A semiconductor power device and its fabrication method
By forming a thin silicon electrode layer and performing mutual solution annealing in the fabrication of AlN power devices, the problems of high on-resistivity and high ohmic contact resistivity of AlN devices are solved, simplifying the process, improving device performance and fault tolerance, and reducing costs.
Patent Information
- Application Number
- CN202611580464.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-10
AI Technical Summary
Existing AlN power devices suffer from high on-resistance and high ohmic contact resistivity. Current technologies struggle to balance process complexity, manufacturing cost, and device performance, failing to meet the mass production requirements of high-performance pure AlN power devices.
Before fabricating the ohmic electrode, a thin electrode layer of silicon material is formed, and it is rapidly annealed to make it intersoluble with the metal stack. Silicon atoms diffuse into the n-type contact layer, increasing the carrier concentration, reducing the ohmic contact resistance and epitaxial layer sheet resistance, simplifying the process flow, and avoiding additional photolithography and high-temperature annealing processes.
This achieved a reduction in ohmic contact resistivity from 0.043 Ωcm² to 0.086 Ωcm², and a reduction in epitaxial layer sheet resistance from 1.88 MΩ/□ to 0.43 MΩ/□. It also simplified process steps, improved device performance and fault tolerance, and reduced costs.
Smart Images

Figure CN123075985A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor technology, and in particular to a semiconductor power device and its fabrication method. Background Technology
[0002] Compared to traditional silicon (Si) semiconductor devices, wide-bandgap semiconductor devices exhibit lower on-resistance and higher energy conversion efficiency at the same voltage level. DC-DC converters, inverters, and other power electronic devices based on wide-bandgap semiconductors offer advantages such as lightweight design and high power density, meeting the application requirements of high-power platforms and fast-charging scenarios, effectively promoting the widespread adoption of electric transportation technology. Furthermore, these materials possess excellent high-temperature resistance and radiation resistance, making them suitable for extreme operating conditions such as aerospace, high-altitude photovoltaics, and wind power, serving as core supporting materials for high-end power equipment.
[0003] The power performance of semiconductor devices is positively correlated with the material's bandgap and carrier mobility. Among them, aluminum nitride (AlN) is a core material for ultra-wide bandgap semiconductors, possessing an ultra-wide bandgap of 6.2 eV and an ultra-high breakdown field strength of 15 MV / cm. A single AlN epitaxial structure can cover the needs of power grid applications across all voltage levels. Currently, AlN single-crystal growth, epitaxy, and device fabrication processes are relatively mature, giving it broad application prospects in high-power fields such as high-voltage power transmission, high-speed rail traction, and aerospace.
[0004] AlN material boasts an extremely high theoretical power factor (BFOM), making it an ideal material for next-generation high-voltage power devices. However, existing AlN devices generally suffer from a high on-resistance, severely limiting their performance and large-scale application. This problem stems from both intrinsic material defects and interfacial contact defects: on the one hand, the Si donor level in AlN is as high as 280 meV, and the high-doping process easily generates self-compensating defects; the electron concentration of existing MOCVD epitaxial AlN is only 10... 15 cm -3 The low carrier concentration leads to a high sheet resistance in the epitaxial film, making it difficult for the electrode and epitaxial film to form effective tunneling conductivity. On the other hand, the electron affinity of AlN is only 0.5~1.9 eV, far lower than the work function of conventional ohmic metals such as Ti / Al. This easily leads to a strong Schottky barrier at the metal-AlN interface, hindering efficient thermionic emission transport. Limited by this dual conductivity mechanism, the room-temperature ohmic contact resistivity of existing AlN devices is generally higher than 10⁻⁶ eV. -1 Ω·cm 2 Therefore, reducing the sheet resistance and ohmic contact resistance of AlN epitaxial films is the core key to overcoming the industrialization barriers of AlN power devices.
[0005] Currently, numerous technical studies have been conducted both domestically and internationally on optimizing AlN ohmic contacts. However, existing solutions struggle to balance process complexity, fabrication costs, and device performance, failing to meet the mass production demands of high-performance pure AlN power devices. Summary of the Invention
[0006] This application provides a semiconductor power device and its fabrication method. The fabrication method of the semiconductor power device can reduce the ohmic contact resistance and epitaxial layer sheet resistance of the device, and does not add any additional process steps. The process is simple and has a high fault tolerance.
[0007] To achieve the above objectives, this application provides the following technical solution: A method for fabricating a semiconductor power device, comprising: A buffer layer and an n-type contact layer are sequentially formed on a substrate. The buffer layer is made of aluminum nitride, and the n-type contact layer is made of aluminum nitride. The n-type contact layer includes a preset ohmic electrode region on the surface opposite to the substrate. An entire electrode stack is formed on the side of the n-type contact layer away from the buffer layer. The electrode stack includes an electrode thin layer, a metal stack, and a protective layer. The electrode thin layer is made of silicon. The metal stack is located on the side of the electrode thin layer away from the n-type contact layer. The protective layer is located on the side of the metal stack away from the electrode thin layer. The electrode stack is patterned, and the orthographic projection of the patterned electrode stack onto the n-type contact layer is located in the preset region of the ohmic electrode. The patterned electrode stack is subjected to rapid annealing, which causes some silicon atoms in the electrode thin layer to diffuse into the n-type contact layer. The electrode thin layer and the metal stack are mutually soluble to form an ohmic electrode, and the ohmic electrode is in ohmic contact with the n-type contact layer.
[0008] This application provides a semiconductor power device and its fabrication method. In the fabrication method of this semiconductor device, before forming the metal stack, a thin electrode layer made of silicon is first formed during the fabrication of the ohmic electrode. After annealing, the thin electrode layer dissolves with the metal stack to form the ohmic electrode. Furthermore, some silicon atoms in the annealed thin electrode layer diffuse into the n-type contact layer. The silicon atoms diffused into the n-type contact layer can increase the carrier concentration near the ohmic electrode, compress the barrier width between the ohmic electrode and the n-type contact layer, and enhance the electron tunneling effect, resulting in a lower ohmic contact resistance between the ohmic electrode and the n-type contact layer. The increased carrier concentration further reduces the sheet resistance of the epitaxial layer. Moreover, the above fabrication method only adds the process of forming a complete thin electrode layer. Compared with related technologies, it does not require additional photolithography and expensive ion implantation and ultra-high temperature annealing processes, nor does it require precise control of the AlGaN gradient layer concentration and Si doping concentration. It does not add any additional process steps, has a simple process with high fault tolerance, and does not require etching a thick AlGaN layer, making it easier to obtain better device performance. Attached Figure Description
[0009] Figure 1 This is a schematic diagram of the structure of an AlN device in related technologies; Figure 2 This is a schematic diagram of another AlN device in the related technology; Figure 3 A flowchart illustrating a method for fabricating a semiconductor power device, as provided in an embodiment of this application; Figures 4 to 6 A schematic diagram illustrating the fabrication state of a semiconductor power device provided in an embodiment of this application; Figure 7 This is a schematic diagram of an electrode stack structure provided in an embodiment of this application; Figure 8 A schematic diagram illustrating the fabrication state of a semiconductor power device provided in an embodiment of this application; Figure 9 Electron microscope images of electrode stack morphology before annealing provided in this application embodiment; Figure 10 STEM-EDS diagrams of element concentration distributions along the depth direction of the annealing front stack provided in this application embodiment; Figure 11 The morphology of the ohmic electrode under an electron microscope after annealing is provided for the embodiments of this application; Figure 12 STEM-EDS diagram of element concentration distribution along the stack depth direction after annealing, provided for embodiments of this application; Figure 13 This is a schematic diagram of the structure of a TLM device provided in an embodiment of this application; Figure 14 IV curves of the 21μm electrode spacing TLM configuration provided in the embodiments of this application after annealing at different annealing temperatures for 30s; Figure 15 IV curves of the 21μm electrode spacing TLM configuration provided in the embodiments of this application, annealed at 1100°C for different times; Figure 16 The ohmic contact resistivity and epitaxial sheet resistance of the TLM device structure with different electrode thicknesses provided in the embodiments of this application; Figures 17 to 20 A schematic diagram illustrating the fabrication state of a semiconductor power device provided in an embodiment of this application; Figure 21 A schematic diagram showing the distribution of the ohmic electrode and anode provided in an embodiment of this application; Figure 22 A comparison of forward IV curves of Schottky diode devices with different ohmic electrodes provided in the embodiments of this application; Figure 23 This is a schematic diagram of the structure of a semiconductor power device provided in an embodiment of this application. Detailed Implementation
[0010] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0011] In related technologies, AlN device structures can be as follows: Figure 1 As shown. The core process flow of this device is as follows: an insulating layer and photoresist pattern are fabricated on the AlN contact layer 011, an ion implantation window is formed, and Si ions are implanted in the contact region A of the AlN contact layer 011. The mixture is then annealed at 1300 °C for at least 4 min. The photoresist and insulating layer are removed, an insulating layer is deposited again, and an ohmic contact window is formed by photolithography. Titanium, aluminum, titanium, and gold layers are sputtered, with thicknesses of 15, 250, 50, and 150 nm respectively, forming the electrode layer 012. Finally, a second annealing is performed at 900 °C. This process improves the interfacial conductivity through ion doping modification, but it increases the number of process steps, requiring thin film deposition, photolithography, ion implantation, cleaning, and high-temperature heat treatment, resulting in a long fabrication cycle. The 1300 °C ultra-high temperature annealing places stringent requirements on the equipment, and ion implantation increases the process cost.
[0012] In another technical solution, the AlN device structure is as follows: Figure 2As shown in the diagram, this method involves sequentially epitaxially growing an 800 nm undoped AlN buffer layer (022) and a 500 nm Si-doped n-AlN functional layer (023) on a SiC substrate (021), followed by the growth of Si-doped Al... x Ga 1-x Gradient layer 024 of N, x The variation range decreased from 1 to 0.55. Combined with a Ti / Al / Ni / Au multilayer electrode 025, the ohmic contact resistivity of the AlN device was reduced to 1.4 × 10⁻⁶. -2 Ω·cm 2 This scheme utilizes the polarization effect to optimize the interfacial conductivity, but it has high process requirements: the concentration gradient of AlGaN in the gradient layer needs to change slowly, the process window for thickness and doping concentration is narrow, the growth parameters of different components are very different, high-temperature epitaxy is prone to causing Si thermal diffusion, and the process fault tolerance is low; at the same time, device fabrication requires etching to remove the AlGaN gradient layer in the channel region, and thick film etching is prone to damaging the underlying AlN channel, introducing defects and leakage channels, which in turn increases the on-resistance of the device.
[0013] To address the aforementioned technical problems, this application provides a method for fabricating a semiconductor power device, such as... Figure 3 As shown, it includes: S301: A buffer layer and an n-type contact layer are sequentially formed on the substrate. The material of the n-type contact layer is n-type doped aluminum nitride. The surface of the n-type contact layer facing away from the substrate includes a predetermined region for the ohmic electrode. Figure 4 As shown, a buffer layer 2 and an n-type contact layer 3 are formed on substrate 1. The substrate can be a sapphire substrate, the material of the buffer layer can be unintentionally doped aluminum nitride, and the material of the n-type contact layer is generally doped with silicon (Si) to provide free electrons.
[0014] S302: A full-layer electrode stack is formed on the side of the n-type contact layer away from the buffer layer. The electrode stack includes an electrode thin layer, a metal stack, and a protective layer. The electrode thin layer is made of silicon. The metal stack is located on the side of the electrode thin layer away from the n-type contact layer, and the protective layer is located on the side of the metal stack away from the electrode thin layer. Figure 6 and Figure 7 As shown, the electrode stack 40 may include an electrode thin layer 41, a metal stack 42 and a protective layer 43, and the metal stack 42 may include multiple film layers.
[0015] S303: Pattern the electrode stack, and the orthogonal projection of the patterned electrode stack onto the n-type contact layer is located in the preset region of the ohmic electrode.
[0016] S304: The patterned electrode stack is subjected to rapid annealing, causing some silicon atoms in the electrode thin layer to diffuse into the n-type contact layer. The electrode thin layer and the metal stack are intersoluble, forming an ohmic electrode, which then makes ohmic contact with the n-type contact layer. Figure 8As shown, the n-type contact layer can serve as an electron transport channel, and the ohmic electrode 4 is in ohmic contact with the n-type contact layer.
[0017] In the semiconductor power device fabrication method provided in this application embodiment, during the fabrication of the ohmic electrode, a thin electrode layer made of silicon is first formed before forming the metal stack. After annealing, the thin electrode layer dissolves with the metal stack to form the ohmic electrode. Furthermore, some silicon atoms in the annealed thin electrode layer diffuse into the n-type contact layer. The silicon atoms diffused into the n-type contact layer can increase the carrier concentration near the ohmic electrode, compress the barrier width between the ohmic electrode and the n-type contact layer, and enhance the electron tunneling effect. This results in a lower ohmic contact resistance between the ohmic electrode and the n-type contact layer, and the increased carrier concentration further reduces the sheet resistance of the epitaxial layer (n-type contact layer). Moreover, the above fabrication method only adds the process of forming a complete thin electrode layer. Compared with related technologies, it does not require additional photolithography and expensive ion implantation and ultra-high temperature annealing processes, nor does it require precise control of the gradient layer concentration and Si doping concentration. It does not add any additional process steps, is simple in process, has high fault tolerance, and does not require etching the AlGaN layer, making it easier to obtain better device performance.
[0018] In this embodiment, step S301 involves sequentially forming a buffer layer and an n-type contact layer on the substrate. Specifically, this involves epitaxially forming the buffer layer and the n-type contact layer on the substrate to form an epitaxial wafer. After forming the epitaxial wafer, it can be sequentially cleaned with an organic solution and buffered oxide etching (BOE) cleaning. The organic solution cleaning process can be as follows: ultrasonically cleaning the epitaxial wafer surface with acetone for 10-20 minutes to remove contaminants, ultrasonically cleaning the epitaxial wafer with isopropanol for 3-6 minutes to remove acetone residue, and finally rinsing with deionized water to remove isopropanol residue and drying with nitrogen. After organic solution cleaning, buffered oxide etching (BOE) solution can be used to remove self-oxides on the epitaxial layer surface for 1-4 minutes, followed by rinsing with deionized water for 2 minutes and drying.
[0019] In this embodiment, before forming a full-layer electrode stack on the side of the n-type contact layer away from the buffer layer, the specific steps may include: forming a groove on the side of the n-type contact layer away from the substrate, the groove being located in the first contact region. After the ohmic electrode is subsequently formed, the ohmic electrode can contact the n-type contact layer through the groove. Specifically, the steps for forming the groove may be: first, forming a first photoresist layer on the n-type contact layer of the epitaxial wafer; then, exposing and developing the first photoresist layer using a first mask; then, etching the n-type contact layer in the developed region to form the groove 31 on the n-type contact layer, such as... Figure 5As shown; then, the first photoresist layer is removed. This can be done by cleaning with N-methylpyrrolidone (NMP) or acetone for 10-20 minutes, followed by a dry stripper to remove all remaining first photoresist layers. Before forming the metal stack, the epitaxial wafer can be further cleaned using BOE cleaning for 1-3 minutes to remove the self-oxidizing layer on the epitaxial wafer surface and then dried.
[0020] In this embodiment, the metal stack in the electrode stack can be a gold-free (Au) stack. In related technologies, the stack forming the cathode is generally a Ti / Al / Ni / Au metal stack; however, Au material is relatively expensive and can contaminate semiconductor process lines, making it incompatible with them. Using a gold-free stack in the metal stack can save costs and ensure compatibility with semiconductor process lines.
[0021] Specifically, the metal stack includes a titanium (Ti) layer, an aluminum (Al) layer, and a titanium (Ti) layer stacked sequentially along a first direction; or, the metal stack includes a titanium (Ti), aluminum (Al), and nickel (Ni) layer stacked sequentially along the first direction; or, the metal stack includes a vanadium (V) layer, an aluminum (Al), and a nickel (Ni) layer stacked sequentially along the first direction; or, the metal stack includes a vanadium (V) layer, an aluminum (Al), and a vanadium (V) layer stacked sequentially along the first direction; or, the metal stack includes a zirconium (Zr) layer, an aluminum (Al), and a nickel (Ni) layer stacked sequentially along the first direction; or, the metal stack includes a zirconium (Zr) layer, an aluminum (Al), and a molybdenum (Mo) layer stacked sequentially along the first direction; the first direction is the direction from the substrate to the buffer layer.
[0022] In this embodiment, the protective layer in the electrode stack can be made of titanium nitride. After annealing, titanium nitride maintains a clear metal layer interface, exhibits high stability, and effectively protects the ohmic electrode. In the prior art, Au is generally used to protect the cathode. Compared to the prior art, the protective layer provided in this embodiment is more cost-effective, saves costs, does not contaminate the semiconductor process line, and is compatible with the semiconductor process line.
[0023] In this embodiment, the thickness of the electrode thin layer can be from 0.5 nm to 6 nm, and the thickness of the protective layer can be from 50 nm to 100 nm.
[0024] Specifically, in step S302, a complete electrode stack is formed on the side of the n-type contact layer away from the buffer layer. This can be achieved using a magnetron sputtering machine with multiple target sites, sequentially forming a thin electrode layer, a metal stack, and a protective layer on the n-type contact layer. Taking a metal stack consisting of sequentially stacked Ti, Al, and Ti layers as an example, the magnetron sputtering machine is equipped with metal targets such as Si, Ti, and Al. By controlling the sputtering time of different targets, an electrode stack including a thin electrode layer, a metal stack, and a protective layer is prepared. The patterned structure of the electrode stack can be a Si / Ti / Al / Ti / TiN stack. The Ti layer in the middle of the stack can be replaced with a metal layer such as a V layer or a Zr layer, with corresponding target additions. The protective layer can be obtained by sputtering Ti metal reacting with N2.
[0025] In this embodiment, the patterning of the electrode stack in step S303 may specifically include the following steps: First, a second photoresist layer is formed on the electrode stack; then, the second photoresist layer is exposed and developed using a second mask to expose the metal stack except for the preset area of the ohmic electrode; then, metal etching is used to remove the metal stack and electrode thin layer in the area outside the preset area of the ohmic electrode. Finally, the second photoresist layer is removed.
[0026] In this embodiment of the application, the annealing temperature of the rapid annealing process in step S304 can be from 650°C to 1100°C, and the annealing time can be from 30s to 90s.
[0027] Specifically, the prepared device can be annealed using a rapid annealing furnace (RTP), which can promote ohmic contact between the ohmic electrode and the n-type contact layer.
[0028] In the embodiments of this application, Figure 9 The image shows the morphology of the electrode stack under an electron microscope before annealing, as provided in the embodiments of this application. The yellow line is the EDS line scanning trajectory. The metal stack 42 in the electrode stack is a stack of Ti layer, Al layer and Ti layer. Figure 10 STEM-EDS images of element concentration distribution along the depth direction of the annealing front stack provided in this application embodiment. Figure 10 Color images are used, with different colors corresponding to different elements, which cannot be distinguished in grayscale images. The stacking depth direction is from the n-type contact layer 3 to the protective layer 43. Figure 10 The x-coordinate of the curve and Figure 9 The spatial positions of the scan paths in the topographic map show a mapping correspondence. Figure 9 and Figure 10 It can be seen that STEM-EDS (surface scan / line scan) before annealing can characterize the elemental distribution of each layer of the electrode stack with clear boundaries and no mixing. Figure 11 The image shows the morphology of the ohmic electrode under an electron microscope after annealing, as provided in the embodiments of this application. The yellow line represents the EDS line scanning trajectory. Figure 12 STEM-EDS images of element concentration distribution along the stack depth direction after annealing, provided for embodiments of this application. Figure 12 Color images are used, with different colors corresponding to different elements, which cannot be distinguished in grayscale images. Figure 12 The x-coordinate of the curve and Figure 11 The spatial positions of the scan paths in the topographic map show a mapping correspondence. Figure 11 and Figure 12 It can be seen that after high-temperature annealing, the electrode thin layer 41 and the metal stack 42 become mutually soluble, forming the ohmic electrode 4. Silicon atoms in the electrode thin layer can diffuse into the n-type contact layer. Si concentrations distributed with depth were detected in the mutually soluble film layer, with stoichiometry between 1% and 2%. Based on SEM and EDS analysis, the total Si concentration by weight in the ohmic electrode 4 can reach over 5%. The protective layer 43 still retains a relatively clear metal layer interface. High-oxygen-content Al-OC and Al-Ti-NOC self-oxidation layers appear above and below the protective layer 43. The thickness of the surface protective layer 43 remains essentially unchanged. EDS analysis shows that this layer incorporates C and O elements after annealing, with atomic percentages generally below 20%. The protective layer 43 exhibits high stability and can protect the underlying structure.
[0029] The semiconductor power device fabrication method provided in the above embodiments can be used to fabricate TLM devices and partial films of Schottky diode (SBD) devices. The TLM device is a transmission line device structure used to measure ohmic contact resistance and epitaxial layer sheet resistance.
[0030] In the embodiments of this application, the structure of the fabricated TLM device 100 is as follows: Figure 13 As shown, a set of ohmic electrodes 4 of the same size and with varying spacing are fabricated on the same platform. The thicknesses of the Si layer (electrode thin layer), Ti layer, Al layer, Ti layer and TiN layer (protective layer) in the ohmic electrodes of the TLM device 100 before annealing can be 0.85 nm, 16.8 nm, 112 nm, 18.0 nm and 53.6 nm, respectively. Figure 14 IV curves for a TLM configuration with a 21 μm electrode spacing after annealing at different annealing temperatures for 30 s are shown. Figure 14Color images were used, with different colors corresponding to different annealing temperatures, which cannot be distinguished in grayscale images. The study found that as the temperature increases, the current increases sequentially at the same voltage, and the corresponding resistance decreases sequentially. For example, when annealed at 650 °C with a 21 μm electrode spacing and a voltage of 30 V, the calculated resistance is 0.981 MΩ. When annealed at 1100 °C for 30 s with the same 21 μm electrode spacing and 30 V, the calculated resistance decreases to 0.389 MΩ. Since the on-resistance is lowest under annealing at 1100 °C, this application further verified the resistance at different annealing times at 1100 °C, such as... Figure 15 As shown, Figure 15 IV curves for different annealing times at an annealing temperature of 1100 °C are shown. Figure 15 Color images are used, with different colors corresponding to different annealing times, which cannot be distinguished by grayscale images. Figure 15 The annealing time ranged from 15 s to 90 s, and it was found that the on-resistance of the device was better in the range of 25 s to 45 s, and the resistance was the lowest in the range of 30 s.
[0031] Furthermore, embodiments of this application compared test data for devices without an electrode thin layer (Si layer) and with electrode thin layers (Si layers) of different thicknesses. The sputtering times of the Si target were adjusted during the fabrication of the ohmic electrode to be 0 s, 30 s, 60 s, and 90 s, respectively. The Si layer thickness measured after 30 s sputtering was 0.85 nm, and the Si layer thickness corresponding to 90 s sputtering was 5.67 nm. Figure 16 As shown, the ohmic contact resistivity ρ corresponds to devices with different Si layer thicknesses. c and epitaxial layer sheet resistance R sh The graph shows the resistivity of the ohmic contact and the sheet resistance of the epitaxial layer, represented by dots and star-shaped dots. After annealing at 1100 °C for 30 s, the device, without a Si layer, yielded an ohmic contact resistivity and an epitaxial layer sheet resistance of 0.237 Ω. cm 2 The value was 1.88 MΩ / □, but after adding a 0.85 nm thick Si layer, the corresponding value decreased to 0.0428 Ω. cm -2 The on-resistivity is 0.435 MΩ / □, corresponding to the lowest on-resistivity. Further increasing the Si layer thickness still significantly improves the on-resistivity compared to devices without a Si layer, but it is slightly higher than when the Si layer thickness is 0.85 nm. At a Si layer thickness of 5.67 nm, the ohmic contact resistivity and epitaxial sheet resistance of the corresponding device are 0.085 Ω. cm 2 And 0.584 MΩ / □.
[0032] Experimental verification shows that the semiconductor power device fabrication method provided in this application reduces the ohmic contact resistance and epitaxial layer sheet resistance of the semiconductor device, with the ohmic contact resistivity reduced to 0.043 Ω. cm 2 Up to 0.086 Ω cm 2 The introduction of the electrode thin layer can reduce the sheet resistance of the epitaxial layer of the device from 1.88 MΩ / □ to 0.43 MΩ / □. Compared with the n-type contact layer directly contacting the metal stack, the Schottky diode device fabricated by the method of this application has lower turn-on voltage and on-resistance, and does not increase the device fabrication steps.
[0033] In this embodiment, the semiconductor power device can be a Schottky diode. The aforementioned ohmic electrode can be the cathode of the Schottky diode. Specifically, in this embodiment, after the rapid annealing process in step S304 during the fabrication of the Schottky diode, the specific steps may include: First: An insulating layer 5 is formed on the side of the ohmic electrode 4 facing away from the substrate 1, such as... Figure 17 As shown; the material of insulating layer 5 can be SiN, and the thickness of insulating layer can be 40 nm to 60 nm.
[0034] Then: the insulating layer 5 is patterned to form through holes 51, such as... Figure 18 As shown.
[0035] Finally: An anode 6 is formed on the side of the insulating layer 5 opposite to the n-type contact layer 3. The anode 6 forms a Schottky contact with the n-type contact layer 3 through the through-hole 51, such as... Figure 19 As shown. On the insulating layer 5, the anode 6 can be a stack of Ni layer, Ti layer and Al layer. The thickness of Ni layer can be 50 nm to 100 nm, the thickness of Ti layer can be 20 nm, and the thickness of Al layer can be 100 nm to 150 nm.
[0036] In this embodiment, step S306 involves etching the insulating layer. Specifically, this process may include: first, forming a third photoresist layer on the insulating layer; then, exposing and developing the third photoresist layer using a third mask to expose the insulating layer on the anode preset area; next, etching the insulating layer to expose the surface of the n-type contact layer, forming vias. Finally, the epitaxial wafer is subjected to NMP cleaning for 10-20 minutes, and the third photoresist layer is removed using a dry photoresist stripper.
[0037] In this embodiment of the application, in S307, an anode is formed on the side of the insulating layer away from the n-type contact layer. The specific steps may include: first, forming a fourth photoresist layer on the insulating layer, exposing and developing the fourth photoresist layer through a fourth mask to expose the anode preset area; then, forming the anode by electron beam evaporation; then, immersing in acetone for about 15 to 30 minutes, and rinsing with isopropanol to remove excess metal outside the anode area to obtain the anode.
[0038] In this embodiment, the semiconductor power device may include at least one repeating unit, and each repeating unit may include a substrate, a buffer layer, an n-type contact layer, an ohmic electrode, an insulating layer, and an anode. When the semiconductor power device includes multiple repeating units, the substrate may include multiple spaced-apart unit partitions, with one repeating unit disposed on each unit partition. During the fabrication of the semiconductor power device, to ensure insulation between each repeating unit, after the anode is formed, the insulating layer and the n-type contact layer located between two adjacent unit partitions can be etched to electrically isolate each repeating unit, such as... Figure 20 As shown.
[0039] In the embodiments of this application, such as Figure 21 The diagram shown is a schematic representation of the distribution structure of the anode 6 and the ohmic electrode 4 in a Schottky diode according to an embodiment of this application. The ohmic electrode 4 can be arranged around the anode 6, and the orthogonal projection of the anode 6 on the substrate is spaced apart from the orthogonal projection of the ohmic electrode 4 on the substrate. The anode 6 and the ohmic electrode are insulated from each other. A cross-sectional view of the above Schottky diode can be shown as follows... Figure 20 As shown.
[0040] Specifically, to verify the performance of the fabricated semiconductor power device, this embodiment compares the performance of Schottky diodes with different ohmic electrodes. For example... Figure 22 The figure shows a comparison of the forward IV curves of Schottky diode devices based on two types of ohmic electrodes: Ti / Al / Ti / TiN stacked layers and Si / Ti / Al / Ti / TiN stacked layers. Figure 22 As can be seen, compared to using an ohmic electrode formed by annealing a Ti / Al / Ti / TiN stack, the turn-on voltage of the SBD device can be reduced to below 2 V using an ohmic electrode formed by annealing a Si / Ti / Al / Ti / TiN stack, while the turn-on voltage of the SBD device with the corresponding ohmic electrode formed by annealing a Ti / Al / Ti / TiN stack is approximately 4 V. Furthermore, improving the ohmic electrode with a Si layer significantly increases the device's forward conduction current, demonstrating the crucial role of the Si layer in enhancing the device's maximum power characteristics.
[0041] This application also includes a semiconductor power device, fabricated using any of the fabrication methods provided by the above-described technical solutions, such as... Figure 23As shown, the semiconductor power device includes: Substrate 1; Buffer layer 2 is located on one side of substrate 1; The n-type contact layer 3 is located on the side of the buffer layer 2 away from the substrate 1; Ohmic electrode 4 is located on the side of n-type contact layer 3 away from buffer layer 2. Ohmic electrode 4 includes a mutual dissolution part and a protective layer located on the side of the mutual dissolution part away from n-type contact layer. The mutual dissolution part is formed by mutual dissolution of electrode thin layer 41 and metal stack 42 located on the side of electrode thin layer 41 away from n-type contact layer 3. The material of electrode thin layer 41 is silicon. Ohmic electrode 4 is in ohmic contact with n-type contact layer 3.
[0042] In the semiconductor power device provided in this application embodiment, the ohmic electrode 4 includes a mutual soluble portion, which is formed by the mutual soluble portion of the electrode thin layer 41 and the metal stack 42 located on the side of the electrode thin layer 41 away from the n-type contact layer 3. The material of the electrode thin layer 41 is silicon. After silicon annealing, it can diffuse into the n-type contact layer, increase the carrier concentration near the ohmic contact electrode, thereby reducing the interface barrier width between the ohmic electrode 4 and the n-type contact layer 3, enhancing the electron tunneling effect, and obtaining a lower ohmic contact resistance between the ohmic electrode 4 and the n-type contact layer 3. The increased carrier concentration further reduces the sheet resistance of the epitaxial layer.
[0043] In this embodiment, the silicon concentration in the ohmic electrode is greater than or equal to 5% by weight, which can better improve the carrier concentration in the first contact region of the n-type contact layer 3.
[0044] Specifically, the protective layer can be made of titanium nitride. After annealing, the protective layer maintains a clear metal interface, exhibits high stability, and effectively protects the ohmic electrode.
[0045] In this embodiment of the application, the semiconductor power device further includes an insulating layer 5 and an anode 6. The insulating layer 5 is located on the side of the ohmic electrode 4 away from the n-type contact layer 3. The insulating layer 5 has a through hole. The anode 6 is located on the side of the insulating layer 5 away from the n-type contact layer 3. The anode 6 is in Schottky contact with the n-type contact layer 3 through the through hole.
[0046] In the aforementioned semiconductor power device, unidirectional rectification is achieved by relying on the Schottky barrier formed between the anode 6 and the n-type contact layer 3. Under forward bias, a positive potential is applied to the anode 6 and a negative potential is applied to the ohmic electrode 4. When the applied voltage exceeds the built-in barrier, electrons are injected from the cathode into the n-type contact layer 3. Electrons are laterally transported to the anode 6 in the n-type contact layer 3, forming a forward conducting current. The buffer layer 2 is a high-resistivity layer that does not participate in conduction and isolates the substrate. Under reverse bias, a negative potential is applied to the anode 6, and the depletion region generated at the Schottky interface extends laterally towards the ohmic electrode 4. The reverse voltage is mainly borne by the depleted n-type contact layer 3, achieving voltage blocking. The buffer layer can suppress parasitic leakage current in the substrate direction.
[0047] Specifically, the above-mentioned ohmic electrode scheme can be widely used in various power and optoelectronic devices such as AlN high electron mobility transistors, AlN light-controlled switches, MOSFETs, AlN lasers, photodetectors, and LEDs.
[0048] Obviously, those skilled in the art can make various modifications and variations to the embodiments of this application without departing from the spirit and scope of this application. Therefore, if these modifications and variations of this application fall within the scope of the claims of this application and their equivalents, this application also intends to include these modifications and variations.
Claims
1. A method for fabricating a semiconductor power device, characterized in that, include: A buffer layer and an n-type contact layer are sequentially formed on a substrate. The material of the n-type contact layer is n-type doped aluminum nitride. The surface of the n-type contact layer opposite to the substrate includes a preset region of ohmic electrodes. An entire electrode stack is formed on the side of the n-type contact layer away from the buffer layer. The electrode stack includes an electrode thin layer, a metal stack, and a protective layer. The electrode thin layer is made of silicon. The metal stack is located on the side of the electrode thin layer away from the n-type contact layer. The protective layer is located on the side of the metal stack away from the electrode thin layer. The electrode stack is patterned, and the orthographic projection of the patterned electrode stack onto the n-type contact layer is located in the preset region of the ohmic electrode. The patterned electrode stack is subjected to rapid annealing, which causes some silicon atoms in the electrode thin layer to diffuse into the n-type contact layer. The electrode thin layer and the metal stack are mutually soluble to form an ohmic electrode, and the ohmic electrode is in ohmic contact with the n-type contact layer.
2. The preparation method according to claim 1, characterized in that, The thickness of the electrode thin layer is from 0.5 nm to 6 nm.
3. The preparation method according to claim 1, characterized in that, The metal stack comprises a titanium layer, an aluminum layer, and a titanium layer stacked sequentially along a first direction; or, The metal stack comprises layers of titanium, aluminum, and nickel stacked sequentially along a first direction; or, The metal stack comprises a vanadium layer, an aluminum layer, and a nickel layer stacked sequentially along a first direction; or, The metal stack comprises a vanadium layer, an aluminum layer, and a vanadium layer stacked sequentially along a first direction; or, The metal stack comprises a zirconium layer, an aluminum layer, and a nickel layer stacked sequentially along a first direction; or, The metal stack includes a zirconium layer, an aluminum layer, and a molybdenum layer stacked sequentially along a first direction; the first direction is the direction from the substrate to the buffer layer.
4. The preparation method according to claim 1, characterized in that, The protective layer is made of titanium nitride.
5. The preparation method according to claim 4, characterized in that, The thickness of the protective layer is 50 nm to 100 nm.
6. The preparation method according to claim 4, characterized in that, The rapid annealing process is carried out at an annealing temperature of 650°C to 1100°C and an annealing time of 30s to 90s.
7. The preparation method according to claim 1, characterized in that, Before forming a complete electrode stack on the side of the n-type contact layer opposite to the buffer layer, the process includes: A groove is formed on the side of the n-type contact layer opposite to the substrate, and the ohmic electrode contacts the n-type contact layer through the groove.
8. The preparation method according to any one of claims 1-7, characterized in that, After forming the ohmic electrode, the process includes: An insulating layer is formed on the side of the ohmic electrode opposite to the substrate; The insulating layer is etched to form through holes; An anode is formed on the side of the insulating layer opposite to the n-type contact layer, and the anode forms a Schottky contact with the n-type contact layer through the through-hole.
9. A semiconductor power device, characterized in that, The semiconductor power device is prepared by the preparation method according to any one of claims 1-8, and comprises: Substrate; A buffer layer is located on one side of the substrate, and the material of the buffer layer is aluminum nitride; An n-type contact layer is located on the side of the buffer layer away from the substrate, and the material of the n-type contact layer is aluminum nitride; An ohmic electrode is located on the side of the n-type contact layer away from the buffer layer. The ohmic electrode includes a mutually soluble portion and a protective layer located on the side of the mutually soluble portion away from the n-type contact layer. The mutually soluble portion is formed by the mutual fusion of an electrode thin layer and a metal stack located on the side of the electrode thin layer away from the n-type contact layer. The material of the electrode thin layer is silicon. The ohmic electrode is in ohmic contact with the n-type contact layer.
10. The semiconductor power device according to claim 9, characterized in that, The silicon concentration in the ohmic electrode is greater than or equal to 5% by weight.
11. The semiconductor power device according to claim 9, characterized in that, The protective layer is made of titanium nitride.
12. The semiconductor power device according to any one of claims 9-11, characterized in that, The semiconductor power device further includes an insulating layer and an anode. The insulating layer is located on the side of the ohmic electrode opposite to the n-type contact layer. The insulating layer has a through-hole. The anode is located on the side of the insulating layer opposite to the n-type contact layer. The anode makes Schottky contact with the n-type contact layer through the through-hole.