Yttrium-zirconium co-doped sulfide solid electrolyte, its preparation method and application
By preparing yttrium zirconium co-doped sulfide solid electrolytes, the problems of low ionic conductivity and insufficient cycle stability of existing solid electrolytes have been solved, achieving high conductivity and long lifespan battery performance, suitable for lithium-ion, sodium-ion batteries and all-solid-state batteries.
Patent Information
- Application Number
- CN202611371732.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-05
- Publication Date
- 2026-11-10
AI Technical Summary
Existing solid electrolytes suffer from low ionic conductivity, insufficient cycle stability, and poor low-temperature performance, and single-element doping offers limited improvement.
Using yttrium-zirconium co-doped sulfide solid electrolytes, based on the chemical formula Lia(YxZr1-x)bClcSd, and combined with ball milling and molten salt synthesis reactions, an electrolyte with a specific crystal structure and high ionic conductivity was prepared.
It significantly improves the ionic conductivity of the electrolyte and the low-temperature performance of the battery, enhances the cycle stability and capacity retention of the battery, and exhibits excellent electrochemical performance, especially under low-temperature conditions.
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and in particular to a yttrium-zirconium co-doped sulfide solid electrolyte, its preparation method, and its application. Background Technology
[0002] With the rapid development of energy storage technology, solid-state batteries have attracted much attention due to their high energy density, long cycle life, and excellent safety performance. One of the core components of a solid-state battery is the solid electrolyte, which is responsible for conducting lithium ions between the positive and negative electrodes while isolating electrons to prevent short circuits. Compared to traditional liquid electrolytes, solid-state electrolytes have higher thermal and chemical stability, thus significantly improving battery safety.
[0003] However, the development of solid-state electrolytes faces numerous challenges. Existing solid sulfide electrolytes (such as Li6PS5Cl and Li6PS5Br) exhibit high ionic conductivity, but still have issues with interfacial stability and mechanical properties. Furthermore, single-element doping has improved performance to some extent, but problems such as insufficient conductivity and limited cycle life remain. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of existing technologies by providing a yttrium-zirconium co-doped sulfide solid electrolyte, which solves the defects of existing solid electrolytes such as low ionic conductivity, insufficient cycle stability, and poor low-temperature performance.
[0005] The present invention also provides a method for preparing a solid electrolyte, which can prepare the above-mentioned solid electrolyte and is simple and low in cost.
[0006] The present invention also provides a secondary battery comprising the above-mentioned solid electrolyte, and therefore, the battery has excellent electrochemical performance.
[0007] The objective of this invention is achieved through the following technical solution: Firstly, this invention provides a yttrium-zirconium co-doped sulfide solid electrolyte, wherein the general chemical formula of the yttrium-zirconium co-doped sulfide solid electrolyte is Lia(YxZr1-x)bClcSd, wherein: 0.5≤(a+b) / (c+d)≤1; 0 < x < 1; a>0, b>0, c>0, d>0.
[0008] Furthermore, the molar ratio of Y:Zr is (0.1–0.9):(0.9–0.1).
[0009] Furthermore, a:b = (2–9.5):1, d:b = (0.5–1.5):1.
[0010] Furthermore, the Li content is 20–40 at%, and the S content is 2–15 at%.
[0011] Furthermore, the yttrium-zirconium co-doped sulfide solid electrolyte is Li6(Y0.5Zr0.5)Cl5S2, Li3(Y0.2Zr0.8)Cl5S, or Li 18 (Y0.7Zr0.3)3Cl 28 At least one of S.
[0012] Furthermore, in the X-ray diffraction pattern, the yttrium-zirconium co-doped sulfide solid electrolyte includes at least 2θ diffraction peaks located at 28.4°–31.7°, 32.8°–37°, 47.1°–52.4°, and 57.3°–64.2°.
[0013] Furthermore, in the X-ray diffraction pattern, the width of the widest diffraction peak of the yttrium-zirconium co-doped sulfide solid electrolyte is ≤1.0°.
[0014] Furthermore, the yttrium-zirconium co-doped sulfide solid electrolyte has an ionic conductivity ≥7 mS / cm at 25°C.
[0015] Secondly, this invention provides a method for preparing a yttrium-zirconium co-doped sulfide solid electrolyte, comprising the following steps: The lithium source, yttrium source, zirconium source, chlorine source, and sulfur source are mixed in stoichiometric ratios to obtain a mixture; Under an inert atmosphere, the mixture is subjected to ball milling, solvent-assisted precipitation reaction, or molten salt synthesis reaction in sequence to obtain the solid electrolyte.
[0016] Furthermore, the process is carried out under an inert atmosphere, specifically an argon or nitrogen atmosphere with a dew point ≤ -60°C; the resulting solid electrolyte is then annealed at 200–400°C.
[0017] Thirdly, the present invention also provides a secondary battery, which includes a positive electrode, a negative electrode and an electrolyte layer, wherein the electrolyte layer includes the above-mentioned yttrium-zirconium co-doped sulfide solid electrolyte or the yttrium-zirconium co-doped sulfide solid electrolyte prepared by the above-mentioned preparation method.
[0018] Furthermore, the secondary battery is a lithium-ion battery, a sodium-ion battery, or a potassium-ion battery.
[0019] Furthermore, when the secondary battery is a lithium-ion battery, its capacity retention rate is ≥40% at -20℃; After 400 cycles of charge-discharge at 0.5C, the capacity retention is ≥80%. Energy density ≥350Wh / kg, volumetric energy density ≥1000Wh / L.
[0020] The solid electrolyte of this invention is doped with Y 3+ The vacancies formed later improved lithium + diffusion pathways of Zr 4+ The introduction of Y and Zr can stabilize the crystal lattice and reduce structural distortion. By introducing synergistic doping of Y and Zr into the Li–Cl–S-based system, the crystal structure and defect concentration can be controlled, the lithium-ion migration channels can be optimized, and the high conductivity and stability of the solid electrolyte can be improved. It can be used in lithium-ion batteries, sodium-ion batteries, and automotive / energy storage all-solid-state batteries, and is particularly suitable for high energy density and extreme temperature applications.
[0021] When used with lithium-ion batteries, it exhibits long lifespan and excellent low-temperature performance, with a capacity retention rate of ≥40% at 0℃ and a cycle life of 400 cycles under 0.5C charge-discharge conditions, with a capacity retention rate of ≥80%, demonstrating excellent low-temperature characteristics and long-cycle stability. Detailed Implementation
[0022] To further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, and not for limiting the scope of the claims of the present invention.
[0023] Unless otherwise specified, all reagents or instruments used in this invention are commercially available products.
[0024] Example 1: Preparation of Li6(Y0.5Zr0.5)Cl5S2 solid electrolyte material 1. Raw material preparation: In an argon atmosphere glove box with a dew point ≤ -60℃, weigh LiCl, YCl3, ZrCl4 and Li2S and mix them in a molar ratio of 6:0.5:0.5:2.
[0025] 2. Ball milling process: The mixture was transferred to a 45 mL stainless steel ball mill jar with zirconia grinding beads at a ball-to-material mass ratio of 10:1. After sealing the ball mill jar, it was removed from the glove box and placed in a high-energy planetary ball mill for continuous ball milling at 500 rpm for 50 h. After ball milling, the ball mill jar was transferred back to the argon glove box, opened, and sampled to obtain the ball-milled powder. The powder was placed in a quartz crucible and annealed at 300 °C for 2 h under argon protection, followed by furnace cooling to obtain yttrium-zirconia co-doped sulfide solid electrolyte powder Li6(Y0.5Zr0.5)Cl5S2.
[0026] 3. XRD characterization: The obtained sample was subjected to powder XRD under Cu-Kα radiation. Its main 2θ diffraction peaks were located at 29.3°, 34.2°, 48.5°, and 61.0°. The half-width at half-maximum (FWHM) of the broad diffraction peaks was 0.72°. The peaks were sharp, indicating that the material had good crystallinity and a spinel-type crystal structure.
[0027] Example 2: Preparation of Li3(Y0.2Zr0.8)Cl5S solid electrolyte material The preparation and testing process of the solid electrolyte in Example 2 is the same as that in Example 1, except that: 1. Raw material ratio: The molar ratio of LiCl:YCl3:ZrCl4:Li2S is 3:0.2:0.8:1.
[0028] 2. Preparation conditions: ball-to-material mass ratio 12:1, ball milling speed 600 rpm, ball milling time 25 h; After ball milling, the powder was annealed at 260℃ for 2 hours under argon protection, and after cooling, the target electrolyte Li3(Y0.2Zr0.8)Cl5S was obtained.
[0029] 3. Structural characterization: XRD analysis showed a Suzuki-type crystal structure; the characteristic diffraction peaks 2θ were 28.9°, 35.1°, 49.0°, and 59.6°, all falling within the diffraction angle range defined in the claims; the widest diffraction peak had a half-width at half-maximum (FWHM) of 0.65°, indicating good crystallinity.
[0030] Example 3: Li 18 (Y0.7Zr0.3)3Cl 28 Preparation of S solid electrolyte materials The preparation and testing process of the solid electrolyte in Example 3 is the same as that in Example 1, except that: 1. Raw material ratio: The molar ratio of LiCl:YCl3:ZrCl4:Li2S is 18:2.1:0.9:1.
[0031] 2. Preparation process: The molten salt synthesis process was employed: the mixture was heated to 600℃ in an inert atmosphere at a heating rate of 8℃ / min and held at that temperature for 1 h; then rapidly quenched and cooled to room temperature; the product was removed and ground in a glove box; annealed at 320℃ for 1.5 h in an argon atmosphere and allowed to cool naturally to obtain Li. 18 (Y0.7Zr0.3)3Cl 28 S Solid electrolyte powder.
[0032] 3. Structural characterization: Powder XRD analysis showed characteristic diffraction peaks at 2θ of 30.1°, 34.7°, 50.2°, and 60.4°; the widest diffraction peak had a half-maximum width (FWHM) of 0.81°, indicating excellent crystallinity.
[0033] Comparative Example 1: Preparation of Li2ZrCl6 solid electrolyte material The preparation process, ball milling, and annealing were kept the same as in Example 1, except that the raw material ratio was changed and only a Zr source was introduced, without adding a Y source or a sulfur source.
[0034] Comparative Example 2: Preparation and Performance Testing of Li3YCl5S Solid Electrolyte Material Using only the Y-doped system, the preparation process is the same as in Example 2.
[0035] The electrochemical performance test results of Examples 1-3, Comparative Examples 1-2, and commercial Li3Cl5S are shown in Table 1.
[0036] Electrical performance testing: 1. Conductivity test: The powder is cold-pressed into a disc with a diameter of 5 mm and a thickness of about 2 mm under a pressure of 380 MPa. Gold electrodes are coated on both sides. The AC impedance spectrum is tested in the frequency range of 1 MHz-100 Hz with an amplitude of 50 mV.
[0037] The room-temperature ionic conductivity was measured to be 1.8 × 10⁻⁶ using impedance spectroscopy. -2 S / cm.
[0038] 2. Battery Assembly and Performance Testing: In an argon-filled glove box, the above-mentioned electrolyte and LiCoO2 cathode material were mixed at a mass ratio of 70:30 to form a composite cathode. The battery configuration was: Li-In alloy anode / Li6(Y0.5Zr0.5)Cl5S2 electrolyte / composite cathode.
[0039] Table 1 ; As shown in Table 1, compared with single-element doping (Y only, Zr only) and undoped Li-Cl-S matrix, the yttrium and zirconium co-doping of this invention significantly improves the room temperature ionic conductivity of the electrolyte, while the low temperature conductivity, battery cycle stability, and low temperature capacity retention are all significantly better than the respective comparative examples. 3+ Doping introduces lithium vacancies, optimizing lithium-ion diffusion channels; Zr 4+ It plays a role in lattice stabilization and suppresses structural distortion during cycling. The two work together to achieve high ionic conductivity of the electrolyte and long cycle life and excellent low-temperature performance of the battery.
[0040] Based on the disclosure in the foregoing specification, those skilled in the art can make appropriate changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the present invention should also fall within the protection scope of the claims of the present invention. Furthermore, although some specific terms are used in this specification, these terms are only for convenience of explanation and do not constitute any limitation on the present invention.
Claims
1. A yttrium-zirconium co-doped sulfide solid electrolyte, characterized in that: The general chemical formula of the yttrium-zirconium co-doped sulfide solid electrolyte is Li a (Y x Zr 1-x bCl c Sd, where: 0.5≤(a+b) / (c+d)≤1; 0<x<1; a>0, b>0, c>0, d>0.
2. The yttrium-zirconium co-doped sulfide solid electrolyte according to claim 1, characterized in that: The molar ratio of Y:Zr is (0.1–0.9):(0.9–0.1).
3. The yttrium-zirconium co-doped sulfide solid electrolyte according to claim 1, characterized in that: The a:b = (2–9.5):1, and the d:b = (0.5–1.5):
1.
4. The yttrium-zirconium co-doped sulfide solid electrolyte according to claim 1, characterized in that: On an atomic percentage basis, the Li content is 20–40 at% and the S content is 2–15 at%.
5. The yttrium-zirconium co-doped sulfide solid electrolyte according to claim 1, characterized in that: The yttrium-zirconium co-doped sulfide solid electrolyte is Li6(Y0.5Zr0.5)Cl5S2, Li3(Y0.2Zr0.8)Cl5S, Li 18 (Y0.7Zr0.3)3Cl 28 At least one of S.
6. The yttrium-zirconium co-doped sulfide solid electrolyte according to claim 1, characterized in that: In the X-ray diffraction pattern, the yttrium-zirconium co-doped sulfide solid electrolyte includes at least 2θ diffraction peaks located at 28.4°–31.7°, 32.8°–37°, 47.1°–52.4°, and 57.3°–64.2°; In the X-ray diffraction pattern, the width of the widest diffraction peak of the yttrium-zirconium co-doped sulfide solid electrolyte is ≤1.0°.
7. The yttrium-zirconium co-doped sulfide solid electrolyte according to claim 1, characterized in that: The yttrium-zirconium co-doped sulfide solid electrolyte has an ionic conductivity of ≥7 mS / cm at 25 °C.
8. A method for preparing a yttrium-zirconium co-doped sulfide solid electrolyte according to any one of claims 1 to 7, characterized in that: Includes the following steps: The lithium source, yttrium source, zirconium source, chlorine source, and sulfur source are mixed in stoichiometric ratios to obtain a mixture; Under an inert atmosphere, the mixture is subjected to ball milling, solvent-assisted precipitation reaction, or molten salt synthesis reaction in sequence to obtain yttrium zirconium co-doped sulfide solid electrolyte.
9. The method for preparing the yttrium-zirconium co-doped sulfide solid electrolyte according to claim 8, characterized in that: The process is carried out under an inert atmosphere, specifically an argon or nitrogen atmosphere with a dew point ≤ -60°C; the resulting yttrium-zirconium co-doped sulfide solid electrolyte is then annealed at 200–400°C.
10. A secondary battery, characterized in that: It includes a positive electrode, a negative electrode, and an electrolyte layer, wherein the electrolyte layer includes the yttrium zirconium co-doped sulfide solid electrolyte according to any one of claims 1-7 or the yttrium zirconium co-doped sulfide solid electrolyte prepared by the preparation method according to claim 8 or 9; The secondary battery is a lithium-ion battery, a sodium-ion battery, or a potassium-ion battery.