A heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive and its preparation method

By using an electrothermal paste with micron-sized spherical microspheres and isocyanate-group pressure-sensitive adhesive layers, the problems of conductive channel interruption and insufficient water resistance caused by emulsion adhesives are solved, achieving low resistance, high strength and stability, suitable for the production of flexible and ultra-thin electrothermal materials.

CN123075752APending Publication Date: 2026-11-10FOSHAN XIUBAO UNDERWEAR TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611472520.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The emulsion adhesive in existing electrothermal pastes causes the conductive channels to be interrupted and has insufficient water resistance, making it impossible to simultaneously meet the requirements of low resistance, high mechanical strength, and stable reliability.

Method used

Micron-sized spherical microspheres are used as the adhesive, and the outer shell is a pressure-sensitive adhesive layer containing isocyanate groups. Combined with components such as conductive carbon black, graphite, and graphene, the bonding is achieved through a combination of hot pressing and moisture curing, which avoids the breakage of the conductive network and enhances the bonding strength in a humid environment.

Benefits of technology

It significantly reduces volume resistivity and contact resistance, improves electrothermal conversion efficiency, enhances bonding strength and water resistance, and is suitable for the preparation of flexible devices and ultrathin films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123075752A_ABST
    Figure CN123075752A_ABST
Patent Text Reader

Abstract

A heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive and its preparation method are disclosed. The paste comprises the following components by weight percentage: 5-35% microsphere adhesive, 5-25% conductive carbon black, 10-35% conductive graphite, 1-10% graphene, 0.5-10% dispersant, 0.1-2% defoamer, 0.1-2% leveling agent, and 20-60% dispersion medium. The microsphere adhesive comprises a polymer microsphere core and a pressure-sensitive adhesive shell. The overall particle size of the microsphere adhesive is D50 = 4μm-6μm. The preparation method includes: S1, first preparing the polymer microsphere core, and then coating its surface with a pressure-sensitive adhesive layer containing isocyanate groups to obtain a core-shell structured microsphere adhesive; S2, mixing and dispersing the conductive carbon black, conductive graphite, graphene, dispersant, defoamer, leveling agent, and dispersion medium to obtain a conductive paste; S3, mixing the microsphere adhesive and the conductive paste evenly to obtain a heat-pressable and moisture-curable electrothermal paste. The electrothermal paste prepared by this invention has the characteristics of low resistance and high electrothermal conversion efficiency, and can be used for the preparation of flexible devices or ultrathin films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrothermal functional paste technology, specifically to a heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive and its preparation method. Background Technology

[0002] Electrothermal pastes are core functional materials for products such as flexible heating devices, battery heating films, and industrial insulation devices. Their core requirements are good coatability, high and stable electrothermal conversion efficiency (low resistance), and excellent mechanical strength and long-term reliability after curing. The basic components of these pastes include conductive fillers (carbon nanotubes, graphene, metal powders, etc.), binders, dispersion media, and a small amount of functional additives. Among these, the binder, as a key component connecting the conductive filler and the substrate, directly affects the film-forming quality, mechanical properties, and electrical conductivity of the paste due to its morphology, dispersibility, and curing characteristics.

[0003] Currently, the most commonly used binder system in electrothermal pastes is emulsion adhesive (such as acrylic emulsion adhesive, styrene-butadiene emulsion adhesive, polyurethane emulsion adhesive, etc.). This system primarily utilizes the excellent dispersibility and coating fluidity of nano-sized particles in emulsion adhesives to enable uniform film formation. Curing methods are mostly thermosetting or room-temperature air drying, where the adhesive particles fuse and cross-link to form a continuous film layer, achieving bonding and fixation between the conductive filler and the substrate. However, while emulsion adhesive-based electrothermal pastes offer processing advantages, they face key challenges in practical applications: First, the particles in the emulsion adhesive are hydrophilic or polar particles. During the mixing process of the slurry, their surface tension makes it easy for the particles to be adsorbed on the surface of the conductive filler or to form an "insulating coating layer" between the filler particles. After curing, these adhesive layers will fill the gaps between the conductive fillers, interrupt the original continuous conductive network, force the current to conduct around the path, significantly increase the volume resistivity and contact resistance of the slurry, and cause the electrothermal conversion efficiency to drop sharply. The resistance value is usually 1 to 2 orders of magnitude higher than the theoretical value.

[0004] Secondly, most emulsion adhesives have insufficient moisture resistance after curing. They are prone to absorbing water and swelling in humid environments or under washing conditions, which leads to decreased adhesion, loss of conductive fillers, further increase in resistance, or even failure.

[0005] In summary, existing electrothermal pastes using emulsion adhesives as binders cannot simultaneously meet the high-end application requirements of "low resistance, high mechanical strength, and stable reliability" due to the disruptive effect of adhesive particles on conductive channels and their water resistance deficiencies. Therefore, developing a microsphere-based electrothermal paste that avoids the drawbacks of emulsion adhesives and combines the functions of hot-press bonding and moisture-curing reinforcement is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0006] To overcome the shortcomings of the prior art, the present invention provides a heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive and its preparation method.

[0007] The technical solution adopted by this invention to solve its technical problem is: A heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive is characterized by comprising the following components by weight percentage: 5-35% microsphere adhesive, 5-25% conductive carbon black, 10-35% conductive graphite, 1-10% graphene, 0.5-10% dispersant, 0.1-2% defoamer, 0.1-2% leveling agent, and 20-60% dispersion medium; wherein the microsphere adhesive is a micron-sized spherical dispersion, the microsphere adhesive comprising a polymer microsphere core and a pressure-sensitive adhesive shell covering the polymer microsphere core, the pressure-sensitive adhesive shell being a pressure-sensitive adhesive layer containing isocyanate groups; and the overall particle size D50 of the microsphere adhesive is 4μm to 6μm.

[0008] Furthermore, the polymer microsphere core is a polystyrene core or a polymethyl methacrylate core; and / or, the pressure-sensitive adhesive layer is an acrylate copolymer containing isocyanate groups.

[0009] Furthermore, the conductive carbon black has a DBP oil absorption value of 50~500 and a particle size of 10~100nm.

[0010] Furthermore, the conductive graphite is one or more of the following: powder, flake, and fibrous forms.

[0011] Furthermore, the graphene is one or more of single-layer graphene, multilayer graphene, reduced graphene, and graphene oxide.

[0012] Furthermore, the dispersant is one or a mixture of two of polyurethane, polycarboxylate, and acrylic copolymer.

[0013] Furthermore, the defoamer is one of organosilicon, mineral oil, or polyether; the leveling agent is one of polyacrylic acid, fluorocarbon, or organosilicon-modified polyether; and the dispersion medium is one of ethyl acetate, butyl acetate, acetone, butanone, isopropyl ether, or sulfoxide.

[0014] A method for preparing the above-mentioned heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive, characterized by comprising the following steps: S1. Synthesis of microsphere adhesive: First, prepare the core of polymer microspheres, and then coat the surface of the core with a pressure-sensitive adhesive layer containing isocyanate groups to obtain core-shell structured microsphere adhesive. S2. Preparation of conductive slurry: Conductive carbon black, conductive graphite, graphene, dispersant, defoamer, leveling agent, and dispersion medium are mixed, stirred, and dispersed, and then ground to a fineness ≤15μm to obtain conductive slurry; S3. Preparation of electrothermal paste: Mix the microsphere adhesive and conductive paste evenly to obtain a heat-pressed and moisture-curable electrothermal paste.

[0015] Furthermore, step S1 specifically includes: S1-1 Core Synthesis: By mass percentage, 20-50 wt% of polymeric monomer, 0.1-3 wt% of initiator AIBN, 1-10 wt% of stabilizer PVP, and 40-80 wt% of ethanol solvent are added to the reactor. After deoxygenation by purging with nitrogen, polymerization is carried out at 60-80℃ for 6-12 hours. After centrifugation, washing, and drying, the polymer microsphere core is obtained. S1-2, Shell Synthesis: Prepare a monomer mixture by mass: 3-8 parts butyl acrylate, 1-3 parts vinyl acetate, 0.1-1 parts methyl methacrylate, 0.5-1 parts ethyl 2-isocyanate, and 0.01-0.3 parts initiator AIBN; prepare a 30-50 wt% ethyl acetate dispersion for the polymer microsphere core, heat to 50-75℃, and add the monomer mixture dropwise at 5 mL / min, with the amount added being 10-40 wt% of the dispersion mass. After the addition is complete, continue the reaction for 4-8 hours, and discharge the microsphere gel.

[0016] Further, in step S2, the stirring speed is 1000~2000 r / min, the dispersion time is 30~60 min, and the slurry is ground 1~2 times with a three-roll mill until the fineness of the slurry reaches below 15 μm; And / or, in step S3, a paddle mixer is used with a speed of 100~500 r / min and a mixing time of 30~60 min.

[0017] The beneficial effects of this invention are: 1. This invention uses micron-sized microsphere adhesive with a particle size D50 of 4~6μm to replace conventional nano-sized emulsion adhesive as the binder for electrothermal paste. The large-particle-size microsphere adhesive does not easily fill the tiny gaps between conductive fillers, avoiding the adhesive layer from breaking the original continuous conductive network, thereby significantly reducing the volume resistivity of the heating layer.

[0018] 2. The microsphere adhesive of the present invention has a spherical structure, which allows the microsphere adhesive to bond with the conductive filler through point contact. It does not spread on the surface of the filler to form a continuous polymer film, thus avoiding the complete insulating coating of conductive particles by traditional long-chain or network-like macromolecular emulsion adhesives. It only provides bonding through local contact points, so that the conductive components can maintain effective contact and communication, thereby significantly reducing contact resistance and improving electrothermal conversion efficiency.

[0019] 3. The microsphere adhesive shell of the present invention is a pressure-sensitive adhesive layer, which enables the electrothermal paste to have pressure-sensitive properties. In the electrode arrangement and heating film encapsulation process, only a short hot pressing is needed to complete the assembly and bonding, without the need for an additional long curing process, which helps to reduce production steps and improve production efficiency.

[0020] 4. The microsphere adhesive shell of the present invention contains active isocyanate groups (-NCO), which can undergo further cross-linking reaction in a humid environment or during water washing, thereby achieving secondary reinforcement of the bonding strength and improving water resistance, effectively meeting the needs of special application scenarios such as water washing and high humidity.

[0021] 5. The electrothermal paste prepared by this invention has the characteristics of low resistance and high electrothermal conversion efficiency. It only requires the preparation of an ultrathin film material to meet the heating requirements. It can be used for the preparation of flexible devices or ultrathin films and is suitable for application scenarios such as wearable devices and medical devices. Attached Figure Description

[0022] The present invention will be further described below with reference to the accompanying drawings and embodiments: Figure 1 This is a schematic diagram of the microsphere adhesive in Example 1; Figure 2 This is a schematic diagram of the preparation process of the heat-pressable-wet-curing electrothermal paste in Example 1; Figure 3 This is a schematic diagram of the preparation process of the heating film in Example 1; Figure 4 is a low-magnification scanning electron microscope image of the microsphere adhesive of Example 1; Figure 5 is a high-magnification scanning electron microscope image of the microsphere adhesive of Example 1. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings.

[0024] It should be noted that if the embodiments of the present invention involve directional indicators (such as up, down, left, right, front, back, top, bottom, inside, outside, vertical, horizontal, longitudinal, counterclockwise, clockwise, circumferential, radial, axial, etc.), the directional indicators are only used to explain the relative positional relationship and movement of the components in a certain specific posture (as shown in the figure). If the specific posture changes, the directional indicators will also change accordingly.

[0025] Furthermore, if the embodiments of this invention involve descriptions such as "first" or "second," these descriptions are for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, features defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. If the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by this invention. Example 1:

[0026] A heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive comprises the following components by weight percentage: 5-35% microsphere adhesive 100, 5-25% conductive carbon black, 10-35% conductive graphite, 1-10% graphene, 0.5-10% dispersant, 0.1-2% defoamer, 0.1-2% leveling agent, and 20-60% dispersion medium; wherein the microsphere adhesive 100 is a micron-sized spherical dispersion, such as... Figure 1 As shown, the microsphere adhesive 100 includes a polymer microsphere core 1 and a pressure-sensitive adhesive shell 2 covering the polymer microsphere core 1. The pressure-sensitive adhesive shell 2 is a pressure-sensitive adhesive layer containing isocyanate groups. The overall particle size D50 of the microsphere adhesive 100 is 4μm to 6μm. The large particle size at the micron level makes it difficult for the microsphere adhesive 100 to fill the tiny gaps between conductive fillers, thereby avoiding the disruption of the conductive network. The spherical structure allows the microsphere adhesive 100 to bond with the conductive filler through point contact, preventing it from spreading on the filler surface to form a continuous polymer film, thus avoiding the complete insulating coating of conductive particles by traditional long-chain or network-like macromolecules.

[0027] Furthermore, the polymer microsphere core 1 is a polystyrene core or a polymethyl methacrylate core; the pressure-sensitive adhesive layer is an acrylate copolymer containing isocyanate groups.

[0028] Furthermore, the conductive carbon black has a DBP oil absorption value of 50~500 and a particle size of 10~100nm.

[0029] Furthermore, the conductive graphite is one or more of the following: powder, flake, and fibrous forms.

[0030] Furthermore, the graphene is one or more of single-layer graphene, multilayer graphene, reduced graphene, and graphene oxide.

[0031] Furthermore, the dispersant is one or a mixture of two of polyurethane, polycarboxylate, and acrylic copolymer.

[0032] Furthermore, the defoamer is one of organosilicon, mineral oil, or polyether; the leveling agent is one of polyacrylic acid, fluorocarbon, or organosilicon-modified polyether; and the dispersion medium is one of ethyl acetate, butyl acetate, acetone, butanone, isopropyl ether, or sulfoxide.

[0033] like Figure 2 As shown, in this embodiment, the preparation method of the above-mentioned heat-pressable and moisture-curable electrothermal paste includes the following steps: S1. Synthesis of microsphere adhesive: First, prepare the polymer microsphere core 1, then coat its surface with a pressure-sensitive adhesive layer containing isocyanate groups to obtain core-shell structured microsphere adhesive 100. SEM image as shown. Figure 4 and Figure 5 As shown; specifically, step S1 includes the following steps: S1-1, Core Synthesis: Weigh 40g styrene, 0.6g azobisisobutyronitrile (AIBN), 3g polyvinylpyrrolidone (PVP-K30), and 80g ethanol, and add them to a reactor equipped with a stirrer, reflux condenser, and heating device. Stir until completely dissolved, purge with nitrogen for 30min to remove oxygen, raise the temperature to 70℃, and polymerize at this temperature for 8h. After the reaction, centrifuge, wash twice with ethanol, and vacuum dry at 60℃ for 12h to obtain the polystyrene core. The above-mentioned polystyrene core is the polymer microsphere core 1, and the above-mentioned styrene is the polymer monomer.

[0034] S1-2, Shell Synthesis: Prepare a monomer mixture by weighing 5.0g butyl acrylate, 2.0g vinyl acetate, 0.3g methyl methacrylate, 0.8g 2-isocyanoethyl acrylate, and 0.08g AIBN, and stirring until homogeneous. Take 25g of the above polystyrene core, add 50g ethyl acetate, and prepare a dispersion of approximately 33wt%. Transfer the dispersion to a reaction vessel and heat to 65℃. Add the entire monomer mixture dropwise at a rate of 5mL / min. After the addition is complete, maintain the temperature for 6 hours to form a pressure-sensitive adhesive layer containing isocyanate groups on the surface of the polymer microsphere core 1, serving as the pressure-sensitive adhesive shell 2, thus obtaining core-shell structured microsphere adhesive 100.

[0035] S2. Preparation of conductive slurry: Conductive carbon black, conductive graphite, graphene, dispersant, defoamer, leveling agent, and dispersion medium are mixed and dispersed at a speed of 1000~2000 r / min for 30~60 min to obtain a slurry mixture. The conductive carbon black, conductive graphite, and graphene together constitute the conductive filler. The slurry mixture is then ground using a three-roll mill, passing through the mill 1~2 times until the slurry fineness reaches below 15μm. The slurry is then filtered to obtain the conductive slurry. In this embodiment, step S2 specifically involves weighing 35g of conductive graphite, 5g of conductive carbon black, 2g of graphene, 0.6g of BYK-190 dispersant, 0.2g of BYK-024 defoamer, 0.2g of organosilicon-modified polyether leveling agent, and 42g of ethyl acetate, and adding them sequentially to the reactor. The mixture is stirred with a disc stirrer at 1500 r / min for 40 min. The slurry was then ground using a three-roll mill, with the roller spacing adjusted to the minimum. After passing through the mill twice, the fineness of the slurry was tested to be ≤15μm. The slurry was then filtered to obtain conductive slurry.

[0036] S3. Preparation of electrothermal paste: Mix the microsphere adhesive 100 obtained in step S1 with the conductive paste obtained in step S2, and stir at a speed of 100~500 r / min for 30~60 min. After stirring and mixing evenly, the heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive is obtained. Specifically, take 20g of the above-mentioned microsphere adhesive 100 particles and 80g of the above-mentioned conductive paste and add them to a mixing container. Use a paddle stirrer, adjust the speed to 300 r / min, and stir for 40 min until evenly mixed to obtain the heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive.

[0037] like Figure 3 As shown, this embodiment also provides a heating film made of a heat-pressable and moisture-curable electrothermal paste. The heating film is composed of an encapsulation film 200, a heating layer 300, and a substrate 400 stacked sequentially from top to bottom; wherein the heating layer 300 is prepared from the aforementioned heat-pressable and moisture-curable electrothermal paste. The preparation steps of this heating film are as follows: S1. Select PET film as substrate 400, apply hot-pressable-wet curable electrothermal paste to the surface of substrate 400, control the wet film thickness by using a doctor blade coating method, and dry it in an oven at 60-80℃ after coating to evaporate and remove the dispersion medium, forming a heating layer 300 with a dry film thickness of about 25μm on the surface of substrate 400. S2. Metal electrodes are arranged on the surface of the heating layer 300, and the electrodes are in reliable contact with the conductive area of ​​the heating layer 300. S3. Take a PET encapsulation film 200 and cover it on the heating layer 300 with electrodes, and encapsulate it using a hot pressing process; using the pressure-sensitive properties of the microsphere adhesive 100 in the heating layer 300, the encapsulation film 200, the heating layer 300, and the substrate 400 are tightly bonded together by hot pressing. S4. Place the hot-pressed film at 25°C and 65% relative humidity for 24 hours. The -NCO active groups on the outer shell of the microsphere adhesive 100 inside the heating layer 300 undergo a moisture-curing crosslinking reaction with the ambient moisture, achieving a secondary improvement in bonding strength, and finally obtaining a complete heating film product. The preparation steps are as follows: Figure 3 As shown. Comparative Example 1:

[0038] The method for preparing the electrothermal paste in this comparative example includes the following steps: S1. Synthesis of microspheres: Weigh 40g styrene, 0.6g azobisisobutyronitrile (AIBN), 3g PVP-K30, and 80g ethanol. Add the above raw materials to a reactor equipped with stirring, reflux condenser, and heating. Stir until completely dissolved, purge with nitrogen for 30min to remove oxygen, raise the temperature to 70℃, and polymerize at a constant temperature for 8h. After the reaction is complete, centrifuge, wash twice with ethanol, and vacuum dry at 60℃ for 12h to obtain polystyrene microspheres (solid content 35%).

[0039] S2. Preparation of conductive slurry: Weigh 35g conductive graphite, 5g conductive carbon black, 0.6g BYK-190 dispersant, 0.2g BYK-024 defoamer, and 30g deionized water, and add them sequentially to the reactor. Stir in a disc at 1500r / min and disperse for 40min. Grind in a three-roll mill with the roller gap adjusted to the minimum, pass through the mill twice, and achieve a fineness ≤15μm. Filter and discharge.

[0040] S3. Preparation of heat-pressable and moisture-curable electrothermal paste: Take 20g of the above polystyrene microspheres and 80g of the above conductive paste and add them to the mixing container. Use a paddle mixer at a speed of 300r / min and stir for 40min to mix evenly to obtain the final electrothermal paste. Comparative Example 2:

[0041] This comparative example demonstrates a method for preparing electrothermal paste. It includes the following steps: S1. Synthetic emulsion adhesive: 5.0g butyl acrylate, 2.0g vinyl acetate, 0.3g methyl methacrylate, 0.8g 2-isocyanoethyl acrylate, and 0.08g AIBN were stirred until homogeneous and set aside. 15g ethyl acetate was added to a reaction vessel and heated to 65℃. The entire monomer mixture was added dropwise at a rate of 5mL / min, with a total addition of 8.18g, which is approximately 10.9wt% of the dispersion. After the addition was complete, the reaction was maintained at this temperature for 6 hours, and the emulsion adhesive (35% solids content) was obtained.

[0042] S2. Preparation of conductive slurry: Weigh 35g conductive graphite, 5g conductive carbon black, 0.6g BYK-190 dispersant, 0.2g BYK-024 defoamer, and 30g deionized water, and add them sequentially to the reactor. Stir in a disc at 1500r / min and disperse for 40min. Grind in a three-roll mill with the roller gap adjusted to the minimum, pass through the mill twice, and achieve a fineness ≤15μm. Filter and discharge.

[0043] S3. Preparation of electrothermal paste: Take 20g of the above-prepared binder and 80g of the above-prepared conductive paste and add them to the mixing container. Use a paddle mixer at a speed of 300r / min and stir for 40min to mix evenly to obtain the final electrothermal paste. Comparative Example 3:

[0044] This comparative example demonstrates a method for preparing electrothermal paste. It includes the following steps: S1 Preparation of Conductive Slurry: Weigh 35g conductive graphite, 5g conductive carbon black, 0.6g BYK-190 dispersant, 0.2g BYK-024 defoamer, and 30g deionized water, and add them sequentially to the reactor. Stir in a disc at 1500r / min and disperse for 40min. Grind in a three-roll mill with the roller gap adjusted to the minimum, pass through the mill twice, and achieve a fineness ≤15μm. Filter and discharge.

[0045] S2 Preparation of electrothermal paste: Take 14g of emulsion adhesive (BASF 7031, solid content 50%) and 80g of the above conductive paste and add them to the mixing container. Use a paddle mixer at a speed of 300r / min and stir for 40min to mix evenly to obtain the final electrothermal paste. Comparative Example 4:

[0046] This comparative example demonstrates a method for preparing electrothermal paste. It includes the following steps: S1. Synthesizing microspheres, step 1 includes the following steps: Step S1-1: Weigh 40g styrene, 0.6g AIBN, 3g PVP-K30, and 80g ethanol. Add the above raw materials to a reactor equipped with stirring, reflux condenser, and heating. Stir until completely dissolved, purge with nitrogen for 30 minutes to remove oxygen, raise the temperature to 70℃, and polymerize at this temperature for 8 hours. After the reaction is complete, centrifuge, wash twice with ethanol, and vacuum dry at 60℃ for 12 hours to obtain the polystyrene microsphere core.

[0047] Step S1-2: Prepare the monomer mixture: 5.0g butyl acrylate, 2.0g vinyl acetate, 0.3g methyl methacrylate, 0.8g ethyl acrylate, and 0.08g AIBN, stir well and set aside. Take 25g of the above polystyrene microsphere core, add 50g ethyl acetate, prepare a 33wt% dispersion, transfer to a reaction vessel, stir and heat to 65℃. Add the entire monomer mixture dropwise at a rate of 5mL / min, with a total addition of 8.18g, approximately 10.9wt% of the dispersion mass. After the addition is complete, maintain the temperature for 6 hours to obtain a core-shell structured microsphere binder with a solid content of approximately 35%.

[0048] S2. Preparation of conductive slurry: Weigh 35g conductive graphite, 5g conductive carbon black, 0.6g BYK-190 dispersant, 0.2g BYK-024 defoamer, and 30g deionized water, and add them sequentially to the reactor. Stir in a disc at 1500r / min and disperse for 40min. Grind in a three-roll mill with the roller gap adjusted to the minimum, pass through the mill twice, and achieve a fineness ≤15μm. Filter and discharge.

[0049] S3. Preparation of electrothermal paste: Take 20g of the above microsphere adhesive, 100g of the above conductive paste, and add them to the mixing container. Use a paddle mixer at a speed of 300r / min and stir for 40min to mix evenly to obtain the final electrothermal paste. Comparative Example 5:

[0050] This comparative example demonstrates a method for preparing electrothermal paste. It includes the following steps: S1. Synthesizing microspheres, step 1 includes the following steps: Step S1-1: Weigh 20g styrene, 20g butyl acrylate, 0.6g AIBN, 3g PVP-K30, and 80g ethanol. Add the above raw materials to a reactor equipped with stirring, reflux condenser, and heating. Stir until completely dissolved, purge with nitrogen for 30 minutes to remove oxygen, raise the temperature to 70℃, and polymerize at this temperature for 8 hours. After the reaction is complete, centrifuge, wash twice with ethanol, and vacuum dry at 60℃ for 12 hours to obtain the non-spherical core of the styrene-butyl acrylate copolymer.

[0051] Step S1-2: Prepare the monomer mixture: Mix 5.0g butyl acrylate, 2.0g vinyl acetate, 0.3g methyl methacrylate, 0.8g 2-isocyanoethyl acrylate, and 0.08g AIBN until homogeneous. Take 25g of the non-spherical core of the above styrene-butyl acrylate copolymer, add 50g ethyl acetate, and prepare a 33wt% dispersion. Transfer the dispersion to a reactor and heat to 65℃. Add the entire monomer mixture dropwise at a rate of 5mL / min, with a total addition of 8.18g, which is approximately 10.9wt% of the dispersion mass. After the addition is complete, maintain the temperature for 6 hours to obtain a core-shell structured microspherical binder (solid content approximately 35%).

[0052] Step S2: Preparation of conductive slurry: Weigh 35g conductive graphite, 5g conductive carbon black, 0.6g BYK-190 dispersant, 0.2g BYK-024 defoamer, and 30g deionized water, and add them sequentially to the reactor. Stir in a disc at 1500r / min and disperse for 40min. Grind in a three-roll mill with the roller gap adjusted to the minimum, pass through the mill twice, and achieve a fineness ≤15μm. Filter and discharge.

[0053] Step S3: Prepare the electrothermal paste: Take 20g of the above microsphere adhesive, 100g of the above conductive paste, and add them to the mixing container. Use a paddle mixer at a speed of 300r / min and stir for 40min to mix evenly to obtain the final electrothermal paste.

[0054] The electrothermal pastes prepared in Example 1 and Comparative Examples 1-5 were coated into heating films with a thickness of 25 μm. The sheet resistance, adhesive strength after hot pressing, adhesive strength after moisture curing, and water resistance were tested. The test conditions were as follows: Sheet resistance was measured at a film thickness of 25 μm, in ohms per square meter; adhesive strength after hot pressing was measured at 80°C, 5 MPa, and a holding pressure of 10 s, with a peel strength measured at 180 degrees Celsius, in Newtons per centimeter; adhesive strength after moisture curing was measured after hot pressing and exposure to air for 24 hours, with a peel strength measured at 180 degrees Celsius, in Newtons per centimeter; water resistance was measured by immersing the heating film in room temperature water for 24 hours, observing its appearance, and testing the retention rate of adhesive strength, categorized as excellent, good, or poor.

[0055] The test results are shown in the table below:

[0056] The data in the table above shows that: Regarding conductivity, the sheet resistance of Examples 1, 1, and 4 was significantly lower than that of Examples 2, 3, and 5, indicating that the micron-sized spherical adhesive can avoid disrupting the conductive network and reduce contact resistance. In contrast, the comparative examples using pure emulsion adhesives or non-core-shell copolymer microspheres had higher sheet resistance, verifying the negative impact of traditional emulsion adhesives and non-core-shell structures on the conductive channels.

[0057] Regarding the hot-press bonding performance, Example 1 and Comparative Example 4 exhibit excellent bonding strength after hot pressing, indicating that the core-shell structure of the pressure-sensitive adhesive shell 2 can provide a good hot-press bonding effect; Comparative Example 1 has extremely low bonding strength due to the absence of the pressure-sensitive adhesive shell 2; the bonding strength of Comparative Examples 2, 3, and 5 is significantly lower than that of the present invention.

[0058] Regarding the enhanced performance of wet curing, the bond strength of Example 1 increased from 9 N / cm to 15 N / cm after wet curing, which is a significant increase. This is because the isocyanate groups in the shell undergo a cross-linking reaction when exposed to moisture, achieving secondary enhancement. The other comparative examples did not show this significant enhancement effect, which verifies that the isocyanate active groups are the core of wet curing enhancement.

[0059] Regarding water resistance, Example 1 exhibits excellent water resistance, thanks to the synergistic effect of the core-shell structure and the moisture-curing crosslinking system; Comparative Examples 1, 3, and 4 show poor water resistance, while Comparative Examples 2 and 5 are only good, all of which are inferior to the solution of this invention.

[0060] The above description is only a preferred embodiment of the present invention. Any technical solution that achieves the purpose of the present invention by essentially the same means is within the protection scope of the present invention.

Claims

1. A heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive, characterized in that: The microspheres comprise, by weight percentage: 5-35% microsphere adhesive 100, 5-25% conductive carbon black, 10-35% conductive graphite, 1-10% graphene, 0.5-10% dispersant, 0.1-2% defoamer, 0.1-2% leveling agent, and 20-60% dispersion medium. The microsphere adhesive 100 is a micron-sized spherical dispersion comprising a polymer microsphere core 1 and a pressure-sensitive adhesive shell 2 covering the polymer microsphere core 1. The pressure-sensitive adhesive shell 2 is a pressure-sensitive adhesive layer containing isocyanate groups. The overall particle size D50 of the microsphere adhesive 100 is 4 μm to 6 μm.

2. The heat-pressable-wet-curing electrothermal paste containing microsphere adhesive according to claim 1, characterized in that: The polymer microsphere core 1 is a polystyrene core or a polymethyl methacrylate core; and / or, the pressure-sensitive adhesive layer is an acrylate copolymer containing isocyanate groups.

3. The heat-pressable-wet-curing electrothermal paste containing microsphere adhesive according to claim 1, characterized in that: The conductive carbon black has a DBP oil absorption value of 50~500 and a particle size of 10~100nm.

4. The heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive according to claim 1, characterized in that: The conductive graphite is one or more of the following: powder, flake, and fibrous forms.

5. The heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive according to claim 1, characterized in that, The graphene is one or more of the following: single-layer graphene, multi-layer graphene, reduced graphene, and graphene oxide.

6. The heat-press-wet-curing electrothermal paste containing microsphere adhesive according to claim 1, characterized in that, The dispersant is one or a mixture of two of polyurethane, polycarboxylate, and acrylic copolymer.

7. The heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive according to claim 1, characterized in that, The defoamer is one of organosilicon, mineral oil, or polyether; the leveling agent is one of polyacrylic acid, fluorocarbon, or organosilicon-modified polyether; and the dispersion medium is one of ethyl acetate, butyl acetate, acetone, butanone, isopropyl ether, or thionyl chloride.

8. A method for preparing a heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive as described in any one of claims 1 to 7, characterized in that, Includes the following steps: S1. Synthesis of microsphere adhesive: First, prepare the core 1 of polymer microspheres, and then coat the surface of the core with a pressure-sensitive adhesive layer containing isocyanate groups to obtain core-shell structured microsphere adhesive 100. S2. Preparation of conductive slurry: Conductive carbon black, conductive graphite, graphene, dispersant, defoamer, leveling agent, and dispersion medium are mixed, stirred, and dispersed, and then ground to a fineness ≤15μm to obtain conductive slurry; S3. Preparation of electrothermal paste: Mix microsphere adhesive 100 with conductive paste evenly to obtain a heat-pressed and moisture-curable electrothermal paste.

9. The method for preparing the heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive according to claim 8, characterized in that, Step S1 specifically includes: S1-1, Core Synthesis: By mass percentage, 20-50 wt% of polymeric monomer, 0.1-3 wt% of initiator AIBN, 1-10 wt% of stabilizer PVP, and 40-80 wt% of ethanol solvent are added to the reactor. After deoxygenation by purging with nitrogen, polymerization is carried out at 60-80℃ for 6-12 h. After centrifugation, washing, and drying, polymer microsphere core 1 is obtained. S1-2, Shell Synthesis: Prepare a monomer mixture by mass: 3-8 parts butyl acrylate, 1-3 parts vinyl acetate, 0.1-1 parts methyl methacrylate, 0.5-1 parts ethyl 2-isocyanate, and 0.01-0.3 parts initiator AIBN; prepare a 30-50 wt% ethyl acetate dispersion for the polymer microsphere core 1, heat to 50-75℃, and add the monomer mixture dropwise at 5 mL / min, with the amount added being 10-40 wt% of the dispersion mass. After the addition is complete, continue the reaction for 4-8 hours, and discharge to obtain microsphere gel 100.

10. The method for preparing the heat-pressable and moisture-curable electrothermal paste containing microsphere adhesive according to claim 8, characterized in that, In step S2, the stirring speed is 1000~2000 r / min, the dispersion time is 30~60 min, and the slurry is ground 1~2 times with a three-roll mill until the fineness of the slurry reaches below 15 μm; And / or, in step S3, a paddle mixer is used with a speed of 100~500 r / min and a mixing time of 30~60 min.