A negative electrode-free lithium-ion battery, its preparation method and power device thereof
By introducing a multifunctional composite electrolyte and welded seam unit design into a negative electrode-free lithium-ion battery, a high-performance SEI film is formed, which solves the problem of interface instability between the negative electrode current collector and the electrolyte, and improves the electrochemical performance and compatibility of the battery.
Patent Information
- Application Number
- CN202611421470.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-10
AI Technical Summary
In negative electrode-less lithium-ion batteries, the interfacial instability between the negative electrode current collector and the electrolyte, including insufficient mechanical strength of the SEI film, electron tunneling, weak interfacial bonding and thermal aging degradation, leads to a decline in battery performance.
An SEI film consisting of a lithium fluoride layer, a flexible organic polymer layer, and a nitrogen oxide layer is formed in situ on the surface of the negative electrode current collector. The current distribution is homogenized and thermal aging degradation is suppressed through the coordinated cooperation of multiple sets of weld seam units and ring welds between the negative electrode tab and the current collector.
It achieves high initial efficiency, long cycle life, low internal resistance and low temperature rise battery performance, and is suitable for various battery systems, with good application prospects and industrialization value.
Smart Images

Figure CN123073173A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of battery materials technology, specifically relating to a negative electrode-free lithium-ion battery, its preparation method, and an electrical device thereof. Background Technology
[0002] Electrodeless lithium-ion batteries use a fully charged positive electrode as the sole active lithium source, directly depositing / stripping metallic lithium onto the negative electrode current collector. Because they eliminate the need for negative electrode active materials, they have extremely high volumetric and gravimetric energy densities and are considered an important technology route for the next generation of high-energy-density batteries.
[0003] One of the core challenges of anode-free lithium-ion batteries is the interfacial instability between the anode current collector and the electrolyte. On the surface of the anode current collector, the natural SEI formed by the reduction and decomposition of conventional carbonate-based electrolytes usually has the following defects: (a) uneven composition, with an excessively high proportion of organic components leading to insufficient mechanical strength, unable to withstand the volume changes of lithium deposition / stripping, resulting in repeated cracking and repair, and continuous consumption of active lithium; (b) discontinuous distribution of inorganic components, which cannot effectively block electron tunneling, leading to continuous reduction of the electrolyte; (c) weak SEI / lithium interface bonding, which is prone to detachment during lithium stripping, exposing fresh lithium surfaces and triggering new side reactions.
[0004] To address these issues, researchers have proposed numerous modification methods: for example, introducing fluoroethylene carbonate (FEC) to form a LiF-rich SEI on the negative electrode surface, but this single system suffers from poor high-voltage stability and continuous consumption; introducing vinylene sulfate (DTD) to improve SEI flexibility, but its use alone results in excessively thick films and increased impedance; introducing lithium nitrate (LiNO3) to enhance SEI ion selectivity, but its solubility in conventional carbonates is limited and it is easily reduced. Furthermore, the type and concentration of lithium salt, the polarity and viscosity of the solvent, the synergistic effect of other auxiliary reagents, and the structure and formation process of the current collector all significantly influence the performance of negative electrode-less lithium-ion batteries.
[0005] More importantly, most of the aforementioned modification studies are based on coin cell half-cells or pouch cells. There is very little research on 21650 (outer diameter 21±0.5mm, height 65±0.5mm) cylindrical cells with all tabs and no negative electrode. The actual current density distribution and local heat accumulation rate of this cylindrical cell are fundamentally different from those of coin cells. At the same time, while the low internal resistance brings high rate potential, it also makes the Joule heat in the current channel of "current collector-connector-terminal" more concentrated. During high-rate discharge, the Joule heat concentration will cause the local temperature rise to be too fast and the peak temperature to be too high, which in turn accelerates the side reactions at the SEI interface and the growth of lithium dendrites, so that the interface advantages of the electrolyte are offset by thermal aging.
[0006] Therefore, how to construct an SEI film with high ionic conductivity, high electronic insulation, high flexibility and high interfacial bonding on the surface of the negative electrode current collector, suppress the thermal aging degradation of SEI / CEI by Joule heating in the overcurrent channel, and make it applicable to various types of negative electrode-free lithium-ion batteries is an urgent technical problem to be solved. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the purpose of this application is to provide a negative electrode-free lithium-ion battery, its preparation method, and an electrical device thereof. In this negative electrode-free lithium-ion battery, on the one hand, a multifunctional composite electrolyte is introduced, enabling the in-situ formation of an SEI film on the surface of the negative electrode current collector, which is composed of a lithium fluoride layer, a flexible organic polymer layer, and a nitrogen oxide layer. This SEI film possesses high ionic conductivity, high electronic insulation, high mechanical strength, high flexibility, and high interfacial adhesion, effectively withstanding volume changes during lithium deposition / stripping without cracking. On the other hand, through the coordinated action of multiple sets of weld seam units spaced circumferentially between the negative electrode tab and the negative electrode current collector, and an annular ring weld in the central region of the negative electrode current collector, the current distribution is homogenized, local hot spots are reduced, and the annular ring weld shortens the current collection path, significantly suppressing the thermal aging and degradation of the SEI / CEI film, and preventing the electrolyte interfacial advantages from diminishing due to heat accumulation. In summary, this electrodeless lithium-ion battery possesses excellent performance characteristics such as high initial efficiency, long cycle life, low internal resistance, and low temperature rise. It is also highly compatible and applicable to various battery systems, including cylindrical, prismatic, and pouch cells, demonstrating promising application prospects and industrialization value.
[0008] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides a negative electrode-free lithium-ion battery, which includes a metal casing, a cell disposed within the metal casing, a positive current collector, and a negative current collector.
[0009] The battery cell includes: Positive electrode sheet.
[0010] A negative electrode current collector without negative electrode active material, the negative electrode current collector having a negative electrode tab, and multiple sets of weld seam units distributed circumferentially between the negative electrode tab and the negative electrode current collector disk.
[0011] The central region of the negative electrode current collector is provided with an annular ring weld, located at the circumferential edge of the central through hole of the negative electrode current collector.
[0012] Diaphragm.
[0013] A multifunctional composite electrolyte, comprising lithium salt, organic solvent and functional additives; wherein the multifunctional composite electrolyte comprises, along the direction away from the negative electrode current collector, a stacked lithium fluoride layer, a flexible organic polymer layer and a nitrogen oxide layer in the SEI film formed in situ on the surface of the negative electrode current collector.
[0014] This application introduces a multifunctional composite electrolyte into a cathode-free lithium-ion battery. This allows for the in-situ formation of an SEI film on the surface of the cathode current collector, layered with lithium fluoride, a flexible organic polymer, and oxide nitride. This SEI film possesses high ionic conductivity, high electronic insulation, high mechanical strength, high flexibility, and high interfacial adhesion, effectively withstanding volume changes during lithium deposition / stripping without cracking. Furthermore, the synergistic effect of multiple circumferentially spaced weld units between the cathode tab and the cathode current collector, along with a ring weld in the central region of the cathode current collector, homogenizes current distribution, reduces local hot spots, and shortens the current collection path using the ring weld, significantly suppressing the thermal aging degradation of the SEI / CEI film and preventing the electrolyte interfacial advantages from diminishing due to heat accumulation. In summary, this cathode-free lithium-ion battery exhibits excellent performance characteristics such as high initial efficiency, long cycle life, low internal resistance, and low temperature rise. It also boasts strong compatibility, applicable to various battery systems including cylindrical, prismatic, and pouch cells, demonstrating promising application prospects and industrialization value.
[0015] It should be noted that the three-layer structure of the SEI membrane can be deeply analyzed by XPS (Ar) + The measurements were obtained by sputtering and cryo-transmission electron microscopy (cryo-TEM), and the specific testing procedures included: After cycling, the battery cells were disassembled in an argon-filled glove box. The negative electrode current collector sample was rinsed with DMC and subjected to XPS depth profiling (Ar). + Sputtering (C1s / F1s / N1s / Li1s spectra) was used to analyze the composition of the three SEI layers; cryo-TEM was used to observe the SEI thickness and crystalline phase distribution; and FIB-SEM was used to observe the density of lithium deposition morphology.
[0016] For example, the positive current collector can be an aluminum alloy current collector or a nickel-plated steel current collector, and the negative current collector can be a copper current collector or a nickel-plated steel current collector.
[0017] For example, multiple weld seam units can be 2, 3 or 4 groups, etc.
[0018] In this application, by arranging the current in parallel groups, the current can be evenly distributed between the negative electrode tab and the current collector, reducing local current density and hot spots, and improving the reliability and safety of overcurrent at high rates.
[0019] In some embodiments, the lithium salt includes any one or a combination of at least two of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium dioxolaneborate (LiBOB), or lithium difluorophosphate (LiPO2F2), preferably a combination of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide.
[0020] This application preferentially uses a combination of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide as a dual lithium salt system, which is beneficial to improving the high-temperature storage stability and low-temperature ionic conductivity of the electrolyte: LiPF6 provides good oxidation stability and cost advantages, while LiFSI has high dissociation degree, which can improve low-temperature ionic conductivity and increase the content of inorganic components such as LiF / Li3N in SEI. The two work together to optimize interface and rate performance.
[0021] In some embodiments, the concentration of lithium salt in the multifunctional composite electrolyte is 0.8-1.2 mol / L, for example, it can be 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L or 1.2 mol / L, etc.
[0022] In some embodiments, the organic solvent includes any one or a combination of at least two of ethylene carbonate (EC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), or dimethyl carbonate (DMC), preferably a combination of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate, or a combination of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate.
[0023] In some embodiments, in the combination of ethylene carbonate, methyl ethyl carbonate, and dimethyl carbonate, the volume ratio of ethylene carbonate, methyl ethyl carbonate, and dimethyl carbonate is (25-35):(45-55):(15-25). The selection range of ethylene carbonate "25-35" can be, for example, 25, 30, or 35. The selection range of methyl ethyl carbonate "45-55" can be, for example, 45, 50, or 55. The selection range of dimethyl carbonate "15-25" can be, for example, 15, 20, or 25.
[0024] In some embodiments, the functional additives include fluorocarbonates, cyclic sulfates, vinylene carbonate (VC), and metal nitrates.
[0025] In this application, fluorocarbonates, cyclic sulfates, vinylene carbonates, and metal nitrates are used as functional additives. The fluorocarbonates (such as FEC) preferentially reduce on the copper foil surface to form a LiF-rich inorganic layer, providing high ionic conductivity and electronic insulation. The cyclic sulfates (such as DTD, TS, etc.) construct a structure rich in Li₂S and LiSO₄. xThe rigid framework of inorganic components enhances the mechanical strength and thermal stability of the SEI; the polymerization of vinylene carbonate (VC) forms a flexible polymer network, improving the SEI's flexibility and interfacial adhesion; the decomposition of metal nitrates (such as LiNO3) produces nitrogen oxide components such as Li3N, reinforcing the inorganic layer and suppressing lithium dendrites. Therefore, through the synergistic effect of the quaternary components, an SEI film consisting of a lithium fluoride layer, a flexible organic polymer layer, and a nitrogen oxide layer is formed in situ on the surface of the negative electrode current collector. This SEI film possesses high ionic conductivity, high electronic insulation, high mechanical strength, high flexibility, and high interfacial adhesion, effectively withstanding volume changes during lithium deposition / stripping without cracking.
[0026] In some embodiments, the multifunctional composite electrolyte further includes an auxiliary film-forming lithium salt.
[0027] In this application, the purpose of adding auxiliary film-forming lithium salt to the electrolyte is to enhance the toughness of the SEI film.
[0028] In some embodiments, the multifunctional composite electrolyte further includes a fluorinated ether cosolvent and / or auxiliary additives. For example, the fluorinated ether cosolvent may be 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) or bis(2,2,2-trifluoroethyl) ether (BTFE), etc.
[0029] In this application, the purpose of introducing a fluorinated ether co-solvent into the electrolyte is to further improve the wetting uniformity and oxidation resistance of the negative electrode current collector.
[0030] In some embodiments, the thickness ratio of the lithium fluoride layer, the flexible organic polymer layer, and the oxynitride layer is 1:(2-5):(1-3), wherein the selection range of the flexible organic polymer layer "2-5" can be, for example, 2, 3, 4, or 5, and the selection range of the oxynitride layer "1-3" can be, for example, 1, 2, or 3.
[0031] In this application, the SEI film formed in situ by the negative electrode current collector has a multilayer structure that satisfies the above thickness ratio. This is beneficial because the volume change of lithium ions during the deposition / stripping process is buffered by the flexible layer, electron tunneling is blocked by the inorganic layer, and the interfacial bonding force is strengthened by the organic layer. This effectively suppresses lithium dendrite and SEI breakage and improves cycle life.
[0032] In some embodiments, in the combination of lithium hexafluorophosphate and lithium bisfluorosulfonylimide, the molar ratio of lithium hexafluorophosphate to lithium bisfluorosulfonylimide is (70-90):(10-30), wherein the range of lithium hexafluorophosphate "70-90" can be, for example, 70, 75, 80, 85 or 90, and the range of lithium bisfluorosulfonylimide "10-30" can be, for example, 10, 15, 20, 25 or 30, preferably (75-85):(15-25).
[0033] In this application, the combination of the above molar ratios in the dual lithium salt system helps to balance high-temperature oxidation stability and low-temperature ionic conductivity, and keeps the content of inorganic components (LiF, Li3N, etc.) in the SEI within an optimized range that is conducive to ion transport and blocks electrons.
[0034] In some embodiments, the fluorocarbonate includes any one or a combination of at least two of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), or fluoroethyl methyl carbonate (FEMC).
[0035] In some embodiments, the cyclic sulfate ester includes any one or a combination of at least two of vinylene sulfate (DTD), a homologue of vinylene sulfate, or propylene sulfate (TS).
[0036] In some embodiments, the metal nitrate includes any one or a combination of at least two of lithium nitrate (LiNO3), potassium nitrate (KNO3), or cesium nitrate (CsNO3).
[0037] In some embodiments, the component content in the functional additive is as follows, based on the total mass of the lithium salt and organic solvent: Fluorinated carbonate 3-12 wt%, for example, 3 wt%, 5 wt%, 8 wt%, 10 wt% or 12 wt%, preferably 5-10 wt%, and more preferably 6-8 wt%.
[0038] The cyclic sulfate is 0.3-2.5 wt%, for example, it can be 0.3 wt%, 0.5 wt%, 1.0 wt%, 2.0 wt% or 2.5 wt%, preferably 0.8-2 wt%, and more preferably 1-1.5 wt%.
[0039] Vinyl carbonate is 0.2-1.8 wt%, for example, it can be 0.2 wt%, 0.5 wt%, 1.0 wt%, 1.5 wt% or 1.8 wt%, preferably 0.5-1.5 wt%, and more preferably 0.8-1.2 wt%.
[0040] Metal nitrates (such as LiNO3) are present in amounts of 0.3-2 wt%, for example, 0.3 wt%, 0.5 wt%, 1.0 wt%, 1.5 wt%, or 2.0 wt%, preferably 0.5-1.5 wt%, and more preferably 0.8-1.2 wt%.
[0041] In the electrolyte provided by this application, each component of the functional additives meets the above mass content, which helps to ensure that each functional additive can play its own film-forming / reinforcing role while avoiding excessive gas generation, increased impedance or decreased negative electrode wettability, thus controlling the SEI composition and structure within the optimal window.
[0042] In some embodiments, the mass content of the auxiliary film-forming lithium salt is 0.1-0.5 wt%, based on the total mass of the lithium salt and organic solvent, for example, it may be 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, or 0.5 wt%.
[0043] In some embodiments, the auxiliary film-forming lithium salt includes lithium difluorooxalate borate (LiDFOB).
[0044] In some embodiments, the mass content of the fluorinated ether cosolvent is 5-15 wt%, based on the total mass of the lithium salt and the organic solvent, for example, it can be 5 wt%, 8 wt%, 10 wt%, 12 wt%, or 15 wt%.
[0045] In some embodiments, the mass content of the auxiliary additive is 0.01-0.5 wt% based on the total mass of the lithium salt and organic solvent, for example, it may be 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.3 wt%, or 0.5 wt%.
[0046] In some embodiments, the auxiliary additives include any one or a combination of at least two of lithium difluorophosphate (LiPO2F2), 1,3-propanesulfonate lactone (1,3-PS), or p-toluenesulfonate (PTS).
[0047] In some embodiments, the weld unit includes at least two parallel welds, such as two, three, or four. It should be noted that industrial CT and cross-sectional metallographic analysis can be used to count the number of welds. In this application, an appropriate number of welds can reduce the interfacial contact resistance and local heat generation without excessively occupying the effective area of the negative electrode current collector, and avoid the formation of overcurrent bottlenecks or excessive weakening of the mechanical strength of the current collector due to too few welds.
[0048] In some embodiments, the weld shape in the weld unit includes any one or a combination of at least two of the following: wavy, radial, or spiral.
[0049] In some embodiments, the width of any weld in the weld unit is 0.25-0.35 mm, for example, 0.25 mm, 0.28 mm, 0.30 mm, 0.33 mm, or 0.35 mm, and the length is 5-7 mm, for example, 5.0 mm, 5.5 mm, 6.0 mm, 6.5 mm, or 7.0 mm. It should be noted that industrial CT and cross-sectional metallographic analysis can be used to determine the width and length of the weld.
[0050] In some embodiments, the thickness of the negative current collector is 0.15-0.3 mm, for example, it can be 0.15 mm, 0.2 mm, 0.25 mm or 0.3 mm.
[0051] In some embodiments, the outer diameter of the annular weld is 4.8-5.4 mm, for example, it can be 4.8 mm, 5.0 mm, 5.1 mm, 5.2 mm or 5.4 mm, etc.
[0052] In some embodiments, the weld width of the annular weld is 0.3-0.36 mm, for example, it can be 0.30 mm, 0.32 mm, 0.33 mm, 0.34 mm or 0.36 mm.
[0053] In some embodiments, the negative electrode current collector is any one of a plain copper foil, a carbon-coated copper foil, a lithiophilic modified copper foil, or a three-dimensional porous copper foil. Compared to plain copper foil, carbon-coated copper foil, lithiophilic modified copper foil, or three-dimensional porous copper foil can further reduce the lithium nucleation overpotential.
[0054] It should be noted that "bright copper foil" refers to a dense copper layer without a carbon coating, a lithium-affinity metal layer, or a porous structure on its surface. The surface roughness Ra of bright copper foil can be 0.2-0.4 μm, such as 0.2 μm, 0.3 μm, or 0.4 μm.
[0055] In some embodiments, the porosity of the three-dimensional porous copper foil is 30-40%, for example, it can be 30%, 35%, or 40%. It should be noted that the porosity can be obtained using the mercury intrusion porosimetry (MIP) method.
[0056] In some embodiments, the lithium-loving modified copper foil includes a copper foil and a lithium-loving layer disposed on both sides of the copper foil, the lithium-loving layer including a silver layer and / or a zinc layer.
[0057] In some embodiments, the positive electrode sheet includes a positive current collector and a layer of positive active material disposed on at least one side surface of the positive current collector.
[0058] In some embodiments, the positive current collector includes a current collector body and lead-out tabs extending outward from the current collector body; the current collector body is provided with multiple sets of weld seam units (e.g., 2 sets, 3 sets, or 4 sets, etc.) for welding to the positive tabs of the positive electrode sheet, and the multiple sets of weld seam units are arranged at intervals along the circumference of the current collector body; a central hole is provided at the center of the current collector body, and the current collector body is also provided with multiple peripheral holes (e.g., 1, 2, or 3, etc.).
[0059] In some embodiments, the positive electrode active material layer includes a positive electrode active material, a conductive agent, and a binder. For example, the positive electrode active material may be an NCM-based high-nickel positive electrode material.
[0060] In some embodiments, the diaphragm includes a porous base membrane and a ceramic coating disposed on both sides of the porous base membrane.
[0061] The use of the aforementioned diaphragm in this application helps to improve thermal stability and electrolyte wettability.
[0062] In some embodiments, the negative electrode-free lithium-ion battery has a full-tab structure.
[0063] In some embodiments, the metal casing is of any one of 21650, 18650, 21700, 4680, 4695 or 46120.
[0064] It should be noted that the battery system provided in this application is applicable to various battery systems, including cylindrical, prismatic, and pouch cells.
[0065] In some embodiments, the AC internal resistance and DC internal resistance of the negative electrode-free lithium-ion battery are each independently 2-4 mΩ, for example, 2 mΩ, 2.5 mΩ, 3 mΩ, 3.5 mΩ or 4 mΩ.
[0066] In some embodiments, the temperature rise rate of the negative electrode-free lithium-ion battery under 10C discharge conditions is ≤4℃ / min, for example, it can be 0.5℃ / min, 1℃ / min, 2℃ / min, 3℃ / min or 4℃ / min, etc., and the surface peak temperature is ≤80℃, for example, it can be 60℃, 65℃, 70℃, 75℃ or 80℃, etc.
[0067] In some embodiments, the negative electrode-free lithium-ion battery has a first-cycle coulombic efficiency of ≥90% under 25±5℃ and 0.1C charge / 0.1C discharge conditions, for example, 90%, 92%, 94%, 96% or 98%.
[0068] In some embodiments, the negative electrode-free lithium-ion battery retains ≥85% of its capacity after 600 cycles at 25±5°C and 0.5C charge / discharge conditions, for example, 85%, 88%, 90%, 92%, or 95%.
[0069] In some embodiments, the negative electrode-free lithium-ion battery retains ≥80% of its capacity after 800 cycles at 25±5°C and 1C charge / 1C discharge conditions, for example, 80%, 82%, 85%, 88%, or 90%.
[0070] Secondly, this application provides a method for preparing a negative electrode-free lithium-ion battery as described in the first aspect, the method comprising the following steps: The device provides a positive electrode sheet, a negative electrode current collector, a separator, and a multifunctional composite electrolyte; the negative electrode current collector has a negative electrode tab; the multifunctional composite electrolyte includes lithium salt, organic solvent, and functional additives.
[0071] The positive electrode, the separator, and the negative current collector are assembled to obtain a battery cell.
[0072] A positive current collector and a negative current collector are provided; the positive electrode tab of the positive electrode sheet is welded to the positive current collector; the negative electrode tab of the battery cell is welded to the negative current collector through multiple sets of weld seam units spaced apart along the circumference of the negative current collector, and at the same time, a ring weld is performed along the circumferential edge of the central through hole of the negative current collector to form a ring weld.
[0073] The welded battery cell is placed into a metal casing, and the positive current collector is welded to the cap of the metal casing to achieve electrical connection. The negative current collector is welded to the bottom of the metal casing to achieve electrical connection. The multifunctional composite electrolyte is then injected.
[0074] A multi-step formation process is performed to form an SEI film in situ on the surface of the negative electrode current collector using the multifunctional composite electrolyte. The SEI film comprises a stacked lithium fluoride layer, a flexible organic polymer layer, and a nitrogen oxide layer along the direction away from the negative electrode current collector.
[0075] This application does not specify the welding method. For example, it can be laser welding, ultrasonic welding, or resistance welding.
[0076] In some embodiments, the specific steps of the multi-step transformation include: At an ambient temperature of 35±3℃ (e.g., 32℃, 33℃, 34℃, 35℃, 36℃, 37℃, or 38℃), the first step involves pre-charging to 3.6-3.9V (e.g., 3.6V, 3.7V, 3.8V, or 3.9V) at 0.01-0.05C (e.g., 0.01C, 0.02C, 0.03C, 0.04C, or 0.05C). The second step involves charging to 4.2V at 0.05-0.1C (e.g., 0.05C, 0.06C, 0.07C, 0.08C, 0.09C, or 0.1C), followed by constant voltage cutoff at 0.01C, and then discharging.
[0077] This application employs a two-step formation process to form the aforementioned layered SEI film in situ on the surface of the negative electrode current collector. The first step involves low-temperature, low-current pre-charging, which preferentially reduces and generates a LiF-rich / nitrogen oxide-rich inorganic inner layer on the copper foil surface. The second step involves heating and constant-current formation to promote the dense growth of a flexible organic polymer outer layer, thus balancing initial efficiency and long-term cycle stability.
[0078] Thirdly, this application provides an electrical device, which includes a negative electrode-free lithium-ion battery as described in the first aspect or a negative electrode-free lithium-ion battery obtained by the preparation method described in the second aspect.
[0079] The numerical range described in this application includes not only the point values listed above, but also any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values included in the range.
[0080] Compared with the prior art, this application has the following advantages: This application introduces a multifunctional composite electrolyte into a cathode-free lithium-ion battery. This allows for the in-situ formation of an SEI film on the surface of the cathode current collector, layered with lithium fluoride, a flexible organic polymer, and oxide nitride. This SEI film possesses high ionic conductivity, high electronic insulation, high mechanical strength, high flexibility, and high interfacial adhesion, effectively withstanding volume changes during lithium deposition / stripping without cracking. Furthermore, the synergistic effect of multiple circumferentially spaced weld units between the cathode tab and the cathode current collector, along with a ring weld in the central region of the cathode current collector, homogenizes current distribution, reduces local hot spots, and shortens the current collection path using the ring weld, significantly suppressing the thermal aging degradation of the SEI / CEI film and preventing the electrolyte interfacial advantages from diminishing due to heat accumulation. In summary, this cathode-free lithium-ion battery exhibits excellent performance characteristics such as high initial efficiency, long cycle life, low internal resistance, and low temperature rise. It also boasts strong compatibility, applicable to various battery systems including cylindrical, prismatic, and pouch cells, demonstrating promising application prospects and industrialization value. Attached Figure Description
[0081] Figure 1 This is a schematic diagram of the structure of the negative electrode-free lithium-ion battery provided in Embodiment 1 of this application.
[0082] Figure 2 This is a schematic diagram of the positive current collector provided in Embodiment 1 of this application.
[0083] Figure 3 This is a schematic diagram of the negative electrode current collector provided in Embodiment 1 of this application.
[0084] Among them, 1-21650 steel shell; 2-battery cell; 3-positive current collector; 31-positive current collector body; 32-lead-out tab; 33-center hole; 34-peripheral hole; 4-negative current collector; 41-center through hole; 5-cap; A-weld unit; B-wavy weld. Detailed Implementation
[0085] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.
[0086] The scope of this application can be defined by lower and upper limits. The selected lower and upper limits define the boundaries of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower and upper limits can be arbitrarily combined to form new ranges. That is, any lower limit can be combined with any upper limit to form a valid range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this application. In addition, if the minimum range values 1 and 2 are listed, and the maximum range values 3, 4 and 5 are also listed, then all ranges of 1~3, 1~4, 1~5, 2~3, 2~4 and 2~5 fall within the scope of this application. In this application, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0~5" means that all real numbers between 0 and 5 have been fully listed in this document, and "0~5" is only a shortened representation of this set of numerical combinations. When a parameter is expressed as an integer ≥2, it is equivalent to listing positive integers that meet the requirements, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. When a parameter is expressed as an integer selected from "2~10", it is equivalent to listing any integer among 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0087] In this application, "at least two combinations" refers to a quantity greater than or equal to 2 unless otherwise specified. For example, "any one or at least two combinations" means any one of the listed items, or a combination of at least two of the listed items formed in a manner that does not conflict and enables the implementation of this application. In this application, unless otherwise specified, the features or solutions corresponding to "and / or" cover any one of two or more related listed items, as well as any and all combinations of the related listed items. The arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a set consisting of A, B, and combinations of A and B, where "containing A and / or B" can be understood, depending on the context of the statement, as containing A, containing B, or simultaneously containing both A and B. In this application, "optional" means that the corresponding feature, component, step or solution is not necessary, that is, it is selected from either "with" or "without". If there are multiple "optional" limitations in a technical solution, unless otherwise specified and there is no technical conflict or mutual constraint, each "optional" limitation is independent and does not affect the others.
[0088] In this application, technical features or solutions described using open-ended terms such as "comprising" or "including" do not exclude additional non-conflicting elements beyond those listed unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond the listed elements. For example, if A includes a1, a2, and a3, unless otherwise specified, this means that A can consist only of a1, a2, and a3, or it can include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3," "A is selected from a1, a2, and a3," and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements." All embodiments and optional embodiments of this application, unless otherwise specified and without technical conflict, can be combined to form new technical solutions, and such combinations fall within the scope of this application. The term "embodiment" as used in this application means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment mutually exclusive with other embodiments. Those skilled in the art can explicitly and implicitly understand that the embodiments described in this application can be combined with other embodiments that do not conflict with existing technologies. The ordinal numbers "first," "second," "third," and "fourth," etc., used in this application in the expressions "first aspect," "second aspect," "third aspect," and "fourth aspect," are for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly specifying the importance or quantity of the indicated technical features. They serve only as a non-exhaustive enumeration and do not constitute a closed limitation on quantity.
[0089] In this application, the order in which the steps are written in the methods described in the various embodiments does not imply a strict execution order. The actual execution order of each step should be determined according to its function and possible internal logic. Unless otherwise specified, all steps in this application can be executed in the order they are written, or in any order without technical conflict. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) executed sequentially, or it may include steps (b) and (a) executed sequentially. If the method also includes step (c), then step (c) can be added to the method in any order without conflict, including but not limited to the execution order of steps (a), (b), and (c), steps (a), (c), and (b), steps (c), (a), and (b), etc.
[0090] Example 1 This embodiment provides a negative electrode-free lithium-ion battery, the structural schematic diagram of which is shown below. Figure 1As shown, the negative electrode-less lithium-ion battery includes a 21650 steel casing 1 (diameter 21mm, height 65mm), a battery cell 2 disposed within the 21650 steel casing 1, a positive electrode current collector 3 (made of aluminum alloy, outer diameter 18.2mm), and a negative electrode current collector 4 (made of copper, its structural schematic diagram is shown in the figure). Figure 3 (As shown).
[0091] The battery cell 2 includes: Positive electrode sheet.
[0092] A negative electrode current collector without negative electrode active material has a negative electrode tab. Four sets of weld seam units A are provided between the negative electrode tab and the negative electrode current collector disk 4, which are distributed circumferentially. Each set of weld seam units A includes three parallel wavy weld seams B. The central area of the negative electrode current collector disk 4 is provided with an annular ring weld located at the circumferential edge of the central through hole 41 of the negative electrode current collector disk 4.
[0093] Diaphragm.
[0094] A multifunctional composite electrolyte, comprising lithium salt, organic solvent and functional additives; the multifunctional composite electrolyte comprises, along the direction away from the negative electrode current collector, a stacked lithium fluoride layer, a flexible organic polymer layer and a nitrogen oxide layer in the SEI film formed in situ on the surface of the negative electrode current collector, with a thickness ratio of 1:3:2.
[0095] The lithium salt comprises LiPF6 and LiFSI in a molar ratio of 80:20; the concentration of the lithium salt in the multifunctional composite electrolyte is 1 mol / L; the organic solvent is a combination of EC, EMC, and DMC in a volume ratio of 30:50:20; based on the total mass of the lithium salt and organic solvent, the functional additive comprises the following components: FEC 7 wt%, DTD 1.2 wt%, VC 1 wt%, and LiNO3 1 wt%; the multifunctional composite electrolyte also includes LiDFOB, with a LiDFOB content of 0.3 wt% based on the total mass of the lithium salt and organic solvent.
[0096] The number of wavy welds B is 12 (forming continuous wavy patterns); the width of each wavy weld B is 0.3 mm and the length is 6 mm; the thickness of the negative electrode current collector 4 is 0.2 mm. The outer diameter of the annular weld is 5.1 mm; the weld width of the annular weld is 0.33 mm.
[0097] The positive electrode includes a positive current collector and positive active material layers disposed on both sides of the positive current collector; the positive current collector is an aluminum foil with a thickness of 13 μm, the aluminum foil has a positive electrode tab, the positive electrode tab is electrically connected to the positive current collector disk 3, and the positive current collector disk 3 is electrically connected to the cap 5 of the 21650 steel shell 1; the structural schematic diagram of the positive current collector disk 3 is shown below. Figure 2 As shown, the device includes a current collector body 31 and lead-out tabs 32 extending outward from the current collector body 31. The current collector body 31 is provided with four sets of weld seam units A for welding to the positive electrode tabs of the positive electrode sheet. The four sets of weld seam units A are arranged at intervals along the circumference of the current collector body 31. Each set of weld seam units A includes three parallel wavy weld seams B. The current collector body 31 has a central hole 33 and three peripheral holes 34. The positive electrode active material layer includes positive electrode active material, conductive carbon black, and polyvinylidene fluoride in a mass ratio of 96:2:2, with the positive electrode active material being LiNi. 0.9 Co 0.05 Mn 0.03 Al 0.02 O2 (NCM90); the single-sided density of the positive electrode is 15 mg / cm³. 2 The compacted density is 3.5 g / cm³. 3 The negative electrode current collector is an electrolytic copper foil with a thickness of 6 μm and a surface roughness Ra of 0.3 μm. The separator includes a porous PE base membrane and an alumina ceramic coating disposed on both sides of the porous PE base membrane. The porous PE base membrane has a thickness of 12 μm, a porosity of 40%, and a Gurley value of 160 s / 100 mL. The alumina ceramic coating has a single-sided thickness of 2 μm (closing temperature ≥135℃, membrane breaking temperature ≥165℃).
[0098] This embodiment also provides a method for preparing the above-mentioned negative electrode-free lithium-ion battery, the method comprising the following steps: (1) Preparation of positive electrode sheet: (a) NiSO4·6H2O, CoSO4·7H2O and MnSO4·H2O were dissolved in deionized water in a molar ratio of Ni:Co:Mn=90:5:3 to prepare a 2 mol / L mixed transition metal salt solution.
[0099] Under nitrogen protection (O2 < 10 ppm), the transition metal mixed salt solution, 5 mol / L NaOH solution, and ammonia (as a pH adjuster) were pumped into a continuous stirred tank reactor (CSTR). The reaction temperature was controlled at 55 ± 1 °C, pH = 11.2 ± 0.1, and stirring speed at 400 rpm, to co-precipitate Ni. 0.9 Co 0.05Mn 0.03 (OH)2 precursor, aged for 2 hours, then filtered and washed (until SO4 saturates are obtained in the wash solution). 2- <5ppm), dried at 80℃ for 12 hours to obtain dried material.
[0100] The dried material was mixed with LiOH·H2O (Li excess 2 mol%) and Al2O3 nanoparticles by planetary ball milling for 30 min. The mixture was then heated to 850℃ in a tube furnace under a pure O2 atmosphere (2 L / min) at a rate of 2℃ / min and held for 12 h. After furnace cooling, the mixture was crushed and sieved (D50 = 10 ± 2 μm) to obtain LiNi. 0.9 Co 0.05 Mn 0.03 Al 0.02 O2 (NCM90).
[0101] (b) The NCM90 was mixed with conductive carbon black and polyvinylidene fluoride at a mass ratio of 96:2:2 and added to N-methylpyrrolidone (NMP). The mixture was dispersed in a planetary mixer (30 rpm revolution / 1500 rpm rotation, 2 h, vacuum degassing for 30 min) to obtain a positive electrode slurry with a solid content of 70 wt%.
[0102] The positive electrode slurry is coated on both sides of a 13μm thick aluminum foil, dried under vacuum at 120℃ for 2 hours, and then rolled to obtain a positive electrode sheet. The positive electrode sheet has a blank area (uncoated aluminum foil), which serves as the positive electrode tab.
[0103] (2) Provide negative electrode current collector: Electrolytic copper foil with a thickness of 6μm was first micro-etched with 3wt% dilute hydrochloric acid for 10s to remove the surface oxide layer, rinsed with deionized water, dehydrated with anhydrous ethanol, and vacuum dried at 80℃ for 4h to control the surface roughness Ra=0.3μm and moisture <50ppm.
[0104] (3) Provide a diaphragm: A porous PE base film is used, and an alumina ceramic coating with a thickness of 2μm is coated on both sides of the porous PE base film.
[0105] (4) Preparation of multifunctional composite electrolyte: In an environment with a dew point temperature ≤ -40℃, EC, EMC, and DMC are mixed in a volume ratio of 30:50:20, then LiPF6 is added to a concentration of 0.8 mol / L, and LiFSI is added to a concentration of 0.2 mol / L. The mixture is magnetically stirred for 30 min until completely dissolved to obtain a basic electrolyte. FEC, DTD, VC, LiNO3, and LiDFOB are added sequentially to the basic electrolyte, stirred evenly, filtered, and sealed for storage at -20℃ in the dark. The water content in the multifunctional composite electrolyte is ≤10 ppm, and the HF content is ≤20 ppm.
[0106] (5) The positive electrode sheet, separator, copper foil and separator are wound with a winding tension of 0.2 N / mm to obtain a core; the tabs on both sides of the core are flattened, and then the negative electrode tabs of the negative current collector are welded to the negative current collector plate by a wavy weld seam using a pulsed laser method, with a welding depth ≥ 0.1 mm and a single-point lap resistance < 0.2 mΩ; at the same time, a ring weld is performed along the circumferential edge of the central through hole of the negative current collector plate to form a ring weld; the positive electrode tabs of the positive electrode sheet are welded to the positive current collector plate.
[0107] The welded battery cell is placed into a 21650 steel shell. The positive current collector is welded to the cap of the metal shell to achieve electrical connection, and the negative current collector is welded to the bottom of the metal shell to achieve electrical connection. The shell is sealed with a groove and a sealing ring, and an injection hole is left.
[0108] (6) In a vacuum chamber (<100Pa), inject the multifunctional composite electrolyte along the injection hole with an injection coefficient of 1.1 and let it stand for 8 hours to fully wet it.
[0109] At an ambient temperature of 35℃, the first step is to precharge to 3.8V at 0.02C and let stand for 30 minutes; the second step is to charge to 4.2V at 0.05C and then keep the voltage constant until 0.01C, followed by discharge to 3V at 0.1C; the gas is then removed by evacuation and sealed.
[0110] Capacity testing was performed at 25℃ and 0.5C charge / discharge conditions, followed by resting at 40℃ for 3 days. Qualified cells with an OCV deviation of <5mV were selected to obtain the negative electrode-free lithium-ion battery.
[0111] Example 2 The difference between this embodiment and embodiment 1 is that the mass content of FEC in the multifunctional composite electrolyte prepared in step (4) is replaced by 3wt% instead of 7wt%.
[0112] The remaining preparation methods and parameters are consistent with those in Example 1.
[0113] Example 3 The difference between this embodiment and embodiment 1 is that the mass content of FEC in the multifunctional composite electrolyte prepared in step (4) is replaced by 5wt% instead of 7wt%.
[0114] The remaining preparation methods and parameters are consistent with those in Example 1.
[0115] Example 4 The difference between this embodiment and embodiment 1 is that the mass content of FEC in the multifunctional composite electrolyte prepared in step (4) is replaced by 12wt% instead of 7wt%.
[0116] The remaining preparation methods and parameters are consistent with those in Example 1.
[0117] Example 5 The difference between this embodiment and embodiment 1 is that in step (4), LiPF6 is added to a concentration of 0.9 mol / L and LiFSI is added to a concentration of 0.1 mol / L, so that the molar ratio of LiPF6 to LiFSI is 90:10.
[0118] The remaining preparation methods and parameters are consistent with those in Example 1.
[0119] Example 6 The difference between this embodiment and embodiment 1 is that in step (4), LiPF6 is added to a concentration of 0.85 mol / L and LiFSI is added to a concentration of 0.15 mol / L, so that the molar ratio of LiPF6 to LiFSI is 85:15.
[0120] The remaining preparation methods and parameters are consistent with those in Example 1.
[0121] Example 7 The difference between this embodiment and embodiment 1 is that in step (4), LiPF6 is added to a concentration of 0.7 mol / L and LiFSI is added to a concentration of 0.3 mol / L, so that the molar ratio of LiPF6 to LiFSI is 70:30.
[0122] The remaining preparation methods and parameters are consistent with those in Example 1.
[0123] Example 8 The difference between this embodiment and embodiment 1 is that each weld unit contains two parallel wavy welds, that is, there are a total of 8 wavy welds between the negative electrode tab and the negative electrode current collector. Each wavy weld has a width of 0.3 mm and a length of 6 mm.
[0124] The remaining preparation methods and parameters are consistent with those in Example 1.
[0125] Example 9 The difference between this embodiment and embodiment 1 is that in step (6), the pre-charge current in the first step is 0.01C.
[0126] The remaining preparation methods and parameters are consistent with those in Example 1.
[0127] Example 10 The difference between this embodiment and embodiment 1 is that in step (6), the pre-charge current in the first step is 0.03C.
[0128] The remaining preparation methods and parameters are consistent with those in Example 1.
[0129] Example 11 The difference between this embodiment and embodiment 1 is that in step (6), the pre-charge current in the first step is 0.05C.
[0130] The remaining preparation methods and parameters are consistent with those in Example 1.
[0131] Example 12 The difference between this embodiment and embodiment 1 is that the FEC in step (4) is replaced with DFEC of equal mass.
[0132] The remaining preparation methods and parameters are consistent with those in Example 1.
[0133] Example 13 The difference between this embodiment and embodiment 1 is that the FEC in step (4) is replaced with FEMC of equal mass.
[0134] The remaining preparation methods and parameters are consistent with those in Example 1.
[0135] Example 14 The difference between this embodiment and embodiment 1 is that the DTD in step (4) is replaced with TS of equal quality.
[0136] The remaining preparation methods and parameters are consistent with those in Example 1.
[0137] Example 15 The difference between this embodiment and embodiment 1 is that the LiNO3 mentioned in step (4) is replaced with an equal mass of potassium nitrate KNO3.
[0138] The remaining preparation methods and parameters are consistent with those in Example 1.
[0139] Example 16 The difference between this embodiment and embodiment 1 is that, in step (4), a fluorinated ether cosolvent TTE is added to the basic electrolyte; based on the total mass of the lithium salt and the organic solvent, the mass content of TTE is 10 wt%.
[0140] The remaining preparation methods and parameters are consistent with those in Example 1.
[0141] Example 17 The difference between this embodiment and embodiment 1 is that, in step (4), an auxiliary additive LiPO2F2 is added to the basic electrolyte; based on the total mass of the lithium salt and organic solvent, the mass content of LiPO2F2 is 0.2wt%.
[0142] The remaining preparation methods and parameters are consistent with those in Example 1.
[0143] Example 18 The difference between this embodiment and embodiment 1 is that the organic solvent in step (4) is replaced by a combination of EC, DEC and EMC in a volume ratio of 30:20:50.
[0144] The remaining preparation methods and parameters are consistent with those in Example 1.
[0145] Comparative Example 1 The difference between this comparative example and Example 1 is that the mass content of FEC in the multifunctional composite electrolyte prepared in step (4) is replaced by 1 wt% instead of 7 wt%.
[0146] The remaining preparation methods and parameters are consistent with those in Example 1.
[0147] Comparative Example 2 The difference between this comparative example and Example 1 is that the mass content of FEC in the multifunctional composite electrolyte prepared in step (4) is replaced by 15wt% instead of 7wt%.
[0148] The remaining preparation methods and parameters are consistent with those in Example 1.
[0149] Comparative Example 3 The difference between this comparative example and Example 1 is that LiFSI is not added in step (4), and the concentration of LiPF6 is 1 mol / L.
[0150] The remaining preparation methods and parameters are consistent with those in Example 1.
[0151] Comparative Example 4 The difference between this comparative example and Example 1 is that in step (4), LiPF6 is added to a concentration of 0.55 mol / L and LiFSI is added to a concentration of 0.45 mol / L, so that the molar ratio of LiPF6 to LiFSI is 55:45.
[0152] The remaining preparation methods and parameters are consistent with those in Example 1.
[0153] Comparative Example 5 The difference between this comparative example and Example 1 is that there are 12 weld seams evenly distributed circumferentially between the negative electrode tab and the negative electrode current collector, which are not grouped.
[0154] The remaining preparation methods and parameters are consistent with those in Example 1.
[0155] Comparative Example 6 The difference between this comparative example and Example 1 is that the central area of the negative electrode current collector does not have an annular weld.
[0156] The remaining preparation methods and parameters are consistent with those in Example 1.
[0157] Comparative Example 7 The difference between this comparative example and Example 1 is that the two steps in step (6) are replaced by the following steps: At 25°C, charge directly to 4.2V with a constant current of 0.5C (with a constant voltage cutoff of 0.01C), and then discharge to 3V with a constant current of 0.1C.
[0158] The remaining preparation methods and parameters are consistent with those in Example 1.
[0159] Performance testing The following tests were performed on the negative electrode-free lithium-ion batteries provided in the above embodiments and comparative examples: 1) Initial coulombic efficiency, test method: 25℃, constant current charging at 0.1C to 4.2V (CV cutoff at 0.02C), discharge at 0.1C to 3V, initial efficiency = first week discharge capacity / first week charge capacity × 100%.
[0160] 2) Capacity retention rate at 600 cycles. Test method: 25℃, 0.5C / 0.5C cycle for 600 cycles (CC-CV charge to 4.2V, cutoff 0.05C; CC discharge to 3.0V), insert a 0.1C reference capacity calibration every 50 cycles, and calculate the capacity retention rate.
[0161] 3) AC internal resistance / DC internal resistance, test method: AC internal resistance ACR is measured with a 1kHz AC impedance meter; DC internal resistance DCIR is calculated by applying a 10s, 1C discharge pulse at 25℃ and 50% SOC, and calculated according to ΔV / ΔI.
[0162] 4) Temperature rise rate / peak surface temperature: The fully charged battery was discharged to 3V at a constant current of 10C in an environment of 25℃. A type K thermocouple (±0.5℃) was attached to the middle of the casing and the corresponding end face of the current collector. The sampling interval was 1s, and the temperature rise rate dT / dt and the peak surface temperature T were recorded. max .
[0163] 5) 800-cycle capacity retention rate, test method: 25℃, 1C / 1C cycle for 800 cycles (CC-CV charge to 4.2V, cutoff 0.05C; CC discharge to 3V), insert a 0.1C reference capacity calibration every 50 cycles, and calculate the capacity retention rate.
[0164] The test results are shown in Table 1.
[0165] Table 1 analyze: As can be seen from the comparison of Examples 1, 2-4 and Comparative Examples 1-2, FEC preferentially reduces (approximately 1.3V vs. Li / Li). +(Near-side defluorination) LiF is supplied to the surface of electrolytic copper foil to construct a high Young's modulus and high interfacial energy SEI underlayer, suppressing lithium dendrite penetration and improving SEI / lithium bonding force; within the protected range of mass content, as FEC increases from 3wt% to 7wt%, the LiF supply is sufficient, the first efficiency increases from 91.0% to 93.5%, and the 600-cycle retention rate increases from 86.0% to 89.0%; when it increases to 12wt% (Example 4), the film thickness increases, the impedance increases slightly (DCIR is 3.4mΩ), the 600-cycle capacity retention rate drops to 86.0%, and the 800-cycle capacity retention rate drops to 81.0%. Although the performance still meets the standard, the long-cycle benefit has decreased significantly. Therefore, the mass content of fluorocarbonate is preferably 5-10wt%, and more preferably 6-8wt%. However, when the mass content is as low as 1wt% (Comparative Example 1), LiF is insufficient, and the SEI repeatedly breaks down and repairs, resulting in continuous lithium consumption. The initial efficiency is 87.5%, and the retention rate after 800 cycles is 58.0%. When the mass content is as high as 15wt% (Comparative Example 2), the SEI is too thick and FEC decomposes to produce gas. The DCIR is 4.6mΩ, and the 10C peak temperature is 84℃.
[0166] As can be seen from the comparison of Examples 1, 5-7 and Comparative Examples 3-4, FSI - The reduction generates inorganic components such as LiF and Li3N to strengthen the SEI. At the same time, LiFSI has a higher degree of dissociation than LiPF6, which improves the ionic conductivity of the electrolyte and reduces interfacial polarization. Within the protection range, when the molar fraction of LiFSI increased from 10% (Example 5) to 20% (Example 1), the DCIR decreased from 3.0 mΩ to 2.8 mΩ, the 600-cycle capacity retention increased from 87.0% to 89.0%, and the 800-cycle capacity retention increased from 82.0% to 84.0%. When further increased to 30% (Example 7), the DCIR further decreased to 2.7 mΩ, the 10C surface peak temperature remained at 72°C, but the 600-cycle capacity retention dropped to 88.5% and the 800-cycle capacity retention dropped to 83.5%, indicating that when the LiFSI proportion is too high, the risk of pitting corrosion in the aluminum foil increases, and the long-cycle benefit decreases. Therefore, the preferred molar ratio of LiPF6 to LiFSI is (75-85):(15-25), at which point the conductivity gain and aluminum corrosion risk reach the optimal balance. When the proportion is 0% (Comparative Example 3), the FSI... - The derivative component was missing, and the capacity retention was 80.0% after 600 weeks; when it accounted for 45% (Comparative Example 4), the ability of LiPF6 to passivate aluminum was diluted, and FSI was reduced. - In the high-potential pitting corrosion of aluminum alloy current collector and positive electrode aluminum foil, the DCIR deteriorated to 5.1mΩ in the mid-to-late stage and the capacity retention rate was only 65.0% at 600 cycles, indicating that the molar fraction of LiFSI in the range of 10-30% is the optimal choice for conductivity gain and aluminum corrosion risk.
[0167] A comparison of Examples 1 and 8 shows that when the number of parallel welds in each weld unit is reduced from 3 to 2, the effective welding area between the negative electrode tab and the negative electrode current collector decreases, and the contact resistance at the welding interface increases. This results in the battery's initial coulombic efficiency decreasing from 93.5% to 93.3%, AC internal resistance increasing from 2.5mΩ to 2.9mΩ, DC internal resistance increasing from 2.8mΩ to 3.2mΩ, temperature rise rate under 10C high-current discharge conditions increasing from 2.9℃ / min to 3.2℃ / min, peak surface temperature of the casing and current collector end face increasing from 72℃ to 76℃, and the 600-cycle capacity retention decreasing from 89.0% to 87.5%, and the 800-cycle capacity retention decreasing from 84.0% to 82.0%. Therefore, having more than 2 parallel welds in a weld unit can ensure sufficient parallel flow channels and suppress localized heat generation without excessively occupying the effective area of the negative electrode current collector.
[0168] As can be seen from the comparison of Examples 1, 9-11 and Comparative Example 7, the first pre-charging stage allows each functional additive to be reduced sequentially and slowly according to the reduction kinetics and diffusion control order, forming a lithium fluoride layer, a flexible organic polymer layer and a nitrogen oxide layer from bottom to top on the surface of the negative electrode current collector, thus forming an SEI film. Specifically, FEC and VC are preferentially adsorbed on the surface of the negative electrode current collector and have fast reduction kinetics, so they are preferentially reduced in the first low-current pre-charging stage, forming a dense lithium fluoride inner layer and a flexible organic polymer middle layer from bottom to top. LiNO3 has low solubility in carbonate solvents and its reduction is diffusion-controlled, so it continues to migrate to the outer surface of the SEI in the second constant-pressure stage and is reduced to form a nitrogen oxide outer layer. Thus, a three-layer sequence structure consistent with the technical solution of this application is obtained, that is, the lithium fluoride layer, the flexible organic polymer layer and the nitrogen oxide layer are sequentially arranged in the direction away from the negative electrode current collector. When the pre-charge current increases from 0.01C to 0.05C, the film formation rate accelerates, the density of the lithium fluoride layer decreases slightly, and the first-cycle efficiency drops from 93.8% to 92.5%. It should be noted that the SEI film formed under the 0.01C condition is the most dense and complete, hence the highest first-cycle efficiency, but the film layer is relatively thicker, and its ion transport impedance is comparable to that under the 0.05C condition (both DC internal resistances are 2.9mΩ). Under the 0.02-0.03C condition, the best balance between density and film thickness can be achieved, with the lowest DC internal resistance (2.8mΩ). If the pre-charge is canceled and replaced with a one-step direct charge at 0.5C (Comparative Example 7), the multi-component functional additives are simultaneously and disorderedly reduced, the SEI is loose and porous, the proportion of organic components is too high, and electron tunneling continuously triggers electrolyte reduction, resulting in a first-cycle efficiency of only 86.5% and a 600-cycle capacity retention of 72.0%. This proves that two-step formation is a necessary condition for the quaternary functional additive system to exert a synergistic effect.
[0169] As shown in Examples 12-18, replacing FEC with DFEC or FEMC, replacing DTD with TS, replacing LiNO3 with KNO3, using TTE as a fluorinated ether co-solvent and LiPO2F2 as an auxiliary additive, or using a combination solvent of ethylene carbonate / diethyl carbonate / methyl ethyl carbonate, all can achieve comprehensive performance of ≥90% initial efficiency, ≥85% capacity retention at 600 cycles, ACR / DCIR at 2-4 mΩ, ≤80°C surface peak temperature at 10°C, and ≥80% capacity retention at 800 cycles (initial efficiency 93.0%-93.8%, 600-cycle capacity retention 88.2%-89.5%, 800-cycle capacity retention 83.0%-84.6%), indicating that the multifunctional composite electrolyte quaternary functional additive system of this application has wide applicability.
[0170] As can be seen from the comparison of Example 1, Comparative Example 5 and Comparative Example 6, if there are 12 welds evenly distributed circumferentially between the negative electrode tab and the negative electrode current collector, without grouping, the welds are discretely distributed and cannot form a parallel current-conducting network. The current is concentrated at each discrete weld position, and the current dispersion and conduction ability are reduced, resulting in a decrease in the battery's initial coulombic efficiency, an increase in AC internal resistance and DC internal resistance, and local heat generation concentration during 10C high-current discharge, with an increase in the temperature rise rate and the peak temperature of the casing. During cycling, the discrete welds are subjected to repeated charging and discharging stress, and microcracks and contact deterioration are prone to occur at the welds, resulting in low capacity retention and decreased long-term cycle stability. If there is no annular weld in the central area of the negative electrode current collector, there is a lack of mechanical support and conductive channel at the center position, and all loads and currents are borne by the outer circumferential welds. The current collector is prone to warping, the risk of weld overload deterioration is aggravated, the battery internal resistance is further increased, the temperature rise is higher, and the cycle life is deteriorated.
[0171] In summary, the technical solution provided in this application enables the 21650 all-tab cylindrical battery without a negative electrode to stably achieve the following comprehensive performance: first-cycle efficiency ≥90%, 600-cycle capacity retention ≥85%, ACR / DCIR both within 2-4mΩ, 10C peak temperature ≤80℃, and 800-cycle capacity retention ≥80%.
[0172] It should be noted that this application illustrates the process method through the above embodiments, but this application is not limited to the above process steps, that is, it does not mean that this application must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to this application, equivalent substitutions of the raw materials used in this application, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of this application.
Claims
1. A negative electrode-free lithium-ion battery, characterized in that, The negative electrode-free lithium-ion battery includes a metal casing, a cell disposed within the metal casing, a positive electrode current collector, and a negative electrode current collector; The battery cell includes: Positive electrode sheet; A negative electrode current collector without negative electrode active material, the negative electrode current collector having a negative electrode tab, and multiple sets of weld seam units distributed circumferentially between the negative electrode tab and the negative electrode current collector disk; The central region of the negative electrode current collector is provided with an annular ring weld, located at the circumferential edge of the central through hole of the negative electrode current collector; Diaphragm; A multifunctional composite electrolyte, comprising lithium salt, organic solvent and functional additives; wherein the multifunctional composite electrolyte comprises, along the direction away from the negative electrode current collector, a stacked lithium fluoride layer, a flexible organic polymer layer and a nitrogen oxide layer in the SEI film formed in situ on the surface of the negative electrode current collector.
2. The negative electrode-free lithium-ion battery according to claim 1, characterized in that, The lithium salt includes any one or a combination of at least two of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium dioxaborate, or lithium difluorophosphate, preferably a combination of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide. And / or, in the multifunctional composite electrolyte, the concentration of lithium salt is 0.8-1.2 mol / L; And / or, the organic solvent includes any one or a combination of at least two of ethylene carbonate, methyl ethyl carbonate, diethyl carbonate, or dimethyl carbonate, preferably a combination of ethylene carbonate, methyl ethyl carbonate, and dimethyl carbonate, or a combination of ethylene carbonate, diethyl carbonate, and methyl ethyl carbonate. And / or, the functional additives include fluorocarbonates, cyclic sulfates, vinylene carbonates, and metal nitrates; And / or, the multifunctional composite electrolyte further includes an auxiliary film-forming lithium salt; And / or, the multifunctional composite electrolyte further includes a fluorinated ether cosolvent and / or auxiliary additives; And / or, the thickness ratio of the lithium fluoride layer, the flexible organic polymer layer, and the oxynitride layer is 1:(2-5):(1-3).
3. The negative electrode-free lithium-ion battery according to claim 2, characterized in that, In the combination of lithium hexafluorophosphate and lithium difluorosulfonyl imide, the molar ratio of lithium hexafluorophosphate to lithium difluorosulfonyl imide is (70-90):(10-30), preferably (75-85):(15-25); And / or, the fluorocarbonate includes any one or a combination of at least two of fluoroethylene carbonate, difluoroethylene carbonate, or fluoroethyl methyl carbonate; And / or, the cyclic sulfate esters include any one or a combination of at least two of vinylene sulfate, vinylene sulfate homologues, or propylene sulfate; And / or, the metal nitrate includes any one or a combination of at least two of lithium nitrate, potassium nitrate, or cesium nitrate; And / or, based on the total mass of the lithium salt and organic solvent, the component content in the functional additive is as follows: Fluorocarbonate 3-12 wt%, preferably 5-10 wt%, more preferably 6-8 wt%; Cyclic sulfate esters: 0.3-2.5 wt%, preferably 0.8-2 wt%, more preferably 1-1.5 wt%; Vinylene carbonate 0.2-1.8 wt%, preferably 0.5-1.5 wt%, more preferably 0.8-1.2 wt%; Metal nitrate 0.3-2 wt%, preferably 0.5-1.5 wt%, more preferably 0.8-1.2 wt%; And / or, based on the total mass of the lithium salt and organic solvent, the mass content of the auxiliary film-forming lithium salt is 0.1-0.5 wt%; And / or, the auxiliary film-forming lithium salt includes lithium difluorooxalate borate; And / or, based on the total mass of the lithium salt and the organic solvent, the mass content of the fluorinated ether co-solvent is 5-15 wt%; And / or, based on the total mass of the lithium salt and organic solvent, the mass content of the auxiliary additive is 0.01-0.5 wt%; And / or, the auxiliary additives include any one or a combination of at least two of lithium difluorophosphate, 1,3-propanesulfonate lactone, or p-toluenesulfonate.
4. The negative electrode-free lithium-ion battery according to any one of claims 1-3, characterized in that, The weld unit includes at least two parallel welds; And / or, in the weld unit, the shape of the weld includes any one or a combination of at least two of the following: wavy, radial, or spiral. And / or, in the weld unit, the width of any weld is 0.25-0.35mm and the length is 5-7mm; And / or, the thickness of the negative electrode current collector is 0.15-0.3 mm; And / or, the outer diameter of the annular weld is 4.8-5.4 mm; And / or, the weld width of the circumferential weld is 0.3-0.36 mm.
5. The negative electrode-free lithium-ion battery according to any one of claims 1-4, characterized in that, The negative electrode current collector is any one of the following: optical copper foil, carbon-coated copper foil, lithium-loving modified copper foil, or three-dimensional porous copper foil; And / or, the positive electrode includes a positive current collector and a positive active material layer disposed on at least one side surface of the positive current collector; And / or, the positive current collector includes a current collector body and lead-out tabs extending outward from the current collector body; the current collector body is provided with multiple sets of weld seam units for welding to the positive tabs of the positive electrode sheet, the multiple sets of weld seam units are arranged at intervals along the circumference of the current collector body; the current collector body is provided with a central hole at the center, and the current collector body is also provided with multiple peripheral holes; And / or, the diaphragm includes a porous base membrane and a ceramic coating disposed on both sides of the porous base membrane; And / or, the negative electrode-free lithium-ion battery has a full tab structure; And / or, the specifications of the metal casing are any one of 21650, 18650, 21700, 4680, 4695 or 46120.
6. The negative electrode-free lithium-ion battery according to any one of claims 1-5, characterized in that, The internal resistance of the negative electrode-free lithium-ion battery is 2-4 mΩ, and its internal resistance is 2-4 mΩ, respectively. And / or, the negative electrode-free lithium-ion battery has a temperature rise rate ≤ 4℃ / min under 10C discharge conditions and a surface peak temperature ≤ 80℃.
7. The negative electrode-free lithium-ion battery according to any one of claims 1-6, characterized in that, The negative electrode-free lithium-ion battery exhibits a first-cycle coulombic efficiency ≥90% under conditions of 25±5℃ and 0.1C charge / 0.1C discharge. And / or, the negative electrode-free lithium-ion battery retains ≥85% of its capacity after 600 cycles at 25±5℃ and 0.5C charge / 0.5C discharge conditions; And / or, the negative electrode-free lithium-ion battery retains ≥80% of its capacity after 800 cycles at 25±5℃ and 1C charge / 1C discharge conditions.
8. A method for preparing a negative electrode-free lithium-ion battery as described in any one of claims 1-7, characterized in that, The preparation method includes the following steps: The device provides a positive electrode sheet, a negative electrode current collector, a separator, and a multifunctional composite electrolyte; the negative electrode current collector has a negative electrode tab; the multifunctional composite electrolyte includes lithium salt, organic solvent, and functional additives. The positive electrode, the separator, and the negative current collector are assembled to obtain a battery cell; A positive current collector and a negative current collector are provided; the positive electrode tab of the positive electrode sheet is welded to the positive current collector; the negative electrode tab of the battery cell is welded to the negative current collector through multiple sets of weld seam units distributed circumferentially along the negative current collector, and at the same time, a ring weld is performed along the circumferential edge of the central through hole of the negative current collector to form a ring weld. The welded battery cell is placed into a metal casing, and the positive current collector is welded to the cap of the metal casing to achieve electrical connection. The negative current collector is welded to the bottom of the metal casing to achieve electrical connection. The multifunctional composite electrolyte is then injected. A multi-step formation process is performed to form an SEI film in situ on the surface of the negative electrode current collector using the multifunctional composite electrolyte. The SEI film comprises a stacked lithium fluoride layer, a flexible organic polymer layer, and a nitrogen oxide layer along the direction away from the negative electrode current collector.
9. The preparation method according to claim 8, characterized in that, The specific steps of the multi-step transformation include: At an ambient temperature of 35±3℃, the first step is to precharge to 3.6-3.9V at 0.01-0.05C, the second step is to charge to 4.2V at 0.05-0.1C and then cut off at a constant voltage of 0.01C, followed by discharge.
10. An electrical appliance, characterized in that, The electrical device includes a negative electrode-free lithium-ion battery as described in any one of claims 1-7 or a negative electrode-free lithium-ion battery obtained by the preparation method as described in any one of claims 8-9.