A liquid-cooled heat sink based on gradient aperture capillary wick and its preparation method

By combining a gradient aperture capillary core structure with a ternary phase change working fluid, the problems of interfacial thermal resistance and capillary permeability of liquid cooling plates in high heat flux density scenarios are solved, achieving a highly efficient heat dissipation effect.

CN123075864APending Publication Date: 2026-11-10SHENZHEN XINDIANJIN OPTOELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611350167.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing liquid cooling plates suffer from problems in high heat flux density scenarios, such as interfacial thermal resistance and the difficulty in simultaneously achieving high capillary force and low permeability of the capillary wick, resulting in insufficient heat dissipation efficiency.

Method used

A gradient pore size capillary core structure is adopted, including a fine pore layer, a transition layer and a coarse pore layer, which increase from bottom to top along the thickness direction. Combined with the uneven morphology and ternary phase change working fluid, the liquid cooling cavity and the phase change cavity are integrated, eliminating interfacial thermal resistance and enhancing capillary force and permeability.

Benefits of technology

It achieves efficient and coordinated heat dissipation, reduces the surface temperature of the heat source, increases the critical heat flux density for burning dry, and enhances heat dissipation capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123075864A_ABST
    Figure CN123075864A_ABST
Patent Text Reader

Abstract

This invention discloses a liquid-cooled heat dissipation plate based on a gradient-pore capillary wick and its preparation method, comprising: a liquid-cooled cavity layer; a phase-change homogeneous temperature vacuum cavity layer filled with a liquid phase-change working fluid; a copper solid base plate layer; a middle partition separating the phase-change homogeneous temperature vacuum cavity layer and the liquid-cooled cavity layer; a capillary wick of gradient-pore metal powder sintered at the bottom of the phase-change homogeneous temperature vacuum cavity layer, wherein the capillary wick comprises, from bottom to top, a fine pore layer, a transition layer, and a coarse pore layer with increasing porosity and pore size along the thickness direction; the total thickness of the capillary wick at the inlet end is less than the total thickness at the outlet end along the coolant flow direction; the surface of the coarse pore layer facing the middle partition has an uneven morphology; this application eliminates the interfacial thermal resistance in the split liquid-cooled plate scheme through structural modification, and solves the problem of difficulty in balancing high capillary force and low permeability of the capillary wick in a thin phase-change cavity, so as to achieve efficient synergistic heat dissipation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of technology, and in particular to a liquid-cooled heat sink based on a gradient aperture capillary wick and its preparation method. Background Technology

[0002] With the continuous increase in heat flux density of high-performance computing chips and power modules, liquid coolers are widely used in heat dissipation applications for high heat flux density devices. The heat dissipation capacity of existing liquid coolers is limited by the combined efficiency of thermal conductivity and forced convection in solid materials, typically exceeding 100 W / cm². 2 In localized hot spots, forced convection of the coolant alone is insufficient to remove heat in time, easily leading to localized overheating. To compensate for the insufficient thermal conductivity of liquid cooling plates, existing technologies have developed solutions that combine vapor chambers with liquid cooling plates.

[0003] However, vapor chambers and liquid cooling plates still have the following shortcomings in practical applications: the vapor chamber and liquid cooling plate are separate structures, and the two are connected by pressing or welding through thermally conductive interface materials. There is additional thermal resistance at the interface, which limits the overall heat dissipation efficiency. At the same time, the performance of the vapor chamber degrades significantly under high power and long-term operation conditions, especially in thin-film designs where the heat transfer capacity decreases more significantly, making it difficult to meet the continuous heat dissipation requirements in high heat flux density scenarios.

[0004] Therefore, it is necessary to provide a solution to the problem of balancing high capillary force and low permeability in thin phase change cavities, so as to achieve efficient synergistic heat dissipation. Summary of the Invention

[0005] In view of this, this application provides a liquid-cooled heat dissipation plate based on a gradient aperture capillary wick and its preparation method, which is used to solve the problem of how to eliminate the interfacial thermal resistance in the split liquid-cooled plate scheme, and at the same time solve the problem of the difficulty in balancing the high capillary force and low permeability of the capillary wick in the thin phase change cavity, so as to achieve efficient synergistic heat dissipation.

[0006] To achieve the above technical objectives, this application adopts the following technical solution: In a first aspect, this application provides a liquid-cooled heat sink based on a gradient aperture capillary wick, comprising, from top to bottom along the thickness direction: The liquid-cooled cavity layer has serpentine or S-shaped flow channels inside for the flow of coolant; A phase change homogeneous temperature vacuum chamber layer, filled with a liquid phase change working fluid; Solid copper base plate layer; The phase change homogenizing vacuum chamber layer and the liquid-cooled chamber layer are separated by an intermediate partition. The bottom of the phase change uniform temperature vacuum cavity layer is provided with a capillary core of metal powder sintered with gradient pore size. The capillary core includes a fine pore layer, a transition layer and a coarse pore layer with increasing porosity and pore size from bottom to top along the thickness direction. Along the coolant flow direction, the total thickness H1 of the capillary wick at the inlet end is less than the total thickness H2 at the outlet end; The surface of the coarse-porous layer facing the intermediate partition has an uneven morphology.

[0007] Preferably, the pore size of the fine-pored layer is 5μm to 25μm and the porosity is 45% to 55%; the pore size of the transition layer is 30μm to 70μm and the porosity is 60% to 70%; and the pore size of the coarse-pored layer is 80μm to 160μm and the porosity is 75% to 88%.

[0008] Preferably, the raised structure with an uneven morphology contacts the intermediate partition.

[0009] Preferably, the liquid phase change working medium is a ternary mixture of ethanol, water and heptanol, wherein the volume ratio of ethanol to water is 40:60 to 75:25, and the mass fraction of heptanol is 0.05% to 0.15%.

[0010] Preferably, the thickness of the phase change uniform temperature vacuum cavity layer is 3-7mm; the total thickness of the liquid cooling heat sink is 10mm-12mm.

[0011] This application provides a method for manufacturing a liquid-cooled heat sink based on a gradient aperture capillary wick, comprising the following steps: S1. A liquid-cooled cavity and a phase-change homogenized vacuum cavity are machined inside a copper substrate; S2. At the bottom of the phase change uniform temperature vacuum chamber, a fine copper powder layer, a medium copper powder layer, and a coarse copper powder layer are laid sequentially from bottom to top. Each layer of copper powder is mixed with a composite pore-forming agent. Along the flow direction of the coolant, the thickness of the fine copper powder layer and the medium copper powder layer is constant, while the thickness of the coarse copper powder layer gradually increases from the inlet end to the outlet end. S3. A pressure plate with an uneven surface is used to apply pressure to the upper surface of the coarse copper powder layer to form an uneven surface; S4. Place the copper substrate in a vacuum sintering furnace for sintering and cooling; S5. Seal the middle partition plate over the space above the phase change uniform temperature vacuum chamber, evacuate the vacuum, fill with liquid phase change working fluid and seal; S6. Seal the upper cover plate over the liquid cooling cavity space to form a coolant flow channel.

[0012] Preferably, in S4, the sintering adopts a pulsed current sintering method with a temperature gradient along the vertical direction, so that the temperature of the fine copper powder layer region is 800℃~850℃, the temperature of the medium copper powder layer region is 850℃~900℃, and the temperature of the coarse copper powder layer region is 900℃~950℃.

[0013] Preferably, the composite pore-forming agent is a mixture of ammonium bicarbonate and ammonium carbonate.

[0014] Preferably, the mass ratio of ammonium bicarbonate to ammonium carbonate in the fine copper powder layer is 4:1, the mass ratio of ammonium bicarbonate to ammonium carbonate in the medium copper powder layer is 3:1, and the mass ratio of ammonium bicarbonate to ammonium carbonate in the coarse copper powder layer is 2:1.

[0015] Preferably, in step S4, during the cooling process, a pressure of 0.1 MPa to 0.5 MPa is applied to the upper surface of the coarse copper powder layer by a graphite press, and the pressure is maintained until the temperature drops below 300°C.

[0016] The beneficial effects of this application are as follows: By integrating the liquid cooling cavity and the phase change homogenizing cavity into the same rectangular metal block and physically isolating them with a partition in the middle, this application eliminates the contact thermal resistance caused by the heat-conducting interface material in the split design, allowing heat to form a continuous metal wall conduction path from the heat source to the coolant; by setting a three-layer gradient capillary core with pore size and porosity increasing from bottom to top along the thickness direction at the bottom of the phase change cavity, the bottom fine pore layer generates high capillary force to adsorb the liquid working fluid onto the evaporation surface, and the top coarse pore layer provides low flow resistance for the smooth escape of steam, thus solving the contradiction between capillary force and permeability that is difficult to balance in thin cavities; through the coarse pores The uneven surface morphology of the layer allows the raised parts to contact the intermediate partition to provide compressive support, while the recessed parts retain steam channels, eliminating the need for independent support columns and avoiding obstruction of steam flow by the support columns. By setting a non-uniform thickness distribution of the capillary core with a thin inlet and a thick outlet along the coolant flow direction, the thin inlet core reduces thermal resistance, while the thick outlet core increases the working fluid storage and evaporation area, matching the temperature field changes of the coolant along the flow direction. By using a ternary mixed working fluid of ethanol, water, and heptanol, ethanol reduces the flow resistance of the working fluid in the coarse-pore layer, and heptanol provides additional reflux driving force, achieving a synergistic enhancement of liquid-cooled forced convection and latent heat exchange of phase change. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the liquid-cooled heat sink of the present invention; Figure 2 This is a partially enlarged cross-sectional view of the liquid-cooled heat sink structure of the present invention; Figure 3 This is a schematic diagram of the contact area between the coarse-porous layer and the intermediate partition plate of the present invention.

[0018] Explanation of reference numerals in the attached figures: 1-Liquid-cooled cavity layer; 2-Flow channel; 3-Phase change uniform temperature vacuum cavity layer; 4-Intermediate partition plate; 5-Solid copper base plate layer; 6-Fine pore layer; 7-Transition layer; 8-Coarse pore layer; 9-Protruding structure; 10-Recessed area. Detailed Implementation

[0019] The embodiments of the technical solution of this application will be described in detail below. The following embodiments are only used to illustrate the technical solution of this application more clearly, and are therefore only examples, and should not be used to limit the scope of protection of this application.

[0020] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0021] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0022] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.

[0023] Unless otherwise explicitly defined and specified herein, all technical and scientific terms used in this application shall have the generally accepted meanings understood by one of ordinary skill in the field of chemical and chemical materials technology (including but not limited to polymer chemistry, inorganic chemistry, organic synthesis, catalysis chemistry, materials processing, and chemical unit operations) based on their professional knowledge and conventional practice. The use of any terminology herein is intended to describe the specific embodiments of this application in the clearest and most accurate manner, so as to fully disclose the technical solution. Such use shall not in any way be construed as a limitation on the scope of the claims, nor does it imply the exclusion of equivalent technical solutions that could be reasonably known by one of skill in the art based on the concept of this application.

[0024] The terms "comprising," "including," "having," "containing," and any grammatical variations or similar expressions used in the specification and claims of this application are all open-ended and non-exhaustive descriptive terms. Their purpose is to explicitly describe the existence of technical features, components, steps, or parts, while explicitly allowing and covering the possibility that other features, components, steps, parts, or any combinations thereof not explicitly listed may exist or be added to the technical solution, as long as such additions do not destroy the integrity and inventiveness of the original technical solution.

[0025] When the terms "embodiments," "some embodiments," or "specific embodiments" are mentioned in the specification, they refer to examples that, in conjunction with the specific parameters, materials, steps, and results described in that section, constitute one or a group of examples for implementing the technical solutions of this application. These embodiments are used for full disclosure and illustrative purposes, not for exhaustive enumeration. Those skilled in the art should understand that, without departing from the overall inventive concept of this application, the various technical features disclosed in different embodiments can be combined, substituted, modified, or deleted to form other implementation methods that are not listed one by one in the specification but also fall within the protection scope of this application.

[0026] Unless otherwise expressly specified and limited, all terms related to chemical process operations, material preparation, processing and analytical testing involved in this application shall be interpreted in the broadest sense based on the conventional understanding of those skilled in the art.

[0027] Regarding numerical values ​​and ranges, all parameter ranges expressed in this application in the form of "from a certain value to a certain value" should be understood as explicitly disclosing the endpoints of the range, each specific numerical point between the endpoints, and all sub-ranges formed by any two numerical points within the range. For example, "30℃ to 80℃" discloses 30, 31, ..., 80℃, as well as sub-ranges such as 30-50℃, 45-70℃, etc. When a numerical value is preceded by "about," "approximately," or similar words, it indicates that the numerical value is allowed to have reasonable errors recognized in the art under the measurement or control conditions, which can generally be understood as the deviation allowed by relevant standards or a normal fluctuation range of ±5% or ±10%.

[0028] like Figure 1 As shown, this application provides a liquid-cooled heat sink based on a gradient aperture capillary wick, comprising, from top to bottom, the following components along the thickness direction: The liquid cooling cavity layer 1 has a serpentine or S-shaped flow channel 2 inside for the flow of coolant; Phase change homogeneous vacuum chamber layer 3, filled with liquid phase change working fluid; 5 layers of solid copper base plate; The phase change uniform temperature vacuum cavity layer 3 and the liquid cooling cavity layer 1 are separated by an intermediate partition plate 4; The bottom of the phase change uniform temperature vacuum chamber layer 3 is provided with a capillary core of metal powder sintered with gradient pore size. The capillary core includes a fine pore layer 6, a transition layer 7 and a coarse pore layer 8 with increasing porosity and pore size from bottom to top along the thickness direction. like Figure 2 As shown, along the coolant flow direction, the total thickness H1 of the capillary wick at the inlet end is less than the total thickness H2 at the outlet end. like Figure 3 As shown, the surface of the coarse-porous layer 8 facing the intermediate partition 4 has an uneven morphology.

[0029] In this application, the liquid-cooled heat sink is a flat rectangular block with a total thickness of 10mm to 12mm. It consists of three stacked layers from top to bottom: an upper liquid-cooled cavity layer 1, a middle phase-change homogeneous temperature vacuum cavity layer 3, and a lower solid copper base plate layer 5. The liquid-cooled cavity layer 1 and the phase-change homogeneous temperature vacuum cavity layer 3 are separated by a thin oxygen-free copper plate (intermediate partition 4), ensuring complete isolation and non-communication between the coolant and the phase-change working fluid at the fluid level, with heat conduction only through the intermediate partition 4. The phase-change homogeneous temperature vacuum cavity layer 3 is a flat, sealed cavity with a gradient-aperture sintered metal powder capillary core at its bottom. The capillary wick consists of three layers from bottom to top: the fine-pore layer 6, which is close to the bottom surface of the cavity, has the smallest pore size and the lowest porosity, generating the highest capillary force to adsorb the liquid working fluid onto the evaporation surface on the heat source side; the coarse-pore layer 8, located on the top layer, has the largest pore size and the highest porosity, providing a low-resistance diffusion channel for steam; and the transition layer 7 lies between the two, achieving a smooth transition in pore size. In the three-layer structure, the copper powder particles in each layer are stacked in more than 10 layers, ensuring the formation of a stable three-dimensional porous network after sintering. Along the flow direction of the coolant, the total thickness of the capillary wick is non-uniformly distributed, being thinner at the inlet end and thicker at the outlet end. The thickness of the fine-pore layer 6 and the transition layer 7 is constant, while only the coarse-pore layer 8 gradually thickens from the inlet end to the outlet end. The surface of the coarse-pore layer 8 facing the intermediate partition 4 has an uneven morphology. The protruding part contacts the intermediate partition 4, providing compressive support to prevent the vacuum cavity from collapsing under atmospheric pressure; the concave part forms a gap with the intermediate partition 4, serving as a lateral diffusion channel for steam.

[0030] This application integrates a liquid-cooled cavity, a phase-change homogenizing vacuum cavity, and a solid copper base plate into a single rectangular metal block. The liquid-cooled cavity and the phase-change cavity are separated by a partition 4, ensuring complete isolation and non-communication between the coolant and the phase-change working fluid at the fluid level. Heat generated by the heat source is conducted to the phase-change cavity via the solid base plate, where the liquid working fluid within the capillary wick absorbs heat and evaporates. The vapor diffuses to the lower surface of the partition 4, condenses, and releases heat. The heat is then carried away by the coolant within the liquid-cooled cavity through forced convection after passing through the partition 4. The entire heat transfer path is a continuous metal wall conduction, without any interfacial filling material. The capillary wick at the bottom of the phase-change cavity is arranged from bottom to top along the thickness direction as a fine-pore layer 6, a transition layer 7, and a coarse-pore layer 8, with porosity and pore size increasing sequentially. The bottom fine-pore layer 6, with a pore size of 5μm to 25μm, generates high capillary force to adsorb the liquid working fluid onto the evaporation surface on the heat source side. The top coarse-pore layer 8, with a pore size of 80μm to 16μm... The 0μm thickness provides low flow resistance for smooth steam escape, thus achieving both high capillary force liquid absorption and low resistance steam exhaust at the same vertical position. The surface of the coarse-pore layer 8 facing the intermediate partition 4 has an uneven morphology. The raised part contacts the intermediate partition 4 to provide pressure resistance support to prevent the vacuum cavity from collapsing under atmospheric pressure. The recessed part forms a gap with the intermediate partition 4 as a steam transverse diffusion channel, so that the same coarse-pore layer 8 can simultaneously achieve the functions of pressure resistance support and steam guidance. Along the flow direction of the coolant, the total thickness H1 at the capillary wick inlet end is less than the total thickness H2 at the outlet end. The thickness of the fine-pore layer 6 and the transition layer 7 is constant, while only the coarse-pore layer 8 gradually thickens from the inlet end to the outlet end. The thin core at the inlet end makes the heat conduction path short and the thermal resistance low when the coolant is mainly subjected to convective heat transfer in the low-temperature section. The thick core at the outlet end makes the working fluid storage large and the evaporation area wide when the coolant is mainly subjected to phase change compensation in the heating section. This matches the temperature field change of the coolant along the flow direction. Through the synergistic effect of the above three-layer integrated design, vertical pore size gradient, surface irregularity of the coarse-pore layer 8, and horizontal thickness gradient, this application eliminates interfacial thermal resistance, resolves the inherent contradiction between capillary force and permeability in thin cavities, eliminates the need for additional support columns and does not obstruct steam flow, and achieves synergistic enhanced heat transfer through liquid-cooled forced convection and latent heat exchange of phase change without increasing pump power consumption.

[0031] In some embodiments, the pore size of the fine-pored layer 6 is 5 μm to 25 μm and the porosity is 45% to 55%; the pore size of the transition layer 7 is 30 μm to 70 μm and the porosity is 60% to 70%; and the pore size of the coarse-pored layer 8 is 80 μm to 160 μm and the porosity is 75% to 88%.

[0032] In this embodiment, the pore size of the fine-pore layer 6 ensures the generation of large capillary pressure in the copper-water system, adsorbing the liquid working fluid onto the evaporation surface on the heat source side; the pore size of the coarse-pore layer 8 allows steam to escape with low resistance; the transition layer 7 is used to achieve a smooth transition in pore size, avoiding additional flow resistance caused by abrupt changes in pore size between the fine-pore layer 6 and the coarse-pore layer 8. The increasing porosity of the three layers ensures sufficient liquid storage at the bottom and unobstructed steam flow at the top.

[0033] In some embodiments, the protruding structure 9 with its uneven morphology contacts the intermediate partition 4.

[0034] In this embodiment, the protruding structure 9 in the concave-convex morphology serves a supporting function, and the recessed area 10 retains the steam channel, eliminating the need for additional welding of solid copper pillars in the prior art, and eliminating the problem of support pillars blocking steam flow.

[0035] In some embodiments, the liquid phase change working fluid is a ternary mixture of ethanol, water and heptanol, wherein the volume ratio of ethanol to water is 40:60 to 75:25, and the mass fraction of heptanol is 0.05% to 0.15%.

[0036] In this embodiment, ethanol is used to reduce the overall viscosity of the working fluid and improve the permeability of the coarse-pore layer 8; water is used to provide high surface tension and high latent heat of vaporization to ensure the capillary driving force and phase change heat carrying capacity of the fine-pore layer 6; heptanol gives the working fluid self-wetting properties and provides additional reflux driving force at a mass fraction of 0.05% to 0.15%.

[0037] In some embodiments, the thickness of the phase change uniform temperature vacuum cavity layer 3 is 3-7 mm; the total thickness of the liquid cooling heat sink is 10 mm to 12 mm.

[0038] This application provides a method for manufacturing a liquid-cooled heat sink based on a gradient aperture capillary wick, comprising the following steps: S1. A liquid-cooled cavity and a phase-change homogenized vacuum cavity are machined inside a copper substrate; S2. At the bottom of the phase change uniform temperature vacuum chamber, a fine copper powder layer, a medium copper powder layer, and a coarse copper powder layer are laid sequentially from bottom to top. Each layer of copper powder is mixed with a composite pore-forming agent. Along the flow direction of the coolant, the thickness of the fine copper powder layer and the medium copper powder layer is constant, while the thickness of the coarse copper powder layer gradually increases from the inlet end to the outlet end. S3. A pressure plate with an uneven surface is used to apply pressure to the upper surface of the coarse copper powder layer to form an uneven surface; S4. Place the copper substrate in a vacuum sintering furnace for sintering and cooling; S5. Seal the middle partition plate 4 over the space above the phase change uniform temperature vacuum chamber, evacuate the vacuum, fill with liquid phase change working fluid and seal; S6. Seal the upper cover plate over the liquid cooling cavity space to form a coolant flow channel 2.

[0039] In this application, the phase change cavity space processed in S1 is a groove with an open top, similar to an open box, which allows for powder spreading and imprinting operations from above without any operational space limitations; in S2, layered powder spreading achieves the distribution of vertical aperture gradient, and by controlling the thickness of the coarse copper powder layer, the scraper gap is small at the inlet and the layer is thin, while the scraper gap is large at the outlet and the layer is thick, thus creating a horizontal thickness gradient. The thickness of the fine copper powder layer and the medium copper powder layer is constant, while only the coarse copper powder layer becomes thicker; in S3, at room temperature, a concave-convex morphology is pressed onto the surface of the powder layer by a pressure plate, and this morphology is fixed in the subsequent sintering; in S4, vacuum sintering forms sintering necks between copper powder particles, and metallurgical diffusion bonding is formed between the layers and between the copper powder and the inner wall of the matrix; S5 and S6 are performed after sintering to seal the phase change working medium inside the cavity and isolate the coolant flow channel 2 from the phase change cavity.

[0040] In some embodiments, the sintering in S4 adopts a pulsed current sintering method with a temperature gradient along the vertical direction, so that the temperature of the fine copper powder layer region is 800℃~850℃, the temperature of the medium copper powder layer region is 850℃~900℃, and the temperature of the coarse copper powder layer region is 900℃~950℃.

[0041] In this embodiment, copper powders of different particle sizes have different shrinkage rates, with fine powder having a larger shrinkage rate and coarse powder having a smaller shrinkage rate. Sintering at a single temperature will cause interlayer stress leading to warping. Pulsed current sintering can achieve a directional temperature gradient within a height of several millimeters, making the linear shrinkage rate of each layer tend to be consistent.

[0042] In some embodiments, the composite pore-forming agent is a mixture of ammonium bicarbonate and ammonium carbonate.

[0043] In this embodiment, the pore-forming agent completely decomposes into gas at 150°C to 350°C, leaving no solid residue and requiring no water washing, thus avoiding chloride ion corrosion and residual carbon pollution.

[0044] In some embodiments, the mass ratio of ammonium bicarbonate to ammonium carbonate in the fine copper powder layer is 4:1, the mass ratio of ammonium bicarbonate to ammonium carbonate in the medium copper powder layer is 3:1, and the mass ratio of ammonium bicarbonate to ammonium carbonate in the coarse copper powder layer is 2:1.

[0045] In this embodiment, the proportion of ammonium bicarbonate in each layer is high, which decomposes preferentially at low temperatures to prevent the fine pores from being filled by the sintering neck; the proportion of ammonium carbonate is high, which decomposes at high temperatures and is synchronized with the sintering of the coarse powder layer.

[0046] In some embodiments, in step S4, during the cooling process, a pressure of 0.1 MPa to 0.5 MPa is applied to the upper surface of the coarse copper powder layer by a graphite press, and the pressure is maintained until the temperature drops below 300°C.

[0047] In this embodiment, there are slight differences in shrinkage between the layers during the sintering and cooling process. If no conformal pressure is applied, the uneven morphology of the upper surface of the coarse-pore layer 8 may produce micron-level dimensional deviations, causing the protrusions to fail to form reliable contact with the intermediate partition 4.

[0048] The following specific embodiments further illustrate this solution. Example

[0049] A liquid-cooled heat sink based on a gradient aperture capillary wick, generally in the shape of a flat rectangular block, comprising, from top to bottom along the thickness direction: Liquid cooling cavity layer 1 is a hollow cavity, which is enclosed by the lower surface of the upper cover plate and the upper surface of the middle partition plate 4. The interior is provided with a serpentine coolant flow channel 2, which is provided with a coolant inlet and outlet, located at both ends in the length direction, and the interface is a G1 / 4 threaded hole. The intermediate partition 4 is made of oxygen-free copper (TU1) thin plate, which matches the sealing edge of the liquid cooling cavity layer 1 and the phase change cavity layer. The intermediate partition 4 completely physically isolates the coolant above from the phase change working fluid below. The phase change homogenizing vacuum chamber layer 3 is a hollow, sealed cavity, enclosed by the lower surface of the intermediate partition plate 4, the upper surface of the lower base plate, and the surrounding side walls. It is filled with a liquid phase change working fluid, and the vacuum level is ≤10. -4 Pa; the liquid phase change working fluid is a ternary mixture of ethanol, water, and heptanol, with a volume ratio of ethanol to water of 70:30 and a mass fraction of heptanol of 0.1%; the bottom of the phase change cavity layer is provided with a gradient-pore size metal powder sintered capillary core, which consists of a fine-pore layer 6, a transition layer 7, and a coarse-pore layer 8 along the thickness direction from bottom to top; the original copper powder particle size of the fine-pore layer 6 is 35 μm, and the pore size after sintering is 15 μm, with a porosity of 50%, and the fine-pore layer 6 is in close contact with the bottom surface of the phase change cavity; the original copper powder particle size of the transition layer 7 is 50 μm, and the pore size after sintering is 50 μm, with a porosity of 60%. 5%; the coarse-porous layer 8 has a non-uniform thickness distribution along the coolant flow direction. At the inlet end, the thickness of the coarse-porous layer 8 is 2.0 mm, and at the outlet end, the thickness of the coarse-porous layer 8 is 2.8 mm. It is transitioned by a smooth slope in the middle. The original copper powder particle size is 150 μm, and the pore size after sintering is 120 μm, with a porosity of 80%; the surface of the coarse-porous layer 8 facing the intermediate partition 4 has an uneven morphology and is arranged in an array; the top of the protrusion contacts the lower surface of the intermediate partition 4 to provide compressive support; the recessed area 10 between the protrusions forms a gap with the intermediate partition 4, which serves as a steam transverse diffusion channel.

[0050] The 5th layer is a solid copper base plate, which is an oxygen-free copper (TU1) solid metal plate with a flat heating surface on its lower surface.

[0051] The manufacturing method of a liquid-cooled heat sink based on a gradient aperture capillary wick includes the following steps: S1. Using TU1 oxygen-free copper material, a rectangular block with external dimensions of 80mm×60mm×11.5mm is manufactured by precision machining (milling) (with a 0.5mm fine grinding allowance). Inside the block, an upper liquid cooling cavity space with a height of 2.8mm, a serpentine flow channel 2 structure, and a lower phase change cavity space with a height of 4.5mm are machined. The phase change cavity space is a groove with an open top, which can be used for subsequent powder spreading operations from above. After machining, the inner wall of the cavity is cleaned, degreased, and acid-washed for activation. S2. High-purity electrolytic copper powder (purity ≥99.8%) was selected and separated into three grades using a vibrating sieve: 35μm fine copper powder, 50μm medium copper powder, and 150μm coarse copper powder. Each particle size of copper powder was annealed at 400°C for 1.5 hours in a hydrogen atmosphere to remove the oxide film and work-hardened layer on the powder surface. After annealing, it was cooled to room temperature under argon protection. Three ratios of ammonium bicarbonate and ammonium carbonate composite pore-forming agents were prepared: for the fine copper powder layer, the mass ratio of ammonium bicarbonate to ammonium carbonate was 4:1, the particle size of the pore-forming agent was 25μm, and the addition amount was 30% by volume; for the medium copper powder layer, the mass ratio of ammonium bicarbonate to ammonium carbonate was 3:1, the particle size of the pore-forming agent was 75μm, and the addition amount was 42% by volume; for the coarse copper powder layer, the mass ratio of ammonium bicarbonate to ammonium carbonate was 2:1, and the pore-forming agent was... The agent has a particle size of 180μm and is added at a volume fraction of 58%. Each layer of copper powder and the corresponding pore-forming agent are mixed in a V-type mixer for 6 hours to ensure uniform dispersion. The copper matrix is ​​placed on an ultrasonic vibration platform (frequency 40kHz, amplitude 30μm). At the bottom of the phase change cavity, a 0.7mm thick layer of fine copper powder is laid from bottom to top, leveled with a programmable movable scraper, and ultrasonically vibrated for 15 seconds. A 0.7mm thick layer of medium copper powder is laid, leveled with a programmable movable scraper, and ultrasonically vibrated for 15 seconds. A coarse copper powder layer is laid with varying thickness along the coolant flow direction, with a thickness of 2.0mm at the inlet end and 2.8mm at the outlet end. A smooth slope transition is formed in the middle by tilting the programmable scraper. After laying, ultrasonically vibrated for 20 seconds. S3. A graphite pressure plate with an array of protrusions 9 (protrusion height 200μm, spacing 2mm) is used to apply a pressure of 0.3MPa to the upper surface of the coarse copper powder layer and hold the pressure for 30s to form a corresponding uneven morphology on the surface of the coarse copper powder layer. After the pressure plate is removed, the uneven morphology is retained in the powder layer. S4. Place the copper substrate after powder spreading in a cold isostatic pressing mold and hold it under 100 MPa pressure for 2 minutes to ensure sufficient strength of the powder compact. Place the pre-pressed assembly in a spark plasma sintering furnace (SPS) and use a pulsed current sintering method with a temperature gradient along the vertical direction, raising the temperature from room temperature to the target temperatures at a rate of 100°C / min. Temperature gradient control: By adjusting the current density of the upper and lower graphite pressure heads and the mold wall thickness design, a temperature gradient is established in the vertical direction. The temperature in the fine copper powder layer area is 830°C, the temperature in the medium copper powder layer area is 880°C, and the temperature in the coarse copper powder layer area is 930°C. The total holding time during the holding stage is 2 hours, and the vacuum degree is ≤5×10⁻⁶. -3 Pa; 30 minutes before the end of the heat preservation, high-purity hydrogen gas (purity ≥99.999%) is introduced into the furnace at a flow rate of 100 mL / min to reduce the copper oxide on the surface of the copper powder and the inner wall of the cavity; after sintering, metallurgical diffusion bonding is formed between the layers of copper powder and between the copper powder and the inner wall of the cavity; during the cooling process, a constant pressure of 0.3 MPa is applied to the upper surface of the coarse copper powder layer by a graphite press, and the pressure is maintained until the temperature drops below 300°C to ensure the dimensional accuracy of the uneven morphology of the upper surface of the coarse pore layer 8; after sintering, the upper and lower surfaces of the copper substrate are precision ground to make the total thickness of the substrate reach 11 mm; S5. A 0.5mm thick oxygen-free copper sheet is used as an intermediate partition 4 to cover the space above the phase change cavity, leaving a 2mm diameter copper tube as a filling tube. The plate is placed in a vacuum brazing furnace, and copper-based brazing filler metal is applied to the edges of the intermediate partition 4. The furnace is then heated to 750°C for vacuum brazing and sealing, ensuring the phase change cavity is in a high vacuum state (10). -4 (Pa level) While keeping the vacuum pump running continuously, a ternary working fluid mixture is injected through the filling capillary tube. The volume ratio of ethanol to water is 70:30, and the mass fraction of heptanol is 0.1%. The injection volume is 50% of the phase change chamber. After injection, the vacuum pump is restarted for a second vacuuming to remove any trace gases that may have been introduced during the injection process. After the second vacuuming, the filling capillary tube is immediately sealed with laser welding to complete the sealing. S6. A 1.2mm thick oxygen-free copper plate with pre-processed serpentine flow channel 2 is used as the upper cover plate and is brazed to seal the upper surface of the middle partition plate 4, so that the lower surface of the upper cover plate and the upper surface of the middle partition plate 4 enclose the coolant flow channel 2. G1 / 4 threaded water nozzle connectors are welded at the coolant inlet and outlet of the cover plate respectively. The lower surface of the solid bottom plate is nickel plated with a thickness of 5μm to prevent oxidation and reduce the contact thermal resistance with the heat source, thus obtaining the liquid cooling heat sink based on the gradient aperture capillary core. Example

[0052] A liquid-cooled heat sink based on a gradient aperture capillary wick is prepared using the same method as in Example 1, except that in step S1, the phase change cavity space is processed to a height of 4.0 mm, and the total thickness of the rectangular block is reserved to be 10.5 mm; in step S2, the thickness of the fine copper powder layer and the medium copper powder layer is 0.6 mm, the thickness of the coarse copper powder layer at the inlet end is 1.8 mm, and the thickness at the outlet end is 2.5 mm; in step S3, the protrusion height of the graphite pressure plate is 150 μm, and the protrusion spacing is 2.5 mm; in step S5, the volume ratio of ethanol to water in the liquid phase change working fluid is 50:50, and the mass fraction of heptanol is 0.08%. Example

[0053] A liquid-cooled heat sink based on a gradient aperture capillary wick is prepared using the same method as in Example 1, except that in step S1, the phase change cavity space is processed to a height of 5.0 mm, and the total thickness of the rectangular block is reserved to be 11.5 mm; in step S2, the thickness of the fine copper powder layer and the medium copper powder layer is 0.8 mm, the thickness of the coarse copper powder layer at the inlet end is 2.2 mm, and the thickness at the outlet end is 3.0 mm; in step S3, the protrusion height of the graphite pressure plate is 250 μm, and the protrusion spacing is 1.5 mm; in step S5, the volume ratio of ethanol to water in the liquid phase change working fluid is 40:60, and the mass fraction of heptanol is 0.12%.

[0054] Comparative Example 1 A liquid-cooled heat sink is prepared in the same way as in Example 1. The difference is that in step S2, the fine copper powder layer, medium copper powder layer and coarse copper powder layer are not distinguished. Only copper powder with a particle size of 80μm is laid. However, the thickness of the inlet end and the thickness of the outlet end are the same as in Example 1.

[0055] Comparative Example 2 A liquid-cooled heat sink is prepared in the same way as in Example 1, except that in step S2, the thickness of the coarse copper powder layer at the inlet and outlet ends is the same, which is 2.4 mm.

[0056] Comparative Example 3 A liquid-cooled heat sink is prepared in the same way as in Example 1, except that step S3 is not included.

[0057] Comparative Example 4 A liquid-cooled heat sink is prepared in the same way as in Example 1, except that the liquid phase change working medium does not include heptanol.

[0058] Testing and Evaluation Test the heat source surface temperature and the critical heat flux density to burn out of different liquid cooling heat sinks; Heat source surface temperature: The liquid cooling heat sink to be tested is installed on a 12mm×12mm simulated heat source. Thermal grease is applied to the contact surface and a constant pressure of 50N~100N is applied. A K-type thermocouple is placed at the center of the contact surface between the heat source and the heat sink to measure the surface temperature of the heat source. The flow rate of the coolant (deionized water) is set to 2L / min and the inlet temperature is 25°C±0.5°C. After the system stabilizes, the simulated heat source is turned on and continuously run at a constant heating power of 300W until thermal equilibrium is reached (the surface temperature fluctuation of the heat source does not exceed ±0.5°C within 5 minutes). The surface temperature of the heat source Ts, the inlet temperature of the coolant Tin, and the outlet temperature Tout are recorded. The total thermal resistance is calculated as R = (Ts− Tin) / Q, where Q is the input thermal power (300W). Each sample is tested 3 times, and the average value is taken as the final result.

[0059] Critical heat flux density for burn-off: After completing the heat source surface temperature test, keep the coolant flow rate (2L / min) and inlet temperature (25°C) constant. Start from 100W and gradually increase the heating power in 20W increments. Run the heat source surface temperature stably for at least 5 minutes at each power point and record the temperature. Continue to increase the power until a sharp temperature rise occurs (the rise rate is ≥1°C / s) or the temperature rise exceeds 10°C within 3 minutes without convergence. Stop heating immediately and record the critical power Pcritical. Calculate the critical heat flux density for burn-off according to CHF = Pcritical / A, where A is the effective heating area of ​​the simulated heat source (12mm × 12mm, i.e., 1.44cm²). Repeat the test 3 times for each sample and take the average value as the final result.

[0060] The results are shown in Table 1.

[0061] Table 1 Test Results ; As can be seen from the comparison between the embodiments and the comparative examples, the embodiments with vertical gradient structure, horizontal thickness gradient, concave and convex morphology and ternary mixed working fluid have lower heat source surface temperature and higher critical heat flux density for burning dry, while the comparative examples lacking any of the above features have significantly reduced performance.

[0062] This application integrates the liquid cooling cavity and the phase change homogenizing cavity into the same rectangular metal block and physically isolates them with a partition plate 4 in the middle. This eliminates the contact thermal resistance caused by the heat-conducting interface material in the separate design, allowing heat to be conducted through a continuous metal wall path from the heat source to the coolant. By setting a three-layer gradient capillary core with increasing pore size and porosity along the thickness direction at the bottom of the phase change cavity, the bottom fine-pore layer 6 generates high capillary force to adsorb the liquid working fluid onto the evaporation surface, while the top coarse-pore layer 8 provides low flow resistance for smooth steam escape. This solves the contradiction between capillary force and permeability in thin cavities. Furthermore, the uneven surface of the coarse-pore layer 8... The morphology allows the raised portion to contact the intermediate partition 4 to provide pressure resistance, while the recessed portion retains the steam channel, eliminating the need for independent support columns and avoiding obstruction of steam flow by the support columns. By setting a non-uniform thickness distribution of the capillary core with a thin inlet and a thick outlet along the coolant flow direction, the thin inlet core reduces thermal resistance, while the thick outlet core increases the working fluid storage and evaporation area, matching the temperature field change of the coolant along the flow direction. By using a ternary mixed working fluid of ethanol, water, and heptanol, ethanol reduces the working fluid flow resistance of the coarse-pore layer 8, and heptanol provides additional reflux driving force, achieving synergistic enhancement of liquid-cooled forced convection and latent heat exchange of phase change.

[0063] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A liquid-cooled heat dissipation plate based on a gradient aperture capillary wick, characterized in that, From top to bottom along the thickness direction, it includes: The liquid-cooled cavity layer has serpentine or S-shaped flow channels inside for the flow of coolant; A phase change homogeneous temperature vacuum chamber layer, filled with a liquid phase change working fluid; Solid copper base plate layer; The phase change uniform temperature vacuum cavity layer and the liquid cooling cavity layer are separated by an intermediate partition. The bottom of the phase change uniform temperature vacuum cavity layer is provided with a capillary core of metal powder sintered with gradient pore size. The capillary core includes, from bottom to top, a fine pore layer, a transition layer and a coarse pore layer with increasing porosity and pore size along the thickness direction. Along the flow direction of the coolant, the total thickness H1 of the capillary at the inlet end is less than the total thickness H2 at the outlet end; The surface of the coarse-porous layer facing the intermediate partition plate has an uneven morphology.

2. The liquid-cooled heat dissipation plate based on a gradient aperture capillary wick according to claim 1, characterized in that, The fine-pore layer has a pore size of 5μm to 25μm and a porosity of 45% to 55%; the transition layer has a pore size of 30μm to 70μm and a porosity of 60% to 70%; and the coarse-pore layer has a pore size of 80μm to 160μm and a porosity of 75% to 88%.

3. The liquid-cooled heat dissipation plate based on a gradient aperture capillary wick according to claim 1, characterized in that, The raised structure with the concave-convex shape contacts the middle partition.

4. The liquid-cooled heat dissipation plate based on a gradient aperture capillary wick according to claim 1, characterized in that, The liquid phase change working fluid is a ternary mixture of ethanol, water and heptanol, wherein the volume ratio of ethanol to water is 40:60 to 75:25, and the mass fraction of heptanol is 0.05% to 0.15%.

5. The liquid-cooled heat sink based on a gradient aperture capillary wick according to claim 1, characterized in that, The thickness of the phase change uniform temperature vacuum cavity layer is 3-7mm; the total thickness of the liquid cooling heat sink is 10mm-12mm.

6. A method for manufacturing a liquid-cooled heat sink based on a gradient aperture capillary wick as described in any one of claims 1-5, characterized in that, Includes the following steps: S1. A liquid-cooled cavity and a phase-change homogenized vacuum cavity are machined inside a copper substrate; S2. At the bottom of the phase change uniform temperature vacuum chamber, a fine copper powder layer, a medium copper powder layer, and a coarse copper powder layer are laid sequentially from bottom to top. Each layer of copper powder contains a composite pore-forming agent. Along the flow direction of the coolant, the thickness of the fine copper powder layer and the medium copper powder layer is constant, while the thickness of the coarse copper powder layer gradually increases from the inlet end to the outlet end. S3. Apply pressure to the upper surface of the coarse copper powder layer using a pressure plate with an uneven morphology to form an uneven morphology; S4. The copper substrate is placed in a vacuum sintering furnace for sintering and cooling; S5. Seal the middle partition plate over the space of the phase change uniform temperature vacuum chamber, evacuate the vacuum, fill with liquid phase change working fluid and seal; S6. The upper cover plate is sealed and covered above the liquid cooling cavity space, forming a coolant flow channel with the liquid cooling cavity space.

7. The method for manufacturing a liquid-cooled heat sink based on a gradient aperture capillary wick according to claim 6, characterized in that, The sintering described in S4 adopts a pulsed current sintering method with a temperature gradient along the vertical direction, so that the temperature of the fine copper powder layer region is 800℃~850℃, the temperature of the medium copper powder layer region is 850℃~900℃, and the temperature of the coarse copper powder layer region is 900℃~950℃.

8. The method for manufacturing a liquid-cooled heat sink based on a gradient aperture capillary wick according to claim 6, characterized in that, The composite pore-forming agent is a mixture of ammonium bicarbonate and ammonium carbonate.

9. The method for manufacturing a liquid-cooled heat sink based on a gradient aperture capillary wick according to claim 6, characterized in that, The mass ratio of ammonium bicarbonate to ammonium carbonate in the fine copper powder layer is 4:1, the mass ratio of ammonium bicarbonate to ammonium carbonate in the medium copper powder layer is 3:1, and the mass ratio of ammonium bicarbonate to ammonium carbonate in the coarse copper powder layer is 2:

1.

10. The method for manufacturing a liquid-cooled heat sink based on a gradient aperture capillary wick according to claim 6, characterized in that, In step S4, during the cooling process, a pressure of 0.1 MPa to 0.5 MPa is applied to the upper surface of the coarse copper powder layer by a graphite press, and the pressure is maintained until the temperature drops below 300°C.