A method for regenerating a positive electrode.
By using a pyrolysis passivation process combining electromagnetic heating and microwave heating, lithium iron phosphate cathode sheets are crushed and aluminum foil is removed. A mixture of carbon dioxide and hydrogen is then introduced to optimize the crystal structure, solving the problem of low pyrolysis efficiency in existing technologies and achieving efficient cathode sheet regeneration and repair.
Patent Information
- Application Number
- CN202611455895.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies for regenerating and repairing lithium iron phosphate cathode sheets using high-temperature pyrolysis processes have low thermal efficiency, resulting in low regeneration and repair efficiency.
A pyrolysis passivation process combining electromagnetic heating and microwave heating is used to break down the positive electrode sheet, remove the aluminum foil, and then introduce a mixture of carbon dioxide and hydrogen under oxygen-free conditions. The positive electrode powder is then repaired by microwave heating, which optimizes the crystal structure and restores the electrochemical activity of the material.
It improves the regeneration and repair efficiency of lithium iron phosphate cathode sheets, ensures uniform heating of cathode powder, removes residual carbon, stabilizes iron valence state, repairs crystal defects, and achieves efficient regeneration and repair.
Smart Images

Figure CN123073244A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of electrode regeneration technology, and more particularly to a method for regenerating a positive electrode. Background Technology
[0002] Discarding lithium iron phosphate batteries after they have reached the end of their lifespan can cause environmental pollution. Therefore, materials used in lithium iron phosphate batteries, such as the lithium iron phosphate cathode sheet, are usually recycled and repaired to facilitate reuse and reduce environmental pollution.
[0003] However, existing technologies for regenerating and repairing lithium iron phosphate cathode sheets through high-temperature pyrolysis have low thermal efficiency, resulting in low regeneration and repair efficiency for lithium iron phosphate cathode sheets. Summary of the Invention
[0004] The purpose of this application is to provide a method for regenerating cathode sheets, aiming to solve the problem of how to improve the regeneration and repair efficiency of lithium iron phosphate cathode sheets.
[0005] To achieve the above objectives, this application adopts the following technical solution: This application provides a method for regenerating a positive electrode sheet. The method includes: crushing the positive electrode sheet and removing the aluminum foil from the positive electrode sheet to obtain clean positive electrode powder; performing pyrolysis passivation treatment on the clean positive electrode powder under anaerobic conditions using an electromagnetic heating pyrolysis process; and introducing a mixture of carbon dioxide and hydrogen into the pyrolysis passivated positive electrode powder under anaerobic conditions, and then repairing the pyrolysis passivated positive electrode powder using a microwave heating repair process.
[0006] The cathode regeneration method provided in this application involves crushing the cathode and removing the aluminum foil. The clean cathode powder is then subjected to pyrolysis passivation via electromagnetic heating. Finally, the passivated cathode powder is repaired using microwave heating. Microwave heating repair has high thermal efficiency, allowing for better and more uniform heating of the cathode powder, thus improving pyrolysis. Simultaneously, a mixture of carbon dioxide and hydrogen is introduced during pyrolysis. Carbon dioxide removes residual carbon from the cathode powder surface while preserving the carbon layer on the electrochemical carbon layer surface, and reconstructs the lithium iron phosphate lattice, restoring the material's electrochemical activity and improving the regeneration and repair effect. Hydrogen ensures the stability of the iron valence state within the cathode powder lattice, repairing the iron valence state and preventing degradation at higher temperatures. By continuously accumulating defects and simultaneously promoting lithium-ion insertion into the crystal lattice, crystal defects such as lithium deficiency and lithium iron inversion are repaired, thereby improving the regeneration and repair effect of cathode powder. It can stably control the pyrolysis temperature of cathode powder, ensuring that cathode powder can be effectively pyrolyzed, and can achieve better regeneration and repair effects on cathode powder.
[0007] In some embodiments, the repair process of the pyrolysis passivated cathode powder by microwave heating includes: conveying the pyrolysis passivated cathode powder into a microwave repair furnace, and heating the microwave repair furnace to between 650°C and 680°C and holding it at that temperature for 40 min to 90 min.
[0008] In some embodiments, the process of introducing a mixture of carbon dioxide and hydrogen into the pyrolysis passivation treated cathode powder includes: introducing a mixture of carbon dioxide and hydrogen at a temperature above 500°C and a carbon dioxide to hydrogen ratio of 90:5 to 90:15 into a microwave repair furnace, while ensuring that 10 Nm³ to 30 Nm³ of hydrogen is introduced per ton of cathode powder.
[0009] In some embodiments, the pyrolysis passivation treatment of clean cathode powder by electromagnetic heating pyrolysis process includes: conveying the clean cathode powder into an electromagnetic heating rotary kiln, and heating the electromagnetic heating rotary kiln to between 400°C and 500°C and holding it at that temperature for 60 min to 120 min.
[0010] In some embodiments, the pyrolysis passivation treatment of clean cathode powder by electromagnetic heating pyrolysis process further includes: introducing a mixture of carbon dioxide and hydrogen gas with a temperature above 500°C and a carbon dioxide to hydrogen ratio of 90:5 to 90:15 into the electromagnetic heating rotary kiln.
[0011] In some embodiments, removing the aluminum foil from the positive electrode sheet to obtain clean positive electrode powder includes: The binder of the broken positive electrode sheet is destroyed by high-temperature pyrolysis, so that the aluminum foil is separated from the lithium iron phosphate material. The mixture of aluminum foil and lithium iron phosphate material is stripped, crushed, and sieved to obtain clean cathode powder.
[0012] In some embodiments, destroying the binder of the broken positive electrode sheet by high-temperature pyrolysis includes: The crushed positive electrode sheet is mixed and stirred with lithium hydroxide solution to wet the positive electrode sheet; The positive electrode sheet after being wetted is pyrolyzed under oxygen-free conditions by superheated steam in order to destroy the binder of the positive electrode sheet. The positive electrode sheet after the adhesive has been damaged is then cooled and dried under oxygen-free conditions.
[0013] In some embodiments, destroying the binder of the broken positive electrode sheet by high-temperature pyrolysis includes: conveying the broken positive electrode sheet into a rotary kiln and heating the rotary kiln to 420°C-460°C under oxygen-free conditions and holding it at that temperature for 60-90 minutes to destroy the binder of the positive electrode sheet; and cooling the positive electrode sheet after the binder has been destroyed under oxygen-free conditions.
[0014] In some embodiments, the regeneration method further includes: conveying the repaired cathode powder to an oxygen-free closed cooling device for cooling; and crushing, sieving, and demagnetizing the cooled cathode powder.
[0015] In some embodiments, the regeneration method further includes: exchanging heat between a mixture of carbon dioxide and hydrogen gas and the cathode powder in an oxygen-free closed cooling device to heat the mixture of carbon dioxide and hydrogen gas to above 500°C; passing the heated mixture of carbon dioxide and hydrogen gas into the cathode powder after pyrolysis passivation treatment to repair the cathode powder; and passing the repaired mixture of carbon dioxide and hydrogen gas into an electromagnetically heated rotary kiln. Attached Figure Description
[0016] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 This is a schematic flowchart illustrating a method for regenerating a positive electrode sheet according to an embodiment of this application; Figure 2 for Figure 1 The flowchart of step S1 is shown below; Figure 3 for Figure 2 A flowchart illustrating step S11; Figure 4 for Figure 2 Another flowchart for step S11. Detailed Implementation
[0018] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0019] The terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, unless otherwise stated, "a plurality of" means two or more.
[0020] In the description of this specification, specific features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments or examples.
[0021] Please see Figure 1 , Figure 1 This is a schematic flowchart illustrating a method for regenerating a positive electrode sheet according to an embodiment of this application. This application provides a method for regenerating a positive electrode sheet for repairing the positive electrode sheet of a lithium iron phosphate battery. The regeneration of the positive electrode sheet (hereinafter referred to as the positive electrode sheet) involves separating the aluminum foil and materials such as lithium, iron, and phosphorus from the positive electrode sheet, thereby regenerating and recycling the lithium iron phosphate materials such as lithium, iron, and phosphorus.
[0022] In some embodiments, the method for regenerating the positive electrode includes: S1: The positive electrode sheet is crushed and the aluminum foil in the positive electrode sheet is removed to obtain clean positive electrode powder. The positive electrode powder is the above-mentioned lithium iron phosphate material in powder form.
[0023] After the positive electrode sheet is crushed, it can be made into smaller sheet-like or powdery particles, which facilitates the subsequent removal of aluminum foil from the positive electrode sheet and the repair of the positive electrode powder.
[0024] In some examples, the process of crushing the positive electrode sheet may include: feeding the clean positive electrode sheet to a shredding device such as a shearing electrode shredder, a hammer-type electrode crusher, or a rotary blade electrode pulverizer to shear and shred the positive electrode sheet into sheet-like particles, such as shredding them into electrode particles of about 100 mm.
[0025] In some examples, please refer to Figure 2 , Figure 2 for Figure 1 The flowchart for step S1 is shown. Removing the aluminum foil from the positive electrode sheet to obtain clean positive electrode powder may include: S11: The binder of the broken positive electrode sheet is destroyed by high-temperature pyrolysis, so that the aluminum foil is separated from the lithium iron phosphate material.
[0026] High-temperature pyrolysis can destroy the binder in the positive electrode, thereby separating the aluminum foil from the lithium iron phosphate material. This allows for further separation of the aluminum foil from the lithium iron phosphate material, resulting in clean lithium iron phosphate material.
[0027] S12: The mixture of aluminum foil and lithium iron phosphate material is stripped, crushed and sieved to obtain clean cathode powder.
[0028] After the aluminum foil and lithium iron phosphate material are separated, a mixture of aluminum foil and lithium iron phosphate material is formed. At this point, it is necessary to separate the aluminum foil and lithium iron phosphate material to obtain clean lithium iron phosphate material, so as to facilitate the regeneration and repair of lithium iron phosphate material.
[0029] Specifically, aluminum foil and lithium iron phosphate material can be separated through peeling, crushing and sieving. The separated lithium iron phosphate material can be in powder form, i.e., clean cathode powder.
[0030] In some examples, the stripping, crushing, and sieving process of the mixture of aluminum foil and lithium iron phosphate material may include: rubbing and stripping the mixture of aluminum foil and lithium iron phosphate material using a rubbing and stripping device to fully separate the aluminum foil from the lithium iron phosphate material, thereby improving the cleanliness of the lithium iron phosphate material.
[0031] The kneading and peeling device may include a housing and spiral blades mounted on the housing. Striking bars are mounted on the shaft of the spiral blades and also on the inner surface of the housing. When the mixture enters the kneading and peeling device, the rotation of the spiral blades propels the mixture, achieving conveying of the mixture. Simultaneously, the spiral blades also squeeze and knead the mixture. During the conveying process, the striking bars on the shaft and housing strike the mixture, thereby effectively separating the aluminum foil from the lithium iron phosphate material. For example, the rotational speed of the spiral blades can be 300-500 revolutions per minute (RPM), such as 300, 350, 400, 450, 500 RPM, etc., to ensure a consistent conveying speed and better kneading and peeling of the mixture. Furthermore, the housing may have multiple sieve holes with a diameter of 1.5-4 mm to initially separate the aluminum foil and lithium iron phosphate material. For example, the sieve hole diameters can be 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, etc.
[0032] Then, the mixture of aluminum foil and lithium iron phosphate material after the glass crumpling process is sorted, for example by cyclone separation or strong magnetic separation, so as to demagnetize and separate the aluminum foil and lithium iron phosphate material.
[0033] Next, the separated lithium iron phosphate material is pulverized, for example, by using an eddy current mill to further pulverize the lithium iron phosphate material to obtain a finer powdered lithium iron phosphate material. For example, the particle size of the powder can be 1-3.5 micrometers, such as 1 micrometer, 1.5 micrometers, 2 micrometers, 2.5 micrometers, 3 micrometers, 3.5 micrometers, etc. Finally, the lithium iron phosphate material is sieved again by cyclone separation, and then subjected to magnetic impurity removal treatment by a strong magnetic separation device, such as a strong magnetic separation device with a magnetic strength of 12000GS, to finally obtain clean powdered lithium iron phosphate material, that is, the clean cathode powder mentioned above.
[0034] By peeling, crushing, and sieving the mixture of aluminum foil and lithium iron phosphate material, a deeper peeling and sieving process can be performed to ensure the cleanliness of the lithium iron phosphate material, thereby ensuring the effectiveness of subsequent regeneration and repair of the lithium iron phosphate material.
[0035] In some embodiments, please refer to Figure 3 , Figure 3 for Figure 2 A schematic diagram of step S11. Destroying the binder of the broken positive electrode sheet through high-temperature pyrolysis includes: S111A: The crushed positive electrode sheet is mixed and stirred with lithium hydroxide solution to wet the positive electrode sheet.
[0036] Lithium hydroxide can be mixed with pure water to prepare a lithium hydroxide solution with a pH value of 9-9.5. Then, 30-50 kg of the lithium hydroxide solution is added to each ton of positive electrode sheet and stirred evenly to wet it. This allows lithium hydroxide to be evenly coated onto the surface of the shredded positive electrode sheet, thus performing a lithium replenishment treatment on the surface of the positive electrode sheet, which facilitates the subsequent repair of the positive electrode powder.
[0037] For example, the pH value of the lithium hydroxide solution prepared by mixing lithium hydroxide with pure water can be 9, 9.2, 9.4, 9.5, etc. The weight of lithium hydroxide solution mixed into each ton of electrode can be 30kg, 35kg, 40kg, 45kg, 50kg, etc.
[0038] S112A: The positive electrode sheet after wet treatment is pyrolyzed under oxygen-free conditions by superheated steam to destroy the binder of the positive electrode sheet.
[0039] After the wet treatment, the positive electrode sheet is conveyed to a closed superheated steam equipment, such as a nitrogen-protected vacuum feeder or a nitrogen-protected screw feeder, via an oxygen-closed feeding device. Superheated steam is then introduced into the superheated steam equipment to decompose the positive electrode sheet and break down the binder. Before introducing superheated steam, high-temperature nitrogen gas (above 200°C, such as 200°C, 250°C, 300°C, etc.) is introduced into the superheated steam equipment to avoid affecting its temperature and to ensure that the superheated steam equipment is in an oxygen-closed environment. For example, the oxygen content in the superheated steam equipment is reduced to below 50 ppm (e.g., 20 ppm, 30 ppm, 40 ppm, 50 ppm, etc.) by the high-temperature nitrogen gas.
[0040] The superheated steam introduced into the superheated steam equipment has a pressure greater than or equal to 0.1 MPa, a temperature between 250℃ and 300℃, and a pyrolysis time controlled between 20 min and 40 min. This ensures sufficient breakdown of the binder on the positive electrode sheet and avoids excessively long decomposition time by the superheated steam, which could lead to corrosion of the aluminum foil. For example, the superheated steam pressure can be 0.1 MPa, 0.15 MPa, 0.2 MPa, etc. The superheated steam temperature can be 250℃, 270℃, 280℃, 300℃, etc. The pyrolysis time can be 20 min, 25 min, 30 min, 35 min, 40 min, etc.
[0041] In some examples, heating devices such as gas heating devices or electric heating devices can be installed on the outside of the superheated steam equipment to ensure that the temperature of the superheated steam equipment is sufficient to fully destroy the adhesive of the positive electrode sheet.
[0042] In some examples, the superheated steam equipment may also be equipped with a conveying screw to stir and transport the positive electrode sheet, so that the positive electrode sheet can be fully heated to better break down the binder of the positive electrode sheet. The conveying screw can rotate at a speed of 2 to 10 revolutions per minute, such as 2, 4, 6, 8, 10 revolutions per minute, etc.
[0043] Superheated steam can effectively disrupt the binder structure within the positive electrode, causing the lithium iron phosphate active material to separate and peel off from the aluminum foil current collector, thus achieving initial separation of the positive electrode material.
[0044] S113A: The positive electrode sheet after the adhesive has been destroyed is cooled and dried under oxygen-free conditions.
[0045] After the superheated steam breaks down the binder of the positive electrode sheet, the bonded positive electrode sheet can be conveyed through an oxygen-free conveying device, such as a nitrogen-protected screw feeder, to an oxygen-free cooling device, such as a pyrolysis cooling furnace, for cooling. The temperature of the positive electrode sheet is reduced to below 145℃ (e.g., 145℃, 140℃, 130℃, 120℃, 110℃, 100℃, etc.). Then, it is conveyed through an oxygen-free conveying device, such as a nitrogen-protected screw feeder, to a drying device, such as a drying oven, for drying and dehydration until the moisture content of the positive electrode sheet is below 3% (e.g., 1%, 2%, 3%, etc.). This ensures that the positive electrode sheet, after the binder is broken down, is in a relatively dry state, facilitating further crushing and separation processing.
[0046] In other embodiments, please refer to Figure 4 , Figure 4 for Figure 2 Another schematic diagram of step S11. Destroying the binder of the broken positive electrode sheet through high-temperature pyrolysis includes: S111B: The crushed positive electrode sheet is conveyed into a rotary kiln, and the kiln is heated to 420℃-460℃ under oxygen-free conditions and held for 60-90 minutes to break down the binder of the positive electrode sheet. For example, the temperature of the rotary kiln can be 420℃, 440℃, 450℃, 460℃, etc. The holding time can be 60 minutes, 70 minutes, 80 minutes, 90 minutes, etc.
[0047] The positive electrode sheet is shredded into flake-shaped particles between 20mm and 80mm (e.g., 20mm, 40mm, 60mm, 80mm, etc.), and then fed into a rotary kiln. Nitrogen gas is introduced into the rotary kiln to reduce the oxygen content inside the kiln to below 10ppm (e.g., 3ppm, 5ppm, 8ppm, 10ppm, etc.). The temperature of the rotary kiln is controlled between 420℃ and 460℃ and held for 60min to 90min. This high-temperature pyrolysis decomposes the binder in the lithium iron phosphate material of the positive electrode sheet, causing the binder to crack and lose its bonding force at the binder interface, thus facilitating the separation of the lithium iron phosphate material from the aluminum foil.
[0048] S112B: The positive electrode sheet after the binder is destroyed is cooled under oxygen-free conditions.
[0049] After the binder is decomposed, the positive electrode sheet is conveyed to the next equipment, such as a kneading and peeling equipment, in an oxygen-closed discharge equipment, such as a nitrogen-protected screw feeder. During this process, the positive electrode sheet can be cooled to below 80°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, etc.
[0050] The above steps can effectively disrupt the binder structure within the positive electrode, causing the lithium iron phosphate active material to separate and peel off from the aluminum foil current collector, thus achieving initial separation of the positive electrode material. Furthermore, cooling the material after separation from the aluminum foil facilitates further processing of the mixture of lithium iron phosphate material and aluminum foil.
[0051] S2: Under anaerobic conditions, the clean positive electrode powder is subjected to pyrolysis passivation treatment through electromagnetic heating pyrolysis process.
[0052] Oxygen-free conditions ensure the safety of the cathode powder pyrolysis process. Electromagnetic heating utilizes the eddy current effect to generate heat from the cathode powder itself, resulting in high heat utilization efficiency. This allows for more effective pyrolysis passivation of the cathode powder, improving the passivation treatment effect. Pyrolysis passivation of the cathode powder can optimize its crystal structure, thereby enhancing the regeneration and repair capabilities.
[0053] In some examples, the pyrolytic passivation treatment of clean cathode powder using electromagnetic heating pyrolysis includes: feeding the clean cathode powder into an electromagnetically heated rotary kiln, and heating the rotary kiln to between 400℃ and 500℃ and holding it at that temperature for 60 min to 120 min. For example, the temperature of the electromagnetically heated rotary kiln can be 400℃, 420℃, 450℃, 480℃, 500℃, etc. The holding time can be 60 min, 80 min, 100 min, 120 min, etc.
[0054] The electromagnetic heating pyrolysis process allows for precise temperature control of the electromagnetic heating rotary kiln between 400℃ and 500℃. This eliminates the need for extremely high temperatures to achieve pyrolysis passivation of the cathode powder, and provides better and more stable temperature control. Holding the cathode powder at 400℃-500℃ for 60-120 minutes in the electromagnetic heating rotary kiln promotes better pyrolysis passivation, thereby improving the regeneration and repair effect of the cathode powder.
[0055] In some examples, the heating rate of the electromagnetically heated rotary kiln can be controlled between 4℃ / min and 6℃ / min during the heating process. For example, the heating rate can be 4℃ / min, 5℃ / min, 6℃ / min, etc. A slight positive pressure, such as 30-60 Pa, is maintained inside the electromagnetically heated rotary kiln. For example, the pressure can be 30 Pa, 40 Pa, 50 Pa, 60 Pa, etc. For instance, nitrogen gas can be introduced into the electromagnetically heated rotary kiln to ensure an oxygen-free environment and maintain the pressure inside the kiln.
[0056] In some examples, the pyrolytic passivation treatment of clean cathode powder via electromagnetic heating pyrolysis further includes: introducing a mixture of carbon dioxide and hydrogen gas at a temperature above 500°C and a carbon dioxide to hydrogen ratio of 90:5-90:15 into an electromagnetically heated rotary kiln. For example, the temperature of the carbon dioxide and hydrogen gas can be 500°C, 520°C, 550°C, 580°C, 600°C, etc. The carbon dioxide to hydrogen ratio can be 90:5, 90:8, 90:10, 90:12, 90:15, etc.
[0057] In the pyrolysis passivation treatment of cathode powder using electromagnetic heating, a mixture of carbon dioxide and hydrogen is introduced into the electromagnetically heated rotary kiln. Maintaining the carbon dioxide:hydrogen ratio at 90:5-90:15 ensures that the amounts of carbon dioxide and hydrogen are within a suitable range. Carbon dioxide acts as an atmosphere conditioner, and the high-temperature reaction between carbon and carbon dioxide generates carbon monoxide, removing residual carbon from the surface of the cathode powder while preserving the carbon layer on the electrochemical carbon layer surface. This prevents excessive reduction and the formation of iron phosphide, further improving the cleanliness and repair effect of the cathode powder. Furthermore, carbon dioxide optimizes heat transfer within the electromagnetically heated rotary kiln, inhibits high-temperature particle agglomeration, and facilitates repair. Inverse defects promote lithium solid phase expansion, enabling lattice reconstruction of lithium iron phosphate and restoring the electrochemical activity of the material, thereby improving the regeneration and repair effect of cathode powder.
[0058] Hydrogen has a reducing effect and can inhibit... It is oxidized again (2FePO4 + Li2O + H2 → 2LiFePO4 + H2O), ensuring the stability of the iron valence state within the lattice of the cathode powder and preventing it from becoming intact. The reaction should be avoided to prevent the formation of... Impurities, which will be generated by failure ( (Fe(II)O) partially reduced to To restore the iron valence state and prevent it from entering a higher temperature state. The continuous accumulation of defects simultaneously promotes lithium-ion insertion into the crystal lattice, repairing crystal defects such as lithium deficiency and lithium iron ion inversion, thereby improving the regeneration and repair effect of cathode powder.
[0059] The temperature of the mixed gas of carbon dioxide and hydrogen is kept above 500℃ to ensure the temperature of the mixed gas and prevent it from affecting the temperature of the electromagnetic heating rotary kiln, thereby ensuring the effect of the pyrolysis passivation treatment of the cathode powder.
[0060] S3: Under anaerobic conditions, a mixture of carbon dioxide and hydrogen gas is introduced into the pyrolysis passivation-treated cathode powder, and the pyrolysis passivation-treated cathode powder is repaired by a microwave heating repair process.
[0061] After undergoing pyrolysis passivation treatment via electromagnetic heating, the cathode powder is again fed into a microwave repair furnace for microwave heating repair. Microwave heating repair has a high heat utilization rate, allowing the cathode powder to be heated more uniformly and thus pyrolyzed more effectively. Simultaneously, a mixture of carbon dioxide and hydrogen is introduced during the pyrolysis process. Carbon dioxide removes residual carbon from the surface of the cathode powder while preserving the carbon layer on the electrochemical carbon layer surface, and it also reconstructs the lithium iron phosphate lattice, restoring the material's electrochemical activity and improving the regeneration and repair effect of the cathode powder. Hydrogen ensures the stability of the iron valence state within the cathode powder lattice, repairing the iron valence state and preventing it from reaching higher temperatures. The continuous accumulation of defects simultaneously promotes lithium-ion insertion into the crystal lattice, repairing crystal defects such as lithium deficiency and lithium iron ion inversion, thereby improving the regeneration and repair effect of cathode powder.
[0062] By crushing the positive electrode sheet and removing the aluminum foil, the clean positive electrode powder is then subjected to pyrolysis passivation treatment using an electromagnetic heating pyrolysis process. Finally, the pyrolysis passivated positive electrode powder is repaired using a microwave heating repair process. This process allows for stable control of the pyrolysis temperature of the positive electrode powder, ensuring effective pyrolysis and achieving better regeneration and repair effects.
[0063] In some examples, the microwave heating repair process for pyrolytic passivated cathode powder includes: conveying the pyrolytic passivated cathode powder into a microwave repair furnace, heating the furnace to between 650℃ and 680℃, and holding at that temperature for 40-90 minutes. For example, the temperature of the microwave repair furnace can be 650℃, 660℃, 670℃, 680℃, etc., and the holding time can be 40 minutes, 60 minutes, 80 minutes, 90 minutes, etc.
[0064] The cathode powder after pyrolysis passivation is heated to a temperature between 650℃ and 680℃ using a microwave heating repair process, and the holding time is between 40min and 90min. This ensures that the cathode powder has sufficient heating temperature and duration, allowing it to be better regenerated and repaired under high-temperature conditions by combining the effects of carbon dioxide and hydrogen, thus improving the regeneration and repair effect of the cathode powder.
[0065] In some examples, the heating rate of the microwave repair furnace can be controlled between 5℃ / min and 20℃ / min. For example, the heating rate can be controlled at 5℃, 10℃, 15℃, 20℃, etc. The microwave repair furnace can maintain a slight positive pressure of 30Pa-60Pa. For example, the pressure can be 30Pa, 40Pa, 50Pa, 60Pa, etc.
[0066] In some examples, the process of introducing a mixture of carbon dioxide and hydrogen into the pyrolysis passivation-treated cathode powder involves: introducing a carbon dioxide and hydrogen mixture at a temperature above 500°C with a carbon dioxide to hydrogen ratio of 90:5-90:15 into the microwave repair furnace, while simultaneously ensuring that 10 Nm³-30 Nm³ of hydrogen is introduced per ton of cathode powder. In some examples, the temperature of the carbon dioxide and hydrogen can be 500°C, 520°C, 550°C, 580°C, 600°C, etc. The carbon dioxide to hydrogen ratio can be 90:5, 90:8, 90:10, 90:12, 90:15, etc. The amount of hydrogen introduced per ton of cathode powder can be 10 Nm³, 15 Nm³, 20 Nm³, 25 Nm³, 30 Nm³, etc.
[0067] In the microwave pyrolysis repair process for cathode powder, a mixture of carbon dioxide and hydrogen is introduced into the microwave repair furnace, maintaining a carbon dioxide:hydrogen ratio of 90:5-90:15. This ensures that the amounts of carbon dioxide and hydrogen are within a suitable range, allowing carbon dioxide to act as an atmosphere conditioner. The high-temperature reaction between carbon dioxide and carbon dioxide generates carbon monoxide, removing residual carbon from the surface of the cathode powder while preserving the carbon layer on the electrochemical carbon layer. This prevents excessive reduction and the formation of iron phosphide, further improving the cleanliness and repair effect of the cathode powder. Furthermore, carbon dioxide optimizes heat transfer within the microwave repair furnace, inhibits high-temperature particle agglomeration, and facilitates repair. Inverse defects promote lithium solid phase expansion, enabling lattice reconstruction of lithium iron phosphate and restoring the electrochemical activity of the material, thereby improving the regeneration and repair effect of cathode powder.
[0068] Hydrogen has a reducing effect and can inhibit... It is oxidized again (2FePO4 + Li2O + H2 → 2LiFePO4 + H2O), ensuring the stability of the iron valence state within the lattice of the cathode powder and preventing it from becoming intact. The reaction should be avoided to prevent the formation of... Impurities, which will be generated by failure ( (Fe(II)O) partially reduced to To restore the iron valence state and prevent it from entering a higher temperature state. The continuous accumulation of defects simultaneously promotes lithium-ion insertion into the crystal lattice, repairing crystal defects such as lithium deficiency and lithium iron ion inversion, thereby improving the regeneration and repair effect of cathode powder.
[0069] The temperature of the mixed gas of carbon dioxide and hydrogen introduced is kept above 500℃ to ensure the temperature of the mixed gas and avoid affecting the temperature of the microwave repair furnace, thereby ensuring the effect of microwave repair of the cathode powder.
[0070] In some embodiments, the exhaust gas from the pyrolysis treatment of the positive electrode sheet using superheated steam, the exhaust gas from the pyrolysis passivation treatment of the positive electrode powder using electromagnetic heating pyrolysis, and the exhaust gas from the repair treatment of the positive electrode powder using microwave heating can be fed into a combustion furnace for combustion. The heat generated by the combustion furnace can be used to dry the positive electrode powder. The exhaust gas generated by the combustion furnace can be discharged after being treated by alkaline spraying and adsorption catalysis.
[0071] In some embodiments, after microwave heating repair treatment of the cathode powder, the cathode regeneration method further includes: conveying the repaired cathode powder to an oxygen-free closed cooling device for cooling treatment. For example, the oxygen-free closed cooling device can be a screw feeder. The repaired cathode powder is conveyed to the screw feeder, and nitrogen gas is simultaneously introduced into the screw feeder to isolate oxygen, thereby controlling the screw feeder to be in an oxygen-free environment. Cooling water channels can be provided on the outer casing of the screw feeder, and cooling water is introduced into the cooling water channels to cool the cathode powder.
[0072] The cooled cathode powder is then subjected to crushing, sieving, and demagnetization treatment. For example, the cooled cathode powder is further crushed by a crusher, then conveyed to a cyclone separator for sieving to further separate impurities, and finally conveyed to a demagnetizing device for demagnetization treatment to obtain pure cathode powder.
[0073] In this way, cooling down the repaired cathode powder facilitates further crushing, sieving, and demagnetizing treatment of the cathode powder. Further crushing, sieving, and demagnetizing treatment of the cathode powder can further improve the cleanliness of the cathode powder and enhance the regeneration and repair effect of the cathode sheet.
[0074] In some embodiments, the method for regenerating the positive electrode further includes: A mixture of carbon dioxide and hydrogen gas is exchanged with the cathode powder in an oxygen-free, sealed cooling device to heat the mixture to over 500°C. The heated mixture is then passed through the pyrolysis-passivated cathode powder to repair it. Finally, the repaired mixture is passed through an electromagnetically heated rotary kiln.
[0075] For example, the casing of the screw feeder can also be equipped with a gas channel to introduce a mixture of carbon dioxide and hydrogen into the gas channel. The high-temperature positive electrode powder inside the screw feeder exchanges heat with the mixture of carbon dioxide and hydrogen, thereby increasing the temperature of the mixture of carbon dioxide and hydrogen to above 500°C.
[0076] By exchanging heat between the cathode powder and a mixture of carbon dioxide and hydrogen in an oxygen-free, closed cooling device, the mixture of carbon dioxide and hydrogen is heated, eliminating the need for a separate heating device for the mixture and saving costs. Furthermore, the heated mixture of carbon dioxide and hydrogen is first passed through the pyrolysis-passivated cathode powder, and then through an electromagnetically heated rotary kiln, allowing for the reuse of the mixture and further reducing costs.
[0077] The above are merely specific embodiments of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.
Claims
1. A method for regenerating a positive electrode, characterized in that, include: The positive electrode sheet is crushed and the aluminum foil in the positive electrode sheet is removed to obtain clean positive electrode powder. Under anaerobic conditions, clean positive electrode powder is subjected to pyrolysis passivation treatment through electromagnetic heating pyrolysis process; Under anaerobic conditions, a mixture of carbon dioxide and hydrogen gas is introduced into the pyrolysis passivation-treated cathode powder, and the pyrolysis passivation-treated cathode powder is repaired by a microwave heating repair process.
2. The regeneration method according to claim 1, characterized in that, The repair process for the pyrolysis passivation-treated cathode powder using microwave heating includes: The pyrolysis passivation treated cathode powder is transported into a microwave repair furnace, and the microwave repair furnace is heated to 650℃-680℃ and held for 40min-90min.
3. The regeneration method according to claim 1 or 2, characterized in that, The mixture of carbon dioxide and hydrogen gas introduced into the pyrolysis passivation treated cathode powder includes: A mixture of carbon dioxide and hydrogen, with a temperature above 500℃ and a carbon dioxide to hydrogen ratio of 90:5-90:15, is introduced into the microwave repair furnace, while ensuring that 10Nm³-30Nm³ of hydrogen is introduced per ton of cathode powder.
4. The regeneration method according to claim 1, characterized in that, The pyrolysis passivation treatment of clean positive electrode powder by electromagnetic heating pyrolysis process includes: Clean cathode powder is conveyed into an electromagnetically heated rotary kiln, and the rotary kiln is heated to 400℃-500℃ and held for 60min-120min.
5. The regeneration method according to claim 4, characterized in that, The pyrolysis passivation treatment of clean positive electrode powder by electromagnetic heating pyrolysis process also includes: A mixture of carbon dioxide and hydrogen, with a temperature above 500℃ and a carbon dioxide to hydrogen ratio of 90:5-90:15, is introduced into an electromagnetically heated rotary kiln.
6. The regeneration method according to claim 1, characterized in that, The process of removing aluminum foil from the positive electrode sheet to obtain clean positive electrode powder includes: The binder of the broken positive electrode sheet is destroyed by high-temperature pyrolysis, so that the aluminum foil is separated from the lithium iron phosphate material. The mixture of aluminum foil and lithium iron phosphate material is stripped, crushed, and sieved to obtain clean cathode powder.
7. The regeneration method according to claim 6, characterized in that, The process of destroying the adhesive of the broken positive electrode sheet through high-temperature pyrolysis includes: The crushed positive electrode sheet is mixed and stirred with lithium hydroxide solution to wet the positive electrode sheet; The positive electrode sheet after being wetted is pyrolyzed under oxygen-free conditions by superheated steam in order to destroy the binder of the positive electrode sheet. The positive electrode sheet after the adhesive has been damaged is then cooled and dried under oxygen-free conditions.
8. The regeneration method according to claim 6, characterized in that, The process of destroying the adhesive of the broken positive electrode sheet through high-temperature pyrolysis includes: The crushed positive electrode sheet is transported into a rotary kiln, and the rotary kiln is heated to 420℃-460℃ under oxygen-free conditions and held for 60min-90min to break the binder of the positive electrode sheet. The positive electrode sheet after the adhesive has been broken is cooled under oxygen-free conditions.
9. The regeneration method according to claim 5, characterized in that, Also includes: The repaired cathode powder is transported to an oxygen-free, closed cooling device for cooling. The cooled cathode powder is then crushed, sieved, and demagnetized.
10. The regeneration method according to claim 9, characterized in that, Also includes: A mixture of carbon dioxide and hydrogen is exchanged with the positive electrode powder in the oxygen-free closed cooling device to heat the mixture of carbon dioxide and hydrogen to above 500°C. The heated mixture of carbon dioxide and hydrogen is passed into the pyrolysis passivation treated cathode powder to repair it. A mixture of carbon dioxide and hydrogen gas, after the cathode powder has been repaired, is introduced into the electromagnetically heated rotary kiln.