A conductive coal-based moisture power generation device based on moisture gradient and its fabrication method
By utilizing the humidity gradient structure and simplified manufacturing process of conductive coal-based wet gas power generation devices, the stability and cost issues of wet gas power generation technology under a wide range of humidity and temperature have been resolved, enabling low-cost large-scale production and stable power output.
Patent Information
- Application Number
- CN202611431936.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-10
AI Technical Summary
Existing wet gas power generation technology has poor adaptability within a wide range of humidity and temperature variations, the devices are prone to degradation, and the manufacturing process is complex, costly, and difficult to achieve large-scale production.
A humidity gradient structure is constructed using a conductive coal-based porous fibrous matrix and a hydrogel layer. Combined with the synergistic regulation of phosphoric acid and various chlorides, the preparation process is simplified, resulting in a conductive coal-based moisture power generation device based on a moisture gradient.
It maintains stable power output over a wide range of humidity and temperature, reduces material costs, simplifies manufacturing processes, is suitable for powering small electronic devices, and supports large-scale production.
Smart Images

Figure CN123074313A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new energy moisture power generation, and in particular to a conductive coal-based moisture power generation device based on a moisture gradient and its preparation method. Background Technology
[0002] Traditional fossil fuels face the dual pressures of resource depletion and environmental pollution. While renewable energy sources (such as solar, wind, and hydropower) have achieved large-scale application, they still have significant limitations: solar energy is limited by sunlight conditions, with power generation efficiency significantly decreasing at night and on cloudy or rainy days; wind power depends on location and wind speed, and is accompanied by noise pollution and ecological impacts; hydropower has stringent geographical requirements, making it difficult to achieve full coverage. Meanwhile, approximately 71% of the Earth's surface is covered by water, and the atmospheric moisture resources in the form of water vapor are enormous (approximately 1.29 x 10⁻⁶). 4 km 3 It has advantages such as wide distribution, recycling, and zero carbon emissions, providing a new direction for the development of new energy sources.
[0003] In recent years, moisture gas power generation (MEG) technology has gradually become a research hotspot. This technology utilizes functional material systems with hydrophilic-hydrophobic gradients, ion-selective transport channels, or interfacial charge separation effects to directly convert the chemical potential energy or phase transition energy of moisture into electrical energy through the adsorption-desorption cycle, ion migration, or charge transfer processes within the material. It possesses potential for device miniaturization, noiseless operation, and strong environmental adaptability. However, current moisture gas power generation technology still faces three major bottlenecks: First, traditional devices exhibit poor adaptability over a wide range of humidity variations, especially with significant performance degradation under low humidity or extreme temperature conditions; second, existing devices are prone to ion concentration gradient saturation or material structure degradation during long-term operation, leading to voltage output attenuation and insufficient stability and durability; third, to generate the gradient, devices require the precise construction of complex structures such as chemical gradients and porous asymmetric electrodes, increasing fabrication difficulty and cost, and hindering large-scale production. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention proposes a conductive coal-based moisture power generation device based on a moisture gradient and its fabrication method. This moisture power generation device exhibits sustained and excellent output performance across a wide range of humidity and temperature variations, and the integrated device can meet the power supply requirements of small electronic devices.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: a conductive coal-based moisture power generation device based on a moisture gradient, characterized in that: the device includes a porous fibrous matrix loaded with conductive coal and a hydrogel layer coated on at least a portion of its surface, forming a humidity gradient structure, thereby generating continuous power output in a humid environment.
[0006] Furthermore, the porous fibrous matrix is preferably one of filter paper, nonwoven fabric, cotton cloth, or sponge.
[0007] Furthermore, the hydrogel layer is a polyvinyl alcohol (PVA)-based hydrogel, comprising water, glycerol (Gly), phosphoric acid (PA), polyvinyl alcohol, and at least one chloride.
[0008] Furthermore, the volume ratio of each component in the hydrogel is: water:glycerol:phosphoric acid = 6:(4-6):(0-1), and the amount of polyvinyl alcohol added is 20%-30% of the water mass.
[0009] Furthermore, the chloride is selected from at least one of NaCl, LiCl, CaCl2, MgCl2 or AlCl3, preferably NaCl, and the molar concentration of the chloride is 0.1-2 mol / L, preferably 1-2 mol / L.
[0010] Furthermore, the present invention also provides a method for preparing the above-mentioned coal-based moisture power generation device based on moisture gradient, comprising the following steps:
[0011] A. Preparation of conductive coal-based nano-carbon solution: Take a certain amount of water into a container, add a dispersant and stir continuously until completely dissolved to form a dispersant solution; add coal powder into the dispersant solution and disperse it evenly by mechanical stirring; then transfer the mixture to a ball mill by a peristaltic pump and ball mill it to the preset particle size to obtain a conductive coal-based nano-carbon solution.
[0012] B. Preparation of carbon paper (carbon cloth): After cleaning the porous fibrous matrix, it is immersed in an alkaline solution for heating treatment, then removed, washed and dried; the dried porous fibrous matrix is immersed in a conductive coal-based nano carbon solution, removed and dried, and this immersion-drying process is repeated 2-6 times to obtain carbon paper (carbon cloth) loaded with conductive coal.
[0013] C. Hydrogel preparation: Mix water, glycerol, and phosphoric acid in proportion, add polyvinyl alcohol and chloride, heat and stir until completely dissolved, and keep warm for later use;
[0014] D. Device assembly: The hydrogel prepared in step C is uniformly coated on one end of the porous fibrous matrix loaded with conductive coal obtained in step B, and after drying, the conductive coal-based moisture power generation device based on humidity gradient is obtained.
[0015] Furthermore, in step A, the dispersant is polyvinylpyrrolidone or sodium cholate.
[0016] Furthermore, in step A, the particle size of the coal powder is 40μm-60μm, and the mass ratio of coal powder to dispersant is 1:0.5-1.
[0017] Furthermore, in step A, the mass concentration of coal-based nano-carbon in the conductive coal-based nano-carbon solution is 5%-10%.
[0018] Furthermore, the alkaline solution mentioned in step B is a 0.5-1 mol / L NaOH solution, the heating temperature is 70-90℃, and the treatment time is 1-2 hours.
[0019] Furthermore, in step C, the heating temperature is 80-95℃, and the stirring time is 2-4 hours.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. This invention uses abundant and inexpensive conductive coal to replace high-cost materials such as graphene and carbon nanotubes, significantly reducing material costs. Combined with a simple coating-drying assembly process, it provides an economical and feasible material solution for the large-scale application of wet gas power generation devices, which is conducive to promoting their large-scale production.
[0022] 2. By constructing a "hydrogel-coal" moisture gradient structure and combining it with the synergistic regulation of phosphoric acid and various chlorides, the device can generate significant voltage output in a wide humidity range (40%-90%) and a wide temperature range (-15-45℃), solving the problems of low output power and easy attenuation of traditional devices.
[0023] 3. This invention can be easily integrated in series or parallel. After large-scale integration, it can directly power commercial small electronic devices (such as LED lights, sensors, etc.) without the need for rectifiers or capacitors. Attached Figure Description
[0024] Figure 1 This is a SEM image of the interface between the hydrogel and conductive coal-loaded filter paper substrate in the moisture-generating device of Embodiment 1 of the present invention.
[0025] Figure 2 This is a test graph showing the voltage performance of the moisture-generating device as a function of humidity in Embodiment 1 of the present invention.
[0026] Figure 3 This is a test graph showing the voltage performance of the moisture generator as a function of temperature in Embodiment 1 of the present invention.
[0027] Figure 4 This is a long-term test diagram of the voltage performance of the moisture generator in Embodiment 1 of the present invention.
[0028] Figure 5 This is a test graph showing the voltage performance of the wet gas power generation device after being connected in series with the number of connected devices in Embodiment 4 of the present invention.
[0029] Figure 6This is a test graph showing the change in current performance of the wet gas power generation device after parallel connection with the number of parallel connections in Embodiment 4 of the present invention.
[0030] Figure 7 This is a diagram of 20 moisture-generating devices connected in parallel to light up LEDs in Embodiment 4 of the present invention. Detailed Implementation
[0031] The present invention will now be described in detail with reference to the accompanying drawings.
[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0033] Example 1
[0034] A conductive coal-based moisture power generation device based on a moisture gradient is fabricated using the following steps:
[0035] S1. Place 500g of water in a container, then add 50g of polyvinylpyrrolidone dispersant to the water. Mechanically stir at 800r / min until completely dissolved to obtain a dispersant solution. Add 50g of coal powder with a particle size of 40μm to the dispersant solution and mechanically stir at 800r / min until uniform. Then, use a peristaltic pump to pump the mixture into a ball mill and ball mill it to a particle size of about 50nm to obtain a conductive coal-based nano-carbon solution with a mass concentration between 5-10%.
[0036] S2. Soak the filter paper in anhydrous ethanol for 1 hour, then immerse it in 0.5 mol / L NaOH solution at 80°C for 2 hours. Remove the impurities, wash with deionized water, and dry. Immerse the dried filter paper in conductive coal solution, remove and dry. Repeat this process 3 times to obtain carbon paper for later use.
[0037] S3. Place 12ml of water, 8ml of glycerol, and 2ml of phosphoric acid in a container, mix thoroughly, then add 3g of polyvinyl alcohol and 0.024mol of sodium chloride. Heat and stir in a 90℃ water bath for 3 hours to dissolve and obtain PVA-based hydrogel. Keep warm for later use.
[0038] S4. Cut the carbon paper into 1cm*3cm pieces, then evenly coat one end of the carbon paper with hydrogel (1cm*1cm). After drying, you will get a moisture generator.
[0039] Furthermore, to clarify the humidity range of the moisture-generating device of this invention, its power generation performance was tested under constant temperature conditions of 25°C at different humidity levels of 40%, 50%, 60%, 70%, 80%, and 90% RH. Figure 2As shown, the results indicate that the device's output voltage remains stable above 0.6V within a humidity range of 40%-80%RH. However, when the humidity increases to 90%RH, the output voltage drops significantly to 0.57V. This is because excessive humidity dilutes the ion concentration gradient, weakening the power generation drive. In summary, this device exhibits stable output performance within a wide humidity range of 40%-80%RH, covering most common indoor and outdoor usage scenarios.
[0040] Furthermore, to clarify the temperature operating range of the moisture-generating device of this invention, its power generation performance was tested at different temperature environments of -15℃, 0℃, 15℃, 30℃, and 45℃ under constant humidity conditions of 60%RH. Figure 3 The results show that the output voltage is 0.54V at -15℃, 0.59V at 0℃, 0.63V at 15℃, 0.65V at 30℃, and 0.66V at 45℃. Overall, the device's output voltage shows a positive correlation with increasing temperature. This device maintains effective output over a wide temperature range of -15℃ to 45℃, covering most common indoor and outdoor usage scenarios.
[0041] Furthermore, to clarify the long-term performance of the moisture-generating device of the present invention, a continuous 200-hour power generation performance test was conducted in a normal temperature environment. Figure 4 As shown, the results indicate that the device's output voltage remained stable above 0.4V throughout the test, demonstrating its good output stability and ability to meet the needs of long-term daily use.
[0042] Example 2
[0043] Example 2 is the same as Example 1, except that the molar mass of sodium chloride added to the hydrogel is 0.012 mol.
[0044] Example 3
[0045] Example 3 is the same as Example 1, except that the chloride added to the hydrogel is replaced with the same molar mass of LiCl, CaCl2, MgCl2, and AlCl3, respectively.
[0046] Example 4
[0047] The devices in multiple embodiments 1 are integrated in series and parallel.
[0048] like Figure 5 , Figure 6As shown, the voltage performance of the devices after series integration and the current performance of the devices after parallel integration were tested. The results show that the output voltage increases significantly with the increase of the number of devices in series, and the output current increases significantly with the increase of the number of devices in parallel. When 20 devices are connected in series, the output voltage can reach about 8.2V; when 10 devices are connected in parallel, the output current can reach more than 500uA. Figure 7 As shown, connecting 20 moisture generators in parallel can power LED lights and illuminate blue LEDs.
[0049] The samples of Example 1, Example 2 and Example 3 of this invention were placed under the same test conditions (25℃, 60%RH) and their output voltage and current were tested. The results are shown in Table 1.
[0050] Table 1. Test results of output performance of samples in Examples 1-3
[0051]
[0052] From Table 1, we can obtain:
[0053] 1. Comparing Example 1 and Example 2, it can be seen that, within a certain range, the output performance of the wet gas power generation device is significantly improved by increasing the sodium chloride content in the hydrogel.
[0054] 2. Comparing Example 1 and Example 3, it can be seen that, under the condition of adding the same molar mass of chloride to the hydrogel, the output voltage and current of the wet gas power generation device with added sodium chloride are the best.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A conductive coal-based moisture power generation device based on a moisture gradient, characterized in that: The device includes a porous fibrous matrix loaded with conductive coal and a hydrogel layer coated on at least a portion of its surface, forming a humidity gradient structure to generate continuous power output in a humid environment.
2. The conductive coal-based moisture power generation device based on moisture gradient according to claim 1, characterized in that: The porous fibrous matrix is one of filter paper, non-woven fabric, cotton cloth or sponge.
3. The conductive coal-based moisture power generation device based on moisture gradient according to claim 1, characterized in that: The hydrogel layer is a polyvinyl alcohol-based hydrogel, comprising water, glycerol, phosphoric acid, polyvinyl alcohol, and at least one chloride.
4. The conductive coal-based moisture power generation device based on moisture gradient according to claim 3, characterized in that: The volume ratio of each component in the hydrogel is water:glycerol:phosphoric acid = 6:(4-6):(0-1), and the amount of polyvinyl alcohol added is 20%-30% of the water mass.
5. The conductive coal-based moisture power generation device based on moisture gradient according to claim 3, characterized in that: The chloride is selected from at least one of sodium chloride, lithium chloride, calcium chloride, magnesium chloride and aluminum chloride, and the molar concentration of the chloride is 0.1-2 mol / L, preferably 1-2 mol / L.
6. The method for preparing a conductive coal-based moisture power generation device based on a moisture gradient according to any one of claims 1-5, characterized in that, Includes the following steps: A. Preparation of conductive coal-based nano-carbon solution: Water is placed in a container, a dispersant is added and stirred continuously until completely dissolved to form a dispersant solution; coal powder is added to the dispersant solution and mechanically stirred to disperse it evenly; then, the mixture is transferred to a ball mill by a peristaltic pump and ball-milled to the preset particle size to obtain a conductive coal-based nano-carbon solution. B. Carbon paper preparation: After cleaning the porous fibrous matrix, it is immersed in an alkaline solution for heating treatment, then removed, washed, and dried; the dried porous fibrous matrix is immersed in a conductive coal-based nano carbon solution, removed, and dried. This immersion-drying process is repeated 2-6 times to obtain carbon paper loaded with conductive coal. C. Hydrogel preparation: Mix water, glycerol, and phosphoric acid in the proportions described in claim 4, add polyvinyl alcohol and chloride, heat and stir until completely dissolved, and keep warm for later use; D. Device assembly: The hydrogel prepared in step C is uniformly coated on one end of the porous fibrous matrix loaded with conductive coal obtained in step B, and after drying, the conductive coal-based moisture power generation device based on humidity gradient is obtained.
7. The preparation method according to claim 6, characterized in that: The dispersant in step A is polyvinylpyrrolidone or sodium cholate; the particle size of the conductive coal powder is 40μm-60μm; the mass ratio of conductive coal powder to dispersant is 1:0.5-1; and the mass concentration of coal-based carbon nanoparticles in the coal-based carbon nanoparticle solution is 5%-10%.
8. The preparation method according to claim 6, characterized in that: The alkaline solution mentioned in step B is a 0.5 mol / L sodium hydroxide solution, the heating temperature is 70-90℃, and the treatment time is 1-2 hours.
9. The preparation method according to claim 6, characterized in that: The heating temperature in step C is 80-95℃, and the stirring time is 2-4 hours.
10. The preparation method according to claim 6, characterized in that: It includes at least two conductive coal-based wet gas power generation devices based on moisture gradient as described in claim 6, wherein the at least two devices are electrically connected in series or parallel to improve the overall output voltage or output current.