A composite electrolyte membrane for semi-solid lithium batteries, its preparation method, and its application.

By using a composite electrolyte membrane of lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt and plasticizer in semi-solid lithium batteries, the problems of high electrolyte-electrode interface impedance and insufficient flexibility are solved, achieving high cycle stability and wide electrochemical window performance of lithium batteries, with good safety and production adaptability.

CN123073142APending Publication Date: 2026-11-10SHENYANG UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611574038.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing semi-solid lithium batteries, the solid-solid interface impedance between the electrolyte and the electrode is large, and the composite electrolyte loses its flexibility, resulting in poor cycle stability.

Method used

A composite electrolyte membrane consisting of lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt, and plasticizer is formed by controlling the proportion of each component and the preparation method. This results in an inorganic/organic composite electrolyte membrane that combines strength and flexibility, thus optimizing the electrode-electrolyte interface contact.

Benefits of technology

It improves the cycle stability and electrochemical window of lithium batteries, inhibits lithium dendrite growth, enhances battery safety and high-voltage performance, and has low manufacturing cost, making it easy to mass-produce.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073142A_ABST
    Figure CN123073142A_ABST
Patent Text Reader

Abstract

This invention provides a composite electrolyte membrane for semi-solid-state lithium batteries, its preparation method, and its application, relating to the field of solid-state electrolyte technology. The composite electrolyte membrane mainly comprises: lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt, and plasticizer. After mixing and stirring these substances in batches until homogeneous, the composite electrolyte membrane is prepared by a casting method. LATP provides lithium-ion transport channels, PVDF-HFP imparts flexibility to the electrolyte membrane, and the lithium salt provides the lithium source. The plasticizer introduces a fluid active lithium-conducting region into the inert framework of PVDF-HFP. This invention provides an inorganic / organic composite electrolyte membrane. By introducing a plasticizer, the LATP-based composite electrolyte membrane at room temperature exhibits both strength and flexibility, thereby inhibiting the growth of lithium dendrites and expanding the operating voltage range of lithium metal batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid electrolyte technology, and more specifically, to a composite electrolyte membrane for semi-solid lithium batteries, its preparation method, and its application. Background Technology

[0002] Against the backdrop of the global new energy vehicle industry's pursuit of higher safety and range, China's solid-state battery industry is entering a phase of parallel industrialization breakthroughs and technological advancements in all-solid-state technology. With the advancement of industrialization, the global solid-state battery equipment market is projected to surge to 107.94 billion yuan by 2030. Furthermore, global shipments of solid-state batteries (semi-solid-state + all-solid-state) are expected to increase from 34 GWh in 2026 to 614 GWh in 2030, exhibiting an exponential expansion trend. The future of China's solid-state battery industry is poised for a period of rapid development.

[0003] Solid-state batteries are a novel battery technology that replaces traditional liquid electrolytes with solid electrolytes. They achieve ion conduction through solid electrolytes, fundamentally revolutionizing the working principle of traditional lithium batteries. Based on the amount of solid electrolyte used, batteries with a liquid content of 5-10 wt% can be called semi-solid-state batteries. The technology path pioneered by semi-solid-state batteries will be the first to achieve industrialization, driving the rapid development of the upstream equipment and materials industry chain. With continuous technological breakthroughs and cost reductions, all-solid-state batteries will gradually move from the laboratory to the market, expanding their applications from high-end electric vehicles to broader scenarios such as energy storage, driving exponential growth in market size.

[0004] Semi-solid batteries primarily use composite electrolytes, including oxides, polymers, and wetting liquids. Oxide solid electrolytes offer high mechanical strength, chemical / electrochemical stability, air stability, and a wider electrochemical window, while also being relatively affordable. Polymer electrolytes, with their superior chemical stability and processability, have garnered significant attention, with PVDF-HFP exhibiting a wide electrochemical window and high ionic conductivity. In current semi-solid battery systems, oxide electrolyte powders and combinations of oxide and polymer electrolyte powders have become mainstream. The inorganic phase provides ion conduction channels and enhances mechanical strength, while the organic phase improves interfacial contact and toughness. However, the practical application of inorganic-organic composite electrolytes in lithium metal batteries still faces two challenges: (1) high solid-solid interface impedance between the electrolyte and electrode; and (2) the need to balance the low ion transference number of polymer electrolytes with the high mechanical strength of inorganic fillers, which leads to a loss of flexibility in the composite electrolyte. These challenges result in poor cycle stability of assembled semi-solid lithium batteries. Therefore, optimizing the composition of composite electrolytes to improve the cycle stability and expand the electrochemical window of lithium batteries is of great significance. Summary of the Invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.

[0006] Therefore, a first aspect of the present invention provides a composite electrolyte membrane suitable for semi-solid lithium batteries, wherein the raw materials of the composite electrolyte membrane include: lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt and plasticizer; The mass percentages of the lithium titanium aluminum phosphate, the polyvinylidene fluoride-hexafluoropropylene, the lithium salt, and the plasticizer are as follows: lithium titanium aluminum phosphate 40%-80%, polyvinylidene fluoride-hexafluoropropylene 10%-40%, lithium salt 5%-30%, and plasticizer 5%-20%.

[0007] In some technical solutions of the present invention, optionally, the weight-average molecular weight of the polyvinylidene fluoride-hexafluoropropylene is one or more of 100,000, 400,000 and 450,000.

[0008] In some technical solutions of the present invention, optionally, the lithium salt is one or more of lithium bis(trifluoromethanesulfonate)imide, lithium bis(fluorosulfonylimide)imide, lithium perchlorate, lithium hexafluorophosphate, and lithium tetrafluoroborate.

[0009] In some technical solutions of the present invention, the plasticizer may optionally be one or more of fluoroethylene carbonate, propylene carbonate, polyethylene glycol, dioctyl adipate, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0010] A second aspect of the present invention provides a method for preparing a composite electrolyte membrane, the method being used to prepare a composite electrolyte membrane for a semi-solid-state lithium battery as described above, the method comprising: According to the mass percentage of the polyvinylidene fluoride-hexafluoropropylene, the lithium salt, and the plasticizer, the lithium salt, the plasticizer, and the polyvinylidene fluoride-hexafluoropropylene are added to a container in the order of the lithium salt, the plasticizer, and the polyvinylidene fluoride-hexafluoropropylene, and stirred at room temperature until they are mixed evenly to obtain a first mixture. According to the mass percentage of lithium titanium aluminum phosphate, lithium titanium aluminum phosphate is added to the first mixture and stirred at room temperature until it is uniformly mixed to obtain the second mixture; The second mixture is applied to a polytetrafluoroethylene mold and coated by a casting method to form a wet film on the polytetrafluoroethylene mold. The wet membrane is dried under vacuum conditions to obtain the composite electrolyte membrane.

[0011] In some technical solutions of the present invention, optionally, when performing the stirring until uniform mixing at room temperature, the stirring is performed using a magnetic stirrer and the stirring speed is set to 100-400 r / min.

[0012] Optionally, in some technical solutions of the present invention, the method of coating by casting includes: The second mixture is coated with a doctor blade, and the coating thickness is controlled to be 50-300 μm to obtain the wet film.

[0013] Optionally, in some technical solutions of the present invention, drying the wet film under vacuum conditions includes: The wet membrane is placed in a vacuum oven, and the temperature of the vacuum oven is controlled at 40-100℃. The wet membrane is dried for 5-20 hours to obtain the composite electrolyte membrane with a thickness of 10-200μm.

[0014] The third aspect of the present invention provides an application of a composite electrolyte membrane for a semi-solid lithium battery, wherein the composite electrolyte membrane is the composite electrolyte membrane of the semi-solid lithium battery described in any of the above technical solutions, and the composite electrolyte membrane of the semi-solid lithium battery is used to prepare a semi-solid lithium battery.

[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention provides an inorganic / organic composite electrolyte membrane. By introducing a plasticizer, the LATP-based composite electrolyte membrane at room temperature possesses both strength and flexibility, thereby inhibiting the growth of lithium dendrites and expanding the operating voltage range of lithium metal batteries.

[0016] 2. This invention provides an inorganic / organic composite electrolyte membrane, which improves the cycle stability of the battery by adding lithium-ion battery electrolyte at the electrode-electrolyte interface.

[0017] 3. The Li||NCM622 battery assembled with the composite electrolyte membrane prepared by the method proposed in this invention has excellent electrochemical performance, with a capacity of over 200mAh g-1 at room temperature and 0.1C rate, stable cycling for 70 cycles, and a capacity of over 190mAh g-1 at 0.5C rate.

[0018] 4. The method for preparing composite electrolyte membranes proposed in this invention is low in cost, high in safety, compatible with existing battery processes, and easy to mass-produce.

[0019] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description

[0020] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1This is a process flow diagram of the electrolyte membrane preparation method of the present invention; Figure 2 This is a flame-retardant test diagram of the composite electrolyte in the experimental examples of this invention; Figure 3 The impedance diagram is shown for the battery assembled with the composite electrolyte in the experimental example of this invention. Figure 4 This is a linear scan LSV plot of the battery assembled with the composite electrolyte in the experimental example of this invention; Figure 5 This is a low-rate cycle test diagram of the battery assembled with the composite electrolyte in the experimental example of this invention; Figure 6 This is a high-rate cycle test diagram of the battery assembled with the composite electrolyte in the experimental example of this invention. Detailed Implementation

[0021] To better understand the above-mentioned objectives, features, and advantages of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be combined with each other.

[0022] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and therefore the scope of protection of the invention is not limited to the specific embodiments disclosed below.

[0023] The following reference Figures 1 to 6 This invention describes a composite electrolyte membrane for a semi-solid lithium battery, its preparation method, and its application, according to some embodiments of the present invention.

[0024] In one embodiment of the present invention, a composite electrolyte membrane for a semi-solid lithium battery is provided. The raw materials of the composite electrolyte membrane include: lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt, and plasticizer; wherein the mass percentages of lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt, and plasticizer are: lithium titanium aluminum phosphate 40%-80%, polyvinylidene fluoride-hexafluoropropylene 10%-40%, lithium salt 5%-30%, and plasticizer 5%-20%.

[0025] In this invention, by controlling the content of lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt, and plasticizer, the prepared inorganic-organic composite electrolyte membrane exhibits excellent cycle stability and an expanded electrochemical window. Specifically: Lithium titanium aluminum phosphate, as an inorganic ceramic fast ion conductor, provides a continuous and rapid transport channel for lithium ions and enhances the mechanical strength of the composite electrolyte membrane. If its content is too high, the proportion of inorganic particles is too large, making it difficult for the polymer matrix to fully coat the membrane, resulting in difficult film formation and a brittle, easily cracked membrane. If the content is too low, the ion transport channels are insufficient, the room temperature ionic conductivity decreases, and the mechanical strength and flame retardant properties deteriorate. Polyvinylidene fluoride-hexafluoropropylene, as an organic polymer matrix, provides a flexible framework for the inorganic phase, improves the interfacial contact between the electrolyte membrane and the electrode, and imparts a certain degree of flexibility to the membrane. If its content is too high, the polymer proportion increases, the ionic conductivity decreases, and the mechanical strength decreases; if the content is too low, the film formation deteriorates, the membrane lacks flexibility, and it is difficult to effectively coat the inorganic particles, resulting in an uneven membrane layer. Lithium salts, as the source of lithium ions, provide freely moving lithium ions after dissociation, contributing to ionic conductivity. When their content is too high, lithium salts tend to aggregate and crystallize, affecting film uniformity and electrochemical stability; when the content is too low, the carrier concentration is insufficient, resulting in low ionic conductivity and increased battery polarization. Plasticizers can dissolve and dissociate lithium salts, reducing the crystallinity of the polymer matrix and forming more amorphous regions conducive to lithium ion jumping, thereby improving ionic conductivity and enhancing the film's flexibility and flame retardant properties. When their content is too high, the film's mechanical strength decreases, and plasticizer precipitation may occur; when the content is too low, the plasticizing effect is insufficient, the improvement in ionic conductivity is limited, and the flame retardant properties are poor. Therefore, by controlling the contents of lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt and plasticizer within the above ranges, the inorganic and organic phases work synergistically, resulting in an inorganic-organic composite electrolyte membrane that combines high room temperature ionic conductivity, good mechanical strength and flexibility, excellent flame retardant properties and a wide electrochemical window, thereby improving the cycle stability and high voltage resistance of semi-solid lithium batteries.

[0026] Optionally, the polyvinylidene fluoride-hexafluoropropylene has a weight-average molecular weight of one or more of 100,000, 400,000, and 450,000.

[0027] Optionally, the lithium salt is one or more of lithium bis(trifluoromethanesulfonate)imide, lithium bis(fluorosulfonylimide), lithium perchlorate, lithium hexafluorophosphate, and lithium tetrafluoroborate.

[0028] Optionally, the plasticizer is one or more selected from fluoroethylene carbonate, propylene carbonate, polyethylene glycol, dioctyl adipate, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0029] In one embodiment of the present invention, such as Figure 1As shown, a method for preparing a composite electrolyte membrane is provided. This method is used to prepare a composite electrolyte membrane for a semi-solid-state lithium battery as described in any of the above embodiments. The preparation method includes: Step 102: According to the mass percentage of the polyvinylidene fluoride-hexafluoropropylene, the lithium salt, and the plasticizer, the lithium salt, the plasticizer, and the polyvinylidene fluoride-hexafluoropropylene are added to the container in the order of the lithium salt, the plasticizer, and the polyvinylidene fluoride-hexafluoropropylene, and stirred at room temperature until they are mixed evenly to obtain the first mixture. Step 104: Add lithium titanium aluminum phosphate to the first mixture according to the mass percentage of the lithium titanium aluminum phosphate, and stir at room temperature until the mixture is homogeneous to obtain the second mixture; Step 106: Apply the second mixture to the polytetrafluoroethylene mold and coat it using a casting method to form a wet film on the polytetrafluoroethylene mold; Step 108: Dry the wet membrane under vacuum conditions to obtain the composite electrolyte membrane.

[0030] In step 102, the lithium salt, the plasticizer, and the polyvinylidene fluoride-hexafluoropropylene (PVDF-HFA) are added to the container in the following order: lithium salt, plasticizer, and PVDF-HFA. The purpose of this order is to add the lithium salt and plasticizer first, allowing the lithium salt to initially disperse or dissolve in the plasticizer to form a premixed system, and then add the PVDF-HFA. If the PVDF-HFA is added directly to the bottom of the container, it tends to adhere to the bottom, leading to difficulties in stirring and uneven dissolution, thus affecting the homogeneity of the first mixture. Adding it last and dispersing it in the premixed system effectively prevents the PVDF-HFA from adhering directly to the bottom of the container, facilitating its full swelling and uniform dispersion during stirring at room temperature, thereby obtaining a uniform and stable first mixture.

[0031] In step 104, lithium titanium aluminum phosphate is added to the first mixture, rather than being added prematurely along with solid components such as lithium salt and polyvinylidene fluoride-hexafluoropropylene. If lithium titanium aluminum phosphate is added too early, it is prone to agglomeration with solids such as lithium salt and polyvinylidene fluoride-hexafluoropropylene, resulting in uneven stirring and poor dispersibility in subsequent processes. Therefore, forming a uniform first mixture in step 102 before adding lithium titanium aluminum phosphate is beneficial for the lithium titanium aluminum phosphate to be fully wetted and uniformly dispersed, thereby obtaining a composite electrolyte membrane with uniform performance.

[0032] In steps 102 and 104, when stirring until homogeneous at room temperature, a magnetic stirrer is used and the stirring speed is set to 100–400 r / min.

[0033] In step 106, the method of casting by scraping includes: using a scraper to coat the second mixture, controlling the coating thickness to be 50-300 μm, to obtain the wet film.

[0034] Specifically, if the coating thickness is too thin, the composite electrolyte membrane may not be able to form, and if the thickness is too thick, the composite electrolyte membrane may be difficult to dry. Therefore, when performing the coating, the coating thickness is selected to be 50-300μm, for example, 50μm, 80μm, 110μm, 140μm, 200μm, 250μm, or 300μm.

[0035] In step 108, drying the wet membrane under vacuum conditions includes: placing the wet membrane in a vacuum oven, controlling the temperature of the vacuum oven at 40-100℃, and drying the wet membrane for 5-20 hours to obtain the composite electrolyte membrane with a thickness of 10-200μm.

[0036] Specifically, excessively high drying temperatures may cause the composite electrolyte membrane to become hard and brittle, lacking flexibility and failing to form a film, while excessively low drying temperatures may result in the liquid portion of the composite electrolyte membrane not being dried, leading to side reactions. Therefore, during the drying process, the drying temperature is determined to be 40-100℃. For example, the drying temperature can be selected as 40℃, 50℃, 60℃, 70℃, 80℃, 90℃, or 100℃ based on the ambient temperature and humidity.

[0037] Excessive drying time may cause the edges of the composite electrolyte membrane to curl up, resulting in an uneven surface that cannot be cut into films; insufficient drying time may cause some of the solution in the composite electrolyte membrane to be difficult to dry, increasing side reactions; therefore, the drying time is determined to be 5-20 hours, for example, the drying time can be selected as 5 hours, 10 hours, 15 hours or 20 hours according to the ambient temperature and humidity.

[0038] In one embodiment of the present invention, an application of a composite electrolyte membrane for a semi-solid lithium battery is provided. The composite electrolyte membrane is the composite electrolyte membrane of the semi-solid lithium battery described in any of the above technical solutions. The composite electrolyte membrane of the semi-solid lithium battery is used to prepare a semi-solid lithium battery. The semi-solid lithium battery includes a positive electrode, a negative electrode, the composite electrolyte membrane described in the above solutions, and a lithium-ion battery electrolyte disposed between the composite electrolyte membrane and the positive electrode and / or the negative electrode.

[0039] The electrolyte used in the lithium-ion battery is one or more of the commercially available conventional electrolytes.

[0040] This invention utilizes lithium aluminum titanium phosphate (LATP) in an inorganic / organic composite electrolyte membrane as an inorganic ceramic fast ion conductor in the system, thereby providing Li +It provides a continuous, rapid channel. The polymer PVDF-HFP provides a flexible framework for the inorganic phase LATP, enabling LATP to be film-formed via casting. Lithium salt is Li... + The source of these ions, and their core function, is to provide freely moving ions. The addition of plasticizers can dissolve and dissociate lithium salts, improve ionic conductivity, and participate in the construction of the SEI film. Simultaneously, it reduces the crystallinity of the polymer matrix, forming more readily available lithium ions. + The leaping "amorphous region" is key to improving ionic conductivity. Therefore, this inorganic-organic composite electrolyte membrane can form a stable SEI film, enabling lithium metal batteries using this membrane to exhibit excellent cycle stability at room temperature and extend the battery's operating voltage range.

[0041] The following are specific embodiments provided by the present invention.

[0042] Example 1

[0043] This embodiment provides an inorganic / organic composite electrolyte membrane for semi-solid lithium batteries and its preparation method.

[0044] The inorganic / organic composite electrolyte membrane, by weight, comprises the following raw materials: 60 parts lithium aluminum titanium phosphate (LATP), 12 parts polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), 18 parts lithium bis(fluorosulfonyl)imide (LiFSI), and 10 parts fluoroethylene carbonate (FEC). The weight-average molecular weight of PVDF-HFP is 400,000. The mass fractions of each component are: LATP 60%, PVDF-HFP 12%, LiFSI 18%, and FEC 10%, totaling 100%.

[0045] The preparation method includes the following steps: S1. In a glove box, add 18 parts LiFSI and 10 parts FEC to a glass bottle and stir magnetically at room temperature until LiFSI is fully dissolved or dispersed. Then add 12 parts PVDF-HFP. The order of addition is: LiFSI → FEC → PVDF-HFP, to avoid PVDF-HFP directly contacting the bottom of the bottle and sticking. Continue stirring magnetically at room temperature at a speed of 200 r / min until a homogeneous mixture without visible solid particles, stratification, or precipitation is formed, obtaining the first mixture.

[0046] S2. Add 60 parts of LATP to the first mixture and continue magnetic stirring at 200 r / min at room temperature until LATP is uniformly dispersed to obtain the second mixture. Adding LATP after dissolving PVDF-HFP can prevent it from prematurely contacting solids such as LiFSI and PVDF-HFP and causing aggregation.

[0047] S3. Place the second mixture on a polytetrafluoroethylene mold, and use a casting method to coat it with a scraper, controlling the coating thickness to be 150 μm, to form a wet film on the polytetrafluoroethylene mold.

[0048] S4. Place the wet membrane in a vacuum oven and vacuum dry it at 60°C for 12 h to obtain an inorganic / organic composite electrolyte membrane with a thickness of about 80 μm.

[0049] The inorganic / organic composite electrolyte membrane prepared in this embodiment has good flexibility and can be cut into the required size, making it suitable for assembling semi-solid lithium metal batteries.

[0050] Example 2

[0051] This embodiment provides an inorganic / organic composite electrolyte membrane for semi-solid lithium batteries and its preparation method.

[0052] The inorganic / organic composite electrolyte membrane, by weight, comprises the following raw materials: 65 parts lithium aluminum titanium phosphate (LATP), 15 parts polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), 12 parts lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and 8 parts propylene carbonate (PC). The weight-average molecular weight of PVDF-HFP is 450,000. The mass fractions of each component are: LATP 65%, PVDF-HFP 15%, LiTFSI 12%, and PC 8%, totaling 100%.

[0053] The preparation method includes the following steps: S1. In a glove box, add 12 parts LiTFSI and 8 parts PC to a glass bottle and magnetically stir at room temperature until LiTFSI is fully dissolved or dispersed. Then add 15 parts PVDF-HFP. The order of addition is: LiTFSI → PC → PVDF-HFP, to avoid PVDF-HFP directly contacting the bottom of the bottle and sticking. Continue magnetic stirring at room temperature at a speed of 300 r / min until a homogeneous mixture without visible solid particles, stratification, or precipitation is formed, obtaining the first mixture.

[0054] S2. Add 65 parts of LATP to the first mixture and continue magnetic stirring at 300 r / min at room temperature until LATP is uniformly dispersed to obtain the second mixture. Adding LATP after dissolving PVDF-HFP can prevent it from prematurely contacting solids such as LiTFSI and PVDF-HFP and causing aggregation.

[0055] S3. Place the second mixture on a polytetrafluoroethylene mold, and use a casting method to coat it with a scraper, controlling the coating thickness to be 200 μm, to form a wet film on the polytetrafluoroethylene mold.

[0056] S4. Place the wet membrane in a vacuum oven and vacuum dry it at 80°C for 10 h to obtain an inorganic / organic composite electrolyte membrane with a thickness of about 100 μm.

[0057] The inorganic / organic composite electrolyte membrane prepared in this embodiment has good flexibility and ionic conductivity, and can be cut into the required size, making it suitable for assembling semi-solid lithium metal batteries.

[0058] The following are performance tests on the samples prepared in Example 2: 1. Flame retardant test The inorganic / organic composite electrolyte membrane prepared in Example 2 was subjected to a combustion test. A flame was brought into contact with the composite electrolyte membrane, and the flame was removed after 2 seconds. Changes in the composite electrolyte membrane before and after the combustion test were recorded. Figure 2 As shown, the composite electrolyte membrane is self-extinguishing.

[0059] 2. Impedance test Impedance testing was performed on the inorganic / organic composite electrolyte membrane prepared in Example 2. A battery was constructed by adding stainless steel sheets to both ends of the composite electrolyte membrane. The diameter of both the composite electrolyte membrane and the stainless steel sheets was 16 mm. The test frequency range was 0.1 Hz to 1,000,000 Hz (electrochemical workstation). The corresponding impedance diagrams at room temperature are shown below. Figure 3 As shown, the inorganic / organic composite electrolyte membrane has a relatively low impedance.

[0060] 3. Linear Scan LSV Test The inorganic / organic composite electrolyte membrane prepared in Example 2 was subjected to linear sweep voltammetry (LSV) testing. A battery was constructed by adding lithium plates and stainless steel plates to both ends of the composite electrolyte membrane. The diameter of the lithium plate was 12 mm, the diameter of the inorganic / organic composite electrolyte membrane was 16 mm, and the diameter of the stainless steel plate was 16 mm. The scan rate was 0.01 V s⁻¹ (electrochemical workstation). The corresponding LSV test graph is shown below. Figure 4 As shown, the electrochemical window of the inorganic / organic composite electrolyte membrane is 4.9 V.

[0061] Example 3

[0062] This embodiment provides a method for preparing a semi-solid lithium metal coin cell and its electrochemical performance testing.

[0063] I. Preparation of the positive electrode sheet Lithium nickel cobalt manganese oxide (NCM622), acetylene black, and polyvinylidene fluoride were added to N-methylpyrrolidone at a mass ratio of 8:1:1 and stirred until homogeneous to obtain a positive electrode slurry. The positive electrode slurry was coated onto one side of an aluminum foil and vacuum dried at 120°C to remove N-methylpyrrolidone, yielding a positive electrode sheet. The positive electrode sheet was cut into circular pieces with a diameter of 12 mm, and the active material loading was approximately 2.12 mg / cm³. 2 .

[0064] II. Battery Assembly Using a lithium metal sheet as the negative electrode and the inorganic / organic composite electrolyte membrane prepared in Example 2 as the electrolyte membrane, the electrolyte membrane is cut into circular pieces with a diameter of 16 mm. In a glove box, the positive electrode sheet, the electrolyte membrane, and the negative lithium sheet are stacked sequentially, and lithium-ion battery electrolyte is dropped between the electrolyte membrane and the positive and / or negative lithium sheet. In this embodiment, the lithium-ion battery electrolyte is a commercially available high-voltage electrolyte. The above-described stacked structure is then installed in a CR2032 coin cell casing to assemble a semi-solid-state lithium metal coin cell.

[0065] The following are performance tests on the samples prepared in Example 3: 1. Loop testing The lithium metal battery of Example 3 was tested at room temperature. The charging cutoff voltage was 4.4V, and the discharging cutoff voltage was 3.0V. The charging and discharging current was set to 0.1C. Figure 5 As shown, the semi-solid-state battery prepared according to Example 3 has a discharge specific capacity of over 200 mAh g⁻¹ at room temperature and a capacity retention rate of 90.06% after 70 cycles; the charge / discharge current is set to 0.5C, such as... Figure 6 As shown, the semi-solid battery prepared according to Example 3 has a discharge specific capacity of over 190 mAh g-1 at room temperature, and a capacity retention rate of 96.71% after 25 charge-discharge cycles.

[0066] The results show that the composite electrolyte membrane provided by this invention has excellent flame retardant properties. By introducing a plasticizer, the ionic conductivity is improved and the crystallinity of the polymer is reduced, which not only enhances the flexibility of the inorganic / organic composite electrolyte membrane but also provides room temperature cycling stability and extends cycle life. By introducing a lithium-ion battery electrolyte to optimize the electrode / electrolyte interface contact, high ionic conductivity is achieved while reducing the desolvation energy barrier of lithium ions at the electrode / electrolyte interface, effectively reducing the battery's internal resistance. The lithium-ion battery electrolyte can also suppress interfacial side reactions and construct a stable SEI film, thereby inhibiting the growth of lithium dendrites. The lithium metal battery assembled with this inorganic / organic composite electrolyte membrane has a wide operating voltage range, high cycle stability, and capacity retention, significantly improving the cycle performance and safety performance of lithium metal batteries. The preparation process of this invention is simple and low-cost, compatible with existing processes, and has great application prospects.

[0067] In the claims, description, and accompanying drawings of this invention, the term "plural" refers to two or more. Unless otherwise explicitly defined, the terms "upper," "lower," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and simplifying the descriptive process, and are not intended to indicate or imply that the device or element referred to must have the described specific orientation, or be constructed and operated in a specific orientation. Therefore, these descriptions should not be construed as limiting the invention. The terms "connected," "installed," "fixed," etc., should be interpreted broadly. For example, "connected" can be a fixed connection between multiple objects, a detachable connection between multiple objects, or an integral connection; it can be a direct connection between multiple objects or an indirect connection between multiple objects through an intermediate medium. For those skilled in the art, the specific meaning of the above terms in this invention can be understood based on the specific circumstances described above.

[0068] In the claims, description, and accompanying drawings of this invention, the terms "one embodiment," "some embodiments," "specific embodiment," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In the claims, description, and accompanying drawings of this invention, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0069] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A composite electrolyte membrane for a semi-solid lithium battery, characterized in that, The raw materials for the composite electrolyte membrane include: lithium titanium aluminum phosphate, polyvinylidene fluoride-hexafluoropropylene, lithium salt, and plasticizer; The mass percentages of the lithium titanium aluminum phosphate, the polyvinylidene fluoride-hexafluoropropylene, the lithium salt, and the plasticizer are as follows: lithium titanium aluminum phosphate 40%-80%, polyvinylidene fluoride-hexafluoropropylene 10%-40%, lithium salt 5%-30%, and plasticizer 5%-20%.

2. The composite electrolyte membrane of the semi-solid lithium battery according to claim 1, characterized in that, The polyvinylidene fluoride-hexafluoropropylene has a weight-average molecular weight of one or more of 100,000, 400,000, and 450,000.

3. The composite electrolyte membrane of the semi-solid lithium battery according to claim 1, characterized in that, The lithium salt is one or more of lithium bis(trifluoromethanesulfonate)imide, lithium bis(fluorosulfonylimide), lithium perchlorate, lithium hexafluorophosphate, and lithium tetrafluoroborate.

4. The composite electrolyte membrane of the semi-solid lithium battery according to claim 1, characterized in that, The plasticizer is one or more of the following: fluoroethylene carbonate, propylene carbonate, polyethylene glycol, dioctyl adipate, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

5. A method for preparing a composite electrolyte membrane, characterized in that, The preparation method is used to prepare the composite electrolyte membrane of the semi-solid lithium battery as described in claim 1, and the preparation method includes: According to the mass percentage of the polyvinylidene fluoride-hexafluoropropylene, the lithium salt, and the plasticizer, the lithium salt, the plasticizer, and the polyvinylidene fluoride-hexafluoropropylene are added to a container in the order of the lithium salt, the plasticizer, and the polyvinylidene fluoride-hexafluoropropylene, and stirred at room temperature until they are mixed evenly to obtain a first mixture. According to the mass percentage of lithium titanium aluminum phosphate, lithium titanium aluminum phosphate is added to the first mixture and stirred at room temperature until it is uniformly mixed to obtain the second mixture; The second mixture is applied to a polytetrafluoroethylene mold and coated by a casting method to form a wet film on the polytetrafluoroethylene mold. The wet membrane is dried under vacuum conditions to obtain the composite electrolyte membrane.

6. The method for preparing the composite electrolyte membrane of the semi-solid lithium battery according to claim 5, characterized in that, When performing the stirring at room temperature until the mixture is homogeneous, a magnetic stirrer is used, and the stirring speed is set to 100-400 r / min.

7. The method for preparing the composite electrolyte membrane of the semi-solid lithium battery according to claim 5, characterized in that, The method of coating by casting includes: The second mixture is coated with a doctor blade, and the coating thickness is controlled to be 50-300 μm to obtain the wet film.

8. The method for preparing the composite electrolyte membrane of the semi-solid lithium battery according to claim 5, characterized in that, The step of drying the wet film under vacuum conditions includes: The wet membrane is placed in a vacuum oven, and the temperature of the vacuum oven is controlled at 40-100℃. The wet membrane is dried for 5-20 hours to obtain the composite electrolyte membrane with a thickness of 10-200μm.

9. The application of a composite electrolyte membrane in a semi-solid lithium battery, characterized in that, The composite electrolyte membrane is the composite electrolyte membrane of the semi-solid lithium battery according to any one of claims 1 to 4, and the composite electrolyte membrane of the semi-solid lithium battery is used to prepare a semi-solid lithium battery.