High-frequency high-speed pcb substrate, method for manufacturing the same, and application thereof

By coating a mixed resin solution onto an LCP insulating substrate and performing chemical electroplating to form a metallic copper layer, the problems of poor adhesion and insufficient dielectric properties of high-frequency PCBs for AI servers are solved, achieving high-frequency and high-speed signal transmission and thermal stability, making it suitable for high-frequency and high-speed communication equipment for AI servers.

CN123075813APending Publication Date: 2026-11-10JIANGMEN DEZHONGTAI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611342645.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing high-frequency PCBs for AI servers suffer from high raw material costs, complex processes, poor thermal stability, unadjustable dielectric properties, and poor adhesion between copper foil and LCP, making it difficult to meet the requirements of high-frequency and high-speed signal transmission.

Method used

A modified coating is formed by coating a mixed resin solution onto the surface of an LCP insulating substrate and then performing chemical electroplating. A metallic copper layer is then grown directly on the modified coating, replacing the traditional hot-pressing bonding of copper foil. This is combined with plasma treatment to strengthen the interfacial bonding.

Benefits of technology

It achieves a high-frequency, high-speed PCB substrate with high bonding strength, low dielectric loss, and excellent thermal stability, which is suitable for AI servers, meets the needs of high-frequency and high-speed signal transmission, and has a simple and controllable process, making it easy to mass-produce.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application provides a high-frequency high-speed PCB substrate and a preparation method and application thereof, and belongs to the technical field of printed circuit board preparation. The preparation method comprises the following steps: S1, coating a mixed resin solution on a liquid crystal polymer insulating base material, and drying to obtain a base material containing an LCP coating layer; and S2, performing chemical electroplating on the base material containing the LCP coating layer to obtain a base material containing a metal layer. The high-frequency high-speed PCB substrate obtained by the application is mainly used in the preparation of AI servers. The preparation method provided by the application is characterized in that a mixed resin solution containing a high-melting-point LCP resin is coated on the surface of an LCP insulating base material, and a modified coating layer is formed by drying, so that the processability of the surface of the base material is improved; then, a specific chemical electroplating process is adopted to grow a copper layer directly on the modified coating layer, so that the traditional copper foil hot-pressing lamination is replaced, and finally, a high-frequency high-speed PCB substrate with high bonding force, low dielectric loss and excellent thermal stability is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of printed circuit board manufacturing technology, and particularly relates to a high-frequency, high-speed PCB substrate, its manufacturing method, and its application. Background Technology

[0002] With the rapid development of information and communication technologies, the performance requirements for printed circuit boards (PCBs) are constantly increasing. Especially in the field of AI servers, the demand for high-frequency, high-speed signal transmission and large-capacity data processing is growing, placing higher demands on the dielectric properties, heat dissipation performance, and structural stability of copper-clad laminates.

[0003] Current high-frequency PCBs for AI servers mostly use a combination of hydrocarbon resin (PCH) / polytetrafluoroethylene (PTFE) resin, Hyper Very Low Profile-5 (HVLP5) copper foil, and quartz fiber cloth. This approach suffers from high raw material costs and complex processes. PTFE requires adhesive to bond the copper foil, has poor thermal stability, and is subject to EU environmental regulations on per- and polyfluoroalkyl substances (PFAS). Furthermore, it has poor thermal conductivity and unadjustable dielectric properties. There is an urgent need to develop a copper clad laminate preparation method with excellent overall performance and simple, low-cost processes.

[0004] In recent years, liquid crystal polymers (LCPs) have been widely used in the field of high-frequency copper-clad laminates due to their excellent dielectric properties. However, conventional LCP-based copper-clad laminates still have some problems, such as poor adhesion between the copper foil and LCP, easy peeling or blistering, which affects the application quality of PCBs. In addition, the dielectric constant and dielectric loss of existing LCP-based copper-clad laminate materials still cannot meet the higher-level technical requirements under high-frequency and high-speed transmission conditions.

[0005] To address these issues, researchers have been exploring new copper-clad laminate (CCL) structures and fabrication methods. Currently, multi-layer lamination is a widely discussed approach for CCL fabrication. This method uses a soluble fluoropolymer film as an adhesive layer, sequentially stacking other cut-to-sheet materials and subjecting them to prolonged static pressing in a high-temperature press to ultimately form a complete laminated CCL. While this approach attempts to improve interfacial bonding and dielectric performance, it suffers from drawbacks such as cumbersome production processes, long production cycles, high manufacturing costs, and suboptimal overall performance of the resulting CCLs, making large-scale production difficult.

[0006] Therefore, developing a novel copper clad laminate preparation method that can simultaneously take into account dielectric properties, heat dissipation performance, roughness, structural stability, environmental friendliness, and simple and low-cost production process has become the current research focus and challenge. Summary of the Invention

[0007] In view of the problems of existing PTFE high-frequency copper clad laminates, such as environmental control, high cost, the need for adhesives affecting thermal stability, and poor interface adhesion after copper foil lamination of traditional LCP copper clad laminates, this invention provides a method for manufacturing AI servers and high-frequency high-speed PCB substrates.

[0008] This invention proposes a method for preparing a high-frequency, high-speed PCB substrate, comprising the following steps:

[0009] S1. After coating the mixed resin solution onto the liquid crystal polymer insulating substrate, dry it to obtain a substrate containing an LCP coating. S2. The above-mentioned substrate containing LCP coating is subjected to chemical electroplating to obtain a substrate containing a metal layer.

[0010] Further, in S1, the mixed resin solution is prepared from raw materials comprising the following parts by weight: 1-30 parts of high heat-resistant thermoplastic resin, 0-20 parts of functional filler, 0-10 parts of dispersant, 0-10 parts of emulsifier, and 50-95 parts of solvent; and / or, In S1, the high heat-resistant thermoplastic resin is selected from liquid crystal polymer resin or phenolphthalein-based polyaryletherketone resin.

[0011] Further, in S1, the liquid crystal polymer resin is a fully aromatic polyester; preferably, the melting point of the liquid crystal polymer resin is greater than 260°C; and / or, In S1, the glass transition temperature of the phenolphthalein-based polyaryletherketone resin is not lower than 220℃; and / or, In S1, the liquid crystal polymer insulating substrate is selected from liquid crystal polymer fiber cloth or liquid crystal polymer film; and / or, In S1, the functional filler is selected from at least one of hollow glass microspheres, polytetrafluoroethylene, diamond, boron nitride, and aluminum nitride; and / or, In S1, the D50 particle size of the functional filler is 0.01–15 μm; and / or, In S1, the solvent is selected from at least one of N-methylpyrrolidone and N,N-dimethylformamide.

[0012] Further, in S1, the coating is a single-sided or double-sided coating of the liquid crystal polymer insulating substrate; and / or, In S1, the thickness of the coating obtained after coating reaches 1–50 μm on one side; and / or, In S1, the drying temperature is 60-80°C; the drying time is 30-60 minutes.

[0013] Further, in S2, the chemical electroplating specifically includes: performing a chemical wet pretreatment on the substrate containing the LCP coating, followed by electrolytic electroplating. Preferably, the chemical electroplating specifically includes: subjecting the substrate containing the LCP coating to roughening treatment, reduction treatment, activation treatment, and desizing treatment in sequence; then using the substrate after desizing treatment as the cathode and copper foil as the anode, electrochemically depositing a metal layer using an electroplating solution containing metal salts until the metal layer reaches the target thickness.

[0014] Further, in S2, the chemical electroplating is performed on one or both sides of the substrate containing the LCP coating; and / or, In S2, the thickness of the metal layer on one side is 0.5–200 μm; and / or, In S2, the metal in the electroplating solution containing the metal salt is selected from at least one of gold, silver, copper, chromium, or nickel; and / or, Preferably, in S2, the electroplating solution containing metal salts is an electroplating solution containing copper salts; the copper salt-containing electroplating solution comprises 150-250 g / L copper sulfate, 30-40 g / L sulfuric acid, and 80-120 mL / L hydrochloric acid; and / or, In S2, the electrochemical deposition temperature is 20~30℃ and the electrochemical deposition time is 40~50min.

[0015] Further, in S2, the roughening treatment includes: immersing the LCP-coated substrate in a high-chromic acid roughening solution for etching, thereby forming micropits with an average diameter of 0.01~0.5μm on the substrate surface; and / or, In S2, the reduction treatment includes: treating the roughened substrate with an aqueous solution of sodium borohydride; preferably, the concentration of the sodium borohydride aqueous solution is 0.5~2 g / L; and / or, In S2, the activation process includes: activating the substrate after reduction rinsing using a Pd-Sn activation solution; Preferably, the Pd-Sn activation solution contains 250 mL / L hydrochloric acid, 5 g / L stannous chloride, and 15 ppm colloidal palladium; more preferably, the activation temperature is 30-40°C, and the activation time is 1-10 min; and / or, In S2, the descaling process includes: descaling the activated substrate using a descaling solution; preferably, the descaling solution is a hydrochloric acid solution of 50~100g / L; more preferably, the descaling temperature is 30~40℃ and the descaling time is 5~10min.

[0016] Furthermore, it also includes S3, performing surface treatment on the substrate containing the metal layer to obtain the finished product.

[0017] The surface treatment includes polishing the metal coating, plasma treatment, and finally interface bonding treatment. Preferably, the interface bonding treatment specifically involves depositing a titanium dioxide intermediate layer on the surface of the metal layer using a plasma-enhanced chemical vapor deposition process.

[0018] This invention also proposes a high-frequency, high-speed PCB substrate prepared by any of the above-described preparation methods.

[0019] This invention also proposes the application of any of the above-described high-frequency, high-speed PCB substrates in AI servers.

[0020] This invention has the following advantages: The method for preparing a high-frequency, high-speed PCB substrate proposed in this invention involves first coating a mixed resin solution containing high-melting-point LCP resin onto the surface of an LCP insulating substrate, drying it to form a modified coating, and improving the surface processability of the substrate; then, using a specific chemical electroplating process (roughening-reduction-activation-descending-electrochemical copper plating), a metallic copper layer is directly grown on the modified coating, replacing the traditional hot-press bonding of copper foil, ultimately obtaining a high-frequency, high-speed PCB substrate with high adhesion, low dielectric loss, and excellent thermal stability.

[0021] In the above preparation method, a metal layer with a thickness of 0.5–200 μm is formed by coating a mixed resin solution onto an LCP insulating substrate and then performing chemical electroplating. This effectively reduces the risk of solder joint cracking during PCB engraving and improves the structural stability and reliability of the PCB. Furthermore, the good compatibility between the mixed resin solution (containing LCP resin) and the LCP insulating substrate enhances the bonding force between the metal layer and the resin layer, effectively solving the problem of peeling or blistering that commonly occurs in traditional LCP-based copper-clad laminates, ensuring the long-term stability of the PCB. In addition, the use of thermoplastic resin and the addition of functional fillers (such as hollow glass microspheres) in the mixed resin solution allows for precise control of the PCB's dielectric properties, linear thermal expansion coefficient, or thermal conductivity, meeting the needs of high-frequency, high-speed signal transmission in the AI ​​server field. In summary, this preparation method is simple and controllable, easy to scale up for mass production, and the prepared PCB exhibits excellent comprehensive performance, meeting the application requirements under harsh environments such as cross-cut adhesion testing and high / low temperature conditions. Detailed Implementation

[0022] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Unless otherwise specified, the embodiments and features in the embodiments of the present invention can be combined with each other.

[0023] On one hand, embodiments of the present invention propose a method for preparing a high-frequency, high-speed PCB substrate, comprising the following steps: S1. After coating the mixed resin solution onto the liquid crystal polymer (LCP) insulating substrate, dry it to obtain a substrate containing an LCP coating. S2. The above-mentioned substrate containing LCP coating is subjected to chemical electroplating to obtain a substrate containing a metal layer.

[0024] The method for preparing a high-frequency, high-speed PCB substrate proposed in this invention involves first coating the surface of an LCP insulating substrate with a mixed resin solution containing high-melting-point LCP resin or PEKC resin, and then drying it to form a modified coating, thereby improving the surface processability of the substrate. Next, a specific chemical electroplating process (roughening-reduction-activation-descending-electrochemical copper plating) is used to directly grow a metal layer on the modified coating, replacing the traditional hot-press bonding of copper foil. The result is a high-frequency, high-speed PCB substrate with high adhesion, low dielectric loss, and excellent thermal stability, suitable for AI servers and other high-frequency, high-speed communication equipment.

[0025] In embodiment S1 of this invention, the LCP insulating substrate itself has high chemical inertness, making it difficult to achieve a strong adhesion of the metal layer through direct electroplating. This invention addresses the fundamental compatibility issue by modifying the LCP substrate surface through coating with a mixed resin solution (LCP or PEKC). When both the coating matrix and the substrate are LCP, their compatibility is better, and the coating bonds firmly to the substrate. By adjusting the type, particle size, and amount of functional fillers, the overall dielectric constant Dk, dielectric loss Df, coefficient of thermal expansion, and thermal conductivity of the board can be flexibly controlled. Furthermore, the coating provides a moderately roughable surface, providing an interface foundation for subsequent electroplating without excessively damaging the bulk LCP substrate, thus ensuring the overall high-frequency performance of the board remains intact.

[0026] In one embodiment of the present invention, in S1, the mixed resin solution is prepared from raw materials comprising the following parts by weight: 1-30 parts of high heat-resistant thermoplastic resin, 0-20 parts of functional filler, 0-10 parts of dispersant, 0-10 parts of emulsifier, and 50-95 parts of solvent.

[0027] In one embodiment of the present invention, in S1, the high heat-resistant thermoplastic resin is selected from liquid crystal polymer (LCP) resin or phenolphthalein polyarylether-Ketone (PEKC) resin.

[0028] In a preferred embodiment of the present invention, in S1, the high heat-resistant thermoplastic resin is selected from liquid crystal polymer resin. In this embodiment of the present invention, when the coating substrate and the base material are both LCP, their compatibility is better, and the coating and the base material are firmly bonded.

[0029] Specifically, in S1, the liquid crystal polymer resin (LCP resin) is a fully aromatic polyester; the melting point of the liquid crystal polymer resin is greater than 260℃; specifically, the melting point of the liquid crystal polymer resin is greater than 280℃. This is mainly to meet the requirements of subsequent applications for the PCB substrate. The molecular weight of the liquid crystal polymer resin is greater than 10,000.

[0030] Specifically, the glass transition temperature of phenolphthalein-based polyaryletherketone resin (PEKC resin) is not lower than 220°C. In this embodiment of the invention, PEKC resin is an amorphous polyaryletherketone, has no melting point, and does not possess liquid crystal properties.

[0031] In one embodiment of the present invention, in S1, the liquid crystal polymer insulating substrate is selected from liquid crystal polymer (LCP) fiber cloth or liquid crystal polymer (LCP) film. It should be noted that LCP is a liquid crystal polymer.

[0032] In one embodiment of the present invention, in S1, the functional filler is selected from at least one of hollow glass microspheres, polytetrafluoroethylene, diamond, boron nitride, and aluminum nitride.

[0033] Preferably, in S1, the D50 particle size of the functional filler is 0.01 to 15 μm.

[0034] In one embodiment of the present invention, in S1, the solvent is selected from at least one of N-methylpyrrolidone (NMP) and N,N-dimethylformamide (DMF).

[0035] In one embodiment of the present invention, in S1, the method for preparing the mixed resin solution includes: dissolving the liquid crystal polymer resin in a solvent, adding a functional filler, adding a dispersant and an emulsifier, and mixing to obtain a mixed resin solution.

[0036] In one embodiment of the present invention, in S1, the coating is a single-sided or double-sided coating of the liquid crystal polymer insulating substrate. Preferably, the coating is a double-sided coating of the liquid crystal polymer insulating substrate.

[0037] In one embodiment of the present invention, in S1, the thickness of the coating obtained after coating reaches 1 to 50 μm on one side.

[0038] In one embodiment of the present invention, in S1, the drying temperature is 60-80°C; and the drying time is 30-60 minutes.

[0039] In embodiment S2 of the present invention, the substrate containing LCP coating is chemically electroplated, abandoning the traditional process of hot-pressing copper foil bonding, and copper layer growth is directly achieved on the surface of modified LCP coating, avoiding the problems of adhesive layer and high cost metal foil dependence caused by the pressing process.

[0040] In one embodiment of the present invention, in S2, the chemical electroplating specifically includes performing a chemical wet pretreatment on the substrate containing the LCP coating, followed by electrolytic electroplating.

[0041] In one embodiment of the present invention, S2 specifically includes: subjecting the substrate containing the LCP coating to roughening treatment, reduction treatment, activation treatment, and desizing treatment in sequence; then using the substrate after desizing treatment as the cathode and copper foil as the anode, electrochemically depositing a metal layer using an electroplating solution containing metal salts until the metal layer reaches the target thickness.

[0042] In one embodiment of the present invention, in S2, the chemical electroplating is to perform chemical electroplating on one or both sides of the substrate containing the LCP coating.

[0043] In one embodiment of the present invention, in S2, the thickness of the metal layer on one side is 0.5 to 200 μm.

[0044] In one embodiment of the present invention, in S2, the metal in the electroplating solution containing the metal salt is selected from at least one of gold, silver, copper, chromium or nickel.

[0045] Preferably, in S2, the electroplating solution containing metal salt is an electroplating solution containing copper salt; the electroplating solution containing copper salt contains 150~250g / L copper sulfate, 30~40g / L sulfuric acid, and 80~120mL / L hydrochloric acid.

[0046] In one embodiment of the present invention, in step S2, the electrochemical deposition temperature is 20~30°C, and the electrochemical deposition time is 40~50 min. Specifically, in step S2, the electrochemical deposition temperature is 25°C, and the electrochemical deposition time is 45 min.

[0047] Specifically, in S2, the metal layer is electrochemically deposited and then rinsed with water.

[0048] In one embodiment of the present invention, in S2, the roughening process includes: immersing the substrate containing the LCP coating in a high-chromic acid type roughening solution for etching, so that micropits with an average diameter of 0.01~0.5μm are formed on the surface of the substrate.

[0049] In one embodiment of the present invention, specifically in S2, micropits with an average diameter of 0.12 μm are formed on the surface of the substrate.

[0050] Specifically, in S2, the high-chromic acid type roughening solution contains 400 g / L chromic anhydride and 400 g / L sulfuric acid.

[0051] Specifically, in S2, the roughening treatment temperature is 65℃ and the roughening treatment time is 5min.

[0052] Specifically, in S2, after roughening is completed, rinse with clean water.

[0053] In one embodiment of the present invention, in S2, the reduction process includes treating the roughened substrate with an aqueous solution of sodium borohydride.

[0054] In one embodiment of the present invention, in step S2, the concentration of the sodium borohydride aqueous solution is 0.5~2 g / L. Specifically, in step S2, the concentration of the sodium borohydride aqueous solution is 1 g / L.

[0055] Specifically, in S2, the reduction treatment temperature is room temperature (10~30).

[0056] Specifically, in S2, the reduction process takes 10 minutes.

[0057] Specifically, in S2, rinse with clean water after the reduction is complete.

[0058] In one embodiment of the present invention, in S2, the final substrate containing the metal layer is either a single side of the substrate with a copper metal layer or both sides of the substrate with a copper metal layer.

[0059] In one embodiment of the present invention, S2, the activation process includes: activating the substrate after reduction rinsing using a Pd-Sn activation solution.

[0060] Specifically, in S2, the Pd-Sn activation solution contains 250 mL / L hydrochloric acid, 5 g / L stannous chloride, and 15 ppm colloidal palladium.

[0061] In one embodiment of the present invention, in step S2, the activation temperature is 30~40℃ and the activation time is 1~10min. Specifically, in step S2, the activation temperature is 35℃ and the activation time is 4min.

[0062] Specifically, in S2, after activation, rinse with clean water.

[0063] In one embodiment of the present invention, S2, the debonding process includes: debonding the activated substrate using a debonding solution.

[0064] In one embodiment of the present invention, in step S2, the descaling solution is a hydrochloric acid solution with a concentration of 50-100 g / L. Specifically, in step S2, the descaling solution is a hydrochloric acid solution with a concentration of 80 g / L.

[0065] In one embodiment of the present invention, in step S2, the depolymerization temperature is 30~40℃, and the depolymerization time is 5~10 min. Specifically, in step S2, the depolymerization temperature is 35℃, and the depolymerization time is 8 min.

[0066] Specifically, in S2, rinse with water after degumming is complete.

[0067] In one embodiment of the present invention, S2 further includes post-processing, which specifically involves: passivating the product obtained by chemical electroplating, washing with water, drying, and drying at 60°C for 30 minutes.

[0068] Specifically, in S2, the passivation treatment temperature is room temperature (10~30℃).

[0069] Specifically, in S2, the passivation solution used for the passivation treatment is an aqueous solution containing 3 g / L benzotriazole.

[0070] Specifically, in S2, the passivation treatment time is 20 minutes.

[0071] In one embodiment of the present invention, a combination of vacuum plating and chemical electroplating can be used. Specifically, a 50nm thick metal layer is first deposited using a vacuum plating process, followed by chemical electroplating to deposit a metal layer of the target thickness. Because vacuum plating has a slow deposition rate and high cost, it is not suitable for directly preparing micron-thick copper layers. Generally, it is only used as a seed layer, which is then thickened using the chemical electroplating method proposed in this application to obtain the metal layer of the target thickness.

[0072] In one embodiment of the present invention, the method for preparing the high-frequency, high-speed PCB substrate further includes the following step: S3, performing surface treatment on the substrate containing the metal layer to obtain the finished product. In this embodiment of the present invention, the outer surface of the metal layer is polished and plasma activated in sequence, and then a titanium dioxide intermediate layer is deposited on the surface of the metal layer using plasma-enhanced chemical vapor deposition (PECVD). The above treatment strengthens the interfacial bonding reliability between the coating and the resin system.

[0073] In one embodiment of the present invention, in S3, the surface treatment includes first polishing the metal coating, then performing plasma treatment, and finally performing interface bonding treatment.

[0074] In one embodiment of the present invention, in step S3, a polishing process is performed to make the surface roughness Ra less than 0.5 μm.

[0075] In one embodiment of the present invention, during plasma treatment in step S3, the gas composition is hydrogen, tetrafluoromethane, and oxygen in a volume ratio of 2:1:1, the gas flow rate is 50 mL / min, the power is 300 W, and the absolute vacuum degree is 0.5 × 10⁻⁶. -6 Pa, temperature 120℃, time 10 minutes.

[0076] In one embodiment of the present invention, in step S3, the interface bonding treatment specifically involves depositing a titanium dioxide intermediate layer on the surface of the metal layer using plasma-enhanced chemical vapor deposition (PECVD). In this embodiment, the interface bonding treatment improves the adhesion between the metal layer and the resin layer.

[0077] Preferably, in S3, the temperature of the plasma-enhanced chemical vapor deposition process is 400~450℃.

[0078] Preferably, in S3, the thickness of the titanium dioxide intermediate layer is 10 nm.

[0079] In another aspect, embodiments of the present invention also provide high-frequency, high-speed PCB substrates prepared by any of the above-mentioned preparation methods.

[0080] Furthermore, this invention also proposes the application of any of the aforementioned high-frequency, high-speed PCB substrates in AI servers. AI servers have much higher requirements for copper foil adhesion than ordinary consumer-grade and industrial-grade PCBs. The core challenge is ensuring that the copper foil and substrate do not delaminate or peel under the harsh conditions of high frequency, high speed, high thermal conductivity, and long-term thermal cycling, thus maintaining signal transmission and structural reliability. The high-frequency, high-speed PCB substrate prepared by this invention, using an LCP substrate combined with a modified resin coating and electroplating metallization process, possesses both low dielectric constant and dielectric loss, ensuring complete transmission of high-frequency signals; high coating adhesion, and a linear thermal expansion coefficient that better matches the copper foil, effectively reducing thermal stress and suppressing board warping; a high glass transition temperature, resulting in excellent high-temperature dimensional stability; and the ability to control thermal conductivity through filler compounding, making it suitable for the demanding 24 / 7 high-power continuous load requirements of AI servers.

[0081] The present invention will now be described in detail with reference to the embodiments.

[0082] Test Example 1 Test methods for PCB substrates Peel strength: Tested according to ASTM B533-85(2024), measuring the peel strength of the copper foil layer at 90°. Record the data for both sides of a double-sided panel, or the smaller peel strength value for a single-sided panel.

[0083] Glass transition temperature Tg: Tested according to ISO 6721-11:2019.

[0084] Dielectric constant Dk and dielectric loss Df: The separated dielectric resonator method (SPDR) was used. In this embodiment of the invention, the instrument used was an Agilent N5230A, and the measurement frequency was 10 GHz. The dielectric properties of the bare plate before electroplating were tested.

[0085] Surface roughness: Surface roughness is tested using the stylus method according to GB / T1031-2009 standard.

[0086] Linear thermal expansion coefficient: Tested according to ISO 11359-2, with a test temperature of -40℃ to 150℃.

[0087] Thermal conductivity: Tested in accordance with IEC 63609-2.

[0088] Example 1 A method for fabricating an AI server PCB substrate includes the following steps: 1. A mixed resin solution is coated on both sides of an LCP fiber cloth (the LCP fiber cloth is obtained by spinning, post-treatment and weaving LCP resin, and the thickness of the cloth is 20μm) and the solvent is dried (drying at 70℃ for 45 minutes) to obtain a substrate containing an LCP coating. The mixed resin solution contains 10% LCP resin and 90% NMP; it is obtained by dissolving LCP resin in N-methylpyrrolidone (NMP).

[0089] It should be noted that the LCP resins used in this invention are all fully aromatic polyesters, model L1000 resin, purchased from Jiangmen Dezhongtai Engineering Plastics Technology Co., Ltd., with a melting point of 335℃.

[0090] 2. A substrate containing an LCP coating is subjected to chemical electroplating to obtain a substrate containing a copper layer; specifically including: (1) Coarsening The dried substrate was placed in a roughening tank and continuously immersed in an etching solution to form micropits with an average diameter of 0.12 μm (using the optical surface roughness test method). The etching solution in the roughening tank was a high-chromic acid type roughening solution containing 400 g / L chromic anhydride and 400 g / L sulfuric acid, and was treated at 65°C for 5 min.

[0091] (2) Reduction process The roughened substrate was placed in a reduction bath for reduction treatment, and then rinsed with clean water in a cleaning bath. The reduction solution was a 1 g / L sodium borohydride aqueous solution, and the process was carried out at room temperature for 10 minutes.

[0092] (3) Activation treatment The obtained product was placed in an activation tank for activation treatment, and then rinsed with clean water in a cleaning tank. The activation solution in the activation tank was a Pd-Sn activation solution, specifically containing 250 mL / L hydrochloric acid, 5 g / L stannous chloride, and 15 ppm colloidal palladium. The temperature was 35℃, and the activation time was 4 min. The colloidal palladium was a commercially available product, and commercially available products can achieve comparable technical effects.

[0093] (4) Degumming treatment The obtained product was sent to a degumming tank for degumming treatment, and then rinsed with clean water in a washing tank. The degumming solution in the degumming tank was 80 g / L hydrochloric acid, the temperature was 35℃, and the time was 8 min.

[0094] (5) Chemical deposition Electrochemical deposition of copper layers on both sides of the treated product was performed until the thickness of the copper layer on each side reached 1 μm. The electroplating process used the desizing product as the cathode and the copper foil as the anode. The electroplating solution contained 200 g / L copper sulfate, 35 g / L sulfuric acid, and 100 mL / L hydrochloric acid. The plating time was 45 min at 25°C. After electroplating, the composite shielding film was rinsed in a water washing tank.

[0095] (6) Post-processing The chemically deposited product was passivated in a passivation tank, then washed with water in a water washing tank, and finally dried in a dryer at 60°C for 30 min. The passivation temperature was room temperature, the passivation solution was an aqueous solution containing 3 g / L benzotriazole, and the passivation time was 20 min.

[0096] The obtained product was tested according to Test Example 1, and the results are shown in Table 1.

[0097] Example 2 A method for fabricating an AI server PCB substrate includes the following steps: Same as Example 1, except that, In step 1, the substrate was replaced with a 25μm LCP film instead of a 20μm LCP fiber cloth; the mixed resin solution was supplemented with functional filler hollow glass microspheres, specifically, the LCP resin content was 10%, the NMP content was 85%, and the hollow glass microspheres (model HS70, manufactured by Zhengzhou Shenglait, D50 particle size 10μm, true density 0.75g / cm³) were added. 3 The content of ) is 5%; after coating, the coating thickness is adjusted from 1μm for each surface to 15μm for each surface.

[0098] In step 2, the thickness of each side of the double-sided copper layer obtained by electroplating reaches 1 μm.

[0099] In step 3, the substrate containing the copper layer obtained in step 2 is subjected to surface treatment to obtain the finished product.

[0100] The surface treatment includes first polishing the metal coating (to achieve a surface roughness Ra of less than 0.5 μm), followed by plasma treatment (the gas composition is hydrogen, tetrafluoromethane, and oxygen in a volume ratio of 2:1:1, the gas flow rate is 50 mL / min, the power is 300 W, and the absolute vacuum degree is 0.5 × 10⁻⁶). -6 Pa, temperature 120℃, time 10 minutes), and finally interface bonding treatment (depositing a titanium dioxide intermediate layer on the copper layer surface using plasma enhanced chemical vapor deposition (PECVD) at 400~450℃, with a titanium dioxide intermediate layer thickness of 10nm).

[0101] In this embodiment of the invention, the bonding force between the metal layer and the resin layer is improved through interface bonding treatment.

[0102] The obtained product was tested according to Test Example 1, and the results are shown in Table 1.

[0103] Example 3 A method for fabricating an AI server PCB substrate includes the following steps: Similar to Example 1, except that in step 1, the substrate was replaced with a 25μm LCP film instead of a 20μm LCP fiber cloth; PEKC resin (manufacturer: Heilongjiang Yingchuang New Materials Co., Ltd.) and silica filler were added to the mixed resin solution, specifically, the content of LCP resin was 10%, the content of PEKC resin was 10%, the content of NMP was 70%, and the content of silica (D50 particle size 100nm) was 10%; the coating thickness after coating was adjusted from 1μm on each side to 0.5μm on each side. In step 2, the thickness of the double-sided copper layer obtained by electroplating was adjusted from 1 μm to 0.5 μm.

[0104] The obtained product was tested according to Test Example 1, and the results are shown in Table 1.

[0105] Example 4 A method for fabricating an AI server PCB substrate includes the following steps: Similar to Example 1, except that in step 1, two inorganic fillers, diamond and silica, are added to the mixed resin solution. Specifically, the content of LCP resin is 5%, the content of NMP is 85%, the content of diamond (D50 particle size 200nm) is 5%, and the content of silica (D50 particle size 50nm) is 5%. The drying conditions are adjusted from 70℃, 45min to 80℃, 90min. The coating thickness after coating is adjusted from 1μm on each side to 1.5μm on each side.

[0106] In step 2, the thickness of each side of the double-sided copper layer obtained by electroplating reaches 1 μm.

[0107] The obtained product was tested according to Test Example 1, and the results are shown in Table 1.

[0108] Comparative Example 1 Same as Example 4, except that the LCP fiber cloth is replaced with glass fiber cloth.

[0109] The obtained product was tested according to Test Example 1, and the results are shown in Table 1.

[0110] Comparative Example 2 Similar to Example 4, step 2 is entirely replaced by laminating with HVLP-5 copper foil with a thickness of 9μm.

[0111] The obtained product was tested according to Test Example 1, and the results are shown in Table 1.

[0112] Comparative Example 3 The commercially available M9 PCB board, model MEGTRON9, is manufactured by Panasonic Electric Works and is produced using a combination process of hydrocarbon resin, quartz fiber cloth, and HVLP5 ultra-low profile copper foil.

[0113] The obtained product was tested according to Test Example 1, and the results are shown in Table 1.

[0114] Comparative Example 4 Same as Example 4, except that no LCP resin was added to the mixed resin solution.

[0115] Table 1

[0116] Based on the test data from Embodiments 1-4 and Comparative Examples 1-4 of the present invention, it can be concluded that... In Examples 1-3, the AI ​​server PCB substrates prepared by using LCP fiber cloth or LCP film as a substrate, combined with modified resin coating and electroplating metallization process, can achieve an overall coating adhesion of 9-12 N / cm, which is significantly better than ordinary glass fiber substrate, HVLP-5 copper foil lamination sample and commercially available M9 board. In Example 2, performance can be directionally controlled by adjusting the type of filler. Adding hollow glass microspheres can reduce the dielectric constant to 2.4 and obtain excellent high-frequency dielectric properties, but it will reduce the thermal conductivity.

[0117] In Example 4, the combination of diamond and silicon dioxide can increase the thermal conductivity to 0.82 W / mK while maintaining a low dielectric constant and dielectric loss, making it more suitable for high-power heat dissipation requirements.

[0118] The linear thermal expansion coefficients of the various embodiments of the present invention are in the range of (16~19)×10⁻⁶. -7 / K is more compatible with the thermal expansion coefficient of commonly used copper foil in PCBs, and the glass transition temperature is maintained at 232-238℃, which is much higher than the 135℃ of commercially available M9 board. It has outstanding high-temperature dimensional stability and the overall surface roughness is better than that of the laminated copper foil sample.

[0119] Comparative Example 1 confirms that replacing ordinary fiberglass cloth leads to an overall deterioration in dielectric properties, loss, and bonding strength. Comparative Example 2 confirms that compared to traditional copper foil lamination, the coating modification-electroplating scheme of this invention significantly improves the interface anchoring effect. Comparative Example 3 confirms that although commercially available M9 sheets have excellent dielectric properties, they suffer from drawbacks such as low glass transition temperature, weak coating adhesion, and insufficient thermal conductivity. Comparative Example 4 confirms that LCP resin plays an indispensable role in the final performance of the product. Therefore, the technical solution of this invention is more suitable for the high-load operation of AI servers 24 / 7.

[0120] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a high-frequency, high-speed PCB substrate, characterized in that, Includes the following steps: S1. After coating the mixed resin solution onto the liquid crystal polymer insulating substrate, dry it to obtain a substrate containing an LCP coating. S2. The above-mentioned substrate containing LCP coating is subjected to chemical electroplating to obtain a substrate containing a metal layer.

2. The preparation method according to claim 1, characterized in that, In S1, the mixed resin solution is prepared from raw materials comprising the following parts by weight: 1-30 parts of high heat-resistant thermoplastic resin, 0-20 parts of functional filler, 0-10 parts of dispersant, 0-10 parts of emulsifier, and 50-95 parts of solvent; and / or, In S1, the high heat-resistant thermoplastic resin is selected from liquid crystal polymer resin or phenolphthalein-based polyaryletherketone resin.

3. The preparation method according to claim 2, characterized in that, In S1, the liquid crystal polymer resin is a fully aromatic polyester; preferably, the melting point of the liquid crystal polymer resin is greater than 260°C; and / or, In S1, the glass transition temperature of the phenolphthalein-based polyaryletherketone resin is not lower than 220℃; and / or, In S1, the liquid crystal polymer insulating substrate is selected from liquid crystal polymer fiber cloth or liquid crystal polymer film; and / or, In S1, the functional filler is selected from at least one of hollow glass microspheres, polytetrafluoroethylene, diamond, boron nitride, and aluminum nitride; and / or, In S1, the D50 particle size of the functional filler is 0.01–15 μm; and / or, In S1, the solvent is selected from at least one of N-methylpyrrolidone and N,N-dimethylformamide.

4. The preparation method according to claim 1, characterized in that, In S1, the coating is a single-sided or double-sided coating of the liquid crystal polymer insulating substrate; and / or, In S1, the thickness of the coating obtained after coating reaches 1–50 μm on one side; and / or, In S1, the drying temperature is 60-80°C; the drying time is 30-60 minutes.

5. The preparation method according to claim 1, characterized in that, In S2, the chemical electroplating specifically includes: performing a chemical wet pretreatment on the substrate containing the LCP coating, followed by electrolytic electroplating. Preferably, the chemical electroplating specifically includes: subjecting the substrate containing the LCP coating to roughening treatment, reduction treatment, activation treatment, and desizing treatment in sequence; then using the substrate after desizing treatment as the cathode and copper foil as the anode, electrochemically depositing a metal layer using an electroplating solution containing metal salts until the metal layer reaches the target thickness.

6. The preparation method according to claim 5, characterized in that, In S2, the chemical electroplating is performed on one or both sides of the substrate containing the LCP coating; and / or, In S2, the thickness of the metal layer on one side is 0.5–200 μm; and / or, In S2, the metal in the electroplating solution containing the metal salt is selected from at least one of gold, silver, copper, chromium, or nickel; and / or, Preferably, in S2, the electroplating solution containing metal salts is an electroplating solution containing copper salts; the copper salt-containing electroplating solution comprises 150-250 g / L copper sulfate, 30-40 g / L sulfuric acid, and 80-120 mL / L hydrochloric acid; and / or, In S2, the electrochemical deposition temperature is 20~30℃ and the electrochemical deposition time is 40~50min.

7. The preparation method according to claim 5, characterized in that, In S2, the roughening treatment includes: immersing the LCP-coated substrate in a high-chromic acid roughening solution for etching, thereby forming micropits with an average diameter of 0.01~0.5μm on the substrate surface; and / or, In S2, the reduction treatment includes: treating the roughened substrate with an aqueous solution of sodium borohydride; preferably, the concentration of the sodium borohydride aqueous solution is 0.5~2 g / L; and / or, In S2, the activation treatment includes: activating the reduced-rinsed substrate using a Pd-Sn activation solution; preferably, the Pd-Sn activation solution contains 250 mL / L hydrochloric acid, 5 g / L stannous chloride, and 15 ppm colloidal palladium; more preferably, the activation temperature is 30~40℃, and the activation time is 1~10 min; and / or, In S2, the descaling process includes: descaling the activated substrate using a descaling solution; preferably, the descaling solution is a hydrochloric acid solution of 50~100g / L; more preferably, the descaling temperature is 30~40℃ and the descaling time is 5~10min.

8. The preparation method according to claim 1, characterized in that, It also includes S3, which involves surface treatment of the substrate containing the metal layer to obtain the finished product. The surface treatment includes polishing the metal coating, plasma treatment, and finally interface bonding treatment. Preferably, the interface bonding treatment specifically involves depositing a titanium dioxide intermediate layer on the surface of the metal layer using a plasma-enhanced chemical vapor deposition process.

9. The high-frequency, high-speed PCB substrate prepared by the preparation method according to any one of claims 1 to 8.

10. The application of the high-frequency, high-speed PCB substrate as described in claim 9 in an AI server.