An electrolyte membrane, a secondary battery, and an electrical device.
By distributing inorganic solid electrolyte particles in a polymer matrix and forming COM covalent bonds, the problem of high interfacial impedance of all-solid electrolytes is solved, and the high ionic conductivity and mechanical strength are improved, thereby enhancing the safety and stability of secondary batteries.
Patent Information
- Application Number
- CN202611289758.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-10
AI Technical Summary
Traditional liquid electrolytes pose safety hazards such as leakage and flammability and explosion. Furthermore, all-solid electrolytes have high interfacial impedance between the inorganic and organic phases, and existing interfacial modification methods are complex and costly, making it difficult to achieve large-scale production.
By distributing inorganic solid electrolyte particles in a polymer matrix and forming COM covalent bonds on their surface, a continuous, low-impedance lithium-ion transport channel is constructed, and a one-step thermal treatment process is used to achieve interface cleaning and chemical bonding.
It significantly reduces interfacial impedance, improves the ionic conductivity and mechanical strength of the electrolyte membrane, enhances resistance to lithium dendrite penetration, and improves the cycle stability and safety of secondary batteries.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This application belongs to the field of battery technology, and particularly relates to an electrolyte membrane, a secondary battery, and an electrical device. Background Technology
[0002] With the rapid development of electric vehicles and the large-scale energy storage market, the demand for high-safety, high-energy-density rechargeable lithium batteries is becoming increasingly urgent. Traditional liquid electrolytes pose safety hazards such as leakage and flammability / explosion, driving all-solid-state batteries to become a key development direction for next-generation battery technology. Among various solid electrolytes, organic-inorganic composite polymer electrolytes (CPEs) have received extensive research due to their combination of the good flexibility and film-forming properties of organic polymers with the high ionic conductivity and mechanical strength of inorganic solid electrolytes. However, their practical application is limited by significant internal interfacial impedance. This bottleneck stems primarily from three aspects: First, highly active inorganic solid electrolyte particles (especially LLZO) are extremely sensitive to air. Upon exposure, an insulating layer of lithium carbonate and lithium hydroxide impurities quickly forms on their surface. This insulating impurity layer is difficult to remove efficiently and thoroughly, severely hindering the cross-interfacial transport of lithium ions like a "wall." Second, due to significant differences in surface energy, polarity, and other physicochemical properties between inorganic solid electrolytes and organic polymers, their compatibility is poor. Mixing them usually results in a simple physical mixture, forming a loose "point contact" weak bonding interface. This interface contains a large number of voids... The interface of gaps and defects not only restricts the effective transport channels of lithium ions, resulting in high internal impedance, but also easily becomes a site for preferential growth of lithium dendrites. Third, existing interface modification methods (such as pre-acid washing, ball milling, or surface coating of solid electrolytes) have obvious limitations. Their processes are complex, adding extra production steps and costs, and they have poor compatibility with large-scale production. Furthermore, the pre-treated solid electrolyte may face the risk of secondary pollution in subsequent processes. At the same time, physical ball milling may damage the crystal structure of the solid electrolyte, and the compatibility between the pre-coating layer and the polymer matrix is also difficult to guarantee, so the interface problem has not been fundamentally solved. Summary of the Invention
[0003] In order to solve at least one of the problems existing in the prior art, one of the objectives of this application is to provide an electrolyte membrane that can enhance the simple physical mixing between organic and inorganic phases into a strong chemical bond, thereby reducing interfacial voids and constructing a continuous, low-impedance lithium-ion transport channel.
[0004] The second objective of this application is to provide a secondary battery.
[0005] The third objective of this application is to provide an electrical appliance.
[0006] To achieve the above objectives, the technical solution adopted in this application is as follows: An electrolyte membrane, comprising: A polymer matrix containing -CO- segments; Inorganic solid electrolyte particles are distributed in the polymer matrix, and the inorganic solid electrolyte particles contain a functional metal element M, wherein the functional metal element M includes at least one of a transition metal element, a group IIIA metal element, or a group IVA metal element. The inorganic solid electrolyte particles and the polymer matrix have COM covalent bonds.
[0007] The electrolyte membrane according to the first aspect of this application has at least the following beneficial effects: This application elevates the simple physical mixing between the organic and inorganic phases to a robust chemical bond, creating strong molecular bridge connections and continuous high-speed ion channels. It forms a gradient interface structure extending from the surface of the inorganic solid electrolyte particles to the polymer matrix, which not only effectively reduces interfacial porosity and optimizes and strengthens the two-phase interface, but also constructs a continuous, low-impedance lithium-ion transport channel, significantly reducing interfacial impedance and effectively improving the room-temperature ionic conductivity of the electrolyte membrane. Furthermore, it significantly enhances the mechanical strength of the interface and its resistance to lithium dendrite penetration, thereby improving the overall electrochemical performance of the electrolyte membrane.
[0008] In some embodiments of this application, the polymer matrix includes one of polyethylene oxide, polypropylene oxide, poly(1,3-dioxolane), polytetrahydrofuran, homopolymer formaldehyde, polyvinyl carbonate, or poly(ε-caprolactone).
[0009] In some embodiments of this application, the functional metal element includes at least one of lanthanum, zirconium, tantalum, aluminum, germanium, or titanium.
[0010] In some embodiments of this application, the inorganic solid electrolyte particles include at least one of lithium lanthanum zirconium oxide, lithium lanthanum titanium oxide, lithium lanthanum zirconium tantalum oxide, lithium titanium aluminum phosphate, or lithium germanium aluminum phosphate.
[0011] In some embodiments of this application, an inorganic interface layer is further provided on the surface of the inorganic solid electrolyte particles, and the inorganic interface layer contains lithium fluoride compounds.
[0012] In some embodiments of this application, the mass ratio of the inorganic solid electrolyte particles to the inorganic interface layer is 1:(0.1~0.25).
[0013] In some embodiments of this application, the thickness of the inorganic interface layer is 3nm to 10nm.
[0014] In some embodiments of this application, lithium salts are also distributed in the polymer matrix; the lithium salts include at least one of lithium fluorophosphate, lithium sulfonylimide, lithium borate, or lithium organic sulfonate.
[0015] In some embodiments of this application, the lithium fluorophosphate salt includes lithium hexafluorophosphate, lithium difluorophosphate, or a combination thereof.
[0016] In some embodiments of this application, the sulfonylimide lithium salt includes lithium bis(trifluoromethanesulfonylimide), lithium bis(fluorosulfonylimide), or a combination thereof.
[0017] In some embodiments of this application, the borate lithium salt includes lithium dioxoborate, lithium difluorooxalate borate, or a combination thereof.
[0018] In some embodiments of this application, the organic sulfonate lithium salt includes lithium trifluoromethanesulfonate, lithium perfluorobutylsulfonate, or a combination thereof.
[0019] In some embodiments of this application, the lithium salt includes sulfonylimide lithium salts, and at least one of lithium fluorophosphate, lithium borate, and organic sulfonate lithium salts.
[0020] In some embodiments of this application, the mass ratio of the sulfonylimide lithium salt to the total mass of other types of lithium salts is (5~10):1.
[0021] In some embodiments of this application, the electrolyte membrane comprises, by mass parts: 40 to 80 parts of polymer matrix, 10 to 30 parts of inorganic solid electrolyte particles, and 5 to 15 parts of lithium salt.
[0022] In some embodiments of this application, the density of the electrolyte membrane is 1.5 g / cm³. 3 ~3.0g / cm 3 .
[0023] In some embodiments of this application, the ionic conductivity of the electrolyte membrane is 1.0 × 10⁻⁶. -4 S / cm ~ 1.0 × 10 -3 S / cm.
[0024] In some embodiments of this application, the lithium-ion transference number of the electrolyte membrane is 0.4 to 0.7.
[0025] In some embodiments of this application, the tensile strength of the electrolyte membrane is 1 MPa to 30 MPa.
[0026] In some embodiments of this application, the elongation at break of the electrolyte membrane is 50% to 300%.
[0027] The second aspect of this application provides a secondary battery, including a positive electrode, a negative electrode, and an electrolyte membrane as described in the first aspect of this application, wherein the electrolyte membrane is disposed between the positive electrode and the negative electrode; the secondary battery has a DC internal resistance ≤56mΩ under discharge conditions of 25°C and 0.2C.
[0028] The secondary battery according to the second aspect of this application has at least the following beneficial effects: This application constructs a stable COM covalent bond connection between inorganic solid electrolyte particles and polymer matrix, forming an excellent chemical bond interface layer, which significantly reduces the interfacial impedance of organic-inorganic electrolyte and greatly improves the ionic conductivity of electrolyte membrane, resulting in a secondary battery with strong cycle stability and high capacity.
[0029] In some embodiments of this application, after the secondary battery has been cycled for 1000 hours, the volume expansion rate of the electrolyte membrane is ≤10%.
[0030] A third aspect of this application provides an electrical device including the secondary battery described in the second aspect of this application.
[0031] The electrical equipment according to the third aspect of this application has at least the following beneficial effects: This application utilizes a rechargeable battery with strong cycle stability and high capacity to provide an electrical device equipped with such a battery. Its battery life is significantly improved, its performance is not easily degraded with long-term use, it does not require frequent battery replacement, the whole machine has a long service life and low maintenance cost, it is suitable for long-term stable operation under various working conditions, and the user experience and product economy are greatly improved. Detailed Implementation
[0032] The embodiments of this application are described in detail below. These embodiments are exemplary and are only used to explain this application, and should not be construed as limiting this application. The term "comprising" and other equivalent descriptive methods used in the specification and claims of this application are intended to cover a non-exclusive inclusion, which includes both the content explicitly described in the specification and claims and steps or units that are not described in the specification and claims but are inherent in the product, method, or structure.
[0033] A first aspect of this application provides an electrolyte membrane, comprising: The polymer matrix contains -CO- segments; Inorganic solid electrolyte particles are distributed in a polymer matrix. The inorganic solid electrolyte particles contain a functional metal element M, which includes at least one of a transition metal element, a group IIIA metal element, or a group IVA metal element. There are COM covalent bonds between the inorganic solid electrolyte particles and the polymer matrix.
[0034] This application elevates the simple physical mixing between the organic and inorganic phases to a robust chemical bond, creating strong molecular bridge connections and continuous high-speed ion channels. It forms a gradient interface structure extending from the surface of the inorganic solid electrolyte particles to the polymer matrix, which not only effectively reduces interfacial porosity and optimizes and strengthens the two-phase interface, but also constructs a continuous, low-impedance lithium-ion transport channel, significantly reducing interfacial impedance and effectively improving the room-temperature ionic conductivity of the electrolyte membrane. Furthermore, it significantly enhances the mechanical strength of the interface and its resistance to lithium dendrite penetration, thereby improving the overall electrochemical performance of the electrolyte membrane.
[0035] Metal ions (such as Zr) on the surface of inorganic solid electrolyte particles 4+ La 3+ The oxygen atom in the polymer matrix has empty orbitals (Lewis acid), and the oxygen atom in the polymer matrix has a lone pair of electrons (Lewis base). The two can form a covalent bond (COM). Specific analysis is as follows: First, the metal ions on the surface of inorganic solid electrolyte particles exhibit Lewis acidity, for example, LLZO (Li7La3Zr2O). 12 The surface of the Zr is exposed 4+ La 3+ These are metal cations, which possess empty d or f orbitals and are typical Lewis acid sites with the ability to accept electron pairs. First-principles calculations show that inorganic solid electrolyte particles such as LLZO have a large number of coordinate-unsaturated metal sites on their surface, and these sites have high reactivity.
[0036] Secondly, polymer matrices containing -CO- segments have coordination capabilities. For example, the oxygen atoms in polyethylene oxide (PEO) have lone pairs of electrons and are good Lewis bases. When the -CO- segments approach the surface of inorganic solid electrolyte particles, the lone pairs of electrons of their oxygen atoms will coordinate with the empty orbitals of surface metal ions to form coordinate bonds (M←O coordination).
[0037] Finally, COM covalent bonds are formed, and under Lewis acid catalysis of metal ions, the coordinated activated polymer matrix generates alkoxy anions (-CO). - ), and M metal ions (such as Zr) on the surface of inorganic solid electrolyte particles. 4+ La 3+ COM covalent bonds are formed between polymer chains (e.g., etc.) to chemically anchor the polymer chains to the surface of inorganic particles.
[0038] Methods for characterizing COM bonds include XPS (binding energy shift), FT-IR (characteristic peak changes), MAS NMR (chemical shift), TGA (residual after washing), TEM (interface morphology), and DFT calculations (theoretical prediction). In some embodiments of this invention, XPS and FT-IR are used to characterize COM bonds.
[0039] In some embodiments of this application, the polymer matrix includes one of polyethylene oxide (PEO), polypropylene oxide, poly(1,3-dioxolane) (PDOL), polytetrahydrofuran, homopolymer formaldehyde, polyvinyl carbonate (PVCA), or poly(ε-caprolactone).
[0040] The polymer matrix used in this application can form a more stable chemical bond with inorganic solid electrolyte particles, thereby improving the electrochemical performance of the electrolyte membrane.
[0041] In some embodiments of this application, the polymer matrix is formed by ring-opening polymerization of oxygen-containing heterocyclic monomers.
[0042] During ring-opening polymerization, oxygen-containing heterocyclic monomers can react with functional metal elements in inorganic solid electrolyte particles to form COM covalent bonds, thereby achieving covalent bonding between the polymer matrix and the inorganic solid electrolyte particles. Specifically, the oxygen atom of the oxygen-containing heterocyclic monomer has a lone pair of electrons, acting as a Lewis base, while the metal ions on the surface of the inorganic solid electrolyte particles have empty orbitals, acting as Lewis acids. The two form COM covalent bonds through coordination-ring-opening polymerization. When the oxygen-containing heterocyclic monomer molecule approaches the surface of the inorganic solid electrolyte particle, its oxygen atom's lone pair of electrons coordinates to the empty orbitals of the surface metal ions, forming a coordination bond (M←O coordination). Simultaneously, the CO bond on the oxygen-containing heterocyclic monomer ring is polarized and weakened due to the shift of the oxygen atom's electron cloud towards the metal ion, increasing ring strain and creating conditions for the subsequent ring-opening reaction. Under the catalysis of the metal ion's Lewis acid, the coordinated-activated oxygen-containing heterocyclic monomer undergoes ring opening, generating an alkoxy anion (-O...). - It can attack the next oxygen-containing heterocyclic monomer to undergo ring-opening polymerization, or react with surface metal ions to form COM covalent bonds, chemically anchoring the polymer chain to the surface of inorganic particles.
[0043] In some embodiments of this application, the oxygen-containing heterocyclic monomer includes at least one of epoxy monomers, cyclic carbonates, or cyclic lactones.
[0044] In some embodiments of this application, the epoxy monomer includes at least one of ethylene oxide, propylene oxide, 1,3-dioxolane, tetrahydrofuran, or trioxymethylene.
[0045] In some embodiments of this application, the cyclic carbonate includes at least one of vinylene carbonate, ethylene carbonate, or propylene carbonate.
[0046] In some embodiments of this application, the cyclic lactone includes at least one of ε-caprolactone, β-proprolactone, γ-butyrolactone, or δ-valerolactone.
[0047] This application uses the aforementioned oxygen-containing heterocyclic monomer, which undergoes a coordination-ring-opening polymerization reaction with inorganic solid electrolyte particles to form more stable COM covalent bonds, thereby improving the electrochemical performance of the electrolyte membrane.
[0048] In some embodiments of this application, the functional metal element includes at least one of lanthanum, zirconium, tantalum, aluminum, germanium, or titanium.
[0049] This application uses the aforementioned functional metal elements, resulting in stronger covalent bonds, better interfacial performance, and an electrolyte membrane with superior electrochemical performance.
[0050] In some embodiments of this application, the inorganic solid electrolyte particles include at least one of lithium lanthanum zirconium oxide (LLZO), lithium lanthanum titanium oxide (LLTO), lithium lanthanum zirconium tantalum oxide (LLZTO), lithium titanium aluminum phosphate (LATP), or lithium germanium aluminum phosphate (LAGP).
[0051] Among them, the chemical formula of lithium lanthanum zirconium oxide (LLZO) is Li 7-x La3Zr 2-x O 12 Where 0 ≤ x ≤ 0.6; specifically, it could be Li7La3Zr2O 12 .
[0052] The chemical formula of lithium lanthanum titanium oxide (LLTO) is Li. 3y La 2 / 3-y TiO3, where 0 ≤ y ≤ 0.3; specifically, it can be Li 0.33 La 0.56 TiO3.
[0053] The chemical formula of lithium lanthanum zirconium tantalum oxide (LLZTO) is Li. 5+z La3Zr z Ta 2-z O 12 Where 0 ≤ z ≤ 1.4; specifically, it can be Li 6.5 La3Zr 1.5 Ta 0.5 O 12 .
[0054] Lithium aluminum titanium phosphate (LATP) has the chemical formula Li. 1+m Al m Ti 2-m(PO4)3, where 0 ≤ m ≤ 0.5; specifically, it can be Li 1.3 Al 0.3 Ti 1.7 (PO4)3.
[0055] Lithium aluminum germanium phosphate (LAGP) has the chemical formula Li. 1+n Al n Ge 2-n (PO4)3, where 0 ≤ n ≤ 0.5; specifically, it can be Li 1.3 Al 0.3 Ge 1.7 (PO4)3.
[0056] This application uses the aforementioned inorganic solid electrolyte particles, whose surface metal ions can form more stable covalent bonds with oxygen atoms in the polymer matrix, resulting in better interfacial performance and thus obtaining an electrolyte membrane with superior electrochemical performance.
[0057] In some embodiments of this application, an inorganic interface layer is further provided on the surface of the inorganic solid electrolyte particles, and the inorganic interface layer contains lithium fluoride compounds.
[0058] The inorganic interface layer of this application is not a dense, defect-free, continuous thick film, but rather a nanoscale thin layer generated in situ on the surface of inorganic solid electrolyte particles. When this inorganic interface layer exists in the form of an ultrathin layer, there is charge transfer and interaction between it and the upper organic film. This interaction not only does not block chemical bonding, but also provides a more uniform and stable interface environment for subsequent grafting. While lithium fluoride compounds are chemically inert and do not react with the polymer matrix or oxygen-containing heterocyclic monomers, the inorganic interface layer possesses a low lithium-ion diffusion barrier and excellent electronic insulation. Its presence can stabilize the activated surface of the inorganic solid electrolyte particles, preventing recontamination during polymerization. The polymer chains can form COM covalent bonds with metal ions on the surface of the inorganic solid electrolyte particles through defect sites or grain boundaries in the inorganic interface layer. Furthermore, this inorganic interface layer itself is a lithium-philic interface phase, which can improve the interfacial compatibility between the inorganic solid electrolyte particles and lithium metal, and inhibit lithium dendrite growth. Therefore, the inorganic interface layer of this application has a dual role: it serves as both a protective and functional layer for the cleaned surface, and it also promotes subsequent chemical grafting.
[0059] In some embodiments of this application, the lithium fluoride compound includes lithium fluoride (LiF).
[0060] In some embodiments of this application, the inorganic interface layer is formed by the thermal decomposition of functional additives on the surface of inorganic solid electrolyte particles.
[0061] This application introduces functional additives as multifunctional reaction media, which trigger an ordered, tandem chemical reaction sequence through one-step heat treatment, thereby achieving a seamless connection from "deep cleaning" to "molecular grafting" on the surface of inorganic solid electrolyte particles.
[0062] Functional additives can decompose at alkaline sites on the surface of inorganic solid electrolyte particles under thermal action, forming active fluorides (mainly hydrogen fluoride). These active fluorides can selectively etch and remove impurities (such as Li2CO3) from the surface of inorganic solid electrolyte particles in situ, achieving "targeted surgery" removal of interfacial impurities, resulting in a clean surface. The removal effect is direct, efficient, and thorough, avoiding structural damage that may be caused by physical methods, and fundamentally solving the problem of interfacial ion blockage. Furthermore, a lithium-loving inorganic interfacial layer (mainly composed of lithium fluoride compounds, such as LiF) can be simultaneously constructed on the cleaned surface, achieving both surface cleaning and functionalization.
[0063] In some embodiments of this application, the functional additive includes at least one of fluorocarbonates, fluoroethers, fluorocarboxylic acid esters, or fluorosulfonates.
[0064] In some embodiments of this application, fluorocarbonates include at least one of fluoroethylene carbonate, difluoroethylene carbonate, bis(2,2,2-trifluoroethyl) carbonate, or methyltrifluoroethyl carbonate.
[0065] In some embodiments of this application, the fluorinated ethers include at least one of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl) ether, methyl perfluorobutyl ether, or trifluoroethoxyethylene fluorinated vinyl ether.
[0066] In some embodiments of this application, fluorinated carboxylic acid esters include at least one of trifluoroethanol propionate, difluoroethanol propionate, trifluoroethanol hexanoate, or difluoroethanol hexanoate.
[0067] In some embodiments of this application, fluorosulfonates include at least one of propyl 2,2,3,3,3-pentafluorotrifluoromethanesulfonate, 2,2,3,3-tetrafluoropropyltrifluoromethanesulfonate, 2,2-difluoroethyltrifluoromethanesulfonate, or hexafluoroisopropyltrifluoromethanesulfonate.
[0068] In some specific embodiments of this application, the functional additives include at least one of fluoroethylene carbonate, difluoroethylene carbonate, bis(2,2,2-trifluoroethyl) carbonate, methyltrifluoroethyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether or bis(2,2,2-trifluoroethyl) ether.
[0069] In some embodiments of this application, the mass ratio of inorganic solid electrolyte particles to inorganic interface layer is 1:(0.1~0.25); for example, it can be any value or a range between 1:0.1, 1:0.12, 1:0.15, 1:0.17, 1:0.2, 1:0.22 or 1:0.25.
[0070] In some embodiments of this application, the thickness of the inorganic interface layer is 3nm to 10nm; for example, it can be any value of 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm or 10nm or a range between any two; in some specific embodiments of this application, the thickness of the inorganic interface layer is 3nm to 8nm.
[0071] This application employs an inorganic interface layer with appropriate mass ratio and thickness, which has a uniform and compact structure and can basically or completely cover the surface of inorganic solid electrolyte particles to form a complete interface structure and improve the electrochemical performance of the electrolyte membrane.
[0072] The thickness of the inorganic interface layer can be measured using the high-resolution transmission electron microscopy (HRTEM) cross-sectional method.
[0073] In some embodiments of this application, lithium salts are also distributed in the polymer matrix.
[0074] Adding lithium salts to the polymer matrix can provide migratable lithium ions, forming a lithium ion conduction carrier for the electrolyte membrane, reducing the activation energy of lithium ion migration, forming a continuous lithium ion transport channel, and improving the ionic conductivity of the electrolyte membrane.
[0075] In some embodiments of this application, the lithium salt includes at least one of lithium fluorophosphate, lithium sulfonylimide, lithium borate, or organic sulfonate lithium salt.
[0076] In some embodiments of this application, lithium fluorophosphate salts include lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiDFP), or combinations thereof.
[0077] In some embodiments of this application, sulfonylimide lithium salts include lithium bis(trifluoromethanesulfonylimide) (LiTFSI), lithium bis(fluorosulfonylimide) (LiFSI), or combinations thereof.
[0078] In some embodiments of this application, the borate lithium salt includes lithium dioxoborate (LiBOB), lithium difluorooxalate borate (LiDFOB), or a combination thereof.
[0079] In some embodiments of this application, the organic sulfonate lithium salt includes lithium trifluoromethanesulfonate (LiCF3SO3), lithium perfluorobutylsulfonate (LiC4F9SO3), or combinations thereof.
[0080] In some embodiments of this application, the lithium salt includes sulfonylimide lithium salts, and at least one of lithium fluorophosphate, lithium borate, and organic sulfonate lithium salts.
[0081] In some embodiments of this application, the mass ratio of the sulfonylimide lithium salt to the total mass of other types of lithium salts is (5~10):1; for example, it can be any value of 5:1, 6:1, 7:1, 8:1, 9:1, or 10:1, or a range between any two. Specifically, the other types of lithium salts include at least one of lithium fluorophosphate, lithium borate, or organic sulfonate lithium salts.
[0082] This application uses a mixture of sulfonylimide lithium salts and other types of lithium salts, which has better distribution uniformity in the polymer matrix and further improves the ionic conductivity of the electrolyte membrane.
[0083] In some embodiments of this application, the electrolyte membrane comprises, by mass parts: 40 to 80 parts of polymer matrix, 10 to 30 parts of inorganic solid electrolyte particles, and 5 to 15 parts of lithium salt.
[0084] In some embodiments of this application, the mass fraction of the polymer matrix can be any value or a range between 40, 45, 50, 55, 60, 65, 70, 75 or 80 parts; in some specific embodiments of this application, the mass fraction of the polymer matrix is 50 to 70 parts.
[0085] In some embodiments of this application, the mass fraction of the inorganic solid electrolyte particles can be any value or a range between 10, 12, 15, 17, 20, 22, 25, 27 or 30 parts; in some specific embodiments of this application, the mass fraction of the inorganic solid electrolyte particles is 15 to 25 parts.
[0086] In some embodiments of this application, the mass fraction of lithium salt can be any value of 5, 7, 9, 10, 11, 13, or 15 parts, or a range between any two; in some specific embodiments of this application, the mass fraction of lithium salt is 7 to 13 parts.
[0087] In some embodiments of this application, the electrolyte membrane further includes 2 to 5 parts by mass of an inorganic interface layer; for example, it can be any value or a range between 2, 2.5, 3, 3.5, 4, 4.2, 4.5 or 5 parts by mass; in some specific embodiments of this application, the inorganic interface layer is 2.5 to 4.2 parts by mass.
[0088] In some embodiments of this application, the electrolyte membrane comprises, by mass parts: 40 to 80 parts of polymer matrix, 10 to 30 parts of inorganic solid electrolyte particles, 5 to 15 parts of lithium salt, and 2 to 5 parts of inorganic interface layer.
[0089] In some specific embodiments of this application, the electrolyte membrane comprises, by mass parts: 50 to 70 parts of polymer matrix, 15 to 25 parts of inorganic solid electrolyte particles, 7 to 13 parts of lithium salt, and 2.5 to 4.2 parts of inorganic interface layer.
[0090] In some embodiments of this application, the thickness of the electrolyte membrane is 20 μm to 100 μm; for example, it can be any value or a range between 20 μm, 40 μm, 50 μm, 60 μm, 80 μm or 100 μm; in some specific embodiments of this application, the thickness of the electrolyte membrane is 40 μm to 60 μm.
[0091] The thickness of the electrolyte membrane can be tested using a micrometer (with a measurement accuracy of 0.001 mm, taking the average of no less than 5 different positions) or a scanning electron microscope (SEM) cross-sectional method (which can simultaneously observe the overall uniformity of the membrane).
[0092] In some embodiments of this application, the density of the electrolyte membrane is 1.5 g / cm³. 3 ~3g / cm 3 For example, it could be 1.5g / cm³. 3 1.7g / cm 3 2g / cm 3 2.2g / cm 3 2.5g / cm 3 2.7g / cm 3 Or 3g / cm 3 The density of the electrolyte membrane is any value in the range or any value between two of these ranges. A density within the above range helps ensure sufficient compactness of the electrolyte membrane, thereby effectively suppressing lithium dendrite penetration and reducing the risk of internal short circuits in the battery. Simultaneously, a suitable density reduces porosity and defects within the membrane, improving the mechanical strength and ion transport efficiency of the electrolyte. This avoids a loose electrolyte membrane structure or insufficient mechanical properties due to excessively low density, and also avoids increased membrane brittleness and decreased processing performance due to excessively high density.
[0093] The density of the electrolyte membrane can be tested using the specific gravity bottle method, and can be found in GB / T 1033.1-2008.
[0094] In some embodiments of this application, the ionic conductivity of the electrolyte membrane is 1×10⁻⁶. -4 S / cm ~ 1×10 -3 S / cm; for example, it could be 1×10-4 S / cm, 1.2×10 -4 S / cm, 1.5×10 -4 S / cm, 1.7×10 -4 S / cm or 1×10 -3 Any value in S / cm or a range between any two. An ionic conductivity of the electrolyte membrane within the above range is beneficial for ensuring efficient lithium-ion transport within the electrolyte membrane, significantly reducing ohmic polarization of the electrolyte, and improving the rate performance and energy efficiency of the entire battery. Simultaneously, high ionic conductivity helps achieve normal charge and discharge of the battery at room temperature, reduces heat accumulation caused by obstructed ion transport, and improves battery safety and cycle stability.
[0095] The ionic conductivity of the electrolyte membrane can be tested by electrochemical impedance spectroscopy (EIS) using a symmetrical cell constructed with a stainless steel (SS) blocking electrode at a test temperature of 25°C.
[0096] In some embodiments of this application, the lithium-ion transference number of the electrolyte membrane is 0.4 to 0.7; for example, it can be any value of 0.4, 0.5, 0.6, or 0.7, or a range between any two. A lithium-ion transference number within this range is beneficial for suppressing the migration of ionic liquid cations or anions within the electrolyte, reducing concentration polarization, improving the selective transport efficiency of lithium ions, thereby reducing concentration polarization at the interface and extending the cycle life of the battery. A higher lithium-ion transference number also means fewer side reactions and a more stable interface, which helps improve the rate performance and safety performance of the full battery.
[0097] The lithium-ion transference number of the electrolyte membrane can be tested using the Bruce-Vincent potentiostatic steady-state polarization method.
[0098] In some embodiments of this application, the tensile strength of the electrolyte membrane is 1 MPa to 30 MPa; for example, it can be any value or a range between 1 MPa, 5 MPa, 10 MPa, 15 MPa, 20 MPa, 25 MPa, or 30 MPa. Having a tensile strength within this range helps ensure the electrolyte membrane maintains its structural integrity during battery assembly, charge-discharge cycles, and mechanical vibrations, resists stress caused by changes in electrode material volume, and prevents membrane rupture leading to internal short circuits. Simultaneously, sufficient tensile strength is a prerequisite for achieving ultra-thin electrolyte membranes, thereby improving the battery's mass energy density and volumetric energy density.
[0099] In some embodiments of this application, the elongation at break of the electrolyte membrane is 50% to 300%; for example, it can be any value or a range between 50%, 100%, 150%, 200%, 250%, or 300%. An elongation at break within this range is beneficial for imparting good flexibility and deformation adaptability to the electrolyte membrane, enabling it to maintain structural integrity without brittle fracture when the battery is bent, wound, or subjected to pressure. This is particularly suitable for applications involving flexible batteries and pouch batteries. Simultaneously, an appropriate elongation at break helps alleviate interfacial stress caused by volume expansion and contraction of the electrode materials during charging and discharging, maintaining close contact between the electrolyte and the electrodes, thereby ensuring the long-term cycle stability of the battery.
[0100] The tensile strength and elongation at break of the electrolyte membrane can be tested with reference to GB / T 1040.1-2025 and GB / T 1040.3-2006.
[0101] In some embodiments of this application, the electrolyte membrane is prepared by a method comprising the following steps: mixing inorganic solid electrolyte particles, oxygen-containing heterocyclic monomers, functional additives, solvents and optional lithium salts to obtain a precursor dispersion; subjecting the precursor dispersion to a first heat treatment, a second heat treatment and a curing treatment in sequence to obtain the electrolyte membrane.
[0102] This application provides a highly integrated one-step mixing production process that mixes various components to form an integrated reaction system and achieves a synergistic "cleaning-grafting-curing" reaction through staged heat treatment. It ingeniously integrates complex interface engineering into a simple staged heat treatment process, which greatly simplifies the process flow, avoids the cost and secondary pollution risk of inorganic solid electrolyte particle pretreatment, has excellent compatibility with industrial production processes, meets the urgent needs of large-scale production, and can remove interface impurities in situ and efficiently and build a strong chemically bonded interface layer during electrolyte preparation to obtain a high-performance electrolyte membrane.
[0103] This application employs a staged heat treatment method to form a specific interface layer on the surface of inorganic solid electrolyte particles, which ultimately enables the inorganic solid electrolyte particles and the polymer matrix to form a stable COM covalent bond connection, effectively solving the technical problem of high interface impedance and obtaining an electrolyte membrane with high ionic conductivity and excellent cycle stability.
[0104] Specifically, the first heat treatment, as the "cleaning and activation stage," allows functional additives to decompose at the alkaline sites on the surface of inorganic solid electrolyte particles under thermal action, forming active fluorides (mainly hydrogen fluoride). These active fluorides can selectively etch and remove impurities (such as Li₂CO₃) from the surface of the inorganic solid electrolyte particles in situ, achieving surface cleaning. Simultaneously, a lithium-loving inorganic interface layer (mainly composed of LiF) is constructed on the cleaned surface, achieving both surface cleaning and functionalization. The second heat treatment, as the "grafting and construction stage," forms an inorganic interface layer on the surface of the cleaned and activated inorganic solid electrolyte particles, significantly enhancing catalytic activity. This effectively initiates in-situ ring-opening polymerization of oxygen-containing heterocyclic monomers in the system, forming strong COM covalent bonds and "growing" a thin and dense polymer electrolyte graft layer on the surface of the inorganic solid electrolyte particles. The curing treatment, as the "forming and curing stage," allows the in-situ generated grafted polymer layer to diffuse and entangle with the surrounding polymer, forming a stable three-dimensional network polymer matrix, resulting in the final electrolyte membrane.
[0105] In some embodiments of this application, inorganic solid electrolyte particles, oxygen-containing heterocyclic monomers, functional additives, solvents, and optionally lithium salts are mixed in a protective gas atmosphere. Specifically, the protective gas includes at least one of nitrogen, argon, or helium.
[0106] This application mixes the components evenly to construct a precursor dispersion, forming an "integrated" reaction system that combines the cleaning agent and the reactive monomer. The precursor dispersion is placed in a high-temperature environment, and the in-situ interface reaction is triggered by staged heat treatment to achieve a synergistic reaction of "cleaning-grafting-curing".
[0107] In some embodiments of this application, the temperature of the first heat treatment is 60°C to 80°C; for example, it can be any value of 60°C, 65°C, 70°C, 75°C or 80°C or a range between any two; in some specific embodiments of this application, the temperature of the first heat treatment is 65°C to 75°C.
[0108] In some embodiments of this application, the duration of the first heat treatment is 1h to 4h; for example, it can be any value or a range between 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h; in some specific embodiments of this application, the duration of the first heat treatment is 1.5h to 2.5h.
[0109] In some embodiments of this application, the temperature of the second heat treatment is 80°C to 100°C; for example, it can be any value of 80°C, 85°C, 90°C, 95°C or 100°C or a range between any two; in some specific embodiments of this application, the temperature of the second heat treatment is 85°C to 95°C.
[0110] In some embodiments of this application, the duration of the second heat treatment is 1h to 4h; for example, it can be any value or a range between 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h; in some specific embodiments of this application, the duration of the second heat treatment is 1.5h to 2.5h.
[0111] In some embodiments of this application, the curing temperature is 50°C to 70°C; for example, it can be any value of 50°C, 55°C, 60°C, 65°C or 70°C or a range between any two; in some specific embodiments of this application, the curing temperature is 55°C to 65°C.
[0112] In some embodiments of this application, the curing time is 1h to 4h; for example, it can be any value or a range between 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h; in some specific embodiments of this application, the curing time is 1.5h to 2.5h.
[0113] In some embodiments of this application, the solvent includes at least one of acetonitrile, N-methylpyrrolidone, dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, dimethyl sulfoxide, acetone, or ethyl acetate.
[0114] The second aspect of this application provides a secondary battery, including a positive electrode, a negative electrode, and an electrolyte membrane according to the first aspect of this application.
[0115] This application constructs a stable COM covalent bond connection between inorganic solid electrolyte particles and polymer matrix, forming an excellent chemical bond interface layer, which significantly reduces the interfacial impedance of organic-inorganic electrolyte and greatly improves the ionic conductivity of electrolyte membrane, resulting in a secondary battery with strong cycle stability and high capacity.
[0116] In some embodiments of this application, an electrolyte membrane is disposed between the positive electrode and the negative electrode.
[0117] In some embodiments of this application, the DC internal resistance of the secondary battery under 25°C and 0.2C discharge conditions is ≤56mΩ; specifically, it can be 1mΩ~50mΩ; for example, it can be any value or a range between 1mΩ, 5mΩ, 10mΩ, 20mΩ, 30mΩ, 40mΩ, 50mΩ or 56mΩ.
[0118] The DC internal resistance (DCR) of a secondary battery under discharge conditions of 25℃ and 0.2C can be tested using the constant current discharge method. The specific test method is as follows: Place the battery under test in a constant temperature environment of 25±2℃ and discharge the battery with a constant current at a rate of 0.2C. Simultaneously record the open circuit voltage U0 of the battery before the start of discharge and the terminal voltage U1 at the end of discharge. Calculate the DC internal resistance according to Ohm's law: DCR=(U0-U1) / I, where I is the applied discharge current (A). Each sample is tested in parallel three times, and the average value is taken as the final result.
[0119] In some embodiments of this application, after 1000 hours of cycling, the volume expansion rate of the electrolyte membrane of the secondary battery is ≤10%; specifically, it can be 1% to 10%; for example, it can be any value of 1%, 2%, 4%, 6%, 8% or 10% or any range between two.
[0120] After 1000 hours of cycling, the volume expansion rate of the electrolyte membrane in a secondary battery can be indirectly determined using the thickness method. The specific test method is as follows: Before the cycling test, cut the electrolyte membrane into rectangular samples of a specified size (e.g., 2cm × 2cm). Using a micrometer or micrometer, select at least 5 measurement points evenly on the sample surface, measure the thickness at each point, and take the average value as the initial thickness T0. Simultaneously measure the initial length L0 and width W0 of the sample, and calculate the initial volume V0 = L0 × W0 × T0. Cycle the assembled secondary battery at 25±2℃ with a set rate (e.g., 0.2C / 0.2C) for 1000 hours. After cycling, disassemble the battery in a glove box, carefully remove the electrolyte membrane, and then dry it in a vacuum oven at 60℃ for 12 hours. After drying, the thickness of the sample was measured at at least 5 points using the same method, and the average value was recorded as the thickness after cycling, T1. Simultaneously, the length L1 and width W1 after cycling were measured, and the volume after cycling, V1, was calculated as V1 = L1 × W1 × T1. The volume expansion rate was calculated using the following formula: Volume expansion rate (%) = (V1 - V0) / V0 × 100%; three batteries were tested in parallel for each sample, and the average value was taken as the final result.
[0121] This application does not impose any particular restrictions on the selection of the positive electrode sheet; conventional positive electrode sheets in the art can be used. In some embodiments of this application, the positive electrode sheet may be a nickel-cobalt-manganese (NCM) ternary positive electrode, a lithium cobalt oxide positive electrode, a lithium nickel oxide positive electrode, a lithium manganese oxide positive electrode, etc.
[0122] This application does not impose any particular restrictions on the selection of the negative electrode sheet; conventional negative electrode sheets in the art can be used. In some embodiments of this application, the negative electrode sheet may be a graphite negative electrode, a lithium titanate negative electrode, a silicon-carbon negative electrode, a silicon-oxygen negative electrode, a lithium metal negative electrode, etc.
[0123] This application does not impose any particular restrictions on the choice of diaphragm; conventional diaphragms in the art can be used. In some embodiments of this application, the diaphragm may be a polypropylene membrane, a polyethylene membrane, a polyvinylidene fluoride membrane, a spandex membrane, an aramid membrane, etc.
[0124] In some embodiments of this application, the secondary battery includes a lithium-ion battery; in some specific embodiments of this application, the lithium-ion battery includes a liquid lithium-ion battery, a solid lithium-ion battery, or a semi-solid lithium-ion battery.
[0125] A third aspect of this application provides an electrical device, including a secondary battery as described in the second aspect of this application.
[0126] This application utilizes a rechargeable battery with strong cycle stability and high capacity to provide an electrical device equipped with such a battery. Its battery life is significantly improved, its performance is not easily degraded with long-term use, it does not require frequent battery replacement, the whole machine has a long service life and low maintenance cost, it is suitable for long-term stable operation under various working conditions, and the user experience and product economy are greatly improved.
[0127] This application does not impose any particular restrictions on the selection of electrical equipment; it can be any conventional electrical equipment in the art. In some embodiments of this application, the electrical equipment can be application devices such as vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, and power tools. Vehicles can be new energy vehicles, which can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc.; spacecraft include airplanes, rockets, space shuttles, and spacecraft, etc.; electric toys include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc.; power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc.
[0128] The following specific embodiments further illustrate the content of this application in detail. It should also be understood that the following embodiments are only for further explanation of this application and should not be construed as limiting the scope of protection of this application. Any non-essential improvements and adjustments made by those skilled in the art based on the principles described in this application fall within the scope of protection of this application. The specific process parameters, etc., in the following examples are merely examples within a suitable range; that is, those skilled in the art can make appropriate selections based on the description herein, and are not intended to be limited to the specific data in the examples below. Unless otherwise specified, the raw materials, reagents, or apparatus used in the following embodiments and comparative examples can be obtained from conventional commercial channels or by existing known methods.
[0129] Example 1 An electrolyte membrane, with the following specific composition: The polymer matrix is specifically polyethylene oxide (PEO), which contains -CO- segments and is formed by ring-opening polymerization of ethylene oxide monomers; lithium salt lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) is also distributed in the polymer matrix. Inorganic solid electrolyte particles, distributed within the aforementioned polymer matrix, specifically lithium lanthanum zirconium oxide particles (LLZO, Li7La3Zr2O). 12 Its surface is provided with an inorganic interface layer whose main component is lithium fluoride. This inorganic interface layer is formed by the thermal decomposition of fluoroethylene carbonate on the surface of lithium lanthanum zirconium oxide particles, and its thickness is 4 nm. The inorganic solid electrolyte particles and the polymer matrix are connected by COM (M=La and Zr) covalent bonds, which form a chemical grafting layer (COM bonded layer) on the surface of the inorganic interface layer. The thickness of the electrolyte membrane is 50 μm.
[0130] The specific method for preparing the above-mentioned electrolyte membrane is as follows: 1) By mass fraction, 20 parts of inorganic solid electrolyte particles, lithium lanthanum zirconium oxide (Li7La3Zr2O), were added. 12 60 parts of LLZO, 60 parts of monomeric ethylene oxide (EO), 10 parts of lithium salt bis(trifluoromethanesulfonyl)imide lithium (LiTFSI), and 10 parts of functional additive fluoroethylene carbonate (FEC) were uniformly mixed and dispersed in N-methylpyrrolidone solvent at a solvent-to-solute mass ratio of 3:2. The mixture was stirred at 500 r / min for 1 hour to obtain a precursor dispersion. 2) Place the precursor dispersion at 70℃ and stir uniformly for 2 hours; this step can induce the functional additive to decompose and generate active fluoride HF, etch and remove impurities such as Li2CO3 on the surface of inorganic solid electrolyte particles in situ, and build a lithium-loving inorganic interface layer (main component is LiF, mass part is 2.8 parts) on the cleaned surface. 3) Continue heating the precursor dispersion to 90°C and stir for 2 hours to initiate the ring-opening polymerization of the monomer, forming an organic graft layer containing COM (M=La and Zr) covalent bonds; 4) The dispersion after the reaction was completed was coated with a doctor blade to a thickness of 400 μm and baked at 60 °C for 2 hours to finally obtain a composite electrolyte membrane with a thickness of 50 μm.
[0131] In the above embodiments, after LLZO is etched with HF to remove Li2CO3 impurities, the surface-coordinated unsaturated La... 3+ Zr 4+Metal ions, acting as Lewis acid active sites, activate the monomer and initiate ring-opening polymerization by accepting lone pair electrons from oxygen atoms in the EO monomer, ultimately forming CO-La / CO-Zr covalent bonds that link the polymer to the LLZO surface. An inorganic interface layer (primarily composed of LiF) forms a lithiophilic interface phase on the cleaned LLZO surface, improving compatibility with the anode and inhibiting dendrite growth. It also protects the activated surface from secondary contamination. Furthermore, its nanoscale thickness and inherent defect sites allow the metal cation active centers to remain exposed and in contact with the monomer, ensuring the smooth progress of the polymerization reaction.
[0132] Example 2 An electrolyte membrane, differing from Example 1 in that the thickness of the inorganic interface layer is 6.5 nm; in the preparation method, FEC is replaced with an equal mass of the functional additive difluoroethylene carbonate (DFEC), and the temperature of step 2) is adjusted to 75°C, resulting in an inorganic interface layer with a mass fraction of 4.2 parts; all other conditions are the same as in Example 1.
[0133] Example 3 An electrolyte membrane, which differs from Example 1 in that the thickness of the inorganic interface layer is 6 nm; in the preparation method, the mass fraction of FEC is adjusted to 20 parts, and the temperature of step 2) is adjusted to 75°C, and the mass fraction of the generated inorganic interface layer is 3.8 parts; all other conditions are the same as in Example 1.
[0134] Example 4 An electrolyte membrane, differing from Example 1, has its mass fractions of LLZO, EO, and LiTFSI adjusted to 25 parts, 50 parts, and 13 parts, respectively; all other conditions are the same as in Example 1.
[0135] Example 5 An electrolyte membrane, differing from Example 1 in that the mass fractions of LLZO, EO, and LiTFSI are adjusted to 15 parts, 70 parts, and 7 parts, respectively; all other conditions are the same as in Example 1.
[0136] Example 6 An electrolyte membrane differs from Example 1 in that the polymer matrix is poly(1,3-dioxolane) (PDOL), which is formed by ring-opening polymerization of 1,3-dioxolane monomer; in the preparation method, the monomer is replaced with an equal mass of 1,3-dioxolane (DOL); all other conditions are the same as in Example 1.
[0137] Example 7 An electrolyte membrane differs from Example 1 in that the polymer matrix is polyvinyl carbonate (PVCA), which is formed by ring-opening polymerization of vinylene carbonate; in the preparation method, the monomer is replaced with an equal mass of vinylene carbonate (VC); all other conditions are the same as in Example 1.
[0138] Example 8 An electrolyte membrane, differing from Example 1 in that the inorganic solid electrolyte particles are lithium titanium aluminum phosphate (LATP, Li 1.3 Al 0.3 Ti 1.7 (PO4)3), the inorganic solid electrolyte particles are connected to the polymer matrix by COM (M=Al and Ti) covalent bonds; in the preparation method, the inorganic solid electrolyte particles are replaced with an equal mass of lithium titanium aluminum phosphate; other conditions are the same as in Example 1.
[0139] Example 9 An electrolyte membrane, differing from Example 1 in that the inorganic solid electrolyte particles are lithium lanthanum zirconium tantalum oxide (LLZTO, Li 6.5 La3Zr 1.5 Ta 0.5 O 12 In this preparation method, the inorganic solid electrolyte particles and the polymer matrix are connected by COM (M=La, Zr and Ta) covalent bonds; the inorganic solid electrolyte particles are replaced with an equal mass of lithium lanthanum zirconium tantalum oxide; all other conditions are the same as in Example 1.
[0140] Example 10 An electrolyte membrane, differing from Example 1 in that the lithium salt is lithium bisfluorosulfonylimide (LiFSI); in the preparation method, the lithium salt is replaced with an equal mass of lithium bisfluorosulfonylimide (LiFSI); all other conditions are the same as in Example 1.
[0141] Example 11 An electrolyte membrane differs from Example 1 in that the lithium salt is lithium dioxoborate (LiBOB); in the preparation method, the lithium salt is replaced with an equal mass of lithium dioxoborate (LiBOB); all other conditions are the same as in Example 1.
[0142] Example 12 An electrolyte membrane differs from Example 1 in that the lithium salt is a mixed lithium salt of lithium bis(trifluoromethanesulfonylimide) (LiTFSI) and lithium dioxoborate (LiBOB), with a mass ratio of LiTFSI to LiBOB of 6:1; in the preparation method, the lithium salt is replaced with the above-mentioned mixed lithium salt; all other conditions are the same as in Example 1.
[0143] Example 13 An electrolyte membrane differs from Example 1 in that the lithium salt is a mixed lithium salt of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium dioxoborate (LiBOB), with a mass ratio of LiTFSI to LiBOB of 9:1; in the preparation method, the lithium salt is replaced with the above-mentioned mixed lithium salt; all other conditions are the same as in Example 1.
[0144] Comparative Example 1 An electrolyte membrane differs from Example 1 in that the inorganic solid electrolyte particles have residual Li2CO3 impurities on their surface, no effective inorganic interface layer on their surface, and no COM covalent bond between the inorganic solid electrolyte particles and the polymer matrix; FEC is not added in the preparation method; all other conditions are the same as in Example 1.
[0145] In Comparative Example 1, without the addition of FEC, it is impossible to generate an inorganic interface layer whose main component is lithium fluoride, nor can it initiate the ring-opening polymerization of monomers to form an organic graft layer.
[0146] Comparative Example 2 An electrolyte membrane differs from Example 1 in that the inorganic solid electrolyte particles have residual Li2CO3 impurities on their surface, no effective inorganic interface layer on their surface, and no COM covalent bond between the inorganic solid electrolyte particles and the polymer matrix; in the preparation method, FEC is replaced with an equal mass of ethylene carbonate (EC); all other conditions are the same as in Example 1.
[0147] In Comparative Example 2, ethylene carbonate does not have the ability to decompose upon heating to produce HF, and cannot generate an inorganic interface layer whose main component is lithium fluoride, nor can it initiate the ring-opening polymerization of monomers to form an organic graft layer.
[0148] Comparative Example 3 An electrolyte membrane differs from Example 1 in that there is no COM covalent bond between the inorganic solid electrolyte particles and the polymer matrix; the adsorption is purely physical.
[0149] The preparation method of the electrolyte membrane in this example is as follows: 1) First, pretreat LLZO powder separately with dilute hydrogen fluoride (HF) solution, then wash and dry; 2) By mass, 20 parts of treated LLZO, 60 parts of ethylene oxide, and 10 parts of lithium bis(trifluoromethanesulfonylimide) are uniformly mixed to obtain a mixture, which is then dispersed in N-methylpyrrolidone solvent at a mass ratio of solvent to mixture of 3:2. The mixture is stirred at 500 r / min for 1 hour to obtain a precursor dispersion; FEC is not added in this step. 3) Place the precursor dispersion at 70℃ and stir evenly for 2 hours; 4) After heating to 90℃, continue stirring for 2 hours; 5) The dispersion after the reaction was completed was coated with a doctor blade to a thickness of 400 μm and baked at 60 °C for 2 hours to finally obtain a composite electrolyte membrane with a thickness of 50 μm.
[0150] In Comparative Example 3, FEC was not added. Instead, HF was used for pretreatment to clean the surface of the inorganic solid electrolyte particles, which could form an inorganic interface layer with lithium fluoride as the main component. However, the reaction process was discontinuous, and it was difficult to induce the formation of a chemically grafted organic layer on the surface of the inorganic solid electrolyte particles. It was only physical adsorption.
[0151] Comparative Example 4 An electrolyte membrane differs from Example 1 in that the inorganic solid electrolyte particles have residual Li2CO3 impurities on their surface, no effective inorganic interface layer on their surface, and no COM covalent bond connection between the inorganic solid electrolyte particles and the polymer matrix.
[0152] The preparation method of the electrolyte membrane in this example is as follows: 1) By mass, 20 parts LLZO, 60 parts ethylene oxide, and 10 parts lithium bis(trifluoromethanesulfonylimide) are mixed evenly to obtain a mixture, which is then dispersed in N-methylpyrrolidone solvent at a mass ratio of 3:2 to obtain a dispersion; FEC is not added in this step. 2) Add 3% of the cationic polymerization initiator aluminum trifluoromethanesulfonate ((CF3SO3)3Al) to the above dispersion and stir at 500 r / min for 1 hour to mix it evenly and form a precursor dispersion. 3) The precursor dispersion was directly heated to 90°C and stirred for 2 hours; in this step, aluminum trifluoromethanesulfonate, as a Lewis acid, initiated the ring-opening polymerization of ethylene oxide to form a polyoxyethylene matrix and encapsulate LLZO therein; 4) The dispersion after the reaction was completed was coated with a doctor blade to a thickness of 400 μm and baked at 60 °C for 2 hours to finally obtain a composite electrolyte membrane with a thickness of 50 μm.
[0153] In Comparative Example 4, without the addition of FEC, it is impossible to generate an inorganic interface layer whose main component is lithium fluoride. The monomer polymerization is initiated by conventional initiators to form a polymer layer, but it is only a physical encapsulation and cannot form a chemically grafted organic graft layer.
[0154] Comparative Example 5 An electrolyte membrane differs from Example 1 in that the inorganic interface layer is incomplete, and an effective COM covalent bond connection cannot be formed between the inorganic solid electrolyte particles and the polymer matrix.
[0155] The preparation method of the electrolyte membrane in this example is as follows: 1) By mass, 20 parts LLZO, 60 parts ethylene oxide, 10 parts lithium bis(trifluoromethanesulfonylimide) and 10 parts fluoroethylene carbonate are mixed evenly to obtain a mixture, which is then dispersed in N-methylpyrrolidone solvent at a mass ratio of solvent to mixture of 3:2. The mixture is stirred at 500 r / min for 1 hour to obtain a precursor dispersion. 2) The above precursor dispersion is directly heated to 80°C and stirred at a constant speed of 500 r / min for 4 hours; in this step, the same temperature is maintained throughout the entire process without any stages. 3) The dispersion after the reaction was completed was coated with a doctor blade to a thickness of 400 μm and baked at 60 °C for 2 hours to finally obtain a composite electrolyte membrane with a thickness of 50 μm.
[0156] In Comparative Example 5, a single-step constant-temperature heat treatment was used, and the cleaning and grafting processes occurred simultaneously, resulting in an incomplete formation of the inorganic interface layer and a loose organic graft layer with low coverage, which could not form an effective covalent bond connection.
[0157] Performance testing (1) Ionic conductivity test process at 25℃ The ionic conductivity was measured using electrochemical impedance spectroscopy (EIS). A symmetrical cell was constructed using a stainless steel (SS) blocked electrode, and the test temperature was 25℃. The specific steps are as follows: 1) Testing battery assembly The electrolyte membranes prepared in each embodiment and comparative example were cut into circular pieces with a diameter of 16 mm. In an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), the electrolyte membranes were placed between two stainless steel blocking electrodes to assemble a 2032 type coin cell (SS|electrolyte|SS). To ensure good interfacial contact, appropriate pressure was applied during assembly to ensure tight adhesion between the electrodes and the electrolyte membrane.
[0158] 2) Test Condition Settings The assembled coin cells were transferred to a constant temperature chamber and allowed to stand at 25±0.5℃ for 2 hours to allow the system to reach thermal equilibrium. EIS testing was performed using an electrochemical workstation with the following parameters set: applied AC voltage amplitude: 10mV; test frequency range: 10... 6 Hz to 0.1Hz.
[0159] 3) Data processing and conductivity calculation The intersection of the high-frequency semicircle and the real axis is read from the obtained Nyquist spectrum; this intersection corresponds to the bulk resistance (R) of the electrolyte. The ionic conductivity (σ) is calculated using the following formula: σ = L / (R×S); Where: σ: ionic conductivity (S / cm); L: Electrolyte membrane thickness (cm), measured by a micrometer. R: Volume resistance (Ω), obtained from EIS spectrum; S: Effective contact area between the electrolyte membrane and the electrode (cm²) 2 ), that is, the area of the stainless steel electrode; Each sample was tested in parallel three times, and the average value was taken as the final result.
[0160] (2) Test process of capacity retention of Ni92 / / SiC full cell after 100 cycles at 0.2C 1) Full battery assembly The electrolyte membranes prepared in the various embodiments and comparative examples were used to assemble Ni92 / / SiC all-solid-state batteries: In an argon-filled glove box, the Ni92 / / SiC all-solid-state batteries were assembled in the following order: negative electrode shell, spring plate, gasket, negative electrode sheet, electrolyte membrane, positive electrode sheet, gasket, and positive electrode shell. Ni92 refers to NCM92 positive electrode, with the chemical formula LiNi. 0.92 Co 0.04 Mn 0.04 O2; SiC refers to a mixture of silicon-based materials (elemental silicon) and carbon-based materials (artificial graphite). In this embodiment, the mass percentage of elemental silicon in SiC is 15%, and the mass percentage of artificial graphite is 85%.
[0161] 2) Formation and testing conditions Transfer the assembled battery to the battery testing system and test it according to the following procedure: 1. Formation stage: After standing in a constant temperature chamber at 25±1℃ for 4 hours, the film is charged to 4.3V with a small current of 0.05C (1C=200mA / g) and then discharged to 2.8V with a constant current. This cycle is repeated twice to form a stable SEI film.
[0162] 2. Cyclic performance test: Test temperature: 25±2℃; Charge / discharge rate: 0.2C constant current charging to 4.3V, followed by constant voltage charging until the current drops to 0.05C; let stand for 10 minutes; 0.2C constant current discharging to 2.8V; let stand for 10 minutes; Number of cycles: 100 consecutive charge-discharge cycles; Data logging: Records the discharge capacity for each cycle.
[0163] 3) Calculation of capacity retention rate: The capacity retention rate (%) is calculated using the following formula: Capacity retention rate = (Discharge capacity at 100th cycle / Discharge capacity at 1st cycle) × 100%; The discharge capacity of the first cycle was taken from the discharge capacity of the first 0.2C cycle after formation. Three batteries were tested in parallel for each sample, and the average value was taken as the final result. The standard deviation was also recorded.
[0164] 4) Test termination conditions During the test, the battery's coulombic efficiency and voltage curve changes are monitored simultaneously. If the battery experiences a short circuit, abnormal voltage fluctuations, or a sharp capacity decay (more than 20% decay in a single cycle), the test is terminated prematurely.
[0165] The relevant technical parameters of the electrolyte membranes in the examples and comparative examples, as well as the performance test results, are shown in Tables 1 and 2. In Table 1, A:B (mass ratio) refers to the mass ratio of inorganic solid electrolyte particles to the inorganic interface layer.
[0166] Table 1. Specific composition of each embodiment and comparative example.
[0167] Table 2 Performance test results of each embodiment and comparative example
[0168] The following conclusions can be drawn from analyzing Table 2: Examples 1-13 successfully constructed a gradient interface (COM bonded layer) with covalent bonds between inorganic solid electrolyte particles and a polymer matrix, transforming the simple physical mixing of organic and inorganic phases into a robust chemical bond with an ionic conductivity of (5.8~9.5)×10⁻⁶. -4 S / cm, density is 2.05~2.32 g / cm³ 3 The lithium-ion transference number was 0.45–0.55, the tensile strength was 8.5–18.5 MPa, the elongation at break was 95–250%, the battery capacity retention was 88.5–95.8%, the DC internal resistance was 38.7–55.6 mΩ, and the electrolyte membrane volume expansion rate was 4.2–7.5%. All of these results were significantly better than those of Comparative Examples 1–5, which had interface defects. The ionic conductivity of Comparative Examples 1–5 was ≤4.2 × 10⁻⁶. -5 S / cm, density ≤1.95g / cm³ 3 The battery exhibits the following properties: lithium-ion transference number ≤ 0.35, tensile strength ≤ 7.2 MPa, elongation at break ≥ 260%, capacity retention ≤ 80.5%, DC internal resistance ≥ 85.4 mΩ, and electrolyte membrane volume expansion ≥ 14.2%. This demonstrates the crucial role of constructing COM covalent bonds between inorganic solid electrolyte particles and the polymer matrix.
[0169] Examples 2-3 adjusted the thickness and mass ratio of the inorganic interface layer; Examples 4-5 adjusted the mass ratio of each component; Examples 6-7 adjusted the type of polymer matrix; Examples 8-9 adjusted the type of inorganic solid electrolyte particles; Examples 10-13 adjusted the type of lithium salt. The performance of the prepared electrolyte membranes changed to some extent but remained at a high level. This proves that the embodiments of this application obtained high-performance electrolyte membranes by controlling the structural composition and material types of the electrolyte membrane, which have wide applicability and stable technical effects.
[0170] Comparative Example 1 did not contain any functional additives, while Comparative Example 2 contained EC. As a result, there was no COM covalent bond between the inorganic solid electrolyte particles and the polymer matrix, the interface cleaning and grafting failed, and the performance was significantly worse. This shows that by using functional additives as in-situ cleaners and reaction media, an effective inorganic interface layer can be constructed, thereby achieving effective chemical bonding. At the same time, this also fully demonstrates the importance of forming chemical bonds between the organic and inorganic phases.
[0171] Comparative Example 3 achieved surface cleaning of inorganic solid electrolyte particles by pretreatment with HF. Although its performance was better than other comparative examples, it was still far lower than all examples. This proves that only by using functional additives for in-situ continuous reaction can effective COM covalent bond connections be formed, thereby promoting interface stability.
[0172] Comparative Example 4 uses a conventional initiator to initiate monomer polymerization, forming a polymer layer, but it is only a physical encapsulation and cannot form a covalent bond connection between the inorganic solid electrolyte particles and the polymer matrix.
[0173] Comparative Example 5 uses a single-step constant temperature heat treatment, which causes the cleaning and grafting processes to occur simultaneously and interfere with each other. This results in an incomplete formation of the inorganic interface layer, a loose graft layer with low coverage, and an inability to build effective covalent bond connections, leading to a significant deterioration in its ionic conductivity and battery cycle performance.
[0174] Furthermore, the lithium symmetric battery assembled with the electrolyte membrane in the embodiments of this application can be stably cycled for more than 1000 hours at a current density of 0.1 mA / cm², and the specific capacity of the assembled all-solid-state battery is ≥20% higher than that of the traditional composite electrolyte.
[0175] In this embodiment, a gradient interface structure with an inorganic interface layer and a chemical grafting layer was successfully constructed through unique material design and a staged heat treatment process. This fundamentally solved the technical problem of high interfacial impedance of organic-inorganic composite electrolytes and obtained an electrolyte membrane with high ionic conductivity and excellent cycle stability.
[0176] In summary, this application constructs a strong COM covalent bond connection between the organic and inorganic phases, forming a continuous, low-impedance lithium-ion transport channel, which significantly reduces the interfacial impedance, effectively improves the ionic conductivity of the electrolyte membrane, and significantly enhances the mechanical strength of the interface and the resistance to lithium dendrite penetration. This electrolyte membrane can be used to prepare high-performance secondary batteries and electrical devices.
[0177] Finally, it should be noted that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection scope and disclosure scope of this application.
Claims
1. An electrolyte membrane, comprising: A polymer matrix containing -CO- segments; Inorganic solid electrolyte particles are distributed in the polymer matrix, and the inorganic solid electrolyte particles contain a functional metal element M, wherein the functional metal element M includes at least one of a transition metal element, a group IIIA metal element, or a group IVA metal element. The inorganic solid electrolyte particles and the polymer matrix have COM covalent bonds.
2. The electrolyte membrane according to claim 1, characterized in that, At least one of the following conditions must be met: a1. The polymer matrix includes one of polyethylene oxide, polypropylene oxide, poly(1,3-dioxolane), polytetrahydrofuran, homopolymer formaldehyde, polyvinyl carbonate, or poly(ε-caprolactone). a2. The functional metal element M includes at least one of lanthanum, zirconium, tantalum, aluminum, germanium, or titanium; a3. The inorganic solid electrolyte particles include at least one of lithium lanthanum zirconium oxide, lithium lanthanum titanium oxide, lithium lanthanum zirconium tantalum oxide, lithium titanium aluminum phosphate, or lithium germanium aluminum phosphate.
3. The electrolyte membrane according to claim 1, characterized in that, The surface of the inorganic solid electrolyte particles is further provided with an inorganic interface layer, which contains lithium fluoride compounds.
4. The electrolyte membrane according to claim 3, characterized in that, The mass ratio of the inorganic solid electrolyte particles to the inorganic interface layer is 1:(0.1~0.25). And / or, the thickness of the inorganic interface layer is 3nm~10nm.
5. The electrolyte membrane according to claim 1, characterized in that, The polymer matrix also contains lithium salts; the lithium salts include at least one of lithium fluorophosphate, lithium sulfonylimide, lithium borate, or organic sulfonate lithium salts.
6. The electrolyte membrane according to claim 5, characterized in that, At least one of the following conditions must be met: b1. The fluorophosphate lithium salt includes lithium hexafluorophosphate, lithium difluorophosphate, or a combination thereof; b2. The sulfonylimide lithium salt includes lithium bis(trifluoromethanesulfonylimide), lithium bis(fluorosulfonylimide), or a combination thereof; b3. The borate lithium salts include lithium dioxoborate, lithium difluorooxalate borate, or combinations thereof. b4. The organic sulfonate lithium salts include lithium trifluoromethyl sulfonate, lithium perfluorobutyl sulfonate, or combinations thereof.
7. The electrolyte membrane according to claim 5, characterized in that, The lithium salt includes sulfonylimide lithium salts, and at least one of lithium fluorophosphate, borate lithium salts, and organic sulfonate lithium salts.
8. The electrolyte membrane according to claim 7, characterized in that, The mass ratio of the sulfonylimide lithium salt to the total mass of other types of lithium salts is (5~10):
1.
9. The electrolyte membrane according to claim 5, characterized in that, The electrolyte membrane comprises, by mass parts: 40 to 80 parts of polymer matrix, 10 to 30 parts of inorganic solid electrolyte particles, and 5 to 15 parts of lithium salt.
10. The electrolyte membrane according to claim 1, characterized in that, The electrolyte membrane has at least one of the following characteristics: 1) The density of the electrolyte membrane is 1.5 g / cm³. 3 ~3g / cm 3 ; 2) The ionic conductivity of the electrolyte membrane is 1×10⁻⁶. -4 S / cm ~ 1×10 -3 S / cm; 3) The lithium-ion transference number of the electrolyte membrane is 0.4~0.7; 4) The tensile strength of the electrolyte membrane is 1 MPa to 30 MPa; 5) The elongation at break of the electrolyte membrane is 50%~300%.
11. A secondary battery, characterized in that, The secondary battery includes a positive electrode, a negative electrode, and an electrolyte membrane according to any one of claims 1 to 10, wherein the electrolyte membrane is disposed between the positive electrode and the negative electrode; the DC internal resistance of the secondary battery under discharge conditions of 25°C and 0.2C is ≤56mΩ.
12. The secondary battery according to claim 11, characterized in that, After 1000 hours of cycling, the volume expansion rate of the electrolyte membrane in the secondary battery is ≤10%.
13. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 11 or 12.