A graphene electrothermal cloth and its preparation method

By constructing a three-dimensional conductive network of graphene, carbon black, and multi-walled carbon nanotubes, along with metal conductive wire intersection nodes, and combining it with hot-pressing composite of thermoplastic polyurethane film, the problems of easy agglomeration of carbon-based materials and poor rheological properties of slurry in graphene electric heating cloth were solved, resulting in a graphene electric heating cloth with low resistance, fast response, high durability, and good temperature uniformity.

CN123075751APending Publication Date: 2026-11-10HEBEI JUWEI ENENG ELECTRIC HEATING TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611348178.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing graphene heating cloths suffer from problems such as carbon-based materials being prone to agglomeration, insufficient internal cross-linking strength, and poor slurry rheological properties, resulting in slow heating response, low water washability and bending durability, and uneven surface temperature distribution when working over a large area.

Method used

Graphene, carbon black, and multi-walled carbon nanotubes are used as composite conductive fillers. By limiting the ratio of conductive fillers to polyurethane matrix, and combining coupling agents and dispersants, a three-dimensional conductive network structure is constructed. During the weaving process, vertical intersection nodes of metal conductive wires and graphene conductive yarns are set. Combined with hot-pressing composite of thermoplastic polyurethane film, a uniform conductive coating is formed.

Benefits of technology

This invention achieves low sheet resistance, fast power-on heating response, high durability, and good surface temperature uniformity of graphene heating cloth, solving the problems of low durability and uneven temperature of traditional graphene heating cloth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123075751A_ABST
    Figure CN123075751A_ABST
Patent Text Reader

Abstract

This invention relates to the field of electrothermal materials technology, and discloses a graphene electrothermal cloth and its preparation method. The cloth comprises a semi-finished electrothermal cloth and a thermoplastic polyurethane film hot-pressed onto the upper and lower surfaces of the semi-finished cloth. The warp yarns of the semi-finished electrothermal cloth include ordinary polyester yarn and spaced-apart metal conductive wires, while the weft yarns include ordinary polyester yarn and graphene conductive yarn. The graphene conductive yarn and the metal conductive wires are in contact and conductive at the weaving intersections. The preparation method is as follows: first, a coupling agent pre-hydrolyzed solution is prepared; graphene, carbon black, multi-walled carbon nanotubes, plasticizer, and a portion of deionized water are mixed, cooled, kneaded, and extruded; then, an aqueous polyurethane emulsion is dispersed and added, followed by the addition of the pre-hydrolyzed solution to obtain a slurry. This invention results in a finished product with low sheet resistance, fast energized heating response, excellent washability and bending durability, and uniform surface temperature distribution during large-area operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrothermal materials technology, specifically to a graphene electrothermal cloth and its preparation method. Background Technology

[0002] Graphene heating cloth is a novel heating product that combines flexible fabric with graphene conductive material. Graphene, with its excellent electrical and thermal conductivity, is combined with traditional textile fibers, forming a conductive network on the fiber surface or within the fabric through specific processing techniques. Graphene heating cloth is characterized by its soft texture, light weight, foldability, and conformability to the human body, and is widely used in industries such as smart wearables, medical therapy, home heating, and car seat heating.

[0003] The heating principle of graphene electrothermal cloth is based on Joule's law. When a certain voltage is applied across the two ends of the graphene electrothermal cloth, current flows through the internally constructed graphene conductive network, and electrons move directionally under the drive of the electric field. During the movement, electrons collide with the graphene lattice and other carbon-based materials, converting electrical energy into heat energy that is radiated outward. In this process, the heating efficiency and temperature distribution depend on the integrity of the conductive pathway and the uniformity of the coating.

[0004] Existing technologies using carbon-based materials such as graphene, carbon black, and multi-walled carbon nanotubes exhibit strong van der Waals forces, making them prone to aggregation. Traditional one-time mixing and water addition methods struggle to allow dispersants to penetrate deep into the material interstices, resulting in an inability to form uniformly distributed conductive pathways after curing. This leads to high sheet resistance and a slower heating response in the finished product. Furthermore, current processes do not perform independent pre-hydrolysis treatment on the coupling agent, and direct mixing restricts the cross-linking reaction, resulting in insufficient bonding strength between the polyurethane coating and the polyester yarn surface. External moisture easily penetrates, and the resistivity of the heating cloth increases after repeated washing and bending, leading to poor durability in daily use. Traditional pulping processes lack control over the timing of plasticizer addition, resulting in poor rheological properties of the pulp under high shear conditions. When processed by a scraper die, it is difficult to form a uniformly thick conductive coating on the polyester yarn surface. Uneven coating thickness can cause localized hot spots under energization, resulting in uneven surface temperature distribution during large-area operation. Furthermore, existing graphene heating cloths have poor heating uniformity. Due to uneven electrode arrangement and conductive coating, they are prone to problems such as higher edge temperature and lower center temperature.

[0005] Therefore, the purpose of this invention is to provide a graphene electrothermal cloth and its preparation method to overcome the shortcomings of the prior art. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a graphene electric heating cloth and its preparation method, which solves the problems of easy agglomeration of carbon-based materials, insufficient internal cross-linking strength, and poor rheological properties of slurry in existing graphene electric heating cloths, resulting in slow heating response, low water washing and bending durability, and uneven surface temperature distribution when working over a large area.

[0007] To achieve the above objectives, the present invention provides the following technical solution:

[0008] In a first aspect, the present invention provides a graphene electrothermal cloth, which adopts the following technical solution:

[0009] A graphene electric heating cloth is composed of a semi-finished electric heating cloth and a thermoplastic polyurethane film hot-pressed onto the upper and lower surfaces of the semi-finished electric heating cloth.

[0010] The warp yarns of the semi-finished electric heating cloth include ordinary polyester yarns and spaced metal conductive wires, while the weft yarns include ordinary polyester yarns and graphene conductive yarns. The graphene conductive yarns and the metal conductive wires are in contact and connected at the weaving intersection.

[0011] Graphene conductive yarn is made by impregnating polyester yarn with graphene conductive yarn slurry and then curing it.

[0012] The graphene conductive yarn sizing agent is made from raw materials comprising the following parts by weight:

[0013] Graphene 10.00 to 14.00 parts;

[0014] Carbon black 0.80 to 1.50 parts;

[0015] 0.80 to 1.50 parts of multi-walled carbon nanotubes;

[0016] 15.00 to 20.00 parts of anionic aliphatic waterborne polyurethane emulsion;

[0017] Dispersant 0.50 to 0.80 parts;

[0018] 0.03 to 0.08 parts of coupling agent;

[0019] Plasticizer 0.02 to 0.05 parts;

[0020] 0.03 to 0.08 parts of defoamer;

[0021] 61.99 to 72.82 parts of deionized water.

[0022] By adopting the above technical solution, graphene, carbon black and multi-walled carbon nanotubes are used as composite conductive fillers. The graphene sheets play the role of a long-range conductive skeleton in the system, while the carbon black particles can fill between the graphene sheets. With the spatial overlap of the multi-walled carbon nanotubes, the three work together to construct a three-dimensional conductive network structure, which helps to reduce the overall resistance of the yarn.

[0023] Preferably, the graphene conductive yarn sizing agent is made from raw materials comprising the following parts by weight:

[0024] 11.00 to 12.00 parts of graphene;

[0025] Carbon black 1.00 to 1.20 parts;

[0026] 1.00 to 1.20 parts of multi-walled carbon nanotubes;

[0027] 17.14 to 18.00 parts of anionic aliphatic waterborne polyurethane emulsion;

[0028] Dispersant 0.60 to 0.70 parts;

[0029] 0.05 to 0.06 parts of coupling agent;

[0030] Plasticizer 0.03 to 0.04 parts;

[0031] 0.05 to 0.06 parts of defoamer;

[0032] Deionized water: 67.74 to 68.13 parts.

[0033] By adopting the above technical solution and limiting the ratio of conductive filler to polyurethane matrix, it is beneficial to control the variance of sheet resistance of conductive coating, thereby improving the conductivity stability and heat distribution of electric heating cloth to a certain extent.

[0034] Preferably, the metal conductive wire is a tin-plated copper wire, which is used for electrical connection with an external conductor;

[0035] The dispersant is sodium polyacrylate; the coupling agent is 3-methacryloyloxypropyltrimethoxysilane; the plasticizer is dioctyl terephthalate; and the defoamer is polyether-modified polydimethylsiloxane.

[0036] By adopting the above technical solution, the anionic polymer chains contained in sodium polyacrylate are easy to generate electrostatic repulsion and steric hindrance on the graphene surface, thereby playing a stabilizing role; the selected 3-methacryloyloxypropyltrimethoxysilane can usually provide chemical bonding between inorganic carbon materials and organic polyurethane; dioctyl terephthalate helps to increase the degree of freedom of movement of polyurethane polymer chain segments.

[0037] Preferably, the anionic aliphatic waterborne polyurethane emulsion is an aqueous emulsion with a solid content of 30% to 35%, and the anionic aliphatic waterborne polyurethane emulsion is made from raw materials comprising the following parts by weight: 100.0 parts of polytetrahydrofuran ether diol; 33.3 parts of isophorone diisocyanate; 6.7 parts of 2,2-dimethylolpropionic acid; 5.0 parts of triethylamine; and 269.0 to 338.0 parts of deionized water.

[0038] By adopting the above technical solution, the polyurethane emulsion synthesized from polytetrahydrofuran ether diol and isophorone diisocyanate has good hydrolysis resistance and weather resistance, which makes the cured coating less sticky under high temperature heating conditions and less prone to significant swelling under water washing conditions, thereby extending the conventional service life of the electric heating cloth at the substrate material level.

[0039] Preferably, the preparation steps of the anionic aliphatic waterborne polyurethane emulsion are as follows:

[0040] 100.0 parts of polytetrahydrofuran ether diol were dehydrated at 100°C for 2 hours under reduced pressure (gauge pressure not exceeding -0.09 MPa) and then cooled to 60°C.

[0041] Add 33.3 parts of isophorone diisocyanate, heat to 80°C, and react at a constant temperature for 2 hours under nitrogen protection;

[0042] Subsequently, 6.7 parts of 2,2-dimethylolpropionic acid were added, and the reaction was continued at 80°C for 3 hours to obtain a polyurethane prepolymer with isocyanate-terminated groups.

[0043] After cooling the polyurethane prepolymer to 40°C, add 5.0 parts of triethylamine and continue stirring to neutralize and react for 30 minutes.

[0044] Under high-speed shear stirring at 2000 rpm, 269.0 to 338.0 parts of deionized water were added dropwise for phase inversion emulsification and continued to disperse for 60 minutes to obtain anionic aliphatic waterborne polyurethane emulsion.

[0045] By adopting the above technical solution, the preliminary reaction is carried out under reduced pressure dehydration conditions, which helps to reduce the interference of water in the system on the isocyanate groups, making them more inclined to react with hydroxyl groups to form urethane bonds. After introducing hydrophilic groups through chain extenders and neutralizing them with triethylamine, the polyurethane molecular chains are more likely to undergo phase transformation under high-speed shearing and the action of deionized water, thereby forming an aqueous polyurethane emulsion system without the addition of organic solvents.

[0046] Secondly, the present invention provides a method for preparing graphene electrothermal cloth, which adopts the following technical solution:

[0047] A method for preparing a graphene electrothermal cloth includes the following steps:

[0048] Deionized water was extracted from the total amount of deionized water in the graphene conductive yarn sizing agent formulation, and the coupling agent was added in the formulation amount. The mixture was kept warm under heating and stirring conditions to obtain a pre-hydrolyzed solution of the coupling agent.

[0049] A portion of the deionized water in the total amount of the formula is mixed with the dispersant, plasticizer, carbon black and multi-walled carbon nanotubes in the formula amount, and then the graphene in the formula amount is added in batches, and the kneading and extrusion state is maintained under cooling conditions.

[0050] Then, the remaining deionized water of the total amount of the formula is added to it, and the stirring speed is increased simultaneously to continue dispersing, so as to obtain a pre-dispersed slurry.

[0051] After cooling the pre-dispersed slurry and reducing the stirring speed, add the formulated amount of anionic aliphatic waterborne polyurethane emulsion and defoamer to it while maintaining stirring;

[0052] Then, the pre-prepared coupling agent pre-hydrolyzed solution was added dropwise, and after stirring, the mixture was filtered out and allowed to stand and mature at room temperature to obtain graphene conductive yarn sizing agent.

[0053] Polyester yarn is continuously passed through an impregnation tank containing graphene conductive yarn slurry by a stretching device. After the excess graphene conductive yarn slurry on the surface is scraped off by a tungsten steel scraper, it is continuously put into the drying tunnel and baked and cured in sequence to obtain graphene conductive yarn.

[0054] Ordinary polyester yarn and metal conductive wire are used as warp yarns, and ordinary polyester yarn and graphene conductive yarn are used as weft yarns. They are interwoven on a loom in a plain weave pattern, so that the graphene conductive yarn and the metal conductive wire form perpendicularly intersecting conductive nodes, thus weaving a semi-finished electric heating cloth. A layer of thermoplastic polyurethane film is then hot-pressed onto the upper and lower surfaces of the semi-finished electric heating cloth to obtain the finished graphene electric heating cloth.

[0055] Preferably, in the process of preparing the coupling agent pre-hydrolyzed solution, the amount of deionized water extracted accounts for 3.4% to 6.5% of the total deionized water in the formula; after adding the coupling agent, the water is heated and kept constant at 38°C to 48°C, and stirred and kept warm at 150 rpm to 250 rpm for 30 min to 50 min.

[0056] By adopting the above technical solution, setting a constant water temperature and coordinating stirring and heat preservation, a relatively stable hydrolysis environment is provided for the silane coupling agent to control the hydrolysis rate. This reduces the self-condensation phenomenon of silanol groups caused by concentration concentration or temperature fluctuations, thereby retaining some reactivity for subsequent crosslinking.

[0057] Preferably, during the kneading and extrusion process, the stirring speed is adjusted to 400 rpm to 600 rpm, the core temperature of the material is controlled to not exceed 50°C by the jacket cooling water, and the kneading and extrusion time is maintained at 50 min to 70 min; and the amount of deionized water used accounts for 16.5% to 29.0% of the total deionized water in the formula.

[0058] By adopting the above technical solution, controlling the amount of deionized water is to adjust the solid content and viscosity of the system in the early stage, so that during the process of providing shear force to deagglomerate, the jacket cooling water can be used to limit the internal frictional heat generation. This not only slows down the excessive evaporation of slurry water, but also prevents the dispersant from failing at high temperature, thereby maintaining a relatively continuous physical dispersion environment.

[0059] Preferably, during the dispersion process of adding the remaining deionized water, the remaining deionized water is added within 10 to 20 minutes, the stirring speed is increased to 1200 rpm to 1800 rpm, and the dispersion is continued for 35 to 55 minutes; when adding the anionic aliphatic waterborne polyurethane emulsion and defoamer, the reactor is fully cooled to reduce the system temperature to 20°C to 30°C, the stirring speed is reduced to 200 rpm to 400 rpm, and the stirring speed is maintained for 20 to 40 minutes after the addition is completed.

[0060] By employing the above technical solution, the system concentration is gradually adjusted by adding residual deionized water, and the rotation speed is increased to further disperse the initially exfoliated carbon nanomaterials into the fluid. Cooling and slowing the flow rate before adding the polyurethane emulsion are chosen primarily to reduce the adverse effects of high shear force and high temperature on emulsion stability, thereby lowering the risk of demulsification.

[0061] Preferably, in the process of preparing graphene conductive yarn, the baking temperature is 70°C to 90°C and the time is 10 min to 15 min; the curing temperature is 110°C to 140°C and the time is 5 min to 10 min; in the process of hot-pressing a layer of thermoplastic polyurethane film onto the upper and lower surfaces of the electrothermal cloth semi-finished product, the hot-pressing temperature is set to 150°C and the thickness of the thermoplastic polyurethane film is 0.05 mm.

[0062] By employing the above technical solution and setting baking and curing processes at different temperatures, the moisture inside the coating can evaporate relatively steadily, reducing the formation of bubbles or pores due to rapid boiling of moisture. At the same time, the high-temperature environment helps the cross-linked network to gradually form. Finally, the hot-pressing composite operation at 150℃ allows the thermoplastic polyurethane film to melt and flow to a certain extent, thereby forming a mechanical anchor with the voids on the surface of the woven fabric and the conductive coating, achieving the bonding and encapsulation of the finished product.

[0063] This invention provides a graphene electrothermal cloth and its preparation method. It has the following beneficial effects:

[0064] 1. This invention, by setting a step of adding the formulated amount of graphene in batches to a mixture of dispersant, plasticizer, carbon black, multi-walled carbon nanotubes, and a portion of deionized water, and maintaining a kneading and extrusion state under cooling conditions, enables the dispersant to enter the gaps between graphene, carbon black, and multi-walled carbon nanotubes. Under the coating effect of anionic aliphatic waterborne polyurethane emulsion, each component forms a uniformly distributed conductive path after curing, resulting in the finished graphene electric heating cloth having a lower sheet resistance and a faster energized heating response speed.

[0065] 2. This invention prepares a pre-hydrolyzed coupling agent solution by extracting a small amount of deionized water and the formulation amount of coupling agent under heating and stirring conditions. This solution is then dripped into a pre-dispersion slurry containing anionic aliphatic waterborne polyurethane emulsion. This reduces the permeability of external moisture, allowing the resulting graphene electric heating cloth to maintain a low resistance change rate even after multiple conventional water washes and repeated bending, thus improving the daily durability of the cloth.

[0066] 3. This invention adds a specific amount of plasticizer to the formula during the early stage of maintaining the kneading and extrusion state. This allows the plasticizer to fully adhere to the surface of graphene, carbon black, and multi-walled carbon nanotubes under high shear. Combined with the process of the polyester yarn passing through the impregnation tank and being treated by the tungsten steel scraper during preparation, it is beneficial to form a conductive coating with uniform thickness on the surface of the polyester yarn. After the subsequent weaving and hot-pressing composite thermoplastic polyurethane film operation is completed, the uniformity of the coating thickness reduces the generation of local hot spots under the power-on state, ensuring the uniform surface temperature distribution of the electric heating cloth when working over a large area.

[0067] 4. This invention uses metal conductive wires as warp yarns and graphene conductive yarns as weft yarns, which are woven together with ordinary polyester yarns. During the weaving process, a parallel conductive network of longitudinal power supply electrodes and transverse heating elements is constructed, realizing the textile integration of flexible circuits. At the same time, it solves the problem of uneven heating caused by overheating at the edges and cooling at the center in traditional circuits. Attached Figure Description

[0068] Figure 1 This is a structural exploded view of the finished graphene electrothermal cloth of the present invention;

[0069] Figure 2 The particle size distribution curves of the graphene conductive yarn slurry obtained in Example 1, Comparative Example 1, and Comparative Example 3 of the present invention are shown.

[0070] Figure 3 Fourier transform infrared spectra of the cured coating samples of Example 1, Comparative Example 1, and Comparative Example 4 of the present invention;

[0071] Figure 4 The graph shows the apparent viscosity of the graphene conductive yarn slurry obtained in Example 1, Comparative Example 2, and Comparative Example 3 of the present invention as a function of shear rate.

[0072] Figure 5 The graphs show the time-temperature rise curves of the finished graphene electric heating cloths of Example 1, Comparative Example 2, and Comparative Example 3 of the present invention under a constant voltage of 5V.

[0073] Figure 6 The graphs show the resistance change rate of the finished graphene electric heating cloths of Example 1, Comparative Example 1, and Comparative Example 4 of the present invention with the number of water washes.

[0074] Figure 7 The graph shows the surface temperature distribution curves of the finished graphene electrothermal cloth along the diagonal path in Embodiment 1, Comparative Example 2, and Comparative Example 3 of the present invention.

[0075] Among them, 1. Semi-finished electric heating cloth. Detailed Implementation

[0076] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0077] Combination Figure 1 As shown, the graphene electric heating cloth provided by this invention has a three-layer composite structure, including a centrally located electric heating cloth semi-finished product 1 and thermoplastic polyurethane films hot-pressed onto the upper and lower surfaces of the electric heating cloth semi-finished product 1. The electric heating cloth semi-finished product 1 is woven with a plain weave. The warp direction of the electric heating cloth semi-finished product 1 consists of ordinary polyester yarn and spaced-apart metal conductive wires, while the weft direction consists of ordinary polyester yarn and graphene conductive yarns. The metal conductive wires are tin-plated copper wires.

[0078] In the braided structure, graphene conductive yarns and longitudinal metal conductive lines form a cross-shaped contact. The metal conductive lines distributed on both sides of the fabric serve as the positive and negative terminals for power supply, thereby constructing an overall parallel conductive heating grid. In actual use, the external conductive connecting lines are connected to the longitudinal metal conductive lines to introduce power. The upper and lower thermoplastic polyurethane films are tightly bonded to the middle electric heating cloth semi-finished product 1 through a hot pressing process. This not only achieves the bonding and encapsulation of the conductive coating, but also prevents graphene from falling off and oxidizing due to the intrusion of external sweat and moisture, ensuring the resistance stability of long-term use.

[0079] Preparation Example 1:

[0080] This preparation example provides a method for preparing anionic aliphatic waterborne polyurethane emulsion, including the following steps:

[0081] 100.0 parts of polytetrahydrofuran ether diol were placed in a reactor equipped with a mechanical stirrer, thermometer, and condenser. The mixture was dehydrated at 100°C for 2 hours under reduced pressure (gauge pressure not exceeding -0.09 MPa), and then cooled to 60°C. 33.3 parts of isophorone diisocyanate were added to the reactor, and the temperature was raised to 80°C. The reaction was carried out at this temperature for 2 hours under nitrogen protection. Subsequently, 6.7 parts of the hydrophilic chain extender 2,2-dimethylolpropionic acid were added, and the reaction was continued at 80°C for 3 hours to obtain a polyurethane prepolymer with terminal isocyanate groups. The system temperature was lowered to 40°C, and 5.0 parts of triethylamine were added. The mixture was stirred and neutralized for 30 minutes. Under high-speed shear stirring at 2000 rpm, 269.0 parts of deionized water were slowly added dropwise to the system for phase inversion emulsification. The mixture was continuously dispersed for 60 minutes to obtain an anionic aliphatic waterborne polyurethane emulsion with a solid content of 35%.

[0082] Preparation Example 2:

[0083] This preparation example provides a method for preparing anionic aliphatic waterborne polyurethane emulsion, including the following steps:

[0084] 100.0 parts of polytetrahydrofuran ether diol with a number average molecular weight of 2000 were placed in a reactor equipped with a mechanical stirrer, thermometer, and condenser. The mixture was dehydrated at 100°C for 2 hours under reduced pressure (gauge pressure not exceeding -0.09 MPa), and then cooled to 60°C. 33.3 parts of isophorone diisocyanate were added to the reactor, and the temperature was raised to 80°C. The reaction was carried out at this temperature for 2 hours under nitrogen protection. Subsequently, 6.7 parts of the hydrophilic chain extender 2,2-dimethylolpropionic acid were added, and the reaction was continued at 80°C for 3 hours to obtain a polyurethane prepolymer with terminal isocyanate groups. The system temperature was lowered to 40°C, and 5.0 parts of triethylamine were added. The mixture was stirred continuously for 30 minutes to neutralize the reaction. Under high-speed shear stirring at 2000 rpm, 338.0 parts of deionized water were slowly added dropwise to the system for phase inversion emulsification. The mixture was continuously dispersed for 60 minutes to obtain an anionic aliphatic waterborne polyurethane emulsion with a solid content of 30%.

[0085] Example 1:

[0086] This embodiment provides a method for preparing graphene electrothermal cloth, including the following steps:

[0087] (1) Weigh the raw materials: 12.00 parts graphene, 1.00 parts carbon black, 1.00 parts multi-walled carbon nanotubes, 17.14 parts waterborne polyurethane emulsion obtained in Preparation Example 1, 0.60 parts sodium polyacrylate (dispersant), 0.05 parts 3-methacryloyloxypropyltrimethoxysilane (coupling agent), 0.03 parts dioctyl terephthalate (plasticizer), 0.05 parts polyether-modified polydimethylsiloxane (defoamer), and 68.13 parts deionized water;

[0088] (2) Take 3.13 parts from the above deionized water and place it in a mixing tank. Heat and keep the water temperature constant at 40°C. Add 0.05 parts of coupling agent and stir at 200 rpm for 40 min to obtain the coupling agent pre-hydrolyzed solution.

[0089] (3) Add 15.00 parts of deionized water to the main dispersion reactor, along with 0.60 parts of dispersant and 0.03 parts of plasticizer. Then add 1.00 parts of carbon black and 1.00 parts of multi-walled carbon nanotubes and mix them at 1000 rpm. Add 12.00 parts of graphene to the main reactor in 4 batches, adjust the speed to 500 rpm, turn on the jacket cooling water to control the core temperature of the material to not exceed 50°C, and maintain a high viscosity kneading and extrusion state for 60 min.

[0090] (4) The remaining 50.00 parts of deionized water are slowly added dropwise into the main reactor over 15 minutes, while the stirring speed is increased to 1500 rpm and the high-speed dispersion is continued for 45 minutes to obtain the pre-dispersed slurry.

[0091] (5) Turn on the full cooling of the reactor to lower the system temperature to 25°C, reduce the speed to 300 rpm, slowly add 17.14 parts of waterborne polyurethane emulsion, then add 0.05 parts of defoamer, and keep stirring at this speed for 30 min;

[0092] (6) Keep the rotation speed at 300 rpm and drop the pre-hydrolyzed coupling agent solution obtained in step (2) into the main reactor at a uniform speed. Continue stirring for 15 min, filter the solution through a 200-mesh filter, and let it stand and mature at room temperature for 18 h to obtain graphene conductive yarn slurry.

[0093] (7) The polyester yarn is continuously passed through the impregnation tank containing the above slurry by the stretching device, and the excess slurry on the surface is scraped off by the tungsten steel scraper. It is then continuously entered into the drying tunnel and successively baked at 80°C for 10 min and cured at 130°C for 5 min to obtain graphene conductive yarn.

[0094] (8) Ordinary polyester yarn and metal conductive wire (tin-plated copper wire) are used as warp yarns, and ordinary polyester yarn and graphene conductive yarn are used as weft yarns. The yarns are interwoven in plain weave on a loom so that the graphene conductive yarn and the metal conductive wire form a perpendicularly intersecting conductive node. The semi-finished product 1 of electric heating cloth is woven. A layer of thermoplastic polyurethane film with a thickness of 0.05 mm is hot-pressed onto the upper and lower surfaces of the semi-finished product at 150°C to obtain the finished graphene electric heating cloth.

[0095] Example 2:

[0096] This embodiment provides a method for preparing graphene electrothermal cloth, including the following steps:

[0097] (1) Weigh the raw materials: 10.00 parts graphene, 0.80 parts carbon black, 0.80 parts multi-walled carbon nanotubes, 15.00 parts waterborne polyurethane emulsion obtained in Preparation Example 2, 0.50 parts sodium polyacrylate (dispersant), 0.03 parts 3-methacryloyloxypropyltrimethoxysilane (coupling agent), 0.02 parts dioctyl terephthalate (plasticizer), 0.03 parts polyether-modified polydimethylsiloxane (defoamer), and 72.82 parts deionized water;

[0098] (2) Take 2.50 parts from the above deionized water and place it in a mixing tank. Heat and keep the water temperature constant at 38°C. Add 0.03 parts of coupling agent and stir at 150 rpm for 30 min to obtain the coupling agent pre-hydrolyzed solution.

[0099] (3) Add 12.00 parts of deionized water to the main dispersion reactor, along with 0.50 parts of dispersant and 0.02 parts of plasticizer. Then add 0.80 parts of carbon black and 0.80 parts of multi-walled carbon nanotubes and mix them at 800 rpm. Add 10.00 parts of graphene to the main reactor in 3 batches, adjust the speed to 400 rpm, turn on the jacket cooling water to control the core temperature of the material to not exceed 50°C, and maintain a high viscosity kneading and extrusion state for 50 min.

[0100] (4) The remaining 58.32 parts of deionized water were slowly added dropwise into the main reactor over 10 minutes, while the stirring speed was increased to 1200 rpm and the mixture was continuously dispersed at high speed for 35 minutes to obtain a pre-dispersed slurry.

[0101] (5) Turn on the full cooling of the reactor to lower the system temperature to 20°C, reduce the rotation speed to 200 rpm, slowly add 15.00 parts of water-based polyurethane emulsion, then add 0.03 parts of defoamer, and keep the rotation speed at that speed for 20 min;

[0102] (6) Keep the rotation speed at 200 rpm and drop the pre-hydrolyzed coupling agent solution obtained in step (2) into the main reactor at a uniform speed. Continue stirring for 10 min, filter the solution through a 200-mesh filter, and let it stand and mature at room temperature for 12 h to obtain graphene conductive yarn slurry.

[0103] (7) The polyester yarn is continuously passed through the impregnation tank containing the above slurry by the stretching device, and the excess slurry on the surface is scraped off by the tungsten steel scraper. It is then continuously entered into the drying tunnel and baked at 70°C for 15 minutes and cured at 110°C for 10 minutes in sequence to obtain graphene conductive yarn.

[0104] (8) Ordinary polyester yarn and metal conductive wire (tin-plated copper wire) are used as warp yarns, and ordinary polyester yarn and graphene conductive yarn are used as weft yarns. The yarns are interwoven in plain weave on a loom so that the graphene conductive yarn and the metal conductive wire form a perpendicularly intersecting conductive node. The semi-finished product 1 of electric heating cloth is woven. A layer of thermoplastic polyurethane film with a thickness of 0.05 mm is hot-pressed onto the upper and lower surfaces of the semi-finished product at 150°C to obtain the finished graphene electric heating cloth.

[0105] Example 3:

[0106] This embodiment provides a method for preparing graphene electrothermal cloth, including the following steps:

[0107] (1) Weigh the raw materials: 14.00 parts graphene, 1.50 parts carbon black, 1.50 parts multi-walled carbon nanotubes, 20.00 parts waterborne polyurethane emulsion obtained in Preparation Example 1, 0.80 parts sodium polyacrylate (dispersant), 0.08 parts 3-methacryloyloxypropyltrimethoxysilane (coupling agent), 0.05 parts dioctyl terephthalate (plasticizer), 0.08 parts polyether-modified polydimethylsiloxane (defoamer), and 61.99 parts deionized water;

[0108] (2) Take 4.00 parts from the above deionized water and place it in a mixing tank. Heat and keep the water temperature constant at 48°C. Add 0.08 parts of coupling agent and stir at 250 rpm for 50 min to obtain the coupling agent pre-hydrolyzed solution.

[0109] (3) Add 18.00 parts of deionized water to the main dispersion reactor, along with 0.80 parts of dispersant and 0.05 parts of plasticizer. Then add 1.50 parts of carbon black and 1.50 parts of multi-walled carbon nanotubes and mix them at 1200 rpm. Add 14.00 parts of graphene to the main reactor in 5 batches, adjust the speed to 600 rpm, turn on the jacket cooling water to control the core temperature of the material to not exceed 50°C, and maintain a high viscosity kneading and extrusion state for 70 min.

[0110] (4) The remaining 39.99 parts of deionized water were slowly added dropwise into the main reactor over 20 minutes, while the stirring speed was increased to 1800 rpm and the mixture was continuously dispersed at high speed for 55 minutes to obtain a pre-dispersed slurry.

[0111] (5) Turn on the full cooling of the reactor to lower the system temperature to 30°C, reduce the rotation speed to 400 rpm, slowly add 20.00 parts of water-based polyurethane emulsion, and then add 0.08 parts of defoamer dropwise. Keep the rotation speed at this speed and stir for 40 min.

[0112] (6) Keep the rotation speed at 400 rpm and drop the pre-hydrolyzed coupling agent solution obtained in step (2) into the main reactor at a uniform speed. Continue stirring for 20 min, filter the solution through a 200 mesh filter, and let it stand and mature at room temperature for 24 h to obtain graphene conductive yarn slurry.

[0113] (7) The polyester yarn is continuously passed through the impregnation tank containing the above slurry by the stretching device, and the excess slurry on the surface is scraped off by the tungsten steel scraper. It is then continuously entered into the drying tunnel and successively baked at 90°C for 10 min and cured at 140°C for 10 min to obtain graphene conductive yarn.

[0114] (8) Ordinary polyester yarn and metal conductive wire (tin-plated copper wire) are used as warp yarns, and ordinary polyester yarn and graphene conductive yarn are used as weft yarns. The yarns are interwoven in plain weave on a loom so that the graphene conductive yarn and the metal conductive wire form a perpendicularly intersecting conductive node. The semi-finished product 1 of electric heating cloth is woven. A layer of thermoplastic polyurethane film with a thickness of 0.05 mm is hot-pressed onto the upper and lower surfaces of the semi-finished product at 150°C to obtain the finished graphene electric heating cloth.

[0115] Example 4:

[0116] This embodiment provides a method for preparing graphene electrothermal cloth, including the following steps:

[0117] (1) Weigh the raw materials: 11.00 parts graphene, 1.20 parts carbon black, 1.20 parts multi-walled carbon nanotubes, 18.00 parts waterborne polyurethane emulsion obtained in Preparation Example 1, 0.70 parts sodium polyacrylate (dispersant), 0.06 parts 3-methacryloyloxypropyltrimethoxysilane (coupling agent), 0.04 parts dioctyl terephthalate (plasticizer), 0.06 parts polyether-modified polydimethylsiloxane (defoamer), and 67.74 parts deionized water;

[0118] (2) Take 3.50 parts from the above deionized water and place it in a mixing tank. Heat and keep the water temperature constant at 45°C. Add 0.06 parts of coupling agent and stir at 200 rpm for 45 min to obtain the coupling agent pre-hydrolyzed solution.

[0119] (3) Add 16.00 parts of deionized water to the main dispersion reactor, along with 0.70 parts of dispersant and 0.04 parts of plasticizer. Then add 1.20 parts of carbon black and 1.20 parts of multi-walled carbon nanotubes and mix them at 1000 rpm. Add 11.00 parts of graphene to the main reactor in 4 batches, adjust the speed to 550 rpm, turn on the jacket cooling water to control the core temperature of the material to not exceed 50°C, and maintain a high viscosity kneading and extrusion state for 65 min.

[0120] (4) The remaining 48.24 parts of deionized water were slowly added dropwise into the main reactor over 15 minutes, while the stirring speed was increased to 1600 rpm and the mixture was continuously dispersed at high speed for 40 minutes to obtain a pre-dispersed slurry.

[0121] (5) Turn on the full cooling of the reactor to lower the system temperature to 25°C, reduce the rotation speed to 350 rpm, slowly add 18.00 parts of water-based polyurethane emulsion, and then add 0.06 parts of defoamer dropwise. Keep the rotation speed at this speed and stir for 35 minutes.

[0122] (6) Keep the rotation speed at 350 rpm and drop the pre-hydrolyzed coupling agent solution obtained in step (2) into the main reactor at a uniform speed. Continue stirring for 15 min, filter the solution through a 200-mesh filter, and let it stand and mature at room temperature for 20 h to obtain graphene conductive yarn slurry.

[0123] (7) The polyester yarn is continuously passed through the impregnation tank containing the above slurry by the stretching device, and the excess slurry on the surface is scraped off by the tungsten steel scraper. It is then continuously entered into the drying tunnel and baked at 85°C for 12 min and cured at 120°C for 8 min in sequence to obtain graphene conductive yarn.

[0124] (8) Ordinary polyester yarn and metal conductive wire (tin-plated copper wire) are used as warp yarns, and ordinary polyester yarn and graphene conductive yarn are used as weft yarns. The yarns are interwoven in plain weave on a loom so that the graphene conductive yarn and the metal conductive wire form a perpendicularly intersecting conductive node. The semi-finished product 1 of electric heating cloth is woven. A layer of thermoplastic polyurethane film with a thickness of 0.05 mm is hot-pressed onto the upper and lower surfaces of the semi-finished product at 150°C to obtain the finished graphene electric heating cloth.

[0125] Comparative Example 1:

[0126] Compared with Example 1, the difference is that all 68.13 parts of deionized water in the formulation are added to the main reactor at the beginning without water fractionation and high solids kneading; at the same time, the coupling agent is not pre-hydrolyzed, and the plasticizer is not added at the beginning of kneading. Instead, the coupling agent and plasticizer are added at the same time when the waterborne polyurethane emulsion is added. All other aspects are the same.

[0127] Comparative Example 2:

[0128] Compared with Example 1, the difference is that no plasticizer is added during the high-viscosity kneading and extrusion stage. Instead, 0.03 parts of plasticizer are added simultaneously with the addition of the waterborne polyurethane emulsion. All other aspects are the same.

[0129] Comparative Example 3:

[0130] Compared with Example 1, the difference is that 65.00 parts of deionized water used for dispersion in the main reactor are added to the main reactor all at once in the initial stage and directly dispersed at high speed without high solids kneading and extrusion. All other aspects are the same.

[0131] Comparative Example 4:

[0132] Compared with Example 1, the difference is that the pre-hydrolysis step of the coupling agent is omitted; the 3.13 parts of deionized water in step (2) are retained until step (6) when they are added to the main reactor, and 0.05 parts of the original coupling agent solution that has not been pre-hydrolyzed are added at the same time, and the rest is the same as in Example 1.

[0133] Test Example 1:

[0134] (1) Extract the graphene conductive yarn slurry after the preparation steps of each embodiment and comparative example are completed and after static curing is completed as test samples. Take about 5g of each sample and place it in a clean glass sample bottle.

[0135] (2) Add about 30 mL of deionized water to a 50 mL beaker, and use a pipette to add about 0.1 mL of the above test sample into the deionized water. Use a glass rod to stir clockwise at a uniform speed for 3 min for preliminary dilution.

[0136] (3) Place the beaker containing the diluent in an ultrasonic cleaner and sonicate at room temperature and 40 kHz for 2 min. All samples were treated under the same ultrasonic conditions. After treatment, particle size and zeta potential were tested.

[0137] (4) Take out the sample liquid after sonication, use a disposable dropper to draw an appropriate amount of liquid and inject it into the quartz cuvette for dynamic light scattering instrument. The liquid level should be controlled at 2 / 3 of the total height of the cuvette.

[0138] (5) Place the cuvette into the test chamber of the dynamic light scattering instrument (Malvern Zetasizer Nano ZS90), set the test temperature to 25℃ and the equilibration time to 120s. The system will automatically perform light source optimization and focus adjustment and record the light intensity fluctuation signal, record the particle size distribution curve of the sample, and record the apparent volume median particle size D50 and polydispersity index PDI output by the instrument software.

[0139] (6) Take another diluted sample solution that has been degassed by ultrasound and inject it into the folded capillary electrode cell. After removing the air bubbles, put it into the test chamber of the equipment, turn on the electrophoresis light scattering module, apply an electric field at 25°C to measure the electrophoretic mobility of the particles, and the system internally calculates and outputs the Zeta potential value based on the Smoluchowski model. Each group of samples is collected three times and the arithmetic mean is recorded.

[0140] Table 1. Apparent particle size and zeta potential of graphene conductive yarn slurry in each example and comparative example

[0141] sample Apparent volume median particle size D50 (nm) Polydispersion Index (PDI) Zeta potential (mV) Example 1 421.3 0.213 -38.6 Example 2 465.7 0.245 -35.2 Example 3 489.1 0.261 -33.9 Example 4 442.8 0.228 -37.1 Comparative Example 1 1582.4 0.672 -18.4 Comparative Example 2 894.6 0.451 -27.3 Comparative Example 3 1345.2 0.618 -21.5 Comparative Example 4 712.5 0.384 -24.8

[0142] Conclusions and Analysis: Combining Table 1 and Figure 2 It can be seen that the apparent volume median particle size D50 of Examples 1-4 is 421.3-489.1 nm, the PDI is 0.213-0.261, and the Zeta potential is -33.9-38.6 mV. Figure 2 The particle size distribution curves of the examples are mainly concentrated in the smaller particle size range, and the curve width is relatively narrow. The D50 of Example 1 is 421.3 nm and the PDI is 0.213. It has a smaller apparent particle size and a narrower particle size distribution in the example group.

[0143] The D50 of Comparative Example 1 and Comparative Example 3 increased to 1582.4 nm and 1345.2 nm, respectively, and the PDI was 0.672 and 0.618, respectively. Figure 2 The two sets of curves shifted towards larger particle sizes, and their distribution range significantly widened. Comparative Examples 1 and 3 both eliminated the staged water addition and high-solids-content kneading process used in Example 1. (Table 1 and...) Figure 2 The results show that the staged water addition and high solids kneading process are beneficial to reducing the apparent particle size measured under uniform test conditions and reducing the particle size distribution width.

[0144] After adjusting only the timing of plasticizer addition in Comparative Example 2, D50 increased from 421.3 nm in Example 1 to 894.6 nm, and PDI increased from 0.213 to 0.451. Combined with the data changes in Table 1, it can be seen that the particle size distribution range of Comparative Example 2 is wider than that of Example 1, indicating that the timing of plasticizer addition affects the particle size distribution of the slurry after kneading and dispersion.

[0145] In Comparative Example 4, after removing the coupling agent pre-hydrolysis treatment, the D50 was 712.5 nm, the PDI was 0.384, and the Zeta potential was -24.8 mV. The corresponding values ​​in Example 1 were 421.3 nm, 0.213, and -38.6 mV, respectively. This indicates that when the other formulations and process conditions remain consistent, the coupling agent pre-hydrolysis treatment can affect the apparent particle size distribution and Zeta potential of the slurry after uniform pretreatment. The above particle size data are used for relative comparison between different samples and are not used to determine the number of graphene sheets or the true lateral size of graphene.

[0146] Test Example 2:

[0147] (1) Extract the graphene conductive yarn obtained by high temperature curing in the examples and comparative examples, carefully scrape off the cured conductive coating on the surface of the yarn with a scalpel, and collect about 5 mg of dry powder as test samples for later use.

[0148] (2) Weigh about 200 mg of spectral grade potassium bromide powder that has been dried at high temperature, and place it together with the coating test sample collected above in a clean agate mortar. Grind it evenly in the same direction for about 5 minutes until it becomes an extremely fine powder.

[0149] (3) Transfer the uniformly mixed powder into the inner cavity of the stainless steel tablet mold, place it on the test bench of the hydraulic press, slowly apply 12MPa pressure and hold for 1min to press it into a test sheet with uniform thickness and semi-transparent.

[0150] (4) Fix the prepared pellet onto the sample cell support of the Fourier transform infrared spectrometer, and set the instrument scanning range to 4000 cm⁻¹. -1 ~400cm -1 Spectral resolution of 4 cm -1 The background and sample were acquired through 32 cumulative scans.

[0151] (5) After the measurement is completed, baseline correction is performed, and 3320cm is recorded. -1 1720cm -1 1100cm -1 and 1030cm -1 Absorbance of the nearby absorption peak; at 1720 cm⁻¹ -1 Using the nearby absorption peaks as internal standards, A3320 / A1720, A1100 / A1720, and A1030 / A1720 were calculated respectively.

[0152] Table 2. Relative absorbance ratio of FTIR characteristic peaks of the cured coatings in each embodiment and the comparative example.

[0153] sample A3320 / A1720 A1100 / A1720 A1030 / A1720 Example 1 0.859 0.649 0.616 Example 2 0.863 0.634 0.618 Example 3 0.861 0.655 0.625 Example 4 0.856 0.645 0.613 Comparative Example 1 0.860 0.237 0.207 Comparative Example 2 0.862 0.592 0.577 Comparative Example 3 0.861 0.570 0.545 Comparative Example 4 0.868 0.313 0.254

[0154] Conclusions and Analysis: Combining Table 2 and Figure 3 It can be seen that the samples in each group are at 3320cm -1 and 1720cm -1 There are obvious absorption zones in the vicinity, with a maximum of 1720 cm. -1 After using the absorption peak as an internal standard, the A3320 / A1720 ratios of Examples 1-4 and Comparative Examples 1-4 were all in the range of 0.856-0.868, with small differences between groups. Figure 3 3320cm -1 and 1720cm -1 The main absorption bands in the vicinity are basically in the same position, indicating that different preparation processes have not caused significant changes to the main characteristic absorption bands of polyurethane.

[0155] In Examples 1-4, the A1100 / A1720 ratio was 0.634-0.655, and the A1030 / A1720 ratio was 0.613-0.625. In Comparative Example 4, the corresponding values ​​decreased to 0.313 and 0.254, respectively, and in Comparative Example 1, they further decreased to 0.237 and 0.207. Figure 3 Comparative Examples 1 and 4 are located between 1100 and 1030 cm. -1 The absorption intensity in the region was also lower than that in the Example Group. The main difference between Example 1 and Comparative Example 4 was whether the coupling agent underwent pre-hydrolysis treatment. (Table 2 and...) Figure 3 This indicates that pre-hydrolysis treatment of the coupling agent can significantly alter the curing coating at 1100 cm⁻¹. -1 ~1030cm -1 The relative absorption intensity of the region, the COC absorption of the polytetrahydrofuran ether segment and the Si-O related absorption of the silicon-containing structure at 1100 cm⁻¹ -1 ~1030cm -1 The regions overlap.

[0156] Test Example 3:

[0157] (1) Extract the graphene conductive yarn slurry of each example and comparative example after it has been cured for the specified curing time according to the corresponding preparation steps. Use a stainless steel spatula to slowly stir the sample for two minutes to eliminate any possible micro-skin on the surface. After standing for five minutes until the bubbles rise and burst, collect about 10 ml of liquid as a test sample.

[0158] (2) Turn on the main unit of the rotary rheometer and the constant temperature water bath circulation system, install a parallel plate measuring rotor with a diameter of 40mm, and control the temperature of the test platform to be constant at 25℃ through the operating software.

[0159] (3) Use a pipette to draw an appropriate amount of test sample and drop it onto the fixed test stage on the lower layer of the rheometer. Control the upper parallel plate rotor to slowly descend to the set gap position. The gap height is set to 1 mm. Use a scraper to gently scrape off the excess slurry residue overflowing from the edge. Let it stand for 3 minutes to eliminate the internal stress generated when loading the sample.

[0160] (4) Set the shear rate scanning program in the equipment control software, and set the shear rate variation range to 0.1s. -1 up to 100s -1 The acquisition mode was set to logarithmic scan, and the system collected 25 data points evenly within this interval.

[0161] (5) Start the test program. The instrument sensor records the torque required for rotor rotation in real time and converts it into apparent viscosity value. After the test, export the original data table containing shear rate and apparent viscosity.

[0162] Table 3. Apparent viscosity and shear thinning index of conductive yarn sizing materials for each embodiment and comparative example

[0163] sample <![CDATA[0.1s -1 Viscosity at shear rate (Pa·s) <![CDATA[10s -1 Viscosity at shear rate (Pa·s) <![CDATA[100s -1 Viscosity at shear rate (Pa·s) Shear thinning index (η0.1 / η10) Example 1 42.15 8.34 1.87 5.05 Example 2 38.64 7.92 1.76 4.88 Example 3 45.22 9.05 2.11 5.00 Example 4 40.81 8.16 1.94 5.00 Comparative Example 1 18.52 6.78 3.42 2.73 Comparative Example 2 58.74 19.35 5.62 3.04 Comparative Example 3 22.14 7.21 3.05 3.07 Comparative Example 4 33.56 10.42 2.86 3.22

[0164] Conclusions and Analysis: Combining Table 3 and Figure 4 It can be seen that the apparent viscosity of Examples 1 to 4 all decreases with increasing shear rate, starting from 0.1 s⁻¹. -1 Increased to 100s -1 Subsequently, the apparent viscosity of Example 1 decreased from 42.15 Pa·s to 1.87 Pa·s, Example 2 from 38.64 Pa·s to 1.76 Pa·s, Example 3 from 45.22 Pa·s to 2.11 Pa·s, and Example 4 from 40.81 Pa·s to 1.94 Pa·s. The shear thinning index of Examples 1 to 4 ranged from 4.88 to 5.05. Figure 4 The rheological curves in the samples all decreased continuously with increasing shear rate, indicating that the slurry in the example group exhibited significant shear-thinning behavior.

[0165] Comparative Examples 1 and 3 were at 0.1s -1 The apparent viscosities were 18.52 Pa·s and 22.14 Pa·s, respectively, lower than the 42.15 Pa·s of Example 1; the shear thinning indices were 2.73 and 3.07, respectively, also lower than the 5.05 of Example 1. Figure 4 The curve of Comparative Example 3 changes with shear rate by a smaller margin than that of Example 1, and the data in Table 3 show that the apparent viscosity of Comparative Example 1 also changes by a smaller margin. Combined with the one-time water addition method used in the two comparative examples, it can be seen that staged water addition and high solids kneading process affect the viscosity difference of the slurry under low and high shear conditions.

[0166] Combined with Table 3 and Figure 4 It can be seen that Comparative Example 2 is at 0.1s -1 10s -1 and 100s -1 The apparent viscosities of the following samples were 58.74 Pa·s, 19.35 Pa·s, and 5.62 Pa·s, respectively, all higher than those of Example 1, corresponding to a shear thinning index of 3.04. Figure 4 The curve of Comparative Example 2 is generally above that of Example 1, indicating that delaying the addition of the plasticizer increases the overall apparent viscosity of the slurry while decreasing it by 0.1s. -1 up to 10s -1 The percentage change in viscosity within the range, Table 3 and Figure 4 This indicates that the method of adding water and the timing of adding plasticizer both affect the rheological response of the slurry.

[0167] Test Example 4:

[0168] (1) Extract the finished graphene electric heating cloths prepared in each example and comparative example. Use a fabric cutter to cut the electric heating cloths into standard square test pieces of 10cm×10cm at room temperature. Along the two opposite sides (i.e. the left and right edges of the sample pieces) parallel to the longitudinal direction of the metal conductive lines, partially remove the thermoplastic polyurethane film on the surface to expose the metal conductive lines located on both sides of the sample pieces. Lead them out and press them with copper foil conductors to form positive and negative test electrodes.

[0169] (2) Place the prepared square test sample flat on an insulated and heat-insulating test platform. Select 8 non-overlapping test points on the surface of the sample. Remove the thermoplastic polyurethane film on the surface of each test point and avoid the longitudinal metal conductive line area so that the four probes can directly contact the graphene conductive yarn layer. The arrangement direction of the four probes is consistent with the direction of the conductive weft yarn. Measure the weft sheet resistance of each test point and record the sheet resistance value of each point. The recorder automatically calculates and outputs the average sheet resistance and the sheet resistance variance of each sample.

[0170] (3) The test sample with copper foil electrodes is suspended and fixed on the acrylic bracket. The positive and negative test clips of the DC regulated power supply are connected to the copper foil conductors on both sides of the sample (i.e., power is supplied directly to the graphene weft yarn through the longitudinal metal conductive lines on both sides). A K-type thermocouple temperature sensor is attached to the back of the sample at the center position. The other end of the sensor is connected to a multi-channel temperature monitoring instrument.

[0171] (4) Start the data recording program of the temperature monitoring instrument, set the sampling interval to 5s, then turn on the DC regulated power supply and instantly adjust the output constant voltage to 5V, keep it powered on for 600s, record the complete heating process of the sample center temperature during the power-on period, and sort out the original data after the test.

[0172] Table 4. Electrical and electrothermal properties of the finished graphene electrothermal cloths in each embodiment and comparative example.

[0173] Sample Name Average sheet resistance (Ω / sq) Sheet resistance variance Center temperature (°C) after 600 seconds of power-on. Average heating rate over the initial 60 seconds (°C / s) Example 1 14.8 1.25 62.4 0.38 Example 2 16.3 1.41 58.7 0.35 Example 3 13.9 1.18 65.1 0.42 Example 4 15.2 1.33 61.2 0.37 Comparative Example 1 112.4 18.73 33.1 0.08 Comparative Example 2 24.3 5.82 51.6 0.22 Comparative Example 3 86.5 12.41 38.2 0.12 Comparative Example 4 17.6 1.84 56.5 0.31

[0174] Conclusions and Analysis: Combining Table 4 and Figure 5 It can be seen that the average latitudinal sheet resistance of Examples 1-4 is 13.9-16.3 Ω / sq, the center temperature is 58.7-65.1℃ after 600s of energization, and the average heating rate in the initial 60s is 0.35-0.42℃ / s. Figure 5 Example 1 showed a rapid temperature rise in the initial stage of power-on, followed by a gradual decrease in the temperature rise rate. The data in Table 4 also showed that Example 1 had a high initial temperature rise rate. Example 3 had the lowest average latitudinal sheet resistance at 13.9 Ω / sq, while having the highest 600s center temperature of 65.1℃ and the highest initial 60s average temperature rise rate of 0.42℃ / s.

[0175] The average latitudinal sheet resistance of Comparative Examples 1 and 3 were 112.4 Ω / sq and 86.5 Ω / sq, respectively, significantly higher than the 14.8 Ω / sq of Example 1; the corresponding center temperatures after 600 s were 33.1 °C and 38.2 °C, respectively, and the average heating rates after the initial 60 s were 0.08 °C / s and 0.12 °C / s, respectively. According to Table 4, the heating performance of Comparative Example 1 was significantly reduced, and... Figure 5 The overall heating curve of Comparative Example 3 was lower than that of Example 1, indicating that the conductivity and heating performance of the finished electric heating cloth under constant voltage conditions were significantly reduced after the elimination of the staged water addition and high solids kneading process.

[0176] The average latitudinal sheet resistance of Comparative Example 2 was 24.3 Ω / sq, the center temperature was 51.6℃ after 600 s, and the average heating rate for the initial 60 s was 0.22℃ / s. These results fall between those of Example 1 and Comparative Examples 1 and 3. Figure 5 The heating curve of Comparative Example 2 is also located below that of Example 1. The formulations of Example 1 and Comparative Example 2 are consistent, the main difference being the timing of plasticizer addition. (Table 4 and...) Figure 5 This indicates that the timing of plasticizer addition affects the final electrical conductivity and temperature rise performance.

[0177] Combine Table 4 and Figure 5 It can be seen that the average latitudinal square resistance of Comparative Example 4 is 17.6 Ω / sq, the center temperature at 600s is 56.5℃, and the average heating rate at the beginning of 60s is 0.31℃ / s. Compared with Example 1, the resistance increase of Comparative Example 4 is smaller than that of Comparative Examples 1 to 3, but the heating rate and the center temperature at 600s are still reduced.

[0178] Test Example 5:

[0179] (1) Extract the finished graphene electric heating cloth prepared in each example and comparative example, cut it into a strip test piece of 20cm×5cm, with the long side direction consistent with the direction of the conductive weft yarn. Set a test end area of ​​about 1cm wide on each side of the sample piece (parallel to the direction of the metal conductive line), remove the thermoplastic polyurethane film on the surface of the test end area, so that the longitudinal metal conductive lines distributed on both sides of the sample piece are exposed respectively. Clamp the two poles of the resistance tester on the exposed metal conductive lines on both sides respectively, measure the initial resistance value of the overall parallel heating network of the sample piece and record it.

[0180] (2) Place a portion of the test samples in a drum-type fabric washing tester, add standard neutral detergent, set the washing water temperature to 30℃, and each washing cycle includes 30 minutes of continuous rotating washing and 10 minutes of dehydration. After completing 10, 30, and 50 washing cycles, remove the samples and air dry them naturally. After achieving state equilibrium under the same environmental conditions as the initial resistance test, measure the resistance values ​​at both ends again at the same clamping position and calculate the resistance change rate at different washing stages.

[0181] (3) Extract another part of the unwashed test sample, clamp the two ends of the sample onto the upper and lower movable clamps of the flexible material flexural fatigue testing machine, set the instrument's single running trajectory to fold 180 degrees and reset, and adjust the test running frequency to 60 times per minute.

[0182] (4) Start the flexural fatigue testing machine to perform continuous bending operation. When the instrument counter reaches 10,000 cycles, stop the equipment, remove the sample and let it stand for 30 minutes to release the residual internal stress. Connect the micro-ohmmeter to measure the final resistance value after bending and calculate the corresponding resistance change rate. Organize and archive all collected data.

[0183] Table 5. Washability and bending resistance of the finished graphene heating cloths of each embodiment and comparative example

[0184] Sample Name Change in resistivity after 10 washes (%) Change in resistivity after 30 washes (%) Change in resistivity after 50 washes (%) Rate of change in resistance after 10,000 bends (%) Example 1 0.85 2.14 5.21 1.52 Example 2 1.12 2.65 6.34 2.08 Example 3 0.74 1.98 4.87 1.35 Example 4 0.96 2.41 5.92 1.84 Comparative Example 1 14.52 125.63 314.85 58.26 Comparative Example 2 4.65 18.24 32.16 9.47 Comparative Example 3 6.82 27.53 48.91 15.33 Comparative Example 4 11.24 42.15 87.41 24.12

[0185] Conclusions and Analysis: Combining Table 5 and Figure 6 It can be seen that the resistance change rate of Examples 1-4 after 10 washes was 0.74%-1.12%, after 30 washes was 1.98%-2.65%, and after 50 washes was 4.87%-6.34%; the resistance change rate after 10,000 bends was 1.35%-2.08%. Figure 6 The resistance change rate of Example 1 increased slowly with the number of water washes. According to the data in Table 5, each example still maintained a low resistance change after 50 water washes.

[0186] Comparative Example 1 showed resistivity changes of 14.52%, 125.63%, and 314.85% after 10,000 washes, respectively, and a resistivity change of 58.26% after 10,000 bends. Figure 6 The resistance change rate of Comparative Example 1 increased rapidly with the number of water washings, and the gap between it and Example 1 gradually widened. The resistance change rate of Comparative Example 3 was 48.91% after 50 water washings and 15.33% after 10,000 bendings, which was also significantly higher than that of Example 1. Combining the preparation conditions of the two comparative examples, it can be seen that after canceling the graded water addition and high solid content kneading process, the resistance stability of the finished product decreased after repeated water washing and bending.

[0187] The resistance change rate of Comparative Example 2 after 50 washes was 32.16%, and the resistance change rate after 10,000 bends was 9.47%, both higher than that of Example 1. The main process difference between Example 1 and Comparative Example 2 is the timing of plasticizer addition. The results show that the timing of plasticizer addition affects the resistance retention of the finished product after repeated washing and bending.

[0188] Combined with Table 5 and Figure 6 It can be seen that the resistance change rate of Comparative Example 4 after 50 washes was 87.41%, and the resistance change rate after 10,000 bends was 24.12%, both higher than that of Example 1. Figure 6 The water washing resistance change curve of Comparative Example 4 is also significantly higher than that of Example 1. The main difference between Example 1 and Comparative Example 4 is whether the coupling agent has undergone pre-hydrolysis treatment. Therefore, Table 5 and Figure 6 This demonstrates a clear correlation between the pre-hydrolysis treatment of the coupling agent and the finished product's resistance to washing, electrical resistance retention, and bending resistance. Existing test results are used to evaluate macroscopic electrical stability.

[0189] Test Example 6:

[0190] (1) Extract the finished graphene electric heating cloth prepared in each example and comparative example, cut it into a square test sample with a specification of 50cm by 50cm, remove the thermoplastic polyurethane film in an area of ​​about 1cm wide along the two opposite sides parallel to the longitudinal direction of the metal conductive line, so that the metal conductive lines distributed on both sides of the sample are exposed respectively; lead out the exposed metal conductive lines on both sides and press them with copper foil conductors to form positive and negative power supply electrodes, and lay the sample flat and fix it on an insulated and heat-insulating wooden platform in a windless test room with a room temperature of 25℃.

[0191] (2) Use a water-based marker to draw a uniform grid of 5 rows and 5 columns on the sample surface to determine 25 evenly distributed cross test nodes. Use thermally conductive silicone grease and high-temperature resistant polyimide tape to attach and fix 25 K-type high-precision patch thermocouples to the corresponding test nodes. Connect the data lines of all thermocouple probes to the acquisition end of the multi-channel temperature monitoring instrument.

[0192] (3) Turn on the DC regulated power supply and adjust the output voltage to be constant at 12V. Continuously power on the test sample and observe the real-time monitoring screen of the multi-channel temperature monitoring instrument. After the system reaches thermal equilibrium after 30 minutes of continuous power-on, click the software record button to capture the absolute temperature values ​​of 25 test nodes.

[0193] (4) After the test, disconnect the output of the regulated power supply. Perform statistical processing on the 25 temperature data collected for each sample, calculate the average temperature value of the 25 points, select the highest and lowest temperatures recorded in the test area, and calculate the maximum absolute value of the deviation of the single point temperature from the average temperature. Fill the statistical results into the data table.

[0194] Table 6. Surface temperature distribution of finished graphene heating cloths in each embodiment and comparative example.

[0195] Sample Name Average temperature (°C) Maximum temperature (°C) Minimum temperature (°C) Maximum absolute deviation (°C) Example 1 45.2 46.1 44.5 0.9 Example 2 42.8 44.2 41.5 1.4 Example 3 48.1 49.3 46.8 1.3 Example 4 44.6 45.9 43.4 1.3 Comparative Example 1 31.4 37.8 26.5 6.4 Comparative Example 2 39.5 44.7 34.2 5.3 Comparative Example 3 33.7 42.1 28.3 8.4 Comparative Example 4 41.2 43.5 39.1 2.3

[0196] Conclusions and Analysis: Combining Table 6 and Figure 7 It can be seen that after continuous power supply at 12V for 30 minutes in Examples 1-4, the average temperature of the 25 temperature measuring points was 42.8-48.1℃. The difference between the highest and lowest temperatures was small, with the maximum absolute deviation ranging from 0.9 to 1.4℃. Figure 7 The temperature curve along the diagonal of the sample in Example 1 is relatively stable, indicating that Examples 1 to 4 all have good surface temperature uniformity within a 50cm×50cm test area.

[0197] The average temperature of Example 1 was 45.2℃, the highest temperature was 46.1℃, the lowest temperature was 44.5℃, and the maximum absolute deviation was 0.9℃. Example 1 had the smallest maximum absolute deviation among the example groups. Figure 7 The fluctuation range of the corresponding temperature curve is also relatively small.

[0198] Comparative Example 1 had an average temperature of 31.4℃, a maximum temperature of 37.8℃, and a minimum temperature of 26.5℃, with the maximum absolute deviation increasing to 6.4℃. Comparative Example 3 had an average temperature of 33.7℃, a maximum temperature of 42.1℃, and a minimum temperature of 28.3℃, with the maximum absolute deviation reaching 8.4℃. Table 6 shows that the maximum absolute deviation of Comparative Example 1 increased significantly, and... Figure 7The temperature curve of Comparative Example 3 showed significant fluctuations. Considering the preparation conditions of Comparative Example 1 and Comparative Example 3, Table 6 and... Figure 7 This indicates that eliminating the staged water addition and high-solids kneading process will reduce the surface temperature uniformity of large-area electric heating cloth.

[0199] Combined with Table 6 and Figure 7 It can be seen that the maximum absolute value of the deviation in Comparative Example 2 is 5.3℃, which is higher than the 0.9℃ in Example 1. Figure 7 The temperature fluctuation in Comparative Example 2 was also greater than that in Example 1. The main difference between Example 1 and Comparative Example 2 was the timing of the addition of the plasticizer. Therefore, the results show that the timing of the addition of the plasticizer affects the temperature distribution uniformity of the large-area electric heating cloth. The maximum absolute value of the deviation in Comparative Example 4 was 2.3℃, which was higher than that in Example 1, but significantly lower than that in Comparative Examples 1 to 3. This indicates that the temperature uniformity decreased after the removal of the coupling agent pre-hydrolysis treatment, but the decrease was less than the changes caused by the removal of the staged water addition and the high solids kneading process.

Claims

1. A graphene electric heating cloth, characterized in that, It is composed of a semi-finished electric heating cloth (1) and a thermoplastic polyurethane film hot-pressed onto the upper and lower surfaces of the semi-finished electric heating cloth (1); The warp yarn of the semi-finished electric heating cloth (1) includes ordinary polyester yarn and spaced metal conductive yarn, and the weft yarn includes ordinary polyester yarn and graphene conductive yarn. The graphene conductive yarn and the metal conductive yarn are in contact and connected at the weaving intersection. The graphene conductive yarn is made by impregnating polyester yarn with graphene conductive yarn slurry and then curing it. The graphene conductive yarn sizing agent is made from raw materials comprising the following parts by weight: Graphene 10.00 to 14.00 parts; Carbon black 0.80 to 1.50 parts; 0.80 to 1.50 parts of multi-walled carbon nanotubes; 15.00 to 20.00 parts of anionic aliphatic waterborne polyurethane emulsion; Dispersant 0.50 to 0.80 parts; 0.03 to 0.08 parts of coupling agent; Plasticizer 0.02 to 0.05 parts; 0.03 to 0.08 parts of defoamer; 61.99 to 72.82 parts of deionized water.

2. The graphene electrothermal cloth according to claim 1, characterized in that, The graphene conductive yarn sizing agent is made from raw materials comprising the following parts by weight: 11.00 to 12.00 parts of graphene; Carbon black 1.00 to 1.20 parts; 1.00 to 1.20 parts of multi-walled carbon nanotubes; 17.14 to 18.00 parts of anionic aliphatic waterborne polyurethane emulsion; Dispersant 0.60 to 0.70 parts; 0.05 to 0.06 parts of coupling agent; Plasticizer 0.03 to 0.04 parts; 0.05 to 0.06 parts of defoamer; Deionized water: 67.74 to 68.13 parts.

3. The graphene electrothermal cloth according to claim 1, characterized in that, The metal conductive wire is a tin-plated copper wire, and the metal conductive wire is used for electrical connection with an external conductor. The dispersant is sodium polyacrylate; The coupling agent is 3-methacryloyloxypropyltrimethoxysilane; The plasticizer is dioctyl terephthalate; The defoamer is polyether-modified polydimethylsiloxane.

4. The graphene electrothermal cloth according to claim 1, characterized in that, The anionic aliphatic waterborne polyurethane emulsion is an aqueous emulsion with a solid content of 30% to 35%, and is made from raw materials comprising the following parts by weight: 100.0 parts of polytetrahydrofuran ether diol; 33.3 parts of isophorone diisocyanate; 6.7 parts of 2,2-dimethylolpropionic acid; 5.0 parts of triethylamine; 269.0 to 338.0 parts of deionized water.

5. The graphene electrothermal cloth according to claim 4, characterized in that, The preparation steps of the anionic aliphatic waterborne polyurethane emulsion are as follows: 100.0 parts of the polytetrahydrofuran ether diol were dehydrated at 100°C for 2 hours under reduced pressure (gauge pressure not exceeding -0.09 MPa) and then cooled to 60°C. Add 33.3 parts of the isophorone diisocyanate, heat to 80°C, and react at a constant temperature for 2 hours under nitrogen protection; Subsequently, 6.7 parts of the 2,2-dimethylolpropionic acid were added, and the reaction was continued at 80°C for 3 hours to obtain a polyurethane prepolymer with isocyanate-terminated groups. After cooling the polyurethane prepolymer to 40°C, add 5.0 parts of the triethylamine and continue stirring to neutralize and react for 30 minutes. Under high-speed shear stirring at 2000 rpm, 269.0 to 338.0 parts of the deionized water were added dropwise for phase inversion emulsification and continued to disperse for 60 minutes to obtain the anionic aliphatic waterborne polyurethane emulsion.

6. A method for preparing a graphene electrothermal cloth as described in any one of claims 1-5, characterized in that, The process includes the following: Deionized water was extracted from the total amount of deionized water in the graphene conductive yarn sizing agent formulation, and the coupling agent was added in the formulation amount. The mixture was kept warm under heating and stirring conditions to obtain a pre-hydrolyzed solution of the coupling agent. A portion of the deionized water in the total amount of the formula is mixed with the dispersant, plasticizer, carbon black and multi-walled carbon nanotubes in the formula amount, and then the graphene in the formula amount is added in batches, and the kneading and extrusion state is maintained under cooling conditions. Then, the remaining deionized water of the total amount of the formula is added to it, and the stirring speed is increased simultaneously to continue dispersing, so as to obtain a pre-dispersed slurry. The pre-dispersed slurry is cooled down, the stirring speed is reduced, and then the formulated amount of anionic aliphatic waterborne polyurethane emulsion and defoamer are added to it while stirring is maintained; The pre-prepared coupling agent pre-hydrolyzed solution was then added dropwise, and after stirring, the mixture was filtered out and allowed to stand and mature at room temperature in a sealed environment to obtain the graphene conductive yarn slurry. Polyester yarn is continuously passed through an impregnation tank containing graphene conductive yarn slurry by a drawing device. After the excess graphene conductive yarn slurry on the surface is scraped off by a tungsten steel scraper, it is continuously fed into the drying tunnel and baked and cured in sequence to obtain graphene conductive yarn. Ordinary polyester yarn and metal conductive yarn are used as warp yarns, and ordinary polyester yarn and graphene conductive yarn are used as weft yarns. The yarns are interwoven in plain weave on a loom, so that the graphene conductive yarn and the metal conductive yarn form a perpendicularly intersecting conductive node, and the semi-finished product of electric heating cloth (1) is woven. A thermoplastic polyurethane film is hot-pressed onto the upper and lower surfaces of the semi-finished electric heating cloth (1) to obtain the finished graphene electric heating cloth.

7. The preparation method according to claim 6, characterized in that, In the preparation of the coupling agent pre-hydrolyzed solution, the amount of deionized water used accounts for 3.4% to 6.5% of the total deionized water in the formulation. After adding the coupling agent, heat and keep the water temperature constant between 38°C and 48°C, and stir and keep warm for 30 to 50 minutes at a speed of 150 rpm to 250 rpm.

8. The preparation method according to claim 6, characterized in that, During the kneading and extrusion process, the stirring speed is adjusted to 400 rpm to 600 rpm, the core temperature of the material is controlled to not exceed 50°C by the jacket cooling water, and the kneading and extrusion time is maintained for 50 min to 70 min. Furthermore, the amount of deionized water used accounts for 16.5% to 29.0% of the total deionized water in the formula.

9. The preparation method according to claim 6, characterized in that, During the dispersion process of adding the remaining deionized water, the remaining deionized water is added within 10 to 20 minutes, the stirring speed is increased to 1200 rpm to 1800 rpm, and the dispersion is continued for 35 to 55 minutes. When adding the anionic aliphatic waterborne polyurethane emulsion and defoamer, the reactor is fully cooled to reduce the system temperature to 20°C to 30°C, and the stirring speed is reduced to 200 rpm to 400 rpm. After the addition is complete, the stirring speed is maintained for 20 min to 40 min.

10. The preparation method according to claim 6, characterized in that, During the preparation of the graphene conductive yarn, the baking temperature is 70°C to 90°C and the time is 10 min to 15 min. The curing temperature is 110°C to 140°C, and the time is 5 min to 10 min; During the hot-pressing process of the upper and lower surfaces of the electric heating cloth semi-finished product (1) to form a layer of thermoplastic polyurethane film, the hot-pressing temperature is set to 150°C and the thickness of the thermoplastic polyurethane film is 0.05 mm.