A sulfide electrolyte with a surface-modified, heat-removable protective layer, its preparation method, and its application.
By forming a three-stage protective layer on the surface of the sulfide electrolyte and using thermal removal technology, the processing dew point can be relaxed from -60℃ to -30℃ without affecting the conductivity and interfacial impedance. This solves the problems of high dew point requirements and high production costs in the existing technology and enables low-cost mass production.
Patent Information
- Application Number
- CN202611396009.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies struggle to effectively block water vapor without sacrificing conductivity and interfacial impedance. Furthermore, the high dew point requirements of the processing environment lead to high production costs, poor protective layer integrity, and poor process compatibility, making it impossible to meet the processing needs of high dew point environments.
The protective layer molecule adopts a three-segment structure, including anchoring groups, thermal breakage responsive groups, and hydrophobic functional groups. A dense hydrophobic barrier is formed on the surface of the sulfide electrolyte by liquid phase impregnation. The protective layer is thermally removed after processing to avoid residue. The conventional liquid phase impregnation process is compatible with the existing solid-state battery hot pressing process.
Without affecting conductivity and interfacial impedance, the processing dew point was relaxed from -60℃ to -30℃, reducing the construction and operation costs of the drying room, avoiding the increase in interfacial impedance and loss of electrochemical performance caused by permanent modification, and realizing low-cost large-scale mass production.
Smart Images

Figure CN123073149A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid-state battery technology, and in particular to a sulfide electrolyte with a surface-modified thermally removable protective layer, its preparation method, and its application. Background Technology
[0002] Sulfide solid electrolytes can achieve room temperature ionic conductivity of up to 10. -3 -10 -2 S / cm is one of the mainstream technologies for lithium metal solid-state batteries. However, the S in the electrolyte bulk... 2- Chemically reactive, it readily undergoes hydrolysis upon contact with water vapor, releasing H2S gas and significantly reducing its ionic conductivity. Currently, mass production processes in the industry require the entire process to be conducted in ultra-low dew point dry rooms of -60°C or below. The construction and maintenance costs of these dry rooms increase dramatically as the dew point decreases. It is estimated that the construction and maintenance costs of a -30°C dry room are approximately 30% of those of a -60°C dry room. Therefore, dew point requirements are a key factor restricting cost reduction in the mass production of sulfide electrolytes.
[0003] Currently, there are three main technical approaches to improving the air stability of sulfide electrolytes: (1) Bulk element doping: The lattice electronic structure is controlled by doping with halogens or metal cations to reduce hydrolysis activity, but the stability improvement is limited and is usually accompanied by a decrease in ionic conductivity, so the processing dew point cannot be relaxed to above -40℃.
[0004] (2) Inorganic coating on surface: Inorganic coatings such as Al2O3, LiF, and Li3PO4 are deposited on the electrolyte surface through processes such as ALD to physically block water vapor; however, if the coating is too thin, it is easy to break and provides insufficient protection, while if it is too thick, it will significantly increase the interfacial impedance and the coating will remain permanently, which will offset the high conductivity advantage of sulfides.
[0005] (3) Organic polymer modification: A hydrophobic polymer layer is coated on the surface of the powder, which has a good protective effect. However, the polymer is a permanent residue with low ionic conductivity and is prone to side reactions with sulfides and electrode interfaces, causing battery cycle degradation.
[0006] The existing technology has the following main shortcomings: (1) It is difficult to balance protection performance and electrochemical performance: Existing modification schemes are all permanent modifications. The improvement of air stability often comes at the cost of sacrificing conductivity and increasing interfacial impedance. It is impossible to protect the battery during the service life while ensuring that the battery performance is not affected.
[0007] (2) Insufficient protection in high dew point environments: Existing solutions can only provide limited protection in dew point environments below -50℃. In high dew point dry rooms from -40℃ to -30℃, the electrolyte hydrolysis rate is still significantly accelerated, which cannot meet the time requirements for mass production processing.
[0008] (3) Poor integrity of the protective layer. The inorganic coating layer is prone to cracking and falling off during cold pressing, rolling and other processing; the organic modification layer has weak bonding force with the electrolyte surface and is easily worn off during processing, and the protective effect will be greatly reduced after damage.
[0009] (4) Poor compatibility with mass production processes: ALD and other coating processes are expensive and have low capacity, making them difficult to adapt to ton-level powder mass production; wet modification carries the risk of solvent residue, which can easily lead to subsequent battery gas production.
[0010] (5) No differentiated design for processing scenarios: Existing technologies are all designed for the stabilization of electrolytes throughout their entire life cycle, but the actual water vapor risk is only concentrated in the processing links such as powder transportation, film making, and electrode preparation; after the battery is sealed and encapsulated, it will basically no longer come into contact with water vapor, and permanent modification is an unnecessary performance sacrifice. Summary of the Invention
[0011] The purpose of this invention is to provide a sulfide electrolyte with a surface-modified, heat-removable protective layer, its preparation method, and its application. The protective layer molecules can be uniformly adsorbed on the surface of the sulfide electrolyte during the processing stage to form a dense hydrophobic barrier, effectively blocking water vapor intrusion, thereby widening the processing dew point from -60℃ to -30℃, significantly reducing the construction and maintenance costs of the dry room. During the battery hot-pressing assembly stage, the tert-butyl carbonate bonds in the protective layer break upon heating, decomposing into gaseous small molecules and being completely discharged through vacuum, leaving no solid residue on the electrolyte surface. This avoids the increased interfacial impedance and loss of electrochemical performance caused by permanent modification in traditional solutions.
[0012] To achieve the above objectives, the present invention provides a sulfide electrolyte with a surface-modified, thermally removable protective layer, comprising a three-segment structure of a thermally responsive hydrophobic protective layer molecule, the molecular structure of which is as follows: ; Wherein, A is an anchoring group, which is one of thiophosphate monoester group or mercaptoacetic acid group; B is a thermally cleavage-responsive group, which is a tert-butyl carbonate bond; C is a hydrophobic functional group, which is one of C4-C8 perfluoroalkyl or long-chain alkyl.
[0013] Preferably, the molecular structure of the protective layer is: Abbreviated as PFBT-P; The electrolyte is a sulfide electrolyte, namely Li6PS5Cl and Li7P3S. 11 Li 10 GeP2S 12 Li 9.54 Si 1.74 P 1.44 S 11.7Cl 0.3 .
[0014] The above-mentioned method for preparing a sulfide electrolyte with a surface-modified, heat-removable protective layer includes the following steps: S1: Dissolve the protective layer molecules in an anhydrous organic solvent to prepare a modification solution; S2. Add the sulfide electrolyte powder to the modification solution and stir to allow the protective layer molecules to be adsorbed onto the surface of the sulfide electrolyte powder to obtain the modified powder. S3. Separate the modified powder, wash it with anhydrous organic solvent, and then dry it to obtain sulfide electrolyte powder with a removable protective layer.
[0015] Preferably, in S1, the organic solvent is one of n-hexane and dichloromethane, and the mass concentration of the modified solution is 0.5-5 wt%.
[0016] Preferably, in S1, the method for preparing the protective layer molecules is as follows: (1) Under the protection of an inert gas, thiophosphoric chloride is dissolved in anhydrous dichloromethane and cooled to 0°C; (2) Add a solution of nonafluorohexanol and triethylamine in anhydrous dichloromethane dropwise to the solution obtained in step (1) while stirring. During the dropwise addition, control the temperature of the reaction system to ≤5℃. After the dropwise addition is completed, raise the temperature to room temperature and stir the reaction to obtain the intermediate. (3) Cool the intermediate system obtained in step (2) to 0°C, and add an anhydrous dichloromethane solution of tert-butyl monocarbonate and triethylamine dropwise. During the dropwise addition, control the temperature of the reaction system to <5°C. After the dropwise addition is completed, raise the temperature to room temperature and continue stirring to obtain the crude product. (4) The crude product obtained in step (3) was filtered to remove triethylamine hydrochloride. The filtrate was washed with water, saturated brine, and dried. The solvent was removed by rotary evaporation under reduced pressure. The product was then purified by silica gel column chromatography. The target component was collected and the solvent was removed under reduced pressure to obtain PFBT-P.
[0017] Preferably, the molar ratio of nonafluorohexanol to thiophosphoric acid chloride is 1:1, and the molar ratio of triethylamine to thiophosphoric acid chloride is 1.1:1. (2) The dropping time is 1-2 hours, and the stirring time at room temperature is 4 hours; (3) The molar ratio of tert-butyl monocarbonate to thiophosphoric acid chloride is 1:1, and the molar ratio of triethylamine to thiophosphoric acid chloride is 1.1:1; the dropping time is 1.5h, the reaction time is 8-12h with stirring at room temperature, and the reaction of intermediate raw materials is monitored by thin-layer chromatography to ensure complete reaction. In (4), the eluent used in silica gel column chromatography is a gradient mixture of petroleum ether and ethyl acetate, with a gradient volume ratio of 20:1, 10:1, and 5:1.
[0018] The eluent used in silica gel column chromatography was a gradient mixture of petroleum ether and ethyl acetate. Low-polarity impurities were first removed by elution with a petroleum ether-ethyl acetate mixture at a volume ratio of 20:1. Then, the proportion of ethyl acetate was gradually increased, switching to a volume ratio of 10:1, and then to a volume ratio of 5:1 for gradient elution. The target product components were collected by TLC thin-layer chromatography, and the organic phases were combined. The solvent was removed by rotary evaporation under reduced pressure to obtain the crude product of perfluorobutylethyl tert-butyloxycarbonyl thiophosphate triester.
[0019] Preferably, in S2, the mass ratio of sulfide electrolyte powder to modified solution is 1:(5-10), and the mixture is stirred at room temperature for 30-120 min.
[0020] Preferably, in step S3, drying is carried out under vacuum at 80-120°C.
[0021] The above-mentioned application of a surface-modified sulfide electrolyte with a thermally removable protective layer in the preparation of solid-state batteries.
[0022] Preferably, it includes the following steps: T1. A sulfide electrolyte with a heat-removable protective layer on its surface is processed in a dry air environment with a dew point of -30°C to -60°C. The processing includes at least one of the following steps: powder transfer, cold pressing of electrolyte membrane, dry preparation of composite positive electrode sheet and stacking. T2. After processing, hot pressing is performed in a vacuum atmosphere to trigger the removal of the protective layer. The hot pressing temperature is 160-190℃, the pressure is 5-20MPa, and the time is 10-60min. This causes the tert-butyl carbonate bonds in the protective layer molecules to undergo a thermal elimination reaction, decompose into gaseous small molecules, and be completely discharged from the surface of the sulfide electrolyte. T3. The electrolyte membrane with the protective layer removed is stacked with the positive and negative electrodes and assembled, then packaged in a soft pack to obtain the final sulfide solid-state lithium battery.
[0023] Therefore, the present invention employs the above-mentioned sulfide electrolyte with a surface-modified thermally removable protective layer, its preparation method, and its application, which have the following beneficial effects: (1) By designing a protective layer molecule with a three-segment structure of anchoring group, thermal fracture response group and hydrophobic functional group, the molecular-level uniform adsorption is achieved by utilizing the coordination effect of anchoring group with the surface of sulfide electrolyte. A dense hydrophobic barrier is formed in the powder processing stage to effectively block water vapor intrusion. The processing environment can be relaxed from ultra-low dew point to high dew point, significantly reducing the construction and operation and maintenance costs of dry room. (2) During the battery hot-press assembly stage, the tert-butyl carbonate bonds in the protective layer molecules undergo a thermal elimination reaction under heat treatment conditions, and are completely decomposed into gaseous small molecules and completely discharged through the vacuum system. There are no solid residues on the electrolyte surface. This avoids the risk of cracking and falling off caused by cold pressing and rolling of traditional inorganic coating layers, and also eliminates the problems of increased interfacial impedance and electrochemical side reactions caused by permanent residues of organic modification layers. This allows the desulfurized electrolyte to return to its original interfacial state, and the ionic conductivity and interfacial impedance are basically the same as those of the unmodified powder. (3) The conventional liquid phase impregnation process is adopted, which does not require expensive equipment such as ALD. The removal process can reuse the existing solid-state battery hot pressing process, which is highly compatible with the existing dry production line, providing a practical and feasible technical path for the low-cost mass production of sulfide solid electrolytes.
[0024] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0025] Figure 1 This is the mass spectrum of PFBT-P prepared according to the present invention. Detailed Implementation
[0026] The technical solution of the present invention will be further described below with reference to the accompanying drawings and embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention should be considered equivalent substitutions and are included within the protection scope of the present invention. Furthermore, it should be understood that after reading the contents of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims and are all within the protection scope of the present invention.
[0027] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.
[0028] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.
[0029] In this invention, unless otherwise specified, all other test materials and instruments are conventional test materials in the field and can be purchased through commercial channels.
[0030] Test method: Dry room environmental stability test: The electrolyte powder was placed in a dry air environment at 25℃ and corresponding dew point for 24 hours of continuous exposure. The room temperature ionic conductivity was measured by AC impedance spectroscopy, and the conductivity retention rate was calculated. At the same time, the cumulative release was detected by an H2S sensor, and the unit was ppm·m. 3 / g.
[0031] Performance testing after removal: The powder is cold-pressed into an electrolyte membrane, and the protective layer is removed by hot pressing according to the corresponding process. The room temperature ionic conductivity and Li symmetric cell interface impedance are then tested.
[0032] Battery performance testing: Assembled NCM811 positive electrode / lithium metal anode solid-state pouch battery, positive electrode surface capacity 3.0 mAh / cm² 2 1C charge / discharge rate, capacity retention rate tested after 50 cycles.
[0033] Reference parameters: The room temperature ionic conductivity of native, unmodified Li6PS5Cl is 1.80 × 10⁻⁶. -3 S / cm, Li-symmetric cell interfacial impedance 26Ω·cm 2 After 50 cycles at 1C, the capacity retention rate is 94.5%.
[0034] PFBT-P preparation process: 1. Under nitrogen protection, add anhydrous dichloromethane to a dry three-necked flask, add thiophosphoryl chloride (1 eq), and cool to 0℃ (ice bath). 2. Add anhydrous DCM solution of nonafluorohexanol (1 eq) + triethylamine (1.1 eq) slowly dropwise over 1.5 h, keeping the temperature ≤ 5 °C. After the addition is complete, remove from the ice bath and stir at room temperature for 4 h to obtain the intermediate O-nonafluorohexylthiophosphoric acid dichloride system. 3. Cool the mixture to 0°C again in an ice bath, and slowly add anhydrous DCM solution of tert-butyl monocarbonate (1 eq) + remaining triethylamine (1.1 eq) for 1.5 h, keeping the temperature below 5°C. After the addition is complete, raise the temperature to room temperature, and continue stirring under nitrogen protection for 10 h. Monitor the intermediate dichloro feedstock by TLC until it is completely consumed. 4. Post-treatment: The reaction solution was filtered to remove the white solid triethylamine hydrochloride; the organic phase was washed successively with ice water and saturated brine, and dried with anhydrous sodium sulfate. 5. Remove crude dichloromethane by rotary evaporation under reduced pressure; purify the crude product by silica gel column chromatography (eluting agent: petroleum ether / ethyl acetate gradient elution, with a volume ratio of petroleum ether to ethyl acetate of 20:1, 10:1, and 5:1), collect the target component, and remove the solvent again under reduced pressure at low temperature to obtain the colorless, transparent, oily liquid target product PFBT-P.
[0035] The mass spectrum of the prepared PFBT-P is as follows: Figure 1 As shown, the measured peaks of the mass spectrum are highly consistent with the theoretical simulation values (the peak positions and peak shapes are in agreement), proving that the synthesized product is indeed the target compound PFBT-P, and has high purity; the fragment peaks that appear correspond to the characteristic fragments of the detert-butyl group, further confirming the existence of the tert-butyl carbonate bond in the molecule.
[0036] Example 1 This invention provides a sulfide electrolyte with a surface-modified, heat-removable protective layer, the preparation method of which includes the following steps: PFBT-P was used as the protective layer molecule and dissolved in anhydrous n-hexane to prepare a modified solution with a mass concentration of 1 wt%. The solution was then sealed and stirred until completely dissolved.
[0037] Li6PS5Cl sulfide electrolyte powder was slowly added to the above-mentioned modification solution, and the solid-liquid mass ratio was controlled at 1:8. The mixture was stirred with a magnetic stirrer for 60 minutes at room temperature, so that the protective layer molecules could spontaneously and uniformly adsorb onto the powder surface through the coordination of anchoring groups to obtain the modified powder.
[0038] After stirring, the modified powder was centrifuged and washed twice with anhydrous n-hexane to remove unadsorbed free molecules on the surface. Then it was dried in a vacuum environment at 80°C for 6 hours to obtain sulfide electrolyte powder with a heat-removable protective layer on the surface.
[0039] The sulfide electrolyte powder with a heat-removable protective layer was continuously exposed to dry air at 25°C and a dew point of -30°C for 24 hours. After exposure, the powder was cold-pressed into an electrolyte film and then subjected to hot-pressing removal under a vacuum atmosphere at a temperature of 180°C, a pressure of 10 MPa, and a holding time of 30 min. This process caused the tert-butyl carbonate bonds in the protective layer molecules to undergo a thermal elimination reaction, decomposing them into gaseous small molecules that were completely expelled from the electrolyte surface.
[0040] After removing the protective layer, the room-temperature ionic conductivity of the electrolyte membrane was measured using AC impedance spectroscopy. A Li-symmetric cell was assembled to test the interfacial impedance. Finally, an NCM811 cathode / lithium metal anode solid-state pouch cell (cathode areal capacity of 3.0 mAh / cm²) was assembled. 2 ), and perform charge-discharge cycle tests at 1C rate.
[0041] Test results showed that after 24 hours of exposure in a -30℃ dew point environment, the conductivity retention rate was 92.3%; the cumulative H2S release within 24 hours was 0.32 ppm·m³. 3 / g; After hot-pressing removal, the room temperature ionic conductivity is 1.76×10⁻⁶. -3 S / cm represents the room temperature ionic conductivity of the original, unmodified powder (1.80 × 10⁻⁶). -3 The S / cm) is 97.8%; the interface impedance of the Li symmetric cell is 28Ω·cm. 2 The full battery retains 94.1% of its capacity after 50 cycles at 1C.
[0042] Example 2 The only difference between this embodiment and Embodiment 1 is that this embodiment is tested at a dew point of -40°C and the same test method as Embodiment 1 is used for performance testing. All other conditions are the same.
[0043] Test results showed that after 24 hours of exposure in a -40℃ dew point environment, the conductivity retention rate was 95.6%; the cumulative H2S release within 24 hours was 0.19 ppm·m³. 3 / g; After hot-pressing removal, the room temperature ionic conductivity is 1.77×10⁻⁶. -3 The S / cm ratio is 98.3% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell is 27 Ω·cm. 2 The full battery retains 94.3% of its capacity after 50 cycles at 1C rate.
[0044] Example 3 The only difference between this embodiment and Embodiment 1 is that this embodiment is tested at a dew point of -50°C and the same test method as Embodiment 1 is used for performance testing. All other conditions are the same.
[0045] Test results showed that after 24 hours of exposure in a -50℃ dew point environment, the conductivity retention rate was 97.2%; the cumulative H2S release within 24 hours was 0.11 ppm·m³. 3 / g; After hot-pressing removal, the room temperature ionic conductivity is 1.78×10⁻⁶. -3 The S / cm ratio is 98.9% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell is 27 Ω·cm. 2 The full battery retains 94.4% of its capacity after 50 cycles at 1C.
[0046] Example 4 The only difference between this embodiment and Embodiment 1 is that this embodiment is tested at a dew point of -50°C and the same test method as Embodiment 1 is used for performance testing. All other conditions are the same.
[0047] Test results showed that after 24 hours of exposure in a -60℃ dew point environment, the conductivity retention rate was 98.1%; the cumulative H2S release within 24 hours was 0.07 ppm·m 3 / g; After hot-pressing removal, the room temperature ionic conductivity is 1.79×10⁻⁶. -3 The S / cm ratio is 99.4% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell is 26 Ω·cm. 2 The full battery retains 94.5% of its capacity after 50 cycles at 1C.
[0048] Example 5 The only difference between this embodiment and Example 1 is that the concentration of the modification solution is 2 wt%, while all other conditions are the same.
[0049] Test results showed that after 24 hours of exposure in a -30℃ dew point environment, the conductivity retention rate was 95.7%; the cumulative H2S release within 24 hours was 0.18 ppm·m³. 3 / g; After hot-pressing removal, the room temperature ionic conductivity is 1.72×10⁻⁶. -3 The S / cm ratio is 95.6% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell is 31 Ω·cm. 2 The full battery retains 93.5% of its capacity after 50 cycles at 1C.
[0050] Example 6 The only difference between this embodiment and Example 1 is that the concentration of the modification solution is 0.5 wt%, while all other conditions are the same.
[0051] Test results showed that after 24 hours of exposure in a -30℃ dew point environment, the conductivity retention rate was 87.4%; the cumulative H2S release within 24 hours was 0.56 ppm·m 3 / g; After hot-pressing removal, the room temperature ionic conductivity is 1.78×10⁻⁶. -3 The S / cm ratio is 98.9% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell is 27 Ω·cm. 2 The full battery retains 94.2% of its capacity after 50 cycles at 1C rate.
[0052] Example 7 The only difference between this embodiment and Embodiment 1 is that the hot-pressing removal process is carried out at a temperature of 170°C, a pressure of 10 MPa, and a holding time of 45 min. All other conditions are the same.
[0053] Test results showed that after 24 hours of exposure in a -30℃ dew point environment, the conductivity retention rate was 92.1%; after hot-pressing removal, the room temperature ionic conductivity was 1.70 × 10⁻⁶. -3The S / cm ratio is 94.4% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell is 33 Ω·cm. 2 The full battery retains 92.8% of its capacity after 50 cycles at 1C.
[0054] Comparative Example 1 The only difference between this comparative example and Example 1 is that pure Li6PS5Cl sulfide electrolyte powder without any modification was directly placed in a dry air environment at 25°C and a dew point of -30°C for 24 hours for continuous exposure, while all other conditions were the same.
[0055] Test results showed that after 24 hours of exposure in a -30℃ dew point environment, the conductivity retention rate was only 32.7%; the cumulative H2S release within 24 hours reached as high as 3.62 ppm·m³. 3 / g; after exposure, the room temperature ionic conductivity decreased to 0.59×10⁻⁶. -3 S / cm; the interfacial impedance of the Li-symmetric cell increases to 142 Ω·cm 2 The capacity retention rate of the full battery after 50 cycles at 1C rate is only 58.3%.
[0056] Comparative Example 2 The only difference between this comparative example and Example 1 is that pure Li6PS5Cl sulfide electrolyte powder without any modification was directly placed in a dry air environment at 25°C and a dew point of -60°C for 24 hours for continuous exposure, while all other conditions were the same.
[0057] Test results showed that after 24 hours of exposure in a -60℃ dew point environment, the conductivity retention rate was 82.3%; the cumulative H2S release within 24 hours was 0.78 ppm·m³. 3 / g; the room temperature ionic conductivity after exposure is 1.48 × 10⁻⁶ g. -3 The S / cm ratio is 82.3% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell is 39 Ω·cm. 2 The full battery retains 88.7% of its capacity after 50 cycles at 1C.
[0058] Comparative Example 3 In this comparative example, an Al2O3 coating with a thickness of 2 nm was deposited on the surface of Li6PS5Cl sulfide electrolyte powder using atomic layer deposition (ALD) process to obtain Al2O3 inorganically coated sulfide electrolyte powder.
[0059] The Al2O3-coated powder was continuously exposed to dry air at 25°C and a dew point of -30°C for 24 hours.
[0060] After exposure, performance tests were conducted using the same test method as in Example 1 (without hot-pressing removal, as the Al2O3 coating is a permanent coating).
[0061] Test results showed that after 24 hours of exposure in a -30℃ dew point environment, the conductivity retention rate was 71.5%; the cumulative H2S release within 24 hours was 0.93 ppm·m 3 / g; the room temperature ionic conductivity after coating is only 1.21×10⁻⁶. -3 The S / cm ratio is 67.2% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell increases to 87 Ω·cm. 2 The full battery retains 82.6% of its capacity after 50 cycles at 1C.
[0062] Comparative Example 4 In this comparative example, dodecyl mercaptan was used as a modifier, which was dissolved in anhydrous n-hexane to prepare a modification solution with a mass concentration of 1 wt%. Li6PS5Cl sulfide electrolyte powder was added to the above modification solution, and the solid-liquid mass ratio was controlled at 1:8. The mixture was stirred at room temperature for 60 min to allow the dodecyl mercaptan to be adsorbed onto the powder surface.
[0063] After stirring, the modified powder was centrifuged, washed twice with anhydrous n-hexane, and then dried in a vacuum environment at 80°C for 6 hours to obtain sulfide electrolyte powder permanently hydrophobically modified with dodecyl mercaptan.
[0064] The dried powder was placed in a dry air environment at 25°C and a dew point of -30°C for 24 hours for continuous exposure (without thermal removal treatment, as dodecyl mercaptan has no thermally cleaved groups).
[0065] The performance test was conducted using the same test method as in Example 1.
[0066] Test results showed that after 24 hours of exposure in a -30℃ dew point environment, the conductivity retention rate was 78.9%; the cumulative H2S release within 24 hours was 0.68 ppm·m³. 3 / g; the room temperature ionic conductivity after modification is only 0.98×10⁻⁶. -3 The S / cm ratio is 54.4% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell increases to 112 Ω·cm. 2 The full battery retains 76.3% of its capacity after 50 cycles at 1C.
[0067] Comparative Example 5 In this comparative example, perfluorooctyl thiophosphate without thermally cleavable groups was used as the modifying molecule (this molecule does not contain tert-butyl carbonate bonds and cannot be thermally triggered for removal). It was dissolved in anhydrous n-hexane to prepare a modification solution with a mass concentration of 1 wt%. Li6PS5Cl sulfide electrolyte powder was added to the above modification solution, and the solid-liquid mass ratio was controlled at 1:8. The mixture was stirred at room temperature for 60 min.
[0068] After stirring, the modified powder was centrifuged, washed twice with anhydrous n-hexane, and then dried in a vacuum environment at 80°C for 6 hours to obtain the modified sulfide electrolyte powder.
[0069] The dried powder was continuously exposed to dry air at 25°C and a dew point of -30°C for 24 hours. After exposure, the powder was cold-pressed into an electrolyte membrane and subjected to the same hot-pressing process as in Example 1 (180°C, 10MPa, holding for 30 minutes) under a vacuum atmosphere. However, since the molecule does not contain tert-butyl carbonate bonds, the protective layer molecules could not be decomposed and removed after hot pressing.
[0070] The performance test was conducted using the same test method as in Example 1.
[0071] Test results showed that after 24 hours of exposure in a -30℃ dew point environment, the conductivity retention rate was 89.1%; after hot pressing, the room temperature ionic conductivity was only 1.06×10⁻⁶. -3 The S / cm ratio is 58.9% of that of the original unmodified powder; the interfacial impedance of the Li symmetric cell increases to 135 Ω·cm. 2 The full battery retains 71.8% of its capacity after 50 cycles at 1C.
[0072] By comparing Examples 1-7 and Comparative Examples 1-5, it can be concluded that: The protective effect is significantly better than the mass production benchmark: In Example 1 of this invention, the conductivity retention rate reached 92.3% after 24 hours in a dew point environment of -30℃, which is significantly better than the 82.3% of the unmodified powder at a dew point of -60℃. This proves that this solution can achieve better processing stability while significantly reducing the dry room grade.
[0073] No performance loss after removal: The conductivity retention rate after removal in all embodiments is above 94%, the interfacial impedance is close to that of the original powder, and the cycle performance is almost without decay, which is far superior to all permanent modification schemes, verifying the core advantage of "zero residue".
[0074] The dew point gradient law is clear: as the dew point decreases (water vapor decreases), the conductivity retention rate gradually increases, and the H2S release gradually decreases, which is in line with the dynamic law of water vapor corrosion; in dew point environments above -40℃, the protection gain of this solution is more significant.
[0075] The concentration and performance are adjustable: the higher the modification concentration, the stronger the protective effect, but the performance will decrease slightly after removal; 1 wt% is the optimal concentration range, which takes into account both the protective effect and electrochemical performance.
[0076] Thermally broken bonds are a core and essential feature: comparing Comparative Example 5 and Example 1, although molecules without thermally broken bonds have a protective effect, they will remain permanently and significantly degrade electrochemical performance, proving the necessity and ingenuity of the three-segment molecular structure design of this invention.
[0077] Therefore, the present invention employs the above-mentioned surface-modified sulfide electrolyte with a heat-removable protective layer, its preparation method, and its application. The protective layer molecules can be uniformly adsorbed on the surface of the sulfide electrolyte during the processing stage to form a dense hydrophobic barrier, effectively blocking water vapor intrusion, thereby widening the processing dew point from -60℃ to -30℃, significantly reducing the construction and maintenance costs of the dry room. During the battery hot-pressing assembly stage, the tert-butyl carbonate bonds in the protective layer break upon heating, decomposing into gaseous small molecules and being completely discharged through vacuum, leaving no solid residue on the electrolyte surface. This avoids the increase in interfacial impedance and loss of electrochemical performance caused by permanent modification in traditional solutions.
[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A sulfide electrolyte with a surface-modified, heat-removable protective layer, characterized in that: It includes a three-segment thermally responsive hydrophobic protective layer molecule and an electrolyte. The molecular structure of the protective layer is as follows: ; Wherein, A is an anchoring group, which is one of thiophosphate monoester group or mercaptoacetic acid group; B is a thermally cleavage-responsive group, which is a tert-butyl carbonate bond; C is a hydrophobic functional group, which is one of C4-C8 perfluoroalkyl or long-chain alkyl groups.
2. The sulfide electrolyte with a surface-modified, heat-removable protective layer according to claim 1, characterized in that: The molecular structure of the protective layer is: Abbreviated as PFBT-P; The electrolyte is a sulfide electrolyte, namely Li6PS5Cl and Li7P3S. 11 Li 10 GeP2S 12 Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 .
3. A method for preparing a sulfide electrolyte with a surface-modified, thermally removable protective layer as described in any one of claims 1-2, characterized in that: Includes the following steps: S1: Dissolve the protective layer molecules in an anhydrous organic solvent to prepare a modification solution; S2. Add the sulfide electrolyte powder to the modification solution and stir to allow the protective layer molecules to be adsorbed onto the surface of the sulfide electrolyte powder to obtain the modified powder. S3. Separate the modified powder, wash it with anhydrous organic solvent, and then dry it to obtain sulfide electrolyte powder with a removable protective layer.
4. The method for preparing a sulfide electrolyte with a surface-modified, thermally removable protective layer according to claim 3, characterized in that: In S1, the organic solvent is either n-hexane or dichloromethane, and the mass concentration of the modified solution is 0.5-5 wt%.
5. The method for preparing a sulfide electrolyte with a surface-modified, thermally removable protective layer according to claim 3, characterized in that: In S1, the protective layer molecules are prepared as follows: (1) Under the protection of an inert gas, thiophosphoric chloride is dissolved in anhydrous dichloromethane and cooled to 0°C; (2) Add a solution of nonafluorohexanol and triethylamine in anhydrous dichloromethane dropwise to the solution obtained in step (1) while stirring. During the dropwise addition, control the temperature of the reaction system to ≤5℃. After the dropwise addition is completed, raise the temperature to room temperature and stir the reaction to obtain the intermediate. (3) Cool the intermediate system obtained in step (2) to 0°C, and add an anhydrous dichloromethane solution of tert-butyl monocarbonate and triethylamine dropwise. During the dropwise addition, control the temperature of the reaction system to <5°C. After the dropwise addition is completed, raise the temperature to room temperature and continue stirring to obtain the crude product. (4) The crude product obtained in step (3) was filtered to remove triethylamine hydrochloride. The filtrate was washed with water, saturated brine, and dried. The solvent was removed by rotary evaporation under reduced pressure. The product was then purified by silica gel column chromatography. The target component was collected and the solvent was removed under reduced pressure to obtain PFBT-P.
6. The method for preparing a sulfide electrolyte with a surface-modified, thermally removable protective layer according to claim 3, characterized in that: The molar ratio of nonafluorohexanol to thiophosphoric acid chloride is 1:1, and the molar ratio of triethylamine to thiophosphoric acid chloride is 1.1:
1. (2) The dropping time is 1-2 hours, and the stirring time at room temperature is 4 hours; (3) The molar ratio of tert-butyl monocarbonate to thiophosphoric acid chloride is 1:1, and the molar ratio of triethylamine to thiophosphoric acid chloride is 1.1:1; the dropping time is 1.5h, the reaction time is 8-12h with stirring at room temperature, and the reaction of intermediate raw materials is monitored by thin-layer chromatography to ensure complete reaction. In (4), the eluent used in silica gel column chromatography is a gradient mixture of petroleum ether and ethyl acetate, with a gradient volume ratio of 20:1, 10:1, and 5:
1.
7. The method for preparing a sulfide electrolyte with a surface-modified, thermally removable protective layer according to claim 3, characterized in that: In S2, the mass ratio of sulfide electrolyte powder to modified solution is 1:(5-10), and the mixture is stirred at room temperature for 30-120 min.
8. The method for preparing a sulfide electrolyte with a surface-modified, thermally removable protective layer according to claim 3, characterized in that: In S3, drying is carried out under vacuum at 80-120℃.
9. The application of a sulfide electrolyte with a surface-modified thermally removable protective layer as described in any one of claims 1-2 in the preparation of solid-state batteries.
10. The application of the sulfide electrolyte with a surface-modified, heat-removable protective layer according to claim 9, characterized in that: Includes the following steps: T1. A sulfide electrolyte with a heat-removable protective layer on its surface is processed in a dry air environment with a dew point of -30°C to -60°C. The processing includes at least one of the following steps: powder transfer, cold pressing of electrolyte membrane, dry preparation of composite positive electrode sheet and stacking. T2. After processing, hot pressing is performed in a vacuum atmosphere to trigger the removal of the protective layer. The hot pressing temperature is 160-190℃, the pressure is 5-20MPa, and the time is 10-60min. This causes the tert-butyl carbonate bonds in the protective layer molecules to undergo a thermal elimination reaction, decompose into gaseous small molecules, and be completely discharged from the surface of the sulfide electrolyte. T3. The electrolyte membrane with the protective layer removed is stacked with the positive and negative electrodes and assembled, then packaged in a soft pack to obtain the final sulfide solid-state lithium battery.