A composite solid electrolyte material with high ionic conductivity and its preparation method
By introducing a core-shell structured oxide doped phase, compounded lithium salt, and interface modifier into a sulfide solid electrolyte, a composite electrolyte with high ionic conductivity and excellent mechanical properties is constructed. This solves the problem of balancing ionic conductivity, mechanical properties, and interface compatibility in high-energy-density batteries using sulfide electrolytes, thereby improving battery safety and cycle life.
Patent Information
- Application Number
- CN202611342560.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-10
AI Technical Summary
Existing sulfide solid electrolytes are difficult to balance high ionic conductivity, excellent mechanical properties and good interfacial compatibility in high-energy-density batteries, and there are risks of interfacial contact failure, lithium dendrite growth and safety hazards.
A high ionic conductivity composite solid electrolyte material is adopted, which includes a homogeneous solid solution of Li6PS5Cl and Li3PS4, a core-shell structured oxide doped phase, a composite lithium salt and an interface modifier. Through synergistic design, a continuous lithium-ion transport channel is constructed, mechanical properties are enhanced and interfacial side reactions are suppressed.
It achieves high ionic conductivity (2.0×10-3S/cm at room temperature) and excellent mechanical properties (tensile strength 22MPa, flexural strength 38MPa), significantly improving battery cycle life and safety, with low initial interface impedance and long-term stability.
Smart Images

Figure CN123073147A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a high ionic conductivity composite solid electrolyte material and its preparation method. Background Technology
[0002] Solid-state lithium batteries, with their outstanding advantages such as high energy density, high safety, and wide electrochemical window, have become the core development direction of next-generation electrochemical energy storage technology, and have broad application prospects in electric vehicles, grid-scale large-scale energy storage, and portable electronic devices. Solid-state electrolytes, as the core functional components of solid-state lithium batteries, play a dual role in conducting lithium ions and isolating the positive and negative electrodes. Their ionic conductivity, mechanical properties, interfacial compatibility, and chemical stability directly determine the overall performance, cycle life, and safety reliability of the battery. Among various solid-state electrolyte systems, sulfide electrolytes are considered one of the most industrially promising solid-state electrolyte systems due to their high room-temperature ionic conductivity, low interfacial contact resistance, and cold-pressing properties. Typical sulfide materials such as Li6PS5Cl and Li3PS4 have become research hotspots in the field.
[0003] Despite their high intrinsic ionic conductivity, sulfide electrolytes still face several technical bottlenecks in practical battery applications. These include insufficient intrinsic mechanical strength and toughness, making it difficult to adapt to the volume expansion and contraction of the positive and negative electrode active materials during charge-discharge cycles. This leads to microcracks and interfacial contact failures, and makes it difficult to effectively suppress lithium dendrite growth and penetration, posing a safety hazard of battery short circuits. Furthermore, sulfide electrolytes exhibit poor chemical compatibility with highly active lithium metal anodes, leading to persistent side reactions at the interface and the formation of a high-resistivity interfacial passivation layer, significantly increasing battery polarization and accelerating capacity decay.
[0004] To address the aforementioned issues, existing technologies often employ modification methods such as introducing oxide second-phase reinforcement, surface polymer coating, and element doping. However, a single modification scheme can often only optimize a single performance indicator: introducing oxide particles is prone to agglomeration, which not only reduces the reinforcement effect but also blocks the lithium-ion transport path, thus reducing conductivity; when using a rigid oxide coating layer, the modulus difference between it and the sulfide matrix is significant, and interfacial cracking is prone to occur during cycling, leading to impedance rebound; when using polymer coating, the restricted movement of polymer chain segments at room temperature hinders ion transport, which in turn reduces the overall ionic conductivity of the electrolyte, making it impossible to achieve a synergistic improvement in high ionic conductivity, excellent mechanical properties, and good interfacial compatibility. Summary of the Invention
[0005] The purpose of this invention is to overcome the technical defects of existing sulfide solid electrolytes that are difficult to balance ionic conductivity, mechanical properties and interfacial compatibility, and to provide a high ionic conductivity composite solid electrolyte material and its preparation method. Through synergistic design, the comprehensive performance of the electrolyte material is systematically improved to meet the application requirements of high-performance solid lithium metal batteries.
[0006] A high ionic conductivity composite solid electrolyte material comprises, by mass percentage: 73-85 wt% of a sulfide host electrolyte, 5-15 wt% of a core-shell structured oxide doped phase, 6-10 wt% of a compound lithium salt, and 0.5-2 wt% of an interface modifier.
[0007] The sulfide-based main electrolyte is a homogeneous solid solution formed by Li6PS5Cl and Li3PS4, wherein the molar ratio of Li6PS5Cl to Li3PS4 is 1:0.3~0.7.
[0008] The core-shell structured oxide doped phase is composed of nanoparticles consisting of a zirconium-based oxide core and an aluminum-based oxide shell, and the aspect ratio of the nanoparticles is 3~8:1.
[0009] The compound lithium salt is a mixture of lithium bis(trifluoromethanesulfonyl)imide and lithium bis(fluorosulfonyl)imide;
[0010] The interface modifier is a silane coupling agent.
[0011] Furthermore, the zirconium-based oxide core is composed of ZrO2 nanoparticles with a particle size of 20-50 nm; the aluminum-based oxide shell is an Al2O3 layer with a thickness of 5-10 nm. The high-hardness, high-modulus ZrO2 core can form dispersed reinforcing sites within the matrix, effectively improving the overall deformation resistance of the electrolyte. The thin and uniform alumina shell possesses excellent lithium-affinity properties, enabling the construction of continuous lithium-ion transition channels on the particle surface, while simultaneously blocking direct contact between the sulfide matrix and the lithium metal anode, suppressing interfacial side reactions and lithium dendrite nucleation.
[0012] Furthermore, the mass ratio of lithium bis(trifluoromethanesulfonyl)imide to lithium bis(fluorosulfonyl)imide in the composite lithium salt is 2:1 to 1:1. LiFSI can significantly reduce the activation energy of lithium-ion migration and increase the carrier concentration at grain boundaries. LiTFSI has excellent thermal and structural stability, which can compensate for the defect of LiFSI being prone to electrochemical corrosion. The two form a synergistic system within this ratio range, which not only broadens the fast lithium-ion transport channel but also maintains the overall chemical stability of the composite electrolyte.
[0013] Furthermore, the silane coupling agent is γ-aminopropyltriethoxysilane or γ-glycidoxypropyltrimethoxysilane. The silane coupling agent constructs a highly ionic, dense passivated buffer layer at the electrolyte-electrode interface, effectively isolating electrolyte residues, sulfides, and side reactions with metallic lithium, thereby reducing interfacial contact resistance.
[0014] Furthermore, the composite solid electrolyte material is a hot-pressed, densified sheet structure with a thickness of 20-50 μm and a porosity not exceeding 5%. A thickness less than 20 μm is prone to being pierced by lithium dendrites during assembly and charge / discharge processes, significantly increasing the risk of short circuits. A thickness exceeding 50 μm prolongs the lithium-ion conduction distance, increasing battery polarization and reducing rate performance. Controlling the porosity to within 5% significantly reduces the channels for air and moisture intrusion, while shortening the lithium-ion transport distance between particles, ensuring high overall ionic conductivity. The dense sheet structure also improves the overall mechanical continuity of the material, mitigating interface peeling and cracking problems caused by electrode volume expansion during charge / discharge.
[0015] A method for preparing a composite solid electrolyte material with high ionic conductivity includes the following steps:
[0016] S1. Preparation of sulfide solid solution: Li6PS5Cl and Li3PS4 were mixed at a set molar ratio and ball-milled under an inert protective atmosphere, followed by annealing to obtain a uniform sulfide-based electrolyte solid solution powder.
[0017] S2. Preparation of core-shell oxide: Aluminum-based oxide precursors were uniformly coated on the surface of zirconium-based oxide nanocores using a sol-gel process. After high-temperature calcination and crystallization, core-shell structured oxide doped phases were obtained.
[0018] S3. Lithium salt pretreatment: Lithium bis(trifluoromethanesulfonyl)imide and lithium bis(fluorosulfonyl)imide are mixed in a certain proportion and vacuum dried to remove moisture and residual solvent to obtain a compound lithium salt.
[0019] S4. Mixing and surface modification: In an inert atmosphere, the sulfide-based electrolyte solid solution powder, the core-shell structure oxide doped phase and the compound lithium salt are mixed, and the interface modifier is added by spraying. The components are uniformly dispersed and the interface modifier is grafted in situ by planetary ball milling.
[0020] S5. Hot pressing: The mixed powder is placed in a mold and hot-pressed to densify it under a set temperature and pressure. After heat preservation, it is cooled and demolded to obtain a composite solid electrolyte sheet.
[0021] Furthermore, in step S1, the high-energy ball mill operates at a speed of 400-600 r / min, a milling time of 8-12 h, a ball-to-material ratio of 20-30:1, and agate balls are used as the grinding media; the annealing treatment is performed at a temperature of 200-250℃, a holding time of 3-5 h, and the inert protective atmosphere is argon, with an oxygen content ≤1 ppm and a moisture content ≤0.1 ppm in the system.
[0022] Furthermore, in step S2, the sol-gel process uses anhydrous ethanol as the dispersion medium, aluminum isopropoxide as the aluminum source, and the reaction temperature is 60~80℃; the high-temperature calcination temperature is 500~600℃, and the holding time is 2~3h.
[0023] Furthermore, the planetary ball mill has a ball-to-material ratio of 20:1, a rotation speed of 300~400 r / min, and a milling time of 4~6 h; the interface modifier has a spray pressure of 0.3~0.5 MPa, a feed rate of 0.5~1 mL / min, a hot-pressing temperature of 150~180℃, a hot-pressing pressure of 60~80 MPa, and a holding time of 1~2 h.
[0024] Beneficial effects:
[0025] This invention achieves a significant improvement in ionic conductivity through a multi-component synergistic design of a sulfide solid solution matrix, a core-shell structured oxide doped phase, a composite lithium salt system, and an interface modifier. The sulfide solid solution combines the high intrinsic conductivity of Li6PS5Cl with the good flexibility of Li3PS4. The composite lithium salt synergistically modulates the lithium-ion transport environment at grain boundaries and in amorphous regions, reducing the migration energy barrier. Combined with the continuous ion transport auxiliary channels constructed by the core-shell oxide in the matrix, the room-temperature ionic conductivity of the composite electrolyte can reach 2.0 × 10⁻⁶. -3 With a S / cm range, it is significantly superior to conventional single-modified sulfide electrolytes and can fully meet the application requirements of high-rate charge and discharge.
[0026] Simultaneously, it achieves synergistic optimization of mechanical properties and interface stability. The core-shell structured oxide doped phase combines a high-modulus zirconium-based oxide core with a lithium-loving aluminum-based oxide shell. It can effectively improve the tensile and flexural strength of the matrix through dispersion strengthening effect, resisting stress damage caused by electrode volume deformation. It can also inhibit the growth and puncture of lithium dendrites through physical barrier and interface regulation. Silane-based interface modifiers construct a dense and stable high-ion conductivity layer at the electrolyte-electrode interface through chemical bonding, effectively suppressing the occurrence of interface side reactions, keeping the initial interface impedance at a low level, and the impedance increase during long-term cycling is small, significantly improving the cycle life and operational safety of the battery. Attached Figure Description
[0027] Figure 1This is a process flow diagram of the preparation process of the composite solid electrolyte material of the present invention;
[0028] Figure 2 Here is a comparison table of component parameters and performance of Examples 1 to 6: Detailed Implementation
[0029] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the protection scope of the present invention.
[0030] Example 1:
[0031] The high ionic conductivity composite solid electrolyte material of this embodiment comprises, by mass percentage: 80 wt% sulfide host electrolyte, 10 wt% core-shell structured oxide doped phase, 8 wt% compounded lithium salt, and 2 wt% interface modifier. The sulfide host electrolyte is a solid solution of Li6PS5Cl and Li3PS4 in a molar ratio of 1:0.5. The core-shell structured oxide doped phase is ZrO2@Al2O3 nanoparticles, with a ZrO2 core diameter of 30 nm, an Al2O3 shell thickness of 8 nm, and an aspect ratio of 5:1. The compounded lithium salt is a mixture of lithium bis(trifluoromethanesulfonyl)imide and lithium bis(fluorosulfonyl)imide in a mass ratio of 1.5:1. The interface modifier is γ-aminopropyltriethoxysilane.
[0032] The preparation method of this embodiment includes the following steps:
[0033] S1: Preparation of sulfide-based electrolyte: Weigh 0.5 mol Li6PS5Cl and 0.25 mol Li3PS4, mix them in an argon-protected glove box with moisture ≤0.1 ppm and oxygen ≤0.1 ppm, add agate balls (ball-to-material ratio 30:1), and ball mill at 500 r / min for 10 h; then anneal the ball-milled product in an argon atmosphere at 220℃ for 4 h, and obtain a white solid solution powder after natural cooling.
[0034] S2: Preparation of core-shell nanoparticles: 5g of ZrO2 nanoparticles with a particle size of 30nm were dispersed in 100mL of anhydrous ethanol and ultrasonically dispersed for 30min to form a uniform suspension; 8g of aluminum isopropoxide was added and reacted at a constant temperature of 70℃ with stirring for 5h; after the reaction was completed, the product was separated and placed in a muffle furnace and calcined at 550℃ for 2.5h, and after cooling, ZrO2@Al2O3 core-shell structured nanoparticles were obtained.
[0035] S3: Preparation of compound lithium salt: Weigh 4.8g of lithium bis(trifluoromethanesulfonyl)imide and 3.2g of lithium bis(fluorosulfonyl)imide, mix them thoroughly, and then vacuum dry them at 90℃ for 18h to completely remove moisture and residual solvent.
[0036] S4: Mixing and Dispersion: 80g of sulfide-based electrolyte powder, 10g of core-shell nanoparticles, and 8g of compounded lithium salt were added to an argon glove box. At the same time, 2g of γ-aminopropyltriethoxysilane was added by spraying at a pressure of 0.4MPa and a rate of 0.8mL / min. The mixture was dispersed using a planetary ball mill with a ball-to-material ratio of 20:1, a rotation speed of 350r / min, and a milling time of 5h.
[0037] S5: Hot pressing: The uniformly mixed powder is transferred into a polytetrafluoroethylene mold and hot-pressed at 160℃ and 70MPa. After holding at the temperature for 1.5h, it is naturally cooled and demolded to obtain a composite solid electrolyte sheet with a thickness of 30μm.
[0038] The performance of the sample prepared in this embodiment was tested: the ionic conductivity was measured using the AC impedance method, and it was 2.1 × 10⁻⁶ at 25°C. -3 S / cm, reaching 5.3×10 at 50℃ -3 S / cm; Mechanical properties were tested using a universal testing machine: tensile strength 22 MPa, flexural strength 38 MPa, and elongation at break 3.5%; Interface impedance was tested when the battery was assembled with a lithium metal anode to form a symmetrical battery, with an initial contact impedance of 12 Ω·cm. 2 After 1000 cycles, the value is 14 Ω·cm. 2 After being stored in an argon atmosphere for 6 months, the ionic conductivity retention rate was 96%. When equipped with an NCM811 / composite electrolyte / Li metal battery, the initial discharge capacity was 195mAh / g at 25℃ and 0.5C, and the capacity retention rate was 89% after 1000 cycles.
[0039] Example 2:
[0040] The high ionic conductivity composite solid electrolyte material of this embodiment consists of the following components by mass percentage: 80wt% sulfide main electrolyte, 10wt% core-shell structured oxide doped phase, 9wt% compounded lithium salt, and 1wt% interface modifier; the composition of other substances is the same as in Example 1, and the interface modifier is γ-glycidoxypropyltrimethoxysilane.
[0041] The preparation process in this embodiment is the same as in Example 1, except that the interface modifier is replaced with γ-glycidoxypropyltrimethoxysilane and the amount is adjusted to 1 wt%.
[0042] The performance of the sample prepared in this embodiment was tested: the ionic conductivity at 25℃ was 1.9 × 10⁻⁶. -3S / cm, tensile strength 21MPa; initial contact resistance with lithium metal anode is 14Ω·cm. 2 Equipped with NCM811 / composite electrolyte / Li metal battery, the capacity retention rate is 87% after 1000 cycles.
[0043] Example 3:
[0044] The high ionic conductivity composite solid electrolyte material of this embodiment comprises, by mass percentage: 78 wt% sulfide host electrolyte, 12 wt% core-shell structured oxide doped phase, 9 wt% compounded lithium salt, and 1 wt% interface modifier. Specifically, the molar ratio of Li6PS5Cl to Li3PS4 in the sulfide host electrolyte is 1:0.6; the core-shell structured oxide doped phase is ZrO2@Al2O3 nanoparticles with an aspect ratio of 8:1; the mass ratio of lithium bis(trifluoromethanesulfonyl)imide to lithium bis(fluorosulfonyl)imide in the compounded lithium salt is 1:1; and the interface modifier is γ-glycidyl etheroxypropyltrimethoxysilane. The remaining component parameters and preparation process are adapted to those of Example 1.
[0045] The sample prepared in this embodiment was subjected to performance testing: the ionic conductivity at 25℃ was 2.0 × 10⁻⁶. -3 S / cm, tensile strength 23MPa, initial interfacial resistance 13Ω·cm 2 .
[0046] Example 4
[0047] The component ratio was adjusted as follows: the sulfide main electrolyte was 78 wt% (Li6PS5Cl:Li3PS4=1:0.6), the oxide doped phase was 12 wt%, the compound lithium salt was 8 wt% (LiTFSI:LiFSI=1:1), and the interface modifier KH560 was 2 wt%. The aspect ratio of the core-shell particles was adjusted to 8:1.
[0048] Performance test results: Ionic conductivity at 25℃: 2.2 × 10⁻⁶ -3 S / cm, tensile strength 24MPa, initial interfacial resistance 11Ω·cm 2 .
[0049] Example 5
[0050] Adjust the component ratio: 73wt% of sulfide main electrolyte (Li6PS5Cl:Li3PS4=1:0.3), 15wt% of oxide doped phase, 10wt% of compound lithium salt (LiTFSI:LiFSI=1.2:1), and 2wt% of interface modifier KH550.
[0051] Performance test results: Ionic conductivity at 25℃ is 1.8×10⁻⁶ -3S / cm, tensile strength 20MPa, initial interfacial resistance 16Ω·cm 2 .
[0052] Example 6
[0053] Adjust the component ratio: the sulfide main electrolyte is 82wt% (Li6PS5Cl:Li3PS4=1:0.7), the oxide doped phase is 7wt%, the compound lithium salt is 10wt% (LiTFSI:LiFSI=1:1), and the interface modifier KH550 is 1wt%.
[0054] Performance test results: Ionic conductivity at 25℃ is 2.1×10⁻⁶ -3 S / cm, tensile strength 22MPa, initial interfacial resistance 12Ω·cm 2 .
[0055] In summary, changes in the content of each component collectively determine the final performance of the electrolyte by altering the ion conduction network, the state of the two-phase interface, and the mechanical reinforcement effect. The sulfide-based electrolyte constructs a continuous lithium-ion transport pathway; too low a content will cause the conductive network to be interrupted by the insulating doped phase, hindering ion conduction. The core-shell oxide doped phase provides mechanical reinforcement and interface passivation, increasing tensile strength in the 5-12 wt% range; excessive doping will cause particle agglomeration, deteriorating ion conductivity. The compounded lithium salt provides migratable lithium ions; an appropriate compounding ratio can promote lithium salt dissociation and increase carrier concentration; excessive lithium salt easily precipitates and agglomerates, increasing impedance. Interface modifiers improve the wettability of the inorganic-organic interface and reduce interface defects; excessive addition introduces organic insulating impurities, blocking ion channels.
[0056] As a further improvement, the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A composite solid electrolyte material with high ionic conductivity, characterized in that, It comprises, by mass percentage: 73-85 wt% sulfide main electrolyte, 5-15 wt% core-shell structured oxide doped phase, 6-10 wt% compound lithium salt and 0.5-2 wt% interface modifier; The sulfide-based electrolyte is a homogeneous solid solution formed by Li6PS5Cl and Li3PS4, wherein the molar ratio of Li6PS5Cl to Li3PS4 is 1:0.3~0.
7. The core-shell structured oxide doped phase is composed of zirconium-based oxide cores and aluminum-based oxide shells, and the aspect ratio of the nanoparticles is 3~8:
1. The compound lithium salt is a mixture of lithium bis(trifluoromethanesulfonyl)imide and lithium bis(fluorosulfonyl)imide; The interface modifier is a silane coupling agent.
2. The high ionic conductivity composite solid electrolyte material according to claim 1, characterized in that, The zirconium-based oxide core is ZrO2 nanoparticles with a particle size of 20-50 nm; the aluminum-based oxide shell is an Al2O3 layer with a shell thickness of 5-10 nm.
3. The high ionic conductivity composite solid electrolyte material according to claim 1, characterized in that, The mass ratio of lithium bis(trifluoromethanesulfonyl)imide to lithium bis(fluorosulfonyl)imide in the compound lithium salt is 2:1 to 1:
1.
4. The high ionic conductivity composite solid electrolyte material according to claim 1, characterized in that, The silane coupling agent is γ-aminopropyltriethoxysilane or γ-glycidoxypropyltrimethoxysilane.
5. The high ionic conductivity composite solid electrolyte material according to claim 1, characterized in that, The composite solid electrolyte material is a thin sheet structure that has been densified by hot pressing, with a thickness of 20~50μm and a porosity of no more than 5%.
6. A method for preparing a high ionic conductivity composite solid electrolyte material as described in any one of claims 1-5, characterized in that, Includes the following steps: S1. Preparation of sulfide solid solution: Li6PS5Cl and Li3PS4 were mixed at a set molar ratio and ball-milled under an inert protective atmosphere, followed by annealing to obtain a uniform sulfide-based electrolyte solid solution powder. S2. Preparation of core-shell oxides: Aluminum-based oxide precursors were uniformly coated on the surface of zirconium-based oxide nanocores using a sol-gel process. After high-temperature calcination and crystallization, core-shell structured oxide doped phases were obtained. S3. Lithium salt pretreatment: Lithium bis(trifluoromethanesulfonyl)imide and lithium bis(fluorosulfonyl)imide are mixed in a certain proportion and vacuum dried to remove moisture and residual solvent to obtain a compound lithium salt. S4. Mixing and surface modification: In an inert atmosphere, the sulfide-based electrolyte solid solution powder, the core-shell structure oxide doped phase and the compound lithium salt are mixed, and the interface modifier is added by spraying. The components are uniformly dispersed and the interface modifier is grafted in situ by planetary ball milling. S5. Hot pressing: The mixed powder is placed in a mold and hot-pressed to densify it under a set temperature and pressure. After heat preservation, it is cooled and demolded to obtain a composite solid electrolyte sheet.
7. The method for preparing a high ionic conductivity composite solid electrolyte material according to claim 6, characterized in that, In step S1, the high-energy ball mill operates at a speed of 400-600 r / min, a milling time of 8-12 h, a ball-to-material ratio of 20-30:1, and agate balls are used as the grinding media. The annealing treatment is carried out at a temperature of 200-250℃ and a holding time of 3-5 h. The inert protective atmosphere is argon, and the oxygen content and moisture content in the system are ≤1 ppm and ≤0.1 ppm, respectively.
8. The method for preparing a high ionic conductivity composite solid electrolyte material according to claim 6, characterized in that, In step S2, the sol-gel process uses anhydrous ethanol as the dispersion medium and aluminum isopropoxide as the aluminum source, with a reaction temperature of 60~80℃; the high-temperature calcination temperature is 500~600℃, and the holding time is 2~3h.
9. The method for preparing a high ionic conductivity composite solid electrolyte material according to claim 6, characterized in that, The planetary ball mill has a ball-to-material ratio of 20:1, a rotation speed of 300~400 r / min, and a milling time of 4~6 h; the interface modifier has a spray pressure of 0.3~0.5 MPa, a feed rate of 0.5~1 mL / min, a hot pressing temperature of 150~180℃, a hot pressing pressure of 60~80 MPa, and a holding time of 1~2 h.