An electrolyte based on a thermally responsive polymer, its preparation method and application
By using a thermally responsive polymer electrolyte in lithium-ion batteries, and utilizing epoxy ether monomers and polysilazane polymers to form a cross-linked network at high temperatures to seal the pores of the separator, the safety hazards of thermal runaway in lithium-ion batteries are solved, and early active safety protection and normal operation compatibility are achieved.
Patent Information
- Application Number
- CN202611530175.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-10
AI Technical Summary
Existing lithium-ion batteries have difficulty actively cutting off ion transport channels in the early stages of thermal runaway, leading to the continued development of thermal runaway and posing a safety hazard.
The electrolyte is based on a thermally responsive polymer, which contains epoxy ether monomers and polysilazane polymers. When the temperature rises abnormally, it forms a three-dimensional cross-linked network structure, which seals the membrane pores and blocks lithium-ion transport.
When the battery overheats abnormally, the electrolyte can actively respond, quickly cut off the ion transport channels, prevent internal short circuits and exothermic reactions, achieve early safety protection, and maintain normal operating performance at room temperature.
Smart Images

Figure CN123073152A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and more specifically to an electrolyte based on a thermally responsive polymer, its preparation method, and its application. Background Technology
[0002] Lithium-ion batteries, with their outstanding advantages such as high energy density, high operating voltage, long cycle life, and low self-discharge rate, have become one of the most competitive electrochemical energy storage technologies in portable electronic devices, new energy vehicles, grid energy storage, and aerospace. With the rapid development of emerging industries such as new energy vehicles, low-altitude economic aircraft, drones, and intelligent equipment, the market is placing higher demands on the energy density and range of lithium-ion batteries, driving their continuous development towards higher specific energy densities. However, higher energy density means storing more chemical energy per unit volume or unit mass. While improving battery performance, this also further increases the risk of thermal runaway, making thermal safety one of the key bottlenecks restricting the further development of high-energy-density lithium-ion batteries.
[0003] Lithium-ion batteries mainly consist of four core components: the positive electrode, the negative electrode, the separator, and the electrolyte. The separator plays a crucial role in isolating the positive and negative electrodes, preventing direct electron contact, and allowing lithium ions to migrate freely. The electrolyte, on the other hand, is responsible for establishing an efficient ion transport channel between the positive and negative electrodes. When a battery is subjected to abnormal operating conditions such as thermal abuse, mechanical abuse, electrical abuse (e.g., overcharging, external short circuits), or internal defects, a series of strongly exothermic side reactions can be induced inside the battery, ultimately leading to thermal runaway. Under normal circumstances, when the battery temperature rises to about 90 ℃-120 ℃, the solid electrolyte interface film on the negative electrode surface begins to decompose and release heat. As the temperature rises further to about 130 ℃-150 ℃, the polyolefin separator gradually undergoes thermal shrinkage or even melts, causing direct contact between the positive and negative electrodes and inducing an internal short circuit, releasing a large amount of Joule heat in a short period of time. When the temperature continues to rise, the positive electrode active material decomposes and releases oxygen, while the electrolyte undergoes a violent oxidation decomposition reaction, further accelerating the exothermic process. This eventually forms a typical autocatalytic positive feedback process of exothermic, temperature rise, and further exothermic, leading to uncontrollable thermal runaway, accompanied by the release, ejection, ignition, or even explosion of a large amount of flammable gas, posing a serious threat to the safety of people's lives and property.
[0004] Currently, numerous studies have been conducted by scholars both domestically and internationally regarding the thermal safety of lithium-ion batteries. Most solutions remain passive protection measures, only improving battery heat resistance or reducing electrolyte flammability. They fail to actively interrupt ion transport processes within the battery in the early stages of thermal runaway, thus failing to fundamentally prevent the continued development of internal short circuits. Therefore, developing novel intelligent electrolyte systems capable of actively responding and rapidly interrupting ion transport channels in the early stages of abnormal battery temperature rise has become a crucial research direction in the field of high-safety lithium-ion batteries. Summary of the Invention
[0005] The purpose of this invention is to at least solve one of the technical problems existing in the prior art, and to provide an electrolyte based on thermally responsive polymers, its preparation method and application, specifically an electrolyte that enables the battery to work normally at room temperature and thermally shuts down at high temperature, its preparation method and a lithium secondary battery.
[0006] The technical solution of the present invention is as follows: In a first aspect, the present invention provides an electrolyte based on a thermally responsive polymer, the electrolyte comprising an epoxy ether monomer, a polysilazane polymer, a lithium salt, and an organic solvent; The epoxy ether monomers and the polysilazane polymers can react under heating conditions to transform the electrolyte from a liquid state into a three-dimensional cross-linked network structure.
[0007] Optionally, the epoxy ether monomer is one or more of sorbitol glycidyl ether (SPE), bisphenol S diglycidyl ether (BPS-DGE), glycerol triglycidyl ether (GTE), pentaerythritol tetraglycidyl ether (PTGE), trimethylolpropane triglycidyl ether (TMPTGE), and tetramethylbisphenol diglycidyl ether (TMBPDGE).
[0008] Optionally, the polysilazane polymer is one or more of polymethylvinylsilazane (PMVS), polydiphenylsilazane (PDPS), polymethylphenylsilazane (PMPS), polyvinylsilazane (PVS), polydimethylsilazane (PMS), polymethylhydrosilazane (PHS), polyphenylsilazane (PPS), and polymethyl(3,3,3-trifluoropropyl)silazane (PMFS).
[0009] Optionally, the lithium salt is one or more of lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium difluorooxalate borate (LiDFOB), lithium bis(oxalate borate) (LiBOB), and lithium nitrate (LiNO3); Optionally, the organic solvent is one or more of ethylene carbonate (EC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethylene glycol dimethyl ether (DME), and 1,3-dioxolane (DOL).
[0010] Optionally, the components in the electrolyte are expressed in the following proportions by mass fraction: epoxy ether monomers 3%~5%, polysilazane polymers 1%~3%, lithium salts 30%~40%, and organic solvents 52%~66%.
[0011] Optionally, the heating conditions include setting the temperature of the electrolyte above 100°C. That is, when the temperature of the electrolyte is above 100°C, the epoxy ether monomers and polysilazane polymers therein can react to transform the electrolyte from a liquid state into a three-dimensional cross-linked network structure.
[0012] The electrolyte in this invention requires no additional heating when applied to lithium secondary batteries. When the lithium secondary battery is at its normal operating temperature, the electrolyte is liquid and wets the pores of the separator, allowing the battery to function normally. However, when the lithium secondary battery experiences an abnormal temperature rise, the polysilazane polymers and epoxy ether monomers in the electrolyte, upon heating, can form a continuous and dense barrier structure in situ at the separator and electrode interfaces. This fills and / or seals the pores of the separator, blocking the lithium-ion transport path and preventing the lithium secondary battery from functioning properly.
[0013] Secondly, the present invention provides a method for preparing the electrolyte, the method comprising the following steps: The electrolyte is obtained by uniformly mixing epoxy ether monomers, polysilazane polymers, lithium salts, and organic solvents.
[0014] Thirdly, the present invention provides a lithium secondary battery with high-temperature thermal shutdown, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the electrolyte is the above-mentioned electrolyte based on a thermally responsive polymer.
[0015] Optionally, when the lithium secondary battery is at normal operating temperature, the electrolyte is liquid and wets the pores of the separator; When the temperature of the lithium secondary battery is higher than the preset temperature, the polysilazane polymer and epoxy ether monomer in the electrolyte form a continuous and dense barrier structure in situ at the interface between the separator and the electrode, filling and / or sealing the pores of the separator and blocking the transport path of lithium ions.
[0016] Optionally, the cathode material is one or more of lithium iron phosphate, lithium cobalt oxide, nickel cobalt manganese, and nickel cobalt aluminum ternary cathode materials; Optionally, the negative electrode material is one or more of lithium metal, silicon-carbon negative electrode material, lithium titanate, and graphite; Optionally, the diaphragm is one or more of the following: polyethylene porous membrane, polypropylene porous membrane, polyethylene / polypropylene three-layer composite membrane, and glass fiber membrane.
[0017] This invention has at least one of the following beneficial effects: 1. This invention provides an electrolyte system that can actively respond and quickly cut off ion transport channels in the early stage of abnormal temperature rise in a battery. This electrolyte can actively cut off the ion transport process inside the battery in the early stage of thermal runaway, fundamentally preventing the internal short circuit from continuing to develop. Specifically, based on the characteristics of thermally responsive polymer precursors—low viscosity at room temperature and rapid transformation into an infusible and insoluble barrier layer upon temperature stimulation—this invention incorporates epoxy ether monomers and polysilazane polymers into the liquid electrolyte. When the battery is at normal operating temperature, the thermally responsive polymer precursor remains in a low-viscosity liquid state, co-wetting the membrane pores with the electrolyte without affecting normal lithium-ion transport or battery electrochemical performance. However, when the battery temperature rises due to thermal abuse or other reasons, the epoxy ether monomers and polysilazane polymers undergo a cross-linking reaction, and the electrolyte gradually transforms from a liquid state into a highly cross-linked three-dimensional barrier layer network. This forms a continuous and dense barrier structure in situ at the membrane porous structure and electrode interface, filling and sealing the membrane pores, blocking lithium-ion transport paths, significantly suppressing internal short circuits and subsequent exothermic reactions, thereby achieving active safety protection in the early stages of thermal runaway development.
[0018] 2. The electrolyte of this invention, based on thermally responsive polymers, is in a solution state at room temperature and can conduct lithium ions normally. It has good compatibility with existing lithium-ion battery manufacturing processes and is easy to scale up and industrialize. Attached Figure Description
[0019] Figure 1 This is a graph showing the change in electrolyte ionic conductivity with temperature in Embodiment 1 of the present invention.
[0020] Figure 2 This is a graph showing the change in electrochemical impedance of the lithium battery assembled with electrolyte in Example 1 of the present invention as a function of temperature.
[0021] Figure 3 This is a schematic diagram showing the change in the electrolyte structure from a room temperature solution state to a high temperature barrier layer state in Embodiment 1 of the present invention.
[0022] Figure 4 This is a graph showing the charge / discharge specific capacity-cycle variation of the lithium battery assembled with electrolyte in Embodiment 1 of the present invention.
[0023] Figure 5 This is a high-temperature voltage-time variation curve of the lithium-ion battery in Embodiment 1 of the present invention.
[0024] Figure 6 This is a graph showing the specific capacity-cycle variation of the lithium battery assembled with electrolyte at different charging and discharging rates in Embodiment 1 of the present invention.
[0025] Figure 7 This is a graph showing the voltage-charge-discharge specific capacity variation of the lithium-ion battery at room temperature and high temperature in Embodiment 2 of the present invention.
[0026] Figure 8 This is a voltage-time curve of the lithium-ion battery from room temperature to high temperature in Embodiment 2 of the present invention.
[0027] Figure 9 This is a graph showing the change in electrolyte ionic conductivity with temperature in Comparative Example 1 of this invention. Detailed Implementation
[0028] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0029] One embodiment of the present invention provides an electrolyte based on a thermally responsive polymer, the electrolyte comprising an epoxy ether monomer, a polysilazane polymer, a lithium salt, and an organic solvent; The epoxy ether monomers and the polysilazane polymers can react under heating conditions to transform the electrolyte from a liquid state into a three-dimensional cross-linked network structure.
[0030] Thermally responsive polymer precursors possess low viscosity at room temperature and can rapidly transform into an infusible and insoluble barrier layer upon temperature stimulation. Adding such precursor materials to liquid electrolytes allows the precursors to maintain a low-viscosity liquid state at normal battery operating temperatures, co-wetting the separator pores with the electrolyte without affecting normal lithium-ion transport or battery electrochemical performance. However, when the battery temperature rises to a set temperature due to thermal abuse, the reaction between the Si–N bonds in the polysilazane and the epoxy monomers accelerates significantly, accompanied by epoxy ring opening and hydroxyl generation. The newly generated hydroxyl groups further participate in Si–N bond reactions, forming Si–O–C crosslinking reactions, thereby promoting the construction of the epoxy organic network and the polysilazane network. The electrolyte gradually transforms from a liquid state into a highly crosslinked three-dimensional barrier layer network, forming a continuous and dense barrier structure in situ at the separator porous structure and electrode interface. This fills and seals the separator pores, blocking lithium-ion transport paths and significantly suppressing internal short circuits and subsequent exothermic reactions, thus achieving active safety protection in the early stages of thermal runaway. Compared to traditional passive safety strategies such as heat-resistant membranes or flame-retardant additives, electrolytes based on thermally responsive polymers can achieve the dual function of maintaining high ion conduction under normal operating conditions and actively cutting off ion transport under abnormal temperature rise. This is expected to rapidly suppress the further development of thermal runaway from the source of the thermal runaway induction mechanism, providing a new technical approach for building safe, high-energy-density lithium-ion batteries.
[0031] In some embodiments, the epoxy ether monomer is one or more of sorbitol glycidyl ether (SPE), bisphenol S diglycidyl ether (BPS-DGE), glycerol triglycidyl ether (GTE), pentaerythritol tetraglycidyl ether (PTGE), trimethylolpropane triglycidyl ether (TMPTGE), and tetramethylbisphenol diglycidyl ether (TMBPDGE).
[0032] In some embodiments, the polysilazane polymer is one or more of polymethylvinylsilazane (PMVS), polydiphenylsilazane (PDPS), polymethylphenylsilazane (PMPS), polyvinylsilazane (PVS), polydimethylsilazane (PMS), polymethylhydrosilazane (PHS), polyphenylsilazane (PPS), and polymethyl(3,3,3-trifluoropropyl)silazane (PMFS).
[0033] In some embodiments, the lithium salt is one or more of lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6) (LiClO4), lithium difluorooxalate borate (LiDFOB), lithium bis(oxalate borate) (LiBOB), and lithium nitrate (LiNO3); In some embodiments, the organic solvent is one or more of ethylene carbonate (EC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethylene glycol dimethyl ether (DME), and 1,3-dioxolane (DOL).
[0034] In some embodiments, the components of the electrolyte are expressed in the following proportions by mass fraction: epoxy ether monomers 3%–5%, polysilazane polymers 1%–3%, lithium salts 30%–40%, and organic solvents 52%–66%. Preferably, the proportions are: epoxy ether monomers 2%–5%, polysilazane polymers 1%–3%, lithium salts 30%–38%, and organic solvents 57%–72%. More preferably, the proportions are: epoxy ether monomers 3%–4%, polysilazane polymers 2%–4%, lithium salts 32%–36%, and organic solvents 62%–66%.
[0035] In some embodiments, the heating conditions include an electrolyte temperature greater than 100°C, preferably 100°C to 150°C, and more preferably 110°C to 140°C.
[0036] Another embodiment of the present invention provides a method for preparing the electrolyte, the method comprising the following steps: The electrolyte is obtained by uniformly mixing epoxy ether monomers, polysilazane polymers, lithium salts, and organic solvents.
[0037] The preparation method of the electrolyte of the present invention is simple and highly practical.
[0038] In some embodiments, the preparation method of the lithium-ion battery electrolyte with high-temperature thermal shutdown described above includes the following steps: An epoxy ether monomer, polysilazane, lithium salt, and organic solvent are mixed and stirred at 500-1000 r / min for 0.5-2 h to obtain a lithium-ion battery electrolyte with high-temperature thermal shutdown.
[0039] Another embodiment of the present invention provides a lithium secondary battery with high-temperature thermal shutdown, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the electrolyte is the above-mentioned electrolyte based on a thermally responsive polymer.
[0040] In normal use, the electrolyte of the lithium secondary battery of the present invention is in a liquid state, which can wet the pores of the separator and does not affect the normal transport of lithium ions or the electrochemical performance of the battery. When the battery temperature rises to the set temperature due to thermal abuse, the epoxy ether monomers and polysilazane polymers in the electrolyte undergo a cross-linking reaction, which gradually transforms the electrolyte from a liquid state into a highly cross-linked three-dimensional barrier layer network. A continuous and dense barrier structure is formed in situ at the porous structure of the separator and the electrode interface, filling and sealing the pores of the separator, blocking the lithium ion transport path, significantly suppressing internal short circuits and subsequent exothermic reactions, thereby achieving active safety protection in the early stage of thermal runaway.
[0041] In some embodiments, when the lithium secondary battery is at normal operating temperature, the electrolyte is liquid and wets the pores of the separator; When the temperature of the lithium secondary battery is higher than the preset temperature, the polysilazane polymer and epoxy ether monomer in the electrolyte form a continuous and dense barrier structure in situ at the interface between the separator and the electrode, filling and / or sealing the pores of the separator and blocking the transport path of lithium ions.
[0042] Preferably, the preset temperature is 100°C.
[0043] In some embodiments, the cathode material is one or more of lithium iron phosphate, lithium cobalt oxide, nickel cobalt manganese, and nickel cobalt aluminum ternary cathode materials; In some embodiments, the negative electrode material is one or more of lithium metal, silicon-carbon negative electrode material, lithium titanate, and graphite. In some embodiments, the diaphragm is one or more of polyethylene porous membrane, polypropylene porous membrane, polyethylene / polypropylene three-layer composite membrane, and glass fiber membrane.
[0044] The present invention will be further described in detail below with reference to specific embodiments, but the present invention is not limited to the following specific embodiments.
[0045] It is important to note that: 1. Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.
[0046] 2. The performance of the lithium-ion battery electrolytes prepared in the following examples was tested as follows: The ionic conductivity was measured using AC impedance spectroscopy on a CHI 760 electrochemical workstation by assembling a stainless steel / separator / stainless steel battery with stainless steel electrodes and a 30-micron thick polytetrafluoroethylene membrane with 6 mm diameter circular holes as the separator. The charge-discharge cycle test of the lithium battery was obtained by assembling lithium / separator / lithium iron phosphate batteries and testing them on a LAND battery charge-discharge test system.
[0047] Example 1: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 1:1) to obtain a liquid electrolyte.
[0048] Step 2: Mix pentaerythritol tetraglycidyl ether (0.1g) and polyvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0049] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a lithium-ion battery electrolyte with high-temperature thermal shutdown based on thermally responsive polymer.
[0050] The obtained electrolyte was subjected to ionic conductivity testing, and the curve of ionic conductivity versus temperature is shown below. Figure 1 As shown, the electrolyte obtained at room temperature (25℃) still has a strength of 5.4 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.02 × 10⁻⁶. -3 S cm -1 .
[0051] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The resulting electrochemical impedance spectroscopy curves are shown below. Figure 2 As shown, the charge transfer resistance R at room temperature ct The charge transfer resistance R is 25.77 Ω at 115 °C. ct The charge transfer resistance R is 851.72 Ω at 120 °C. ct It is 2302 Ω.
[0052] The obtained electrolyte was subjected to high-temperature change testing. Schematic diagrams of the electrolyte at room temperature and after high temperature are shown below. Figure 3 As shown, the electrolyte obtained at room temperature is in solution form, while the electrolyte obtained at high temperature has a barrier layer structure.
[0053] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and charge-discharge tests were conducted. The resulting charge-discharge specific capacity versus cycle number curves are shown below. Figure 4 As shown, within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate battery has a 90% capacity retention rate after 240 cycles.
[0054] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, which were then subjected to high-temperature charge-discharge tests. The resulting voltage-time variation curves are shown in the figure below. Figure 5 As shown, the voltage dropped from the normal voltage of 3 V to below 2.5 V within 3 minutes at high temperature, proving that the obtained electrolyte-assembled lithium / lithium iron phosphate battery achieved battery thermal shutdown within 3 minutes at high temperature.
[0055] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and charge-discharge tests were conducted. The resulting curves of specific capacity versus cycle number at different charge-discharge rates are shown below. Figure 6 As shown, within the voltage range of 2.5~3.8V at 0.1 C, the lithium / lithium iron phosphate battery exhibits a capacity of 161 mAh g⁻¹. -1 The discharge specific capacity; within the voltage range of 2.5~3.8V at 0.3C, the lithium / lithium iron phosphate battery has a discharge capacity of 155 mAhg. -1 The discharge specific capacity; within the voltage range of 2.5~3.8V at 0.5 C, the lithium / lithium iron phosphate battery has a discharge specific capacity of 151 mAh g. -1 The discharge specific capacity; within the voltage range of 2.5~3.8V at 1C, the lithium / lithium iron phosphate battery has a discharge capacity of 138 mAh g. -1 The discharge specific capacity; within the voltage range of 2.5~3.8V at 2C, the lithium / lithium iron phosphate battery has a discharge capacity of 122mAh g / L. -1 The discharge specific capacity; within the voltage range of 2.5~3.8V at 5C, the lithium / lithium iron phosphate battery has a discharge capacity of 93 mAh g. -1 The specific discharge capacity.
[0056] Example 2: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 1:1) to obtain a liquid electrolyte.
[0057] Step 2: Mix pentaerythritol tetraglycidyl ether (0.1g) and polyvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0058] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (0.8g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0059] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 5.9 × 10⁻⁶.-3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.04 × 10⁻⁶. -3 S cm -1 .
[0060] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 26.58 Ω at 115 °C. ct The charge transfer resistance R is 869.55 Ω at 120 °C. ct It is 2076 Ω.
[0061] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5 to 3.8V at 0.5 C, the lithium / lithium iron phosphate batteries maintained a capacity retention of 92% after 230 cycles.
[0062] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, which were then subjected to high-temperature charge-discharge tests. The resulting voltage-to-capacity variation curves are shown in the figure below. Figure 7 As shown, within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate battery has a capacity of 152mAh g / L. -1 The discharge specific capacity is [not specified]. However, after standing still for 5 minutes at high temperature, the discharge specific capacity is 1.75 mAh g. -1 The electrolyte exhibited a significant high-temperature thermal shutdown effect.
[0063] The lithium / lithium iron phosphate battery assembled with the obtained electrolyte operates normally at room temperature. When the temperature is increased to 120 degrees Celsius, the voltage drops from 3.8 V to 2.4 V. The voltage-time curve is shown in the figure below. Figure 8 As shown, the electrolyte exhibits a significant high-temperature thermal shutdown effect.
[0064] Example 3: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 2:1) to obtain a liquid electrolyte.
[0065] Step 2: Mix pentaerythritol tetraglycidyl ether (0.1g) and polyvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0066] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0067] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 6.3 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.03 × 10⁻⁶. -3 S cm -1 .
[0068] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 30.63 Ω at 115 °C. ct The charge transfer resistance R is 982.35 Ω at 120 °C. ct It is 1892 Ω.
[0069] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, which were then subjected to high-temperature charge-discharge tests. At room temperature and 0.5C, within a voltage range of 2.5–3.8V, the lithium / lithium iron phosphate batteries exhibited a performance of 150 mAh g⁻¹. -1 The discharge specific capacity is [value missing]. However, after standing still for 5 minutes at high temperature, the discharge specific capacity is 0.85 mAh g. -1 The electrolyte exhibited a significant high-temperature thermal shutdown effect.
[0070] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5 to 3.8V at 0.5 C, the lithium / lithium iron phosphate batteries maintained a capacity retention of 91% after 230 cycles.
[0071] Example 4: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 3:1) to obtain a liquid electrolyte.
[0072] Step 2: Mix pentaerythritol tetraglycidyl ether (0.1g) and polyvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0073] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0074] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 5.1 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.06 × 10⁻⁶. -3 S cm -1 .
[0075] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 26.58 Ω at 115 °C. ct The charge transfer resistance R is 763.32 Ω at 120 °C. ct It is 1965 Ω.
[0076] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for high-temperature charge-discharge tests. Under high temperature, the voltage dropped from the normal voltage of 3 V to below 2.5 V within 4 minutes. The obtained electrolyte showed obvious high-temperature thermal shutdown effect of lithium batteries.
[0077] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate batteries maintained a capacity retention of 93% after 220 cycles.
[0078] Example 5: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 4:1) to obtain a liquid electrolyte.
[0079] Step 2: Mix pentaerythritol tetraglycidyl ether (0.1g) and polyvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0080] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0081] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 5.5 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.07 × 10⁻⁶. -3 S cm -1 .
[0082] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for high-temperature charge-discharge tests. Under high temperature, the voltage dropped from the normal voltage of 3 V to below 2.5 V within 4 minutes. The obtained electrolyte showed obvious high-temperature thermal shutdown effect of lithium batteries.
[0083] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5 to 3.8V at 0.5 C, the lithium / lithium iron phosphate batteries exhibited a capacity retention of 92% after 210 cycles.
[0084] Example 6: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 1:1) to obtain a liquid electrolyte.
[0085] Step 2: Mix pentaerythritol tetraglycidyl ether (0.1g) and polyvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0086] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (0.6g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0087] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 5.8 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.02 × 10⁻⁶. -3 S cm -1 .
[0088] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 27.13 Ω at 115 °C. ct The charge transfer resistance R is 951.85 Ω at 120 °C.ct It is 1673 Ω.
[0089] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for high-temperature charge-discharge tests. Under high temperature, the voltage dropped from the normal voltage of 3 V to below 2.5 V within 3 minutes. The obtained electrolyte showed obvious high-temperature thermal shutdown effect of lithium batteries.
[0090] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, which were then subjected to high-temperature charge-discharge tests. At room temperature and 0.5C, within a voltage range of 2.5–3.8V, the lithium / lithium iron phosphate batteries exhibited a performance of 153 mAh g⁻¹. -1 The discharge specific capacity is [value missing]. However, after standing still for 5 minutes at high temperature, the discharge specific capacity is 0.45 mAh g. -1 The electrolyte exhibited a significant high-temperature thermal shutdown effect.
[0091] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate batteries exhibited a capacity retention rate of 91% after 220 cycles.
[0092] Example 7: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 1:1) to obtain a liquid electrolyte.
[0093] Step 2: Mix pentaerythritol tetraglycidyl ether (0.2g) and polyvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0094] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0095] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 4.8 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.02 × 10⁻⁶. -3 S cm -1 .
[0096] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ctThe charge transfer resistance R is 42.53 Ω at 115 °C. ct The charge transfer resistance R is 932.61 Ω at 120 °C. ct It is 2035 Ω.
[0097] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for high-temperature charge-discharge tests. Under high temperature, the voltage dropped from the normal voltage of 3 V to below 2.5 V within 4 minutes. The obtained electrolyte showed obvious high-temperature thermal shutdown effect of lithium batteries.
[0098] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate batteries maintained 95% capacity retention after 200 cycles.
[0099] Example 8: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 1:1) to obtain a liquid electrolyte.
[0100] Step 2: Mix pentaerythritol tetraglycidyl ether (0.2g) and polyvinylsilazane (0.06g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0101] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0102] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 6.5 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.03 × 10⁻⁶. -3 S cm -1 .
[0103] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 33.60 Ω at 115 °C. ct The charge transfer resistance R is 1023.25 Ω at 120 °C. ct It is 1958 Ω.
[0104] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for high-temperature charge-discharge tests. Under high temperature, the voltage dropped from the normal voltage of 3 V to below 2 V within 4 minutes. The obtained electrolyte showed obvious high-temperature thermal shutdown effect of lithium batteries.
[0105] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate batteries exhibited a 90% capacity retention rate after 235 cycles.
[0106] Example 9: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 1:1) to obtain a liquid electrolyte.
[0107] Step 2: Mix pentaerythritol tetraglycidyl ether (0.2g) and polyvinylsilazane (0.08g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0108] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0109] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 4.9 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.05 × 10⁻⁶. -3 S cm -1 .
[0110] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 36.41 Ω at 115 °C. ct The charge transfer resistance R is 966.05 Ω at 120 °C. ct It is 1759 Ω.
[0111] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, which were then subjected to high-temperature charge-discharge tests. At room temperature and 0.5C within a voltage range of 2.5–3.8V, the lithium / lithium iron phosphate batteries exhibited a performance of 149 mAh g⁻¹. -1 The discharge specific capacity is [not specified]. However, after standing still for 5 minutes at high temperature, the discharge specific capacity is 1.25 mAh g.-1 The electrolyte exhibited a significant high-temperature thermal shutdown effect.
[0112] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5 to 3.8V at 0.5 C, the lithium / lithium iron phosphate batteries maintained a capacity retention of 94% after 230 cycles.
[0113] Example 10: This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 1:1) to obtain a liquid electrolyte.
[0114] Step 2: Mix pentaerythritol tetraglycidyl ether (0.2g) and polyvinylsilazane (0.1g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0115] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0116] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 4.5 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 0.01 × 10⁻⁶. -3 S cm -1 .
[0117] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 38.92 Ω at 115 °C. ct The charge transfer resistance R is 1020.15 Ω at 120 °C. ct It is 2260 Ω.
[0118] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for high-temperature charge-discharge tests. Under high temperature, the voltage dropped from the normal voltage of 3 V to below 2.1 V within 4 minutes. The obtained electrolyte showed a significant high-temperature thermal shutdown effect on lithium batteries.
[0119] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, which were then subjected to high-temperature charge-discharge tests. At room temperature and within a voltage range of 2.5–3.8V at 0.5 C, the lithium / lithium iron phosphate batteries exhibited a performance of 152 mAh g⁻¹. -1 The discharge specific capacity is [value missing]. However, after standing still for 5 minutes at high temperature, the discharge specific capacity is 0.35 mAh g. -1 The electrolyte exhibited a significant high-temperature thermal shutdown effect.
[0120] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for charge-discharge testing. Within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate batteries exhibited a 90% capacity retention rate after 220 cycles.
[0121] Example 11 This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 2:1) to obtain a liquid electrolyte.
[0122] Step 2: Mix sorbitol glycidyl ether (0.2g) and polyvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0123] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0124] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 25.83Ω at 115 °C. ct The charge transfer resistance R is 944.85Ω at 120 °C. ct It is 1637Ω.
[0125] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, which were then subjected to high-temperature charge-discharge tests. At room temperature and 0.5C within a voltage range of 2.5–3.8V, the lithium / lithium iron phosphate batteries exhibited a performance of 146 mAh g⁻¹. -1 The discharge specific capacity was [value missing]. However, after standing still for 5 minutes at high temperature, the discharge specific capacity was 0.68 mAh g. -1 The electrolyte exhibited a significant high-temperature thermal shutdown effect.
[0126] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5 to 3.8V at 0.5 C, the lithium / lithium iron phosphate batteries maintained a capacity retention of 91% after 300 cycles.
[0127] Example 12 This embodiment illustrates the method for preparing a high-temperature thermal shutdown lithium-ion battery electrolyte based on a thermally responsive polymer disclosed in this invention, including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 2:1) to obtain a liquid electrolyte.
[0128] Step 2: Mix pentaerythritol tetraglycidyl ether (0.2g) and polymethylvinylsilazane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0129] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0130] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, and temperature-dependent electrochemical impedance spectroscopy was performed. The charge transfer resistance R at room temperature was measured. ct The charge transfer resistance R is 18.76Ω at 115 °C. ct The charge transfer resistance R is 856.24Ω at 120 °C. ct It is 1740Ω.
[0131] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries, which were then subjected to high-temperature charge-discharge tests. At room temperature and 0.5C within a voltage range of 2.5–3.8V, the lithium / lithium iron phosphate batteries exhibited a performance of 141 mAh g⁻¹. -1 The discharge specific capacity was [value missing]. However, after standing still for 5 minutes at high temperature, the discharge specific capacity was 0.96 mAh g. -1 The electrolyte exhibited a significant high-temperature thermal shutdown effect.
[0132] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5 to 3.8V at 0.5 C, the lithium / lithium iron phosphate batteries exhibited a capacity retention of 93% after 290 cycles.
[0133] Comparative Example 1 The difference from Example 1 is that pentaerythritol tetraglycidyl ether is not added, and the specific operation steps are as follows: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 2:1) to obtain a liquid electrolyte.
[0134] Step 2: Mix polymethylvinylsilazane (0.02g) with the liquid electrolyte (1g) obtained in Step 1, stirring at 1000r / min for 30min to obtain the lithium-ion battery electrolyte.
[0135] The ionic conductivity of the obtained electrolyte was tested, and the results are as follows: Figure 9 As shown, the electrolyte obtained at room temperature (25℃) still has a strength of 6.3 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 13.15 × 10⁻⁶. -3 S cm -1 This proves that electrolytes cannot react at high temperatures to form a barrier structure.
[0136] The lithium / lithium iron phosphate batteries assembled with the obtained electrolyte were subjected to charge-discharge tests. Within the voltage range of 2.5 to 3.8V at 0.5 C, the lithium / lithium iron phosphate batteries exhibited a capacity retention of 88% after 270 cycles.
[0137] Comparative Example 2 The difference from Example 1 is that polyvinylsilazane is not added, and the specific operation steps are as follows: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 2:1) to obtain a liquid electrolyte.
[0138] Step 2: Mix pentaerythritol tetraglycidyl ether (0.2g) with the liquid electrolyte (1g) obtained in Step 1, stirring at 1000r / min for 30min to obtain the lithium-ion battery electrolyte.
[0139] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature (25℃) still had a conductivity of 5.8 × 10⁻⁶. -3 S cm -1 The electrolyte obtained at high temperature (120℃) has a strength of 14.92 × 10⁻⁶. -3 S cm -1 This proves that electrolytes cannot react at high temperatures to form a barrier structure.
[0140] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for charge-discharge testing. Within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate batteries exhibited a 90% capacity retention rate after 263 cycles.
[0141] Comparative Example 3 The difference from Example 1 is that "polyvinylsilazane" is replaced with "polysiloborazane", specifically including the following steps: Step 1: Dissolve lithium bis(trifluoromethanesulfonylimide) (0.28 g) in a mixed solution (1 mL) of propylene carbonate / fluoroethylene carbonate (volume ratio 2:1) to obtain a liquid electrolyte.
[0142] Step 2: Mix pentaerythritol tetraglycidyl ether (0.2g) and polysiloxane (0.02g) at a stirring speed of 1000r / min for 30min to obtain a mixed solution.
[0143] Step 3: Mix the mixed solution (0.12g) obtained in Step 2 with the liquid electrolyte (1g) obtained in Step 1 to obtain a high-temperature thermal shutdown lithium-ion battery electrolyte based on thermally responsive polymer.
[0144] The obtained electrolyte was tested for ionic conductivity, and the electrolyte obtained at room temperature still had a conductivity of 5.6 × 10⁻⁶. -3 Scm -1 The electrolyte obtained at high temperature has a strength of 17.23 × 10⁻⁶. -3 S cm -1 This demonstrates that the electrolyte cannot react to form a barrier structure at high temperatures. Therefore, polysiloxane and pentaerythritol tetraglycidyl ether cannot react to form a barrier structure.
[0145] The obtained electrolyte was used to assemble lithium / lithium iron phosphate batteries for charge-discharge testing. Within the voltage range of 2.5~3.8V at 0.5C, the lithium / lithium iron phosphate batteries exhibited a capacity retention of 89% after 250 cycles.
[0146] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. An electrolyte based on a thermally responsive polymer, characterized in that, The electrolyte comprises epoxy ether monomers, polysilazane polymers, lithium salts, and organic solvents; The epoxy ether monomers and the polysilazane polymers can react under heating conditions to transform the electrolyte from a liquid state into a three-dimensional cross-linked network structure.
2. The electrolyte according to claim 1, characterized in that, The epoxy ether monomers are one or more of sorbitol glycidyl ether, bisphenol S diglycidyl ether, glycerol triglycidyl ether, pentaerythritol tetraglycidyl ether, trimethylolpropane triglycidyl ether, and tetramethylbisphenol diglycidyl ether.
3. The electrolyte according to claim 1, characterized in that, The polysilazane polymers are one or more of polymethylvinylsilazane, polydiphenylsilazane, polymethylphenylsilazane, polyvinylsilazane, polydimethylsilazane, polymethylhydrosilazane, polyphenylsilazane, and polymethyl(3,3,3-trifluoropropyl)silazane.
4. The electrolyte according to claim 1, characterized in that, The lithium salt is one or more of lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate, lithium difluorooxalate borate, lithium bis(oxalate borate), and lithium nitrate. The organic solvent is one or more of ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, propylene carbonate, methyl ethyl carbonate, dimethyl carbonate, diethyl carbonate, ethylene glycol dimethyl ether, and 1,3-dioxolane.
5. The electrolyte according to claim 1, characterized in that, The electrolyte contains the following components by mass fraction: epoxy ether monomers 3%~5%, polysilazane polymers 1%~3%, lithium salts 30%~40%, and organic solvents 52%~66%.
6. The electrolyte according to claim 1, characterized in that, The heating conditions include making the temperature of the electrolyte greater than 100°C.
7. The method for preparing the electrolyte according to any one of claims 1 to 6, characterized in that, The preparation method includes the following steps: The electrolyte is obtained by uniformly mixing epoxy ether monomers, polysilazane polymers, lithium salts, and organic solvents.
8. A lithium secondary battery with high-temperature thermal shutdown, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that, The electrolyte is the electrolyte according to any one of claims 1 to 6.
9. The lithium secondary battery according to claim 8, characterized in that, When the lithium secondary battery is at normal operating temperature, the electrolyte is liquid and wets the pores of the separator; When the temperature of the lithium secondary battery is higher than the preset temperature, the polysilazane polymer and epoxy ether monomer in the electrolyte form a continuous and dense barrier structure in situ at the interface between the separator and the electrode, filling and / or sealing the pores of the separator and blocking the transport path of lithium ions.
10. The lithium secondary battery according to claim 8, characterized in that, The cathode material is one or more of lithium iron phosphate, lithium cobalt oxide, nickel cobalt manganese, and nickel cobalt aluminum ternary cathode materials; The negative electrode material is one or more of lithium metal, silicon-carbon negative electrode material, lithium titanate, and graphite. The diaphragm is one or more of the following: polyethylene porous membrane, polypropylene porous membrane, polyethylene / polypropylene three-layer composite membrane, and glass fiber membrane.