtain DOPO@PE composite particles with a hydrophobic organic layer on the surface. Polyarylamide (PA) was dissolved in a DMAC / acetone mixed solvent (DMAC to acetone volume ratio of 7:3), and lithium chloride was added and stirred until homogeneous to obtain a polymer solution. Based on the mass of the polymer solution, the mass percentage of polyarylamide was 12%, and the mass percentage of lithium chloride was 0.5%. DOPO@PE composite particles with a hydrophobic organic layer on the surface were added to a DMAC / acetone mixed solvent (the volume ratio of DMAC to acetone was 7:3) and ultrasonically dispersed at 60℃ and 200W for 30 min to obtain a DOPO@PE dispersion with a mass percentage of 5wt%. The DOPO@PE dispersion was added dropwise to the PA solution and stirred at 200 rpm for 2 hours to obtain the spinning solution; the mass ratio of DOPO@PE composite particles to PA was 25:75. Under conditions of 18kV voltage, 15cm receiving distance, 0.8mL / h propulsion speed, 25℃ ambient temperature, and 28% ambient humidity, the spinning solution was electrospun to obtain a nanofiber membrane with a thickness of 12cm. The nanofiber membrane had a fiber diameter of 500nm and a porosity of 62%. The nanofiber membrane was dried at 80°C and a vacuum degree ≤133 Pa for 4 hours to obtain a nanofiber membrane containing flame retardant material. A nanofiber membrane containing flame-retardant material was placed in a mold and held at 100°C and 10 MPa for 5 minutes. After cooling, a first polymer layer with a thickness of 10 μm was obtained. Based on the mass of the first polymer layer, the mass percentage of polyarylamide was 75% and the mass percentage of flame-retardant material was 25%.
[0221] Comparative Example 3 Except for the preparation of the composite current collector, which differs from Example 2, the rest is the same as Example 2.
[0222] <Preparation of Composite Current Collectors> Preparation of the first polymer layer: Polyarylamide was dissolved in a DMAC / acetone mixed solvent (DMAC to acetone volume ratio of 7:3), and lithium chloride was added and stirred until homogeneous to obtain a spinning solution. Based on the mass of the spinning solution, the mass percentage of polyarylamide was 12%, and the mass percentage of lithium chloride was 0.5%. Under the conditions of 18kV voltage, 15cm receiving distance, 0.8mL / h propulsion speed, 25℃ ambient temperature, and 28% ambient humidity, the spinning solution was electrospun to obtain a nanofiber membrane with a thickness of 12µm. The nanofiber membrane has a fiber diameter of 500nm and a porosity of 62%. The nanofiber membrane was immersed in a 0.1M Zn(NO3)2·6H2O methanol solution, and then transferred to a 0.4M 2-methylimidazole solution. The membrane was then subjected to a hydrothermal reaction at 60℃ for 2 h to form a ZIF-8 coating (based on the mass of the first nanofiber membrane, the loading of the ZIF-8 coating was 42 wt%), thus obtaining the second nanofiber membrane. DOPO solid powder was vacuum dried at 80°C for 4 hours to remove adsorbed moisture; then it was heated and melted at 100°C to obtain liquid DOPO. The second nanofiber membrane was placed in a vacuum drying oven and degassed for 60 min at 80°C and a vacuum degree ≤133 Pa to fully remove air from the pores of the second nanofiber membrane. Open the valve of the DOPO storage tank of the vacuum impregnation device to allow liquid DOPO to flow in under atmospheric pressure and completely immerse the second nanofiber membrane; the liquid DOPO spontaneously permeates into the pores of the second nanofiber membrane under capillary action and fills the gaps between the ZIF-8 crystals; maintain the vacuum degree ≤133 Pa and continue impregnation for 20 min to ensure that DOPO fully fills all the interconnected pores; after impregnation, slowly depressurize to atmospheric pressure to obtain the third nanofiber membrane; The third nanofiber membrane was dried at 80℃ and under a vacuum of ≤133 Pa for 4 hours to solidify DOPO. DOPO solidified in the nanofiber pores, firmly bonding ZIF-8 crystals and polyamide nanofibers together to form composite particles, thus obtaining a nanofiber membrane containing composite particles. The mass ratio of ZIF-8 to DOPO was 2:1. The nanofiber membrane containing composite particles was placed in a mold and held at 100°C and 10 MPa for 5 minutes. After cooling, a first polymer layer with a thickness of 10 μm was obtained. Based on the mass of the first polymer layer, the mass percentage of polyarylamide was 61% and the mass percentage of composite particles was 25%.
[0223] Preparation of the metal layer: Ni / Cu alloy powder (Ni powder to Cu powder mass ratio of 3:1, average particle size of 80 nm), titanium carbide nanowires (aspect ratio of 60) with a mass percentage of 94%, and polyvinylpyrrolidone with a mass percentage of 2% were added to ethanol and ultrasonicated at 600 W for 30 min to obtain a metal layer slurry with a solid content of 40%. Under conditions of 50kV voltage, 15cm spray gun distance, 80℃ substrate temperature, and 0.3MPa carrier gas pressure, the metal layer slurry was sprayed onto one side surface of the first polymer layer to obtain a metal layer with a thickness of 2μm.
[0224] The performance parameters of the composite current collectors obtained in the examples and comparative examples are shown in Table 1.
[0225] Performance testing (1) Surface resistance test: The surface resistance of the composite current collector was measured using the four-probe method (unit: mΩ·cm). -2 Test equipment: Keithley 2400 source meter, four-probe resistivity meter. Test conditions: temperature 25℃, relative humidity 50%. Five points were measured for each sample, and the average value was taken.
[0226] (2) Interlayer peel strength test: The interlayer peel strength between the polymer layer and the metal layer was measured using the 90° peel method (unit: N·cm). -1 Testing equipment: Instron 5967 universal testing machine. Peeling speed: 50 mm / min. Three points were measured for each sample, and the average value was taken.
[0227] (3) 180℃ Thermal Runaway Test: First, preheat the thermal abuse test chamber to room temperature, set the target temperature to 180℃, and the heating rate is usually 5℃ / min (adjustable range 5~20℃ / min). Connect the secondary battery and voltage acquisition device to ensure that there is no risk of short circuit. Next, place the secondary battery in the test chamber. If gas generation needs to be collected, place it in a sealed explosion-proof chamber, connect the pressure sensor and gas sampling pipeline, and check the sealing. Then, start the heating program to heat up to 180℃ at the set rate and hold the temperature for 30 minutes (or adjust according to the standard). At the same time, monitor the secondary battery temperature, voltage, pressure and other parameters in real time and record the data. When the voltage drops rapidly to 0V, the temperature rise rate dT / dt>1℃ / s (lasting for more than 3 seconds), the secondary battery catches fire or explodes, or the temperature exceeds 300℃, it is determined that the secondary battery has thermal runaway and the test is stopped. Finally, plot the temperature-time curve, voltage-time curve, and pressure-time curve. If gas is collected, analyze the components (such as H2, CO, CO2, CH4, etc.) using gas chromatography-mass spectrometry and record key parameters such as thermal runaway trigger temperature, maximum temperature, temperature rise rate, and gas production.
[0228] (4) Conductivity retention test after 500 cycles: The secondary battery was subjected to 500 charge-discharge cycles (voltage range 2.8-4.2V, current density 1C), and the conductivity change before and after the cycles was measured. The retention rate (unit: %) was calculated. Test equipment: Neware battery test system.
[0229] (5) Self-healing efficiency test: The composite current collector sample was bent (bending radius 5mm, bending angle ±90°, 10 cycles), and the conductivity before and after the treatment was measured. The self-healing efficiency (unit: %) was calculated.
[0230] (6) Post-cycle flame retardant efficiency test: After 500 charge-discharge cycles, the composite current collector sample was subjected to a 180℃ thermal runaway test. The thermal runaway time (unit: s) was recorded and compared with the sample that was not cycled to examine the effect of cycle aging on flame retardant performance.
[0231] (7) Surface density and thickness test: Surface density was measured using a precision electronic balance (unit: g·m⁻²); thickness was measured using a micrometer (unit: μm). Five points were measured for each sample, and the average value was taken.
[0232] (8) Thermal runaway temperature test: The secondary battery was placed in a high-temperature oven and heated from 25°C to 400°C at a heating rate of 5°C / min. The temperature at which thermal runaway occurred was recorded (unit:°C). An ARC accelerated calorimeter was used; thermal runaway was determined by dT / dt ≥ 1°C / min, and the temperature was recorded (°C).
[0233] (9) SEM+EDS test: Field emission SEM was used to observe the MOF load morphology, and EDS was used to confirm the distribution of ZIF-8, DOPO, Si, Ti and other elements.
[0234] The test results are shown in Table 2 below.
[0235] Table 1 Table 2 As can be seen from the experimental data in Table 2, the composite current collector of this application can prolong the runaway time of the secondary battery at 180℃. Time can improve the safety performance of secondary batteries and also enhance their capacity retention rate.
[0236] Finally, it should be noted that the above embodiments are used to illustrate the technical solutions of this application and not to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.
Claims
1. A composite current collector, characterized in that, It includes a first polymer layer, a metal layer, and a second polymer layer located between the first polymer layer and the metal layer; The first polymer layer comprises composite particles; The composite particles include flame-retardant materials and metal-organic framework materials, wherein the metal-organic framework materials have a porous structure, and the flame-retardant materials are located on the surface and / or within the pores of the metal-organic framework materials.
2. The composite current collector as described in claim 1, characterized in that, The first polymer layer contains an adhesive, and the adhesive contains disulfide bonds.
3. The composite current collector as described in claim 2, characterized in that, In the first polymer layer, the adhesive has a mass percentage content of 3-10%; And / or, the adhesive comprises at least one of the following: carboxylated chitosan-modified disulfide-containing aqueous polyurethane, 2,2'-dithiodibenzoic acid, polyester polyol containing dithiodipropionate bonds, disulfide dichloride, bis(4-hydroxyphenyl) disulfide, bis(2-hydroxyethyl) disulfide, epoxy resin, sulfur, polyethylene glycol containing dithiodipropionate blocks, and zinc salt of 1-vinyl-3-ethylimidazolium dithiocarboxylate.
4. The composite current collector as described in claim 1, characterized in that, The second polymer layer has silicon-oxygen bonds; there is a Si-OM chemical bond between the second polymer layer and the metal layer, where M is a metal element in the metal layer.
5. The composite current collector as described in claim 1, characterized in that, The thickness of the second polymer layer is 0.2~1.0 μm.
6. The composite current collector as described in claim 1, characterized in that, The second polymer layer comprises the following components in weight percentage: 70-80% second polymer, 20-30% aerogel, and 1-2% silane coupling agent.
7. The composite current collector as described in claim 6, characterized in that, Meet at least one of the following: (1) The glass transition temperature of the second polymer is greater than 300°C; (2) The second polymer includes at least one of polyimide, siloxane-modified polyimide, silsesquioxane polymer, aryl-substituted polysiloxane, geopolymer, organometallic polymer-siloxane hybrid, and silane-polyethylene glycol-acrylate polymer; (3) The silane coupling agent includes at least one of aminosilane coupling agents, vinylsilane coupling agents, and epoxysilane coupling agents; (4) The aerogel includes at least one of inorganic aerogel and organic aerogel.
8. The composite current collector as described in claim 7, characterized in that, Meet at least one of the following: (1) The aminosilane coupling agent includes at least one of aminopropyl-triethoxysilane, aminopropyl-trimethoxysilane, di-(trimethoxysilylpropyl)amine, N-(β-aminoethyl)-γ-aminopropyl-trimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyl-methyl-trimethoxysilane; (2) The vinyl silane coupling agent includes at least one of vinyltrichlorosilane, vinyltriethoxysilane, vinyl-tri-(2-methoxyethoxy)silane, and vinyltrimethoxysilane; (3) The epoxy silane coupling agent includes at least one of γ-glycidylpropyltrimethoxysilane and 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane; (4) The inorganic aerogel includes at least one of silica aerogel, titanium dioxide aerogel, zirconium dioxide aerogel, alumina aerogel, magnesium oxide aerogel, vanadium oxide aerogel, boron nitride aerogel or titanium nitride aerogel. (5) The organic aerogel includes at least one of polymethyl methacrylate aerogel, polystyrene aerogel or polyimide aerogel.
9. The composite current collector as described in claim 1, characterized in that, The first polymer layer further includes a first conductive agent, which comprises a carbon material.
10. The composite current collector as described in claim 9, characterized in that, In the first polymer layer, the mass percentage of the first conductive agent is 10-18%; And / or, the carbon material includes at least one of carbon nanotubes, graphene, carbon nanofibers, and carbon nanotube / graphene hybrid materials.
11. The composite current collector as described in claim 1, characterized in that, In the first polymer layer, the mass percentage of the composite particles is 20-30%.
12. The composite current collector as described in claim 1, characterized in that, The metal layer comprises the following components by mass percentage: 90-95% second conductive agent, 3-5% thermally conductive fiber, and 2-5% dispersant; the second conductive agent comprises metal particles.
13. The composite current collector as described in claim 12, characterized in that, Meet at least one of the following: (a) The average particle size of the metal particles is 50-100 nm; (b) The aspect ratio of the thermally conductive fiber is greater than 30; (c) The thermally conductive fiber includes at least one of SiC fiber, Si3N4 fiber, Mg3N2 fiber, GaN fiber, AlN fiber, and BN fiber; (d) The dispersant includes at least one of polyvinylpyrrolidone, polyacrylic acid, polyacrylamide, lignin sulfonate, sodium carboxymethyl cellulose, hydroxyethyl cellulose, urea, citric acid, and sodium dodecylbenzene sulfonate.
14. The composite current collector as described in claim 1, characterized in that, Meet at least one of the following: (A) The flame retardant material includes at least one of inorganic flame retardant materials and organic flame retardant materials; (B) The metal-organic framework material includes at least one of zeolite imidazole framework, cobalt dimethylimidazolium, iron-containing organometallic framework material, zinc-containing organometallic framework material or chromium-containing organometallic framework material. (C) The thickness of the first polymer layer is 8~10 μm; (D) The thickness of the metal layer is 1~3μm.
15. A secondary battery, characterized in that, It includes a positive electrode, a negative electrode, and a separator, wherein the separator is located between the positive electrode and the negative electrode, and the positive electrode and / or the negative electrode includes a composite current collector as described in any one of claims 1 to 14.
16. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 15.