Functionalized fiber composite skeleton material, preparation method and solid electrolyte membrane
By functionalizing PET fibers by introducing lithium carboxyl groups on the surface and nitrile groups on the surface of Tencel fibers, a porous network composite skeleton material is formed, which solves the problems of interfacial compatibility, mechanical strength and ion transport of PET-based fiber skeleton materials in solid electrolyte composite membranes, and achieves high efficiency in lithium ion migration and conductivity.
Patent Information
- Application Number
- CN202610955240.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-30
- Publication Date
- 2026-11-10
AI Technical Summary
Existing PET-based fiber skeleton materials in solid electrolyte composite membranes suffer from problems such as insufficient interfacial compatibility, difficulty in balancing porosity and mechanical strength, insufficient ion transport regulation, and difficulty in forming a stable synergistic network through fiber blending.
By introducing lithium carboxylate groups on the surface of PET fibers and nitrile groups on the surface of Tencel fibers, a functionalized fiber composite skeleton material is formed. The two types of fibers interweave to form a porous network, which improves interfacial compatibility and mechanical strength, and optimizes ion transport performance.
It achieves excellent mechanical strength and dimensional stability under high porosity, reduces interfacial impedance, improves ionic conductivity and lithium-ion migration efficiency, and solves the problems in the existing technology.
Smart Images

Figure CN123073155A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid-state battery electrolyte materials technology, and more specifically, to a functionalized fiber composite skeleton material, a method for preparing the functionalized fiber composite skeleton material, and a composite solid electrolyte membrane comprising the composite skeleton material. Background Technology
[0002] In composite solid electrolyte systems, porous framework materials are typically introduced as reinforcing support layers to improve the mechanical strength, dimensional stability, and processing performance of the electrolyte membrane. Their pore structure provides space for the wetting and solidification of polymer lithium salt electrolytes and the dispersion and fixation of oxide solid electrolyte particles such as LATP and LLZO, thus contributing to the construction of stable composite ion transport structures. PET nonwoven fabric, due to its good mechanical properties, thermal dimensional stability, pore structure controllability, and mature industrial preparation capabilities, can be considered as one of the options for this type of framework material.
[0003] The existing technologies for improving PET-based fiber skeletons mainly include: plasma surface treatment, chemical grafting modification, physical mixing of multiple fibers, and directly using PET nonwoven fabric as reinforcement.
[0004] However, existing PET-based fiber skeletons still have the following technical problems in solid electrolyte composite membranes: Insufficient interfacial compatibility: PET has limited active sites on its surface, resulting in poor interfacial contact with oxide electrolytes, which easily leads to interfacial defects and increases interfacial impedance; Conflict between porosity and mechanical strength: High porosity is beneficial for ion transport, but it significantly reduces the mechanical strength of the framework material, making it difficult to simultaneously meet the requirements of ion transport and continuous processing; Insufficient ion transport regulation: Existing surface modifications mostly focus on introducing single polar groups (such as hydroxyl and carboxyl groups), which have limited ability to synergistically regulate lithium salt dissociation and ion selective transport; Difficulty in forming a synergistic network through fiber blending: When PET is simply blended with unmodified cellulose fibers, the coordination effect of the two fibers is singular and has limited stability, making it difficult to construct a stable and efficient synergistic ion transport network; Process defects: Some surface modification processes (such as plasma treatment) have problems such as high equipment costs, easy decay of modification effects, or adverse effects on the mechanical properties of the substrate.
[0005] Therefore, there is an urgent need to develop a new type of fiber skeleton material that can simultaneously take into account interfacial compatibility, mechanical strength, porosity, ion transport efficiency, and process economy. Summary of the Invention
[0006] To address the technical problems in existing PET-based fiber skeleton materials, such as poor interfacial compatibility, difficulty in balancing porosity and mechanical strength, insufficient ion transport regulation due to limited surface modification, and the inability of simple fiber blending to form a stable and synergistic ion transport network, this invention provides a functionalized fiber composite skeleton material, a method for preparing the functionalized fiber composite skeleton material, and a composite solid electrolyte membrane containing the composite skeleton material. By introducing lithium carboxylate groups onto the surface of PET fibers, the polarity and density of lithium-containing active sites on the fiber surface are increased, improving its interfacial compatibility with polymer lithium salt electrolytes and inorganic lithium-ion conductor particles. By introducing nitrile groups onto the surface of Tencel fibers, its coordination effect and wetting properties with lithium salt and polar polymer systems are improved. The two types of functionalized fibers interweave to form a porous network, thereby maintaining high porosity while improving the mechanical support capacity, dimensional stability, and electrolyte filling uniformity of the skeleton material, and helping to reduce the interfacial impedance of the composite electrolyte membrane.
[0007] In a first aspect, the present invention provides a functionalized fiber composite skeleton material, comprising: The first fiber is a modified PET fiber with lithium carboxylate groups on its surface; The second fiber is a modified Tencel fiber with a nitrile group on its surface; The first fiber and the second fiber are interwoven within the skeleton material to form a porous structure; The mass ratio of the first fiber to the second fiber is 5:95 to 60:40.
[0008] Furthermore, the mass ratio of the first fiber to the second fiber is 20:80 to 40:60; The first fiber has a length of 0.5–8 mm and a diameter of 5–20 μm; the second fiber has a length of 0.5–6 mm and a diameter of 5–20 μm. The thickness of the skeleton material is 20–100 μm, and the porosity is 60%–85%.
[0009] Furthermore, the diameter of the first fiber and the second fiber are both 0.2 to 5 μm, and the length is both 0.1 to 2 mm. The thickness of the skeleton material is 5 to 20 μm, so as to form a thin composite skeleton material by means of micronized PET fiber and micronized Tencel fiber.
[0010] Furthermore, the composite skeleton material also includes a bonding and reinforcing component, which is selected from one or more of low-melting-point polyester fibers, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, lithium polyacrylate, polyurethane, nanocellulose, and aramid nanofibers, and its addition amount is 0.5% to 10% of the total mass of the first fiber and the second fiber.
[0011] Furthermore, the composite skeleton material has an asymmetric layered structure, including: The first layer near the negative electrode side is the first fiber enrichment layer. An intermediate layer, wherein the intermediate layer is a mixture of a first fiber and a second fiber; The second layer, located near the positive electrode side, is a second fiber-enriched layer.
[0012] In a second aspect, the present invention provides a method for preparing a functionalized fiber composite skeleton material, used to prepare the functionalized fiber composite skeleton material as described in any of the preceding claims, the method comprising: Step S10: Provide modified PET fibers with lithium carboxylate groups on the surface, i.e., the first fiber; Step S20: Provide modified Tencel fibers with acrylonitrile groups on the surface, i.e., the second fiber; Step S30: The obtained first fiber and second fiber are mixed at a mass ratio of 5:95 to 60:40 and dispersed in a dispersion medium to form a uniform fiber suspension; Step S40: The obtained fiber suspension is processed into a wet membrane using wet papermaking, vacuum filtration, or filtration molding methods; Step S50: The wet film is dried and hot-pressed to obtain the functionalized fiber composite skeleton material.
[0013] Furthermore, the dispersion medium is water or a mixture of water and alcohol, and a dispersant is added. The dispersant is selected from one or more of Triton X-100, sodium dodecyl sulfate, polyvinylpyrrolidone, and sodium carboxymethyl cellulose, and the amount added is 0.001% to 0.1% of the total fiber mass. The fiber suspension also contains a bonding and reinforcing component, which is selected from one or more of low-melting-point polyester fibers, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, lithium polyacrylate, polyurethane, nanocellulose, and aramid nanofibers, and its addition amount is 0.5% to 10% of the total mass of the first fiber and the second fiber.
[0014] Furthermore, during the drying and hot-pressing process of the wet film, the drying temperature is 60–120°C, the hot-pressing temperature is 80–180°C, the pressure is 0.5–5 MPa, and the time is 0.5–10 min.
[0015] Furthermore, the first fiber is prepared by the following method: PET fibers are immersed in a NaOH aqueous solution with a concentration of 0.05–1.0 mol / L and treated at 40–90°C for 5–60 min for surface hydrolysis. Then, they are immersed in a lithium-containing compound solution for lithium salting treatment. The lithium-containing compound is selected from one or more of LiOH, Li2CO3, and lithium acetate. The solution concentration is 0.05–1.0 mol / L, the treatment temperature is 30–90°C, and the treatment time is 0.5–8 h, to obtain the first fiber with lithium carboxylate groups on the surface.
[0016] Furthermore, the method also includes: After surface hydrolysis and before lithium salting, the surface-hydrolyzed PET fibers are immersed in an acid solution of 0.01–0.1 mol / L for 5–30 min, wherein the acid solution is selected from one or more of hydrochloric acid, acetic acid, and citric acid.
[0017] Furthermore, the second fiber is prepared by esterification, cyanoethylation, or modification with a nitrile-containing silane coupling agent: The esterification method includes: Tencel fibers are dispersed in a polar aprotic solvent, and cyanoacetic acid, a dehydrating condensing agent and a catalyst are added. The mixture is reacted at 40-90℃ for 4-24 hours under an inert atmosphere to allow the hydroxyl groups on the surface of the Tencel fibers to undergo an esterification reaction with cyanoacetic acid, introducing nitrile functional groups onto the fiber surface. After the reaction, the fibers are washed and dried to obtain the second fiber. Wherein, the polar aprotic solvent is selected from one or more of DMF, DMSO, DMAc, and NMP; the dehydrating condensing agent is selected from one or more of DCC, DIC, EDC, and CDI; the catalyst is selected from one or more of DMAP, pyridine, and triethylamine; and the mass ratio of Tencel fiber to cyanoacetic acid is 1:0.1 to 1:1.0. The cyanoethylation method includes: Tencel fibers are activated in an alkaline solution, then acrylonitrile is added and reacted at 20-60°C for 1-8 hours to allow the hydroxyl groups on the Tencel surface to undergo an addition reaction with acrylonitrile, introducing nitrile functional groups onto the fiber surface. After the reaction, the fibers are acid-washed, water-washed, and dried to obtain the second fiber. The method for modifying nitrile-containing silane coupling agents includes: Tencel fibers are dispersed in a water / alcohol mixture, and a nitrile-containing silane coupling agent is added. The mixture is reacted at 20–80°C for 1–12 hours to allow the hydroxyl groups on the surface of the Tencel fibers to undergo a hydrolysis-condensation reaction with the silane coupling agent, thereby introducing nitrile-containing functional groups onto the fiber surface. After the reaction, the fibers are washed and dried to obtain the second fiber. The nitrile-containing silane coupling agent is selected from one or more of 3-cyanopropyltriethoxysilane and 3-cyanopropyltrimethoxysilane.
[0018] Thirdly, the present invention provides a composite solid electrolyte membrane, comprising the functionalized fiber composite skeleton material as described in any one of the first aspects, and a composite solid electrolyte slurry filling the pores of the skeleton material, wherein the composite solid electrolyte slurry comprises an inorganic lithium-ion conductor, a polymer binder, and a lithium salt. The composite solid electrolyte membrane is prepared by the following method: after vacuum drying of the skeleton material, it is immersed in the composite solid electrolyte slurry and immersed for 5 to 60 minutes under vacuum conditions of -0.05 to -0.1 MPa. After removal, excess slurry on the surface is scraped off, and the membrane is obtained by drying, rolling, hot pressing and vacuum solvent removal treatment.
[0019] Furthermore, the inorganic lithium-ion conductor is selected from one or more of LATP, LLZO, LLZTO, LAGP, Li3PS4, and Li6PS5Cl, with a particle size D50 of 50–1000 nm; the polymer binder is selected from one or more of PVDF-HFP, PEO, PAN, PMMA, PVDF, polycarbonate, and polyionic liquid; and the lithium salt is selected from one or more of LiTFSI, LiFSI, LiPF6, LiBOB, and LiDFOB. Based on the mass of solid components, the content of inorganic lithium-ion conductors is 30%–90%, the content of polymer binders is 5%–50%, and the content of lithium salts is 1%–30%.
[0020] Beneficial effects
[0021] The functionalized fiber composite skeleton material, the preparation method of the functionalized fiber composite skeleton material, and the composite solid electrolyte membrane containing the composite skeleton material provided by the present invention, by mixing modified PET fibers (PET-COOLi) with lithium carboxylate groups on the surface and modified Tencel fibers (Tencel-CN) with nitrile groups on the surface at a specific mass ratio (5:95 to 60:40), a porous skeleton material with interwoven fibers is formed, achieving the following synergistic beneficial effects: First, the fixed carboxylate anions in PET-COOLi fiber can effectively bind anion migration and increase lithium ion migration number. At the same time, its high modulus ensures that the skeleton material still has excellent mechanical strength and dimensional stability under high porosity (60%~85%), meeting the requirements of continuous winding processing.
[0022] Secondly, the nitrile groups on the surface of Tencel-CN fibers have high dipole moments, enabling them to react with Li. + Reversible coordination occurs, providing a continuous hopping transport channel for lithium ions and reducing the migration activation energy; at the same time, the nitrile group improves the wettability of the framework material to the electrolyte slurry and reduces interface defects.
[0023] Third, the two types of fibers form a heterogeneous coordination network in the cross-contact region, consisting of carboxyl group sites, nitrile group sites, and subsequent inorganic electrolyte surface sites, enabling Li... + It can migrate efficiently between different sites, reduce interfacial impedance, and improve the overall ionic conductivity of the composite electrolyte.
[0024] In summary, this solution simultaneously addresses the challenges of poor interfacial compatibility, the contradiction between porosity and strength, and low ion transport efficiency in existing technologies, achieving synergistic optimization of mechanical support and ion transport functions. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0026] Figure 1 A schematic flowchart illustrating a method for preparing a functionalized fiber composite skeleton material according to an embodiment of the present invention; Figure 2 PET modification reaction diagram provided for embodiments of the present invention; Figure 3 A schematic diagram of the modification reaction of Tencel fibers provided for embodiments of the present invention; Figure 4 A schematic diagram of the microstructure of porous framework materials and the heterogeneous ion hopping conduction mechanism provided for embodiments of the present invention; Figure 5 The modified PET XPS full spectrum provided in Example 1 of this invention; Figure 6 The infrared spectra of PET and Tencel blend before and after modification provided in Example 1 of the present invention; Figure 7 This is a SEM cross-sectional view of the composite solid electrolyte filling framework material provided in Embodiment 1 of the present invention; Figure 8 This is a SEM surface image of the composite solid electrolyte filling skeleton material provided in Embodiment 1 of the present invention. Detailed Implementation
[0027] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0028] In this invention, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.
[0029] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are feasible for those skilled in the art. If the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.
[0030] This invention employs two types of fibers with different compositions, properties, and functional orientations as building blocks of the skeletal material, and performs different surface functional modifications on each to achieve clear functional division and synergistic effects in the final composite film. One type of fiber is PET fiber. PET fiber has high modulus, high tensile strength, and good dimensional stability, making it suitable as the main load-bearing and supporting phase in the composite skeletal material. By performing surface hydrolysis and lithium salting treatment on PET fiber, lithium carboxylate groups are formed on its surface, resulting in surface lithium carboxylate-modified PET fiber, denoted as PET-COOLi. In addition to providing the main mechanical support, the fixed carboxylate sites on its surface can also serve as binding / release sites for lithium ions and, to some extent, reduce the migration contribution of anions, thereby improving the lithium ion transference number in the composite electrolyte system. The other type of fiber is Tencel fiber. Tencel fiber belongs to the cellulose-based regenerated fiber family and contains many hydroxyl groups on its surface, exhibiting good hydrophilicity, liquid absorption, and chemical modification capabilities. Acrylonitrile groups were introduced onto the surface of Tencel fibers through esterification, etherification, cyanoethylation, and silane coupling to obtain surface-acrylonitrified Tencel fibers, denoted as Tencel-CN. The acrylonitrile groups possess high dipole moments and can react with Li... + Reversible coordination occurs, providing continuous migration sites for lithium ions and improving the wettability of the framework material to the solid electrolyte slurry and the continuity of ion transport. This invention creates a porous framework material by blending PET-COOLi fibers and Tencel-CN fibers in a certain proportion, allowing the two types of fibers to be interleaved within the membrane. This forms a heterogeneous coordination network in the fiber cross-contact areas, composed of lithium carboxylate sites, nitrile sites, and inorganic electrolyte surface sites from the subsequently filled electrolyte. Li +Reversible coordination and discoordination can occur between different coordination sites, thereby constructing continuous lithium-ion transport channels across fibers and interfaces. Compared with single-functional fiber frameworks or unmodified hybrid frameworks, this bicomponent functionalized framework material can simultaneously achieve mechanical strength, porosity, electrolyte wettability, interfacial compatibility, and lithium-ion migration efficiency.
[0031] To better understand the above technical solution, a detailed explanation of the technical solution is provided below with reference to the accompanying drawings.
[0032] This invention provides a functionalized fiber composite skeleton material, comprising: The first fiber is a modified PET fiber with lithium carboxylate groups on its surface; The second fiber is a modified Tencel fiber with a nitrile group on its surface; The first fiber and the second fiber are interwoven within the skeleton material to form a porous structure; The mass ratio of the first fiber to the second fiber is 5:95 to 60:40.
[0033] The functionalized fiber composite skeleton material provided in this invention includes a first fiber and a second fiber. The first fiber is a modified PET fiber with lithium carboxylate groups on its surface (hereinafter referred to as "first fiber" or "PET-COOLi fiber"), and the second fiber is a modified Tencel fiber with nitrile groups on its surface (hereinafter referred to as "second fiber" or "Tencel-CN fiber"). The first fiber and the second fiber are interleaved within the skeleton material to form a three-dimensional porous structure. Furthermore, the mass ratio of the first fiber to the second fiber is 5:95 to 60:40.
[0034] Within this mass ratio range, the first fiber acts as the mechanically supporting phase, endowing the framework material with good mechanical strength and dimensional stability; the second fiber acts as the ion transport phase, providing continuous nitrile group coordination sites, improving electrolyte wettability and ion conductivity. The staggered distribution of the two types of fibers at the microscale results in the formation of a heterogeneous coordination network in the fiber cross-contact region, composed of lithium carboxylate sites, nitrile group sites, and inorganic particle surface sites subsequently filled in the electrolyte, thereby significantly improving lithium-ion transference number and interfacial ion transport efficiency.
[0035] In a preferred embodiment of the present invention, the mass ratio of the first fiber to the second fiber is 20:80 to 40:60, more preferably 30:70. This preferred ratio can maximize the coordination continuity of nitrile sites while ensuring sufficient mechanical strength of the skeleton material, thereby achieving the best balance between mechanical and electrochemical properties.
[0036] To further optimize the molding process and performance of the skeleton material, this embodiment also optimizes the fiber length and diameter. Specifically, the length of the first fiber is 0.5–8 mm, preferably 1–5 mm; the diameter is 5–20 μm, preferably 8–18 μm. The length of the second fiber is 0.5–6 mm, preferably 1–3 mm; the diameter is 5–20 μm, preferably 5–15 μm. Within this size range, the fibers are easily and uniformly suspended in the dispersion medium, forming a uniform porous network during wet papermaking, and the fiber intersections are firmly bonded after hot pressing, resulting in excellent overall mechanical properties of the skeleton material.
[0037] Accordingly, the thickness of the skeleton material is 20–100 μm, preferably 30–60 μm; the porosity is 60%–85%, preferably 70%–80%. This range of thickness and porosity allows the skeleton material to accommodate sufficient solid electrolyte slurry to ensure ionic conductivity, while maintaining sufficient mechanical strength to resist stress during battery assembly and use.
[0038] For applications requiring extremely thin framework materials (such as portable electronic devices or high volumetric energy density batteries), this invention also provides an embodiment using microfibers. In this embodiment, the diameter of both the first and second fibers is 0.2–5 μm, and the length is 0.1–2 mm, thereby further reducing the thickness of the framework material to 5–20 μm. By employing microfibers of PET and Tencel, it is possible to maintain a high porosity (typically still above 60%) while controlling the film thickness within an ultra-thin range. Furthermore, due to the reduced fiber diameter, the number of contact points between fibers increases, improving the uniformity and flexibility of the framework material.
[0039] To further improve the interlayer bonding strength, anti-dust properties, and subsequent winding processing performance of the skeleton material, the composite skeleton material of the present invention may further include a bonding reinforcement component. The bonding reinforcement component is selected from one or more of low-melting-point polyester fibers, polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyethylene oxide (PEO), lithium polyacrylate, polyurethane, nanocellulose, and aramid nanofibers. These bonding reinforcement components can be uniformly dispersed in the fiber suspension, partially melt or self-adhere during hot pressing, fixing adjacent fibers together, thereby improving the overall strength and anti-delamination ability of the skeleton material without significantly reducing porosity. The amount of the bonding reinforcement component added is 0.5% to 10% of the total mass of the first and second fibers. If the amount added is too low, the reinforcement effect is not obvious; if the amount added is too high, it may clog the pores and reduce ion transport performance.
[0040] To further optimize the compatibility between the framework material and the positive and negative electrode interfaces, this invention also provides a composite framework material with an asymmetric layered structure. This structure includes a first layer near the negative electrode side, an intermediate layer, and a second layer near the positive electrode side. Specifically, the first layer near the negative electrode side is a first fiber (PET-COOLi fiber) enriched layer, meaning that the mass percentage of the first fiber in this layer is significantly higher than that of the second fiber, for example, the first fiber percentage is ≥70%. The intermediate layer is a mixed layer of the first and second fibers, and their ratio can be consistent with the overall mass ratio or adjusted as needed. The second layer near the positive electrode side is a second fiber (Tencel-CN fiber) enriched layer, meaning that the mass percentage of the second fiber in this layer is significantly higher than that of the first fiber.
[0041] The technical benefits of this asymmetric structure are multifaceted: the first fiber-enriched layer on the negative electrode side exhibits higher mechanical strength and dimensional stability, effectively resisting lithium dendrite penetration and reducing the risk of short circuits; the second fiber-enriched layer on the positive electrode side is rich in nitrile groups, providing excellent wettability to polar electrolyte slurries, and exhibiting fewer side reactions between nitrile groups and positive electrode materials (such as high-voltage ternary materials), which is conducive to forming a stable positive electrode / electrolyte interface; the intermediate mixed layer serves as a transition region, ensuring continuous lithium-ion transport from the negative electrode side to the positive electrode side and avoiding increased interfacial impedance due to abrupt changes in composition. Furthermore, the asymmetric structure allows for customized design by adjusting the thickness and fiber ratio of each layer according to the specific battery system (such as lithium metal anode, graphite anode, or different positive electrode materials).
[0042] Please see Figure 1 The present invention also provides a method for preparing a functionalized fiber composite skeleton material, used to prepare the functionalized fiber composite skeleton material as described in any of the preceding embodiments, such as... Figure 1 As shown, the method includes: Step S10: Provide modified PET fibers with lithium carboxylate groups on the surface, i.e., the first fiber; Step S20: Provide modified Tencel fibers with acrylonitrile groups on the surface, i.e., the second fiber; Step S30: The obtained first fiber and second fiber are mixed at a mass ratio of 5:95 to 60:40 and dispersed in a dispersion medium to form a uniform fiber suspension; Step S40: The obtained fiber suspension is processed into a wet membrane using wet papermaking, vacuum filtration, or filtration molding methods; Step S50: The wet film is dried and hot-pressed to obtain the functionalized fiber composite skeleton material.
[0043] The functionalized fiber composite skeleton material of this invention can be prepared using a wet papermaking process, specifically including the following steps: preparing a first fiber and a second fiber separately; mixing the two fibers at a predetermined mass ratio, dispersing them in water or a water / alcohol mixture, and adding an appropriate amount of dispersant (such as Triton X-100, sodium dodecyl sulfate, etc., the amount added being 0.001% to 0.1% of the total fiber mass) to form a uniform fiber suspension; forming a wet film from the suspension using methods such as wet papermaking, vacuum filtration, or filtration molding; subsequently drying at 60–120°C, and then hot-pressing at 80–180°C and 0.5–5 MPa pressure for 0.5–10 minutes to obtain the skeleton material. When it is necessary to prepare an asymmetric layered structure, a layered layup or continuous layered papermaking method can be used to sequentially form a first fiber-enriched layer, a mixed layer, and a second fiber-enriched layer, and then hot-pressing the whole structure for shaping.
[0044] The first fiber (PET-COOLi fiber) is a functionalized fiber obtained by controlled surface hydrolysis of PET fibers followed by lithium salt treatment. The PET fibers are preferably chopped fibers with a length of 0.5–8 mm, more preferably 1–5 mm; the fiber diameter is 5–20 μm, more preferably 8–18 μm. The preparation process and reaction diagram are shown below. Figure 2 As shown, the reaction process is as follows: Alkali treatment generates carboxylates and hydroxyl groups on the PET surface; acidification converts the carboxylates to hydroxyl groups; and lithium salting converts the surface carboxyl groups to lithium carboxylates. The preparation process specifically includes: 1. Surface hydrolysis treatment PET fibers are immersed in an alkaline aqueous solution for controlled surface hydrolysis. The alkaline solution is preferably a NaOH aqueous solution with a concentration of 0.05–1.0 mol / L, more preferably 0.1–0.5 mol / L. The treatment temperature is 40–90℃, more preferably 50–70℃; the treatment time is 5–60 min, more preferably 10–40 min.
[0045] After the above treatment, some ester bonds on the surface of the PET fiber are hydrolyzed, generating polar groups such as carboxylates and hydroxyl groups on the surface, thus providing reaction sites for subsequent lithium salting treatment.
[0046] 2. Acidification treatment
[0047] To improve the effective conversion rate of surface carboxyl groups, acidification treatment is preferably performed after alkali treatment. Specifically, the hydrolyzed PET fibers can be washed with deionized water and then immersed in an acid solution of 0.01–0.1 mol / L for 5–30 min. The acid solution can be selected from one or more of hydrochloric acid, acetic acid, and citric acid. This step can convert the carboxylates on the PET surface into carboxyl groups, improving the uniformity and effectiveness of subsequent lithium salting treatment. After acidification, the fibers are washed until neutral.
[0048] 3. Lithium salting treatment
[0049] PET fibers, after surface hydrolysis and optional acidification, are immersed in a lithium-containing compound solution for lithium salting treatment. The lithium-containing compound can be selected from one or more of LiOH, Li₂CO₃, lithium acetate, and LiTFSI. The concentration of the lithium salting solution can be 0.05–1.0 mol / L, preferably 0.1–0.8 mol / L; the treatment temperature can be 30–90℃, preferably 50–70℃; and the treatment time can be 0.5–8 h, preferably 1–4 h.
[0050] After lithium salt treatment, the carboxyl groups on the surface of PET fibers are converted into lithium carboxylate groups, resulting in PET-COOLi fibers. The weight gain of the obtained PET-COOLi fibers can be 1% to 10%, preferably 2% to 8%.
[0051] This method only modifies the fiber surface at the nanoscale without destroying the internal crystalline structure of the fiber, thus preserving the high modulus properties of PET fiber.
[0052] It should be noted that the functionalization of the PET surface in this invention is essentially a "surface hydrolysis-lithiation" modification, and is not limited to the narrow sense of molecular grafting reaction; any technical solution that forms fixed lithium carboxylate sites on the PET surface through chemical treatment should be regarded as an equivalent alternative to this invention.
[0053] The second fiber (Tencel-CN fiber) is a functionalized fiber obtained by introducing nitrile groups onto the surface of Tencel fibers. The Tencel fibers are preferably chopped fibers with a length of 0.5–6 mm, more preferably 1–3 mm; the fiber diameter is 5–20 μm. Before use, it is preferable to vacuum dry to remove adsorbed moisture and prevent subsequent reactions from becoming damp. It can be prepared by any of the following methods.
[0054] 1. Introducing nitrile groups via esterification
[0055] In a preferred embodiment, the surface of Tencel fibers is modified using a cyanoacetic acid esterification method. The reaction process is as follows: Figure 3As shown, Tencel fibers and cyanoacetic acid undergo a dehydration condensation reaction in a polar aprotic solvent with the aid of a dehydration condensing agent and a catalyst to produce Tencel-CN fibers and urea derivatives.
[0056] Specifically, dried Tencel chopped fibers are dispersed in a polar aprotic solvent, which may be selected from one or more of DMF, DMSO, DMAc, and NMP; cyanoacetic acid, a dehydrating condensing agent, and a catalyst are added, and the reaction is carried out under an inert atmosphere. The dehydrating condensing agent may be selected from one or more of DCC, DIC, EDC, and CDI; the catalyst may be selected from one or more of DMAP, pyridine, and triethylamine. The reaction temperature may be 40–90°C, preferably 60–80°C; the reaction time may be 4–24 h, preferably 6–12 h.
[0057] During this reaction, the hydroxyl groups on the surface of Tencel fibers undergo esterification with cyanoacetic acid, forming a functional layer containing the —OCO—CH2—CN structure on the fiber surface. After the reaction, the fibers are washed sequentially with DMF, ethanol, and deionized water to remove unreacted reagents, catalysts, and byproducts. Subsequently, the fibers are vacuum dried at 50–80 °C to obtain Tencel-CN fibers.
[0058] Preferably, the mass ratio of Tencel fiber to cyanoacetic acid is 1:0.1 to 1:1.0, more preferably 1:0.3 to 1:0.6. The weight gain of the resulting Tencel-CN fiber is preferably 3% to 20%, more preferably 5% to 15%.
[0059] 2. Introducing nitrile groups via cyanoethylation
[0060] In another embodiment, cyanoethylation can be used to introduce nitrile groups. First, the Tencel fibers are activated in an alkaline solution, such as NaOH, KOH, or tetrabutylammonium hydroxide solution. Then, acrylonitrile is added, and the reaction is carried out at 20–60°C for 1–8 hours, causing the hydroxyl groups on the Tencel surface to undergo an addition reaction with acrylonitrile, forming a functional layer containing a —O—CH2—CH2—CN structure on the fiber surface. After the reaction, the fibers are acid-washed, water-washed, and dried to obtain Tencel-CN fibers.
[0061] 3. Modification method using nitrile-containing silane coupling agents
[0062] In another embodiment, the surface of Tencel fibers can be modified using a nitrile-containing silane coupling agent. The nitrile-containing silane coupling agent can be selected from 3-cyanopropyltriethoxysilane, 3-cyanopropyltrimethoxysilane, etc. This reaction can be carried out in a water / alcohol mixture at a temperature of 20–80°C for 1–12 hours. After washing and drying, Tencel-CN fibers with nitrile groups on the surface can also be obtained.
[0063] All three methods can stably introduce nitrile groups into the surface of Tencel fibers, and the reaction conditions are mild, without damaging the fiber's intrinsic strength. The weight gain of the resulting Tencel-CN fibers is generally controlled between 3% and 20%, preferably between 5% and 15%, to ensure sufficient nitrile group density while avoiding excessive reaction that could lead to fiber embrittlement.
[0064] It should be noted that the above-mentioned nitrile group introduction method is only a preferred embodiment. The present invention is not limited to the specific reaction types listed. Any method that can stably introduce nitrile groups or strongly polar groups with similar lithium ion coordination functions on the surface of Tencel fibers can be used as an alternative to the present invention.
[0065] The Tencel-CN fibers and PET-COOLi fibers prepared above are mixed and dispersed in a dispersion medium at a predetermined mass ratio to form a uniform fiber suspension. The dispersion medium can be water, or a mixture of water / ethanol, water / isopropanol, etc. The dispersant can be selected from one or more of Triton X-100, sodium dodecyl sulfate, polyvinylpyrrolidone, and sodium carboxymethyl cellulose, and its addition amount is preferably 0.001% to 0.1%.
[0066] Preferably, the mass ratio of Tencel-CN to PET-COOLi is 5:95 to 60:40, more preferably 20:80 to 40:60, and even more preferably 30:70. During the mixing process, high-speed stirring, ultrasonic dispersion, mechanical dispersion, or other methods can be used to ensure that the two types of fibers are evenly distributed in the suspension.
[0067] To improve the interlayer bonding strength, anti-dust properties, and subsequent winding processing performance of the skeleton material, a bonding reinforcement component can be further added. The bonding reinforcement component can be selected from one or more of low-melting-point polyester fibers, PVDF-HFP, PEO, lithium polyacrylate, polyurethane, nanocellulose, and aramid nanofibers, and its addition amount is preferably 0.5% to 10% of the total fiber mass.
[0068] The above-mentioned uniform suspension is processed into a wet film using wet papermaking, vacuum filtration, filtration molding, or a similar papermaking process. This film is then dried and hot-pressed to obtain a two-component functionalized fiber skeleton material. The preferred drying temperature is 60–120℃; the preferred hot-pressing temperature is 80–180℃; the preferred hot-pressing pressure is 0.5–5 MPa; and the preferred hot-pressing time is 0.5–10 min.
[0069] The thickness of the obtained skeleton material can be 20–100 μm, preferably 30–60 μm; the porosity can be 60%–85%, preferably 70%–80%.
[0070] When thinner skeleton materials are required, micronized PET fibers and micronized Tencel fibers can be used. Conventional fibers can be obtained with the target diameter and length through mechanical grinding or chemical treatment; at this time, the fiber diameter is preferably 0.2-5 μm, the fiber length is preferably 0.1-2 mm, and the corresponding skeleton material thickness can be further reduced to 5-20 μm.
[0071] To further optimize the electrode interface, the framework material can be designed as an asymmetric layered structure.
[0072] In one implementation, a three-layer structure is adopted: 1. The side near the negative electrode is a PET-COOLi enrichment layer; 2. The middle layer is a PET-COOLi / Tencel-CN hybrid layer; 3. The side near the positive electrode is a Tencel-CN enriched layer.
[0073] Among them, the PET-COOLi enriched layer has high mechanical strength and dimensional stability, which can reduce the risk of dendrite puncture on the negative electrode side; the Tencel-CN enriched layer has good hydrophilicity and ion transport capability, which is beneficial to improve electrolyte wetting and interfacial contact on the positive electrode side; the intermediate mixed layer is used to construct a continuous cross-fiber synergistic ion transport network.
[0074] In another embodiment, the Tencel-CN enrichment layer can be disposed on the negative electrode side and the PET-COOLi enrichment layer can be disposed on the positive electrode side (depending on the selected inorganic electrolyte, electrode type and interface stability requirements).
[0075] When LATP is used as an inorganic electrolyte and applied to a lithium metal anode, it is preferable to further provide an LLZO, polymer electrolyte, LiF, Al2O3, Li3PO4 or other interfacial protective layer on the anode side to reduce interfacial side reactions caused by direct contact between LATP and lithium metal.
[0076] The working principle and synergistic mechanism of the bicomponent functionalized fiber skeleton material of the present invention are as follows: By synergistically designing a "mechanically supporting phase" and an "ion transport phase," simultaneous optimization of mechanical and electrochemical properties is achieved. The microstructure of porous framework materials and the heterogeneous ion hopping conduction mechanism are as follows... Figure 4 As shown.
[0077] Among them, PET-COOLi fiber, as the main load-bearing phase, relies on the high modulus and dimensional stability of PET itself to maintain the overall structural integrity and processing strength of the skeleton material even under high porosity conditions. The fixed carboxylate anion sites in the lithium carboxylate groups on the PET surface can serve as reversible binding / release sites for lithium ions and help reduce the migration contribution of anions in the system, thereby improving the lithium ion transference number.
[0078] Tencel-CN fibers possess both good hydrophilicity and ion transport assist functions. The nitrile groups on their surface have high dipole moments, allowing them to react with Li. + Reversible coordination occurs, resulting in Li + It provides continuous coordination migration sites and enhances the adsorption and wetting ability of the framework material for electrolyte slurry.
[0079] In the cross-contact region between the two types of fibers, the lithium carboxylate sites on the PET-COOLi surface, the nitrile sites on the Tencel-CN surface, and the oxygen-containing sites on the surface of the subsequently filled inorganic electrolyte particles can collectively form a heterogeneous coordination interface. + Reversible coordination / decoupling migration can occur between carboxylate groups, nitrile groups, and inorganic electrolyte surface sites, thereby forming continuous ion transport pathways across fibers and interfaces, reducing interfacial impedance, and improving the overall ion transport efficiency of the composite membrane.
[0080] When the Tencel-CN content is too low, there are insufficient nitrile sites, resulting in inadequate continuity of the ion coordination network. When the Tencel-CN content is too high, the proportion of the PET load-bearing skeleton decreases, potentially affecting the tensile strength and dimensional stability of the skeleton material. Therefore, considering porosity, mechanical properties, electrolyte wettability, and ion transport performance, the mass ratio of Tencel-CN to PET-COOLi is preferably controlled between 20:80 and 40:60, more preferably 30:70.
[0081] The present invention also provides a composite solid electrolyte membrane, comprising a functionalized fiber composite skeleton material as described in any of the preceding claims, and a composite solid electrolyte slurry filling the pores of the skeleton material, wherein the composite solid electrolyte slurry comprises an inorganic lithium-ion conductor, a polymer binder, and a lithium salt. The composite solid electrolyte membrane is prepared by the following method: after vacuum drying of the skeleton material, it is immersed in the composite solid electrolyte slurry and immersed for 5 to 60 minutes under vacuum conditions of -0.05 to -0.1 MPa. After removal, excess slurry on the surface is scraped off, and the membrane is obtained by drying, rolling, hot pressing and vacuum solvent removal treatment.
[0082] A composite solid electrolyte membrane can be prepared by impregnating the prepared functionalized fiber composite skeleton material with a composite solid electrolyte slurry. Specifically, an inorganic lithium-ion conductor, a polymer binder, a lithium salt, and an organic solvent are mixed to prepare the composite solid electrolyte slurry. The inorganic lithium-ion conductor can be selected from one or more of LATP, LLZO, LLZTO, LAGP, Li3PS4, and Li6PS5Cl; the particle size of the inorganic conductor is preferably 50-1000 nm, and more preferably 200-500 nm.
[0083] The polymer binder may be selected from one or more of PVDF-HFP, PEO, PAN, PMMA, PVDF, polycarbonate, and polyionic liquid; the lithium salt may be selected from one or more of LiTFSI, LiFSI, LiPF6, LiBOB, and LiDFOB; and the solvent may be selected from one or more of acetonitrile, NMP, DMF, DMSO, THF, and acetone.
[0084] Based on the mass of solid components, the content of inorganic lithium-ion conductor can be 30% to 90%, preferably 70% to 90%; the content of polymer binder can be 5% to 50%, preferably 5% to 15%; and the content of lithium salt can be 1% to 30%.
[0085] The prepared functionalized fiber skeleton material is pre-dried under vacuum at 80–120°C to remove residual moisture and volatiles from the membrane. Then, the skeleton material is immersed in the aforementioned composite electrolyte slurry under a vacuum of -0.05–-0.1 MPa for 5–60 min, preferably 15–30 min; this process can be repeated 1–5 times to improve the uniformity and density of the slurry filling the pores of the skeleton material. After immersion, excess slurry is scraped off the surface, followed by drying, rolling, hot pressing, and vacuum solvent removal treatment to obtain the fiber-reinforced composite solid electrolyte membrane.
[0086] In a preferred embodiment, LATP nanopowder, PVDF-HFP, or PEO can be used as the binder phase, and NMP or acetonitrile can be used as the solvent to prepare the slurry.
[0087] In another implementation, LLZO or LLZTO can be used instead of LATP to improve its compatibility with the lithium metal anode interface.
[0088] The present invention provides a two-component functional fiber composite skeleton material and a composite solid electrolyte membrane, which achieve synergistic optimization of mechanical support and ion transport functions by blending PET-COOLi fiber with fixed anion sites and Tencel-CN fiber with nitrile coordination sites in a specific ratio.
[0089] 1. By differentiating and synergistically combining two types of functional fibers, PET-COOLi and Tencel-CN, an effective division of labor between mechanical support and ion transport functions was achieved.
[0090] 2. Under conditions of high porosity, the skeleton material can still maintain good structural integrity and processing adaptability, which is beneficial for subsequent winding, lamination and battery assembly.
[0091] 3. The nitrile sites on the surface of Tencel fibers, the lithium carboxylate sites on the surface of PET, and the inorganic electrolyte sites together construct a heterogeneous coordination network, which is beneficial to improving lithium-ion transport efficiency and reducing interfacial impedance.
[0092] 4. The fixed anion sites on the PET surface help reduce the contribution of anion migration, thereby improving the lithium ion transference number.
[0093] The preparation process of this invention has good scalability, and is applicable to both wet-process papermaking of fiber membranes and subsequent composite filling of various inorganic / polymer electrolyte systems.
[0094] The present invention will be further described in detail below through specific embodiments. These embodiments are for illustrative purposes only and do not constitute a limitation on the scope of protection of the present invention. Any equivalent substitutions or modifications made based on the concept of the present invention shall fall within the scope of protection of the present invention.
[0095] In the following examples, the PET and Tencel fibers used were commercially available chopped strands, which were vacuum-dried at 80°C for 12 hours before use. All chemical reagents used were of analytical grade.
[0096] Example 1: Basic ratio of skeleton material (PET-COOLi:Tencel-CN=30:70, modified by esterification)
[0097] 1.1 Preparation of Tencel-CN fibers (esterification method)
[0098] 10 g of dried Tencel chopped fibers (1.5 mm in length and 12 μm in diameter) were dispersed in 200 mL of DMF. 5 g of cyanoacetic acid, 8 g of DCC, and 0.5 g of DMAP were added sequentially. The reaction was carried out under nitrogen protection at 75 °C with stirring for 10 hours. After the reaction, the fibers were washed three times each with DMF, anhydrous ethanol, and deionized water, and then vacuum-dried at 60 °C for 12 hours to obtain Tencel-CN fibers. The weight gain was calculated to be 9.2%. Infrared spectroscopy was observed at 2252 cm⁻¹. - The presence of a -C≡N characteristic absorption peak at position ¹ indicates that the nitrile group has been successfully grafted.
[0099] 1.2 Preparation of PET-COOLi Fibers
[0100] 10 g of chopped PET fibers (3 mm in length, 15 μm in diameter) were immersed in 200 mL of 0.2 mol / L NaOH aqueous solution and treated at 65 °C for 25 minutes. After removal, the fibers were washed with deionized water until neutral, then immersed in 0.05 mol / L hydrochloric acid solution for 15 minutes and washed until neutral. The fibers were then immersed in 0.4 mol / L LiOH aqueous solution and reacted at 60 °C for 2.5 hours. After the reaction, the fibers were washed and dried to obtain PET-COOLi fibers with a weight gain of 5.1%.
[0101] Figure 5 The XPS full spectrum of modified PET is shown, displaying the complete X-ray photoelectron spectroscopy (XPS) spectrum of the modified PET surface. The modified PET fiber surface possesses lithium carboxylate groups (-COOLi), and the XPS full spectrum can be used to verify the presence and chemical state of lithium. Analysis of the characteristic peaks in the figure reveals: the O 1s peak indicates the presence of oxygen on the sample surface, possibly in the form of carboxylate or hydroxyl groups; the C 1s peak indicates the presence of carbon on the sample surface, mainly from the carbon skeleton of PET; the appearance of the Li 1s peak directly confirms the presence of lithium on the sample surface, with a lithium content of 4.1 at%, consistent with the presence of lithium carboxylate groups.
[0102] 1.3 Preparation of framework materials
[0103] Tencel-CN fiber and PET-COOLi fiber were mixed at a mass ratio of 30:70, with a total mass of 5 g. The mixed fibers were dispersed in 1 L of deionized water, and 0.005 g of Triton X-100 was added. The mixture was stirred at high speed for 30 minutes to form a homogeneous suspension. Vacuum filtration was used to form the film. The suspension was poured into a Buchner funnel (filter paper pore size 10 μm) and filtered until no obvious water layer was visible on the surface, yielding a wet film. The wet film was dried in a 100℃ forced-air drying oven for 2 hours, and then placed in a hot press and hot-pressed at 160℃ and 1 MPa for 3 minutes to obtain a bicomponent functionalized fiber composite skeleton material.
[0104] Figure 6 The figures show the infrared spectra of PET / Tencel blends before and after modification. The red curve represents the modified PET / Tencel blend sample (sample A), and the black curve represents the unmodified PET / Tencel blend sample (sample B).
[0105] Characteristic peak analysis: 3350cm -1 The -OH stretching vibration peak, mainly originating from Tencel fibers, indicates the presence of hydroxyl groups on the surface of Tencel fibers; 2252 cm⁻¹ -1 The C≡N stretching vibration peak appeared only in the modified sample, indicating that nitrile groups were successfully introduced onto the surface of the modified Tencel fiber; 1715 cm⁻¹ -1The C=O stretching vibration peak originates from the carbonyl group in PET, indicating the presence of PET; 1585 cm⁻¹ -1 and 1390cm -1 COO - The asymmetric stretching vibration peaks were more pronounced in the modified samples, indicating that carboxylate groups were successfully introduced onto the surface of the modified PET fibers.
[0106] By comparing the infrared spectra of the samples before and after modification, it can be confirmed that the modification treatment successfully introduced the target functional groups into the surface of PET and Tencel fibers.
[0107] 1.4 Performance Testing
[0108] The framework material prepared in this embodiment has a thickness of 48 μm, a porosity of 76%, and a tensile strength of 23.5 MPa. After vacuum drying the framework material at 100℃ for 12 hours, it was immersed in a composite solid electrolyte slurry (LATP nanopowder D50=300 nm 70 wt%, PVDF-HFP 15 wt%, LiTFSI 15 wt%, solvent NMP) under a vacuum of -0.09 MPa for 30 minutes. Excess slurry was scraped off, and the material was dried at 80℃. It was then rolled, hot-pressed at 120℃ for 5 minutes, and vacuum-removed to obtain the composite solid electrolyte membrane. Its room temperature ionic conductivity was measured to be 1.26 × 10⁻⁶. -4 The lithium-ion transference number (LTM) is 0.65, and the interfacial impedance (with lithium metal) is 78 Ω·cm². The assembled LiFePO4|Li solid-state battery retained 91.3% of its capacity after 200 cycles at 0.5C and 60℃.
[0109] Cross-sectional view of composite solid electrolyte filled skeleton material as shown in Figure Figure 7 As shown, during the preparation process, the two-component functionalized fibers (modified PET and modified Tencel) form a three-dimensional porous network through a specific method. The two types of fibers are interleaved and distributed, and the electrolyte fills these pores, forming a layered or similar structure, which affects the ionic conductivity, mechanical strength, and contact area between the electrolyte and the electrode of the membrane, thereby affecting the overall performance of the battery.
[0110] Figure 8 The SEM image shows the surface morphology of the composite solid-state electrolyte filling framework material. The surface exhibits a network structure composed of numerous interwoven fine fibers with abundant pores between them. This network structure provides excellent ion transport channels and electrolyte wettability, facilitating rapid lithium-ion movement and uniform electrolyte distribution. Simultaneously, the high porosity also helps increase the specific surface area of the membrane, expanding the contact area between the electrolyte and the electrode, thereby improving battery performance.
[0111] Example 2: Preferred ratio and microfiber thin skeleton material (PET-COOLi:Tencel-CN=40:60, microfiber)
[0112] 2.1 Preparation of microfibers
[0113] Conventional PET fibers and Tencel fibers were mechanically ground and acid-hydrolyzed to obtain micronized fibers: PET-COOLi fibers had a diameter of 0.5~1.5 μm and a length of 0.3~0.8 mm; Tencel-CN fibers had a diameter of 0.5~1.5 μm and a length of 0.3~0.8 mm. The modification steps were the same as in Example 1.
[0114] 2.2 Preparation of framework materials
[0115] Micronized Tencel-CN fibers and micronized PET-COOLi fibers were mixed at a mass ratio of 40:60, with a total mass of 3g. The mixture was dispersed in 1.5 L of a water / ethanol mixture (volume ratio 3:1), and 0.003 g of sodium dodecyl sulfate was added. The mixture was ultrasonically dispersed for 15 minutes. The film was formed using a wet papermaking machine, dried at 80℃, and then hot-pressed at 140℃ and 0.8 MPa for 2 minutes to obtain a thin skeleton material.
[0116] 2.3 Performance Testing
[0117] In this embodiment, the skeleton material has a thickness of only 11 μm, a porosity of 72%, and a tensile strength of 18.2 MPa. The composite solid electrolyte membrane (slurry is the same as in Example 1, but LLZO nanopowder is used to replace part of the LATP, LATP:LLZO = 1:1) has a room temperature ionic conductivity of 1.08 × 10⁻⁶. -4 The film exhibits a capacitance of S / cm, a lithium-ion transference number of 0.61, and an interfacial impedance of 85 Ω·cm². This thin film is suitable for high-volume-density pouch cells, maintaining a capacity retention of 87.6% after 300 cycles at 0.5C.
[0118] Example 3: Skeleton material with added adhesive reinforcing components (PET-COOLi:Tencel-CN=25:75, with added low-melting-point polyester fiber)
[0119] 3.1 Fiber Preparation
[0120] Tencel-CN fiber was prepared by cyanoethylation: 10 g of Tencel fiber (5 mm in length, 10 μm in diameter) was activated in 0.5 mol / L NaOH aqueous solution for 30 minutes, then 15 mL of acrylonitrile was added, and the reaction was carried out at 40°C for 4 hours. After the reaction, the fiber was washed successively with 0.1 mol / L hydrochloric acid and deionized water, and dried to obtain Tencel-CN fiber with a weight gain of 7.8%. PET-COOLi fiber was prepared in the same manner as in Example 1.
[0121] 3.2 Preparation of framework materials
[0122] Tencel-CN fiber and PET-COOLi fiber were mixed at a mass ratio of 75:25, and then 3% of low-melting-point polyester fiber (12 μm in diameter, 5 mm in length, and melting point 128℃) was added. Water was used as the dispersion medium, with 0.008% sodium carboxymethyl cellulose added as a dispersant. After vacuum filtration and molding, the mixture was dried at 100℃ and then hot-pressed at 130℃ and 0.6 MPa for 4 minutes.
[0123] 3.3 Performance Testing
[0124] In this embodiment, the skeleton material has a thickness of 52 μm, a porosity of 74%, and a tensile strength of 27.8 MPa (significantly higher than Example 1 without binder). Due to the binder reinforcement, it exhibits excellent anti-dust performance, with no fiber shedding even after repeated winding. The composite solid electrolyte membrane (with PEO replaced in the slurry, content 12 wt%) has an ionic conductivity of 1.15 × 10⁻⁶ at 60°C. -4 S / cm, migration number 0.63. Stable cycling performance, with 92.7% capacity retention after 200 cycles.
[0125] Example 4: Asymmetric layered framework material (PET-COOLi enriched on the negative electrode side, Tencel-CN enriched on the positive electrode side)
[0126] 4.1 Fiber Preparation
[0127] Tencel-CN fiber was prepared using a nitrile-containing silane coupling agent modification method: 10 g of Tencel fiber (5 mm in length, 8 μm in diameter) was dispersed in 200 mL of a water / ethanol (1:1) mixture, 5 mL of 3-cyanopropyltriethoxysilane was added, the pH was adjusted to 4.5 with acetic acid, and the reaction was carried out at 50 °C for 6 hours. After washing and drying, Tencel-CN fiber was obtained with a weight gain of 6.5%. PET-COOLi fiber was prepared in the same manner as in Example 1.
[0128] 4.2 Preparation of Three-Layer Framework Material
[0129] Continuous layered papermaking process is adopted: First layer (negative electrode side): PET-COOLi fiber and a small amount of Tencel-CN fiber are mixed at a ratio of 90:10, 1.5 g is taken and dispersed in water, and the mixture is formed by papermaking, controlling the wet film thickness to be about 20 μm.
[0130] Intermediate layer: Mix PET-COOLi and Tencel-CN at a ratio of 30:70, take 2 g to disperse, and continue to form the film on the first layer, controlling the wet film thickness to be about 25 μm.
[0131] Second layer (positive electrode side): Mix Tencel-CN and PET-COOLi at a ratio of 85:15, take 1.5 g to disperse, and form on the intermediate layer, controlling the wet film thickness to be about 20 μm.
[0132] The entire wet film was dried at 90°C and then hot-pressed at 150°C and 0.8 MPa for 5 minutes to obtain an asymmetric skeleton material with a total thickness of approximately 55 μm.
[0133] 4.3 Performance Testing
[0134] The asymmetric framework material exhibits an overall tensile strength of 24.1 MPa. The negative electrode surface primarily exposes PET-COOLi, exhibiting high hardness and significant resistance to lithium dendrite penetration. The positive electrode surface primarily exposes Tencel-CN, with contact angle testing showing a wetting angle of only 22° for the electrolyte slurry, far lower than conventional PET nonwoven fabrics (approximately 65°). A LiNi0.8Co0.1Mn0.1O2 (NCM811)|Li battery assembled using the composite solid electrolyte membrane (with 5% LLZTO added to the slurry) maintained a capacity retention of 88.9% after 150 cycles at 2.8–4.3 V and 0.5C, compared to only 75.2% for the homogeneous framework material. This indicates that the asymmetric structure effectively suppressed side reactions at the positive electrode interface.
[0135] Example 5
[0136] 5.1 Preparation of Tencel-CN fibers (esterification method, using boundary fiber length)
[0137] Dry Tencel short-cut fibers were selected, with a length of 6 mm (upper limit of claim 2) and a diameter of 18 μm. The following proportions were used: 10 g Tencel fiber, 200 mL DMF, 5 g cyanoacetic acid, 8 g DCC, and 0.5 g DMAP. The mixture was stirred and reacted at 75°C for 10 hours under nitrogen protection. After the reaction, the fibers were washed and dried to obtain Tencel-CN fiber with a weight gain of 8.5%.
[0138] 5.2 Preparation of PET-COOLi fibers (using boundary concentration and boundary fiber length)
[0139] (1) Surface hydrolysis
[0140] Take short-cut PET fibers, selecting those with a length of 0.5 mm (lower limit of claim 2) and a diameter of 20 μm. Immerse 10 g of PET fibers in 200 mL of 0.05 mol / L NaOH aqueous solution (lower limit of claim 9 concentration) and treat at 40 °C (lower limit of claim 9 temperature) for 60 minutes (upper limit of claim 9 time).
[0141] (2) Acidification treatment
[0142] The hydrolyzed fibers are immersed in 0.01 mol / L hydrochloric acid solution (lower concentration of claim 10) for 30 minutes (upper time of claim 10), and then washed until neutral.
[0143] (3) Lithium salting treatment
[0144] The acidified fibers were immersed in a 0.05 mol / L LiOH aqueous solution (the lower limit concentration of claim 9) and reacted at 30°C (the lower limit temperature of claim 9) for 8 hours (the upper limit time of claim 9). After the reaction, the fibers were washed and dried to obtain PET-COOLi fibers with a weight gain of 2.5% (close to the lower limit).
[0145] 5.3 Preparation of framework materials
[0146] Fiber ratio: Mix the above Tencel-CN fiber and PET-COOLi fiber at a mass ratio of 30:70, with a total mass of 5g (i.e., Tencel-CN 1.5g, PET-COOLi 3.5g).
[0147] Bonding reinforcement component: PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene copolymer) is selected as the bonding reinforcement component, and its addition amount is 0.5% of the total mass of the first and second fibers (lower limit of claim 4). PVDF-HFP is pre-dissolved in a small amount of acetone and then mixed with the fiber suspension.
[0148] Dispersion and molding: The mixed fibers and binder were dispersed in 1 L of deionized water, and 0.005 g of Triton X-100 was added. The mixture was stirred at high speed for 30 minutes. Vacuum filtration molding was used to form the film. The wet film was dried at 100℃ for 2 hours, and then hot-pressed at 80℃ (lower limit of hot-pressing temperature) and 0.5 MPa (lower limit of hot-pressing pressure) for 10 minutes (upper limit of hot-pressing time) to obtain a two-component functionalized fiber composite skeleton material.
[0149] 5.4 Performance Testing
[0150] In this embodiment, the skeleton material has a thickness of 52 μm, a porosity of 73%, and a tensile strength of 24.6 MPa (slightly higher than the 23.5 MPa of Example 1 due to the addition of PVDF-HFP). The composite solid electrolyte membrane (slurry same as in Example 1) has a room temperature ionic conductivity of 1.19 × 10⁻⁶. -4 S / cm, lithium-ion transference number 0.64. Assembled LiFePO4|Li batteries, after 200 cycles at 0.5C and 60℃, maintained a capacity retention of 91.8%.
[0151] Comparative Example 1 (simple mixture of unmodified fibers)
[0152] To demonstrate the synergistic effect of the present invention, a comparative example was provided. Unmodified PET fibers (the same raw material PET as in Example 1, without any surface treatment) and unmodified Tencel fibers (raw Tencel, without acrylamide) were mixed at a mass ratio of 30:70, and a skeleton material was prepared using the same wet papermaking and hot-pressing process as in Example 1. This skeleton material had a thickness of 50 μm, a porosity of 73%, and a tensile strength of 16.2 MPa (significantly lower than the 23.5 MPa of Example 1). The room temperature ionic conductivity of the composite solid electrolyte membrane (slurry the same as in Example 1) was only 5.8 × 10⁻⁶. -5 The lithium-ion transference number (LTM) is 0.38, and the interfacial impedance is as high as 156 Ω·cm². The assembled LiFePO4|Li battery exhibits a capacity retention of only 78.3% after 100 cycles at 0.5C, and only 52.6% after 200 cycles. This comparative example demonstrates that unfunctionalized fiber mixtures cannot form an effective heterogeneous coordination network, and their ion transport performance and interfacial stability are significantly inferior to the scheme of this invention.
[0153] Comparing Example 1 and Comparative Example 1, the results show that the tensile strength of Example 1 (23.5 MPa) is significantly higher than that of Comparative Example 1 (16.2 MPa). This is because the lithium carboxylate groups on the PET-COOLi surface generate additional ionic or hydrogen bonds with adjacent fibers during hot pressing, enhancing the bonding force between fibers. More importantly, the ionic conductivity of Example 1 (0.126 mS / cm) is more than double that of Comparative Example 1 (0.058 mS / cm), the lithium-ion transference number increases from 0.38 to 0.65, and the interfacial impedance is significantly reduced. This directly proves that introducing lithium carboxylate and nitrile functional groups onto the surface can construct a heterogeneous coordination network, significantly improving ion transport efficiency. After 200 cycles, the capacity retention of Example 1 is as high as 91.3%, while that of Comparative Example 1 is only 52.6%, further confirming the decisive influence of functionalization modification on long-term cycle stability.
[0154] Comparing Examples 1, 2, and 3, the ratios of Examples 1 (30:70), 2 (40:60), and 3 (25:75) are different. Performance data shows that: Mechanical properties: The higher the proportion of PET-COOLi, the greater the tensile strength of the skeleton material. Example 2 (40% PET-COOLi) has a thickness of only 11 μm (microfiber), but due to the high proportion of PET-COOLi, it still maintains a strength of 18.2 MPa; Example 1 (30% PET-COOLi) has a strength of 23.5 MPa; Example 3 (25% PET-COOLi), although a binder was added, had a low proportion of PET-COOLi, and its strength might have decreased without the binder. This indicates that PET-COOLi, as the load-bearing phase, has a positive correlation with mechanical properties.
[0155] Ionic conductivity and transport number: Example 1 (30:70) showed the highest conductivity (0.126 mS / cm) and the highest transport number (0.65); Example 2 (40:60) showed slightly lower conductivity, and Example 3 (25:75) was in between. This indicates the existence of an optimal ratio range (approximately 30:70), where the density of nitrile sites and the density of fixed anion sites are optimally balanced, resulting in the most significant synergistic effect. Deviations from this value (towards either side) lead to a slight decrease in performance.
[0156] Cyclic stability: The 200-cycle capacity retention rate (92.7%) of Example 3 (with binder) was slightly higher than that of Example 1 (91.3%), thanks to the binder further stabilizing the fiber network structure and reducing structural relaxation during long-term cycling.
[0157] Comparing Examples 1 and 2, the effect of fiber size on film thickness was analyzed. Example 2 used microfibers (0.5-1.5 μm in diameter, 0.3-0.8 mm in length), with a framework material thickness of only 11 μm, significantly thinner than the 48 μm of Example 1. Although the ionic conductivity (0.108 mS / cm) and transport number (0.61) were slightly lower than those of Example 1, they still met the requirements of most solid-state batteries (typically >0.1 mS / cm). More importantly, the thin framework material is beneficial for reducing battery internal resistance and increasing volumetric energy density. Example 2 retained 87.6% of its capacity after 300 cycles, demonstrating the good durability of the thin film. Therefore, the microfiber approach is particularly suitable for thickness-sensitive high-energy-density batteries while maintaining sufficiently high ionic conductivity.
[0158] Example 3, based on Example 1, added 3% low-melting-point polyester fiber. Results showed that the tensile strength significantly increased from 23.5 MPa to 27.8 MPa (an 18% increase), while the porosity (74%) and thickness (52 μm) remained largely unchanged. Ionic conductivity (0.115 mS / cm) and migration number (0.63) decreased slightly but remained within acceptable ranges. The bonding reinforcement component partially melted during hot pressing, "welding" the fiber intersections together, improving overall structural integrity and thus enhancing dust resistance and long-term cycling stability (92.7% vs 91.3%). Therefore, adding 0.5%–10% bonding reinforcement component is beneficial for applications requiring high strength and winding resistance.
[0159] Example 4 employs a three-layer asymmetric structure (PET-COOLi enrichment on the negative electrode side, intermediate mixing, and Tencel-CN enrichment on the positive electrode side). Compared to homogeneous framework materials, its key advantage lies in simultaneously optimizing the interfaces of both electrodes. The high PET-COOLi content on the negative electrode side provides stronger resistance to lithium dendrite penetration; the high Tencel-CN content on the positive electrode side improves interfacial compatibility with the high-voltage positive electrode (NCM811) and reduces side reactions. In the stringent testing of the NCM811|Li battery, the capacity retention rate after 150 weeks reached 88.9%, while the homogeneous framework material (not shown) only reached approximately 75%. This demonstrates that the asymmetric structure is an effective strategy for adapting to both high-voltage positive electrodes and lithium metal negative electrodes.
[0160] Surface functionalization modification is fundamental to performance improvement: the performance of a simple mixture of unmodified PET / Tencel fibers (Comparative Example 1) is far inferior to any functionalized example, demonstrating the necessity of the synergistic design of the “PET-COOLi + Tencel-CN” bicomponent functional fibers.
[0161] The optimal ratio is 30:70 (PET-COOLi:Tencel-CN): This ratio achieves the best balance of mechanical properties, ionic conductivity and transport number, and is recommended as the first choice for routine applications.
[0162] Microfibers can achieve ultra-thin skeleton materials (5~20 μm), which are suitable for high volumetric energy density batteries while maintaining considerable ion conduction performance.
[0163] Adding 0.5% to 10% of the binder can significantly improve mechanical strength and cycle stability, making it suitable for winding processes with stringent mechanical performance requirements.
[0164] The asymmetric layered structure can independently optimize the positive and negative electrode interfaces, making it particularly suitable for high-voltage positive electrodes (such as NCM811) and lithium metal negative electrode systems.
[0165] The above are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. Any equivalent structural transformations made using the contents of the present invention specification and drawings under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.
[0166] It should be noted that when numerical ranges are involved in this invention, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, preferred embodiments are described in order to avoid redundancy. Although preferred embodiments of this invention have been described, those skilled in the art can make other changes and modifications to these embodiments once they know the basic inventive concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of this invention.
[0167] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from the spirit and scope of this invention; if these modifications and variations of this invention fall within the scope of the claims of this invention and their equivalents, then this invention also intends to include these modifications and variations.
Claims
1. A functionalized fiber composite skeleton material, characterized in that, include: The first fiber is a modified PET fiber with lithium carboxylate groups on its surface; The second fiber is a modified Tencel fiber with a nitrile group on its surface; The first fiber and the second fiber are interwoven within the skeleton material to form a porous structure; The mass ratio of the first fiber to the second fiber is 5:95 to 60:
40.
2. The composite skeleton material according to claim 1, characterized in that, The mass ratio of the first fiber to the second fiber is 20:80 to 40:60; The first fiber has a length of 0.5–8 mm and a diameter of 5–20 μm; the second fiber has a length of 0.5–6 mm and a diameter of 5–20 μm. The thickness of the skeleton material is 20–100 μm, and the porosity is 60%–85%.
3. The composite skeleton material according to claim 1, characterized in that, The diameter of the first fiber and the second fiber are both 0.2 to 5 μm and the length is both 0.1 to 2 mm. The thickness of the skeleton material is 5 to 20 μm, so as to form a thin composite skeleton material by means of micronized PET fiber and micronized Tencel fiber.
4. The composite skeleton material according to claim 1, characterized in that, The composite skeleton material also includes a bonding and reinforcing component, which is selected from one or more of low-melting-point polyester fibers, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, lithium polyacrylate, polyurethane, nanocellulose, and aramid nanofibers, and its addition amount is 0.5% to 10% of the total mass of the first fiber and the second fiber.
5. The composite skeleton material according to claim 1, characterized in that, The composite skeleton material has an asymmetric layered structure, including: The first layer near the negative electrode side is the first fiber enrichment layer. An intermediate layer, wherein the intermediate layer is a mixture of a first fiber and a second fiber; The second layer, located near the positive electrode side, is a second fiber-enriched layer.
6. A method for preparing a functionalized fiber composite skeleton material, characterized in that, The method for preparing the functionalized fiber composite skeleton material according to any one of claims 1 to 5 includes: Step S10: Provide modified PET fibers with lithium carboxylate groups on the surface, i.e., the first fiber; Step S20: Provide modified Tencel fibers with acrylonitrile groups on the surface, i.e., the second fiber; Step S30: The obtained first fiber and second fiber are mixed at a mass ratio of 5:95 to 60:40 and dispersed in a dispersion medium to form a uniform fiber suspension; Step S40: The obtained fiber suspension is processed into a wet membrane using wet papermaking, vacuum filtration, or filtration molding methods; Step S50: The wet film is dried and hot-pressed to obtain the functionalized fiber composite skeleton material.
7. The preparation method according to claim 6, characterized in that, The dispersion medium is water or a mixture of water and alcohol, and a dispersant is added. The dispersant is selected from one or more of Triton X-100, sodium dodecyl sulfate, polyvinylpyrrolidone, and sodium carboxymethyl cellulose, and the amount added is 0.001% to 0.1% of the total fiber mass. The fiber suspension also contains a bonding and reinforcing component, which is selected from one or more of low-melting-point polyester fibers, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, lithium polyacrylate, polyurethane, nanocellulose, and aramid nanofibers, and its addition amount is 0.5% to 10% of the total mass of the first fiber and the second fiber.
8. The preparation method according to claim 6, characterized in that, During the drying and hot-pressing process of the wet film, the drying temperature is 60-120℃, the hot-pressing temperature is 80-180℃, the pressure is 0.5-5MPa, and the time is 0.5-10min.
9. The preparation method according to claim 6, characterized in that, The first fiber is prepared by the following method: PET fibers are immersed in a NaOH aqueous solution with a concentration of 0.05–1.0 mol / L and treated at 40–90°C for 5–60 min for surface hydrolysis. Then, they are immersed in a lithium-containing compound solution for lithium salting treatment. The lithium-containing compound is selected from one or more of LiOH, Li2CO3, and lithium acetate. The solution concentration is 0.05–1.0 mol / L, the treatment temperature is 30–90°C, and the treatment time is 0.5–8 h, to obtain the first fiber with lithium carboxylate groups on the surface.
10. The preparation method according to claim 9, characterized in that, The method further includes: After surface hydrolysis and before lithium salting, the surface-hydrolyzed PET fibers are immersed in an acid solution of 0.01–0.1 mol / L for 5–30 min, wherein the acid solution is selected from one or more of hydrochloric acid, acetic acid, and citric acid.
11. The preparation method according to claim 6, characterized in that, The second fiber is prepared by esterification, cyanoethylation, or modification with a nitrile-containing silane coupling agent. The esterification method includes: Tencel fibers are dispersed in a polar aprotic solvent, and cyanoacetic acid, a dehydrating condensing agent and a catalyst are added. The mixture is reacted at 40-90℃ for 4-24 hours under an inert atmosphere to allow the hydroxyl groups on the surface of the Tencel fibers to undergo an esterification reaction with cyanoacetic acid, introducing nitrile functional groups onto the fiber surface. After the reaction, the fibers are washed and dried to obtain the second fiber. Wherein, the polar aprotic solvent is selected from one or more of DMF, DMSO, DMAc, and NMP; the dehydrating condensing agent is selected from one or more of DCC, DIC, EDC, and CDI; the catalyst is selected from one or more of DMAP, pyridine, and triethylamine; and the mass ratio of Tencel fiber to cyanoacetic acid is 1:0.1 to 1:1.
0. The cyanoethylation method includes: Tencel fibers are activated in an alkaline solution, then acrylonitrile is added and reacted at 20-60°C for 1-8 hours to allow the hydroxyl groups on the Tencel surface to undergo an addition reaction with acrylonitrile, introducing nitrile functional groups onto the fiber surface. After the reaction, the fibers are acid-washed, water-washed, and dried to obtain the second fiber. The method for modifying nitrile-containing silane coupling agents includes: Tencel fibers are dispersed in a water / alcohol mixture, and a nitrile-containing silane coupling agent is added. The mixture is reacted at 20–80°C for 1–12 hours to allow the hydroxyl groups on the surface of the Tencel fibers to undergo a hydrolysis-condensation reaction with the silane coupling agent, thereby introducing nitrile-containing functional groups onto the fiber surface. After the reaction, the fibers are washed and dried to obtain the second fiber. The nitrile-containing silane coupling agent is selected from one or more of 3-cyanopropyltriethoxysilane and 3-cyanopropyltrimethoxysilane.
12. A composite solid electrolyte membrane, characterized in that, The invention includes the functionalized fiber composite skeleton material according to any one of claims 1 to 5, and a composite solid electrolyte slurry filling the pores of the skeleton material, wherein the composite solid electrolyte slurry comprises an inorganic lithium-ion conductor, a polymer binder, and a lithium salt. The composite solid electrolyte membrane is prepared by the following method: after vacuum drying of the skeleton material, it is immersed in the composite solid electrolyte slurry and immersed for 5 to 60 minutes under vacuum conditions of -0.05 to -0.1 MPa. After removal, excess slurry on the surface is scraped off, and the membrane is obtained by drying, rolling, hot pressing and vacuum solvent removal treatment.
13. The composite solid electrolyte membrane according to claim 12, characterized in that, The inorganic lithium-ion conductor is selected from one or more of LATP, LLZO, LLZTO, LAGP, Li3PS4, and Li6PS5Cl, with a particle size D50 of 50–1000 nm; the polymer binder is selected from one or more of PVDF-HFP, PEO, PAN, PMMA, PVDF, polycarbonate, and polyionic liquid; the lithium salt is selected from one or more of LiTFSI, LiFSI, LiPF6, LiBOB, and LiDFOB. Based on the mass of solid components, the content of inorganic lithium-ion conductors is 30%–90%, the content of polymer binders is 5%–50%, and the content of lithium salts is 1%–30%.