Fully Finned GaN-based P-type Multichannel Device with High On-current and its Fabrication Method

By using a fully finned GaN-based P-type multi-channel device structure, and utilizing an N-type heavily doped layer to form a tunnel junction and a fully finned array structure, the problems of ohmic contact and gate control capability of GaN-based P-type channel devices are solved, achieving high on-current and low-cost device design.

CN123076002APending Publication Date: 2026-11-10XIDIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611167822.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-03
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

GaN-based P-channel devices have lower drive capability than N-channel devices, making it difficult to form effective ohmic contacts, which limits the improvement of high conduction current. Furthermore, existing multi-channel structures are difficult to achieve efficient ohmic contacts and gate control capabilities, resulting in increased chip area and cost.

Method used

A fully finned GaN-based P-type multi-channel device structure is adopted. Two-dimensional hole gas channels are formed in the P-type multi-channel epitaxial structure, and tunnel junctions are formed using N-type heavily doped layers. Combined with the fully finned array structure, sidewall contacts of multiple two-dimensional hole gas channels are realized, thereby improving ohmic contact efficiency and gate control capability.

Benefits of technology

It significantly improves the on-current of P-channel devices, reduces the layout area and cost of P-channel devices, achieves driving capability matching between P-type and N-type devices, and simplifies the monolithic integration process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076002A_ABST
    Figure CN123076002A_ABST
Patent Text Reader

Abstract

This invention discloses a fully finned GaN-based P-type multichannel device with high on-current and its fabrication method, comprising: a substrate and a buffer layer on the substrate; a P-type multichannel epitaxial structure located on the buffer layer; a fully finned array structure penetrating the source, gate, and drain regions of the P-type multichannel epitaxial structure to the bottom barrier layer of the P-type multichannel epitaxial structure, dividing it into multiple sub-P-type multichannel epitaxial structures; an N-type heavily doped layer located on the surface and sidewalls of the sub-P-type multichannel epitaxial structures in the source and drain regions, and on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures; source and drain electrodes located on the N-type heavily doped layer in the source and drain regions; a gate dielectric layer located on the surface and sidewalls of the sub-P-type multichannel epitaxial structures between the source and drain regions, and on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures; a gate electrode located on the gate dielectric layer in the gate region; and the width of the finned structure in the source and drain regions being greater than the width of the finned structure in the gate region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor device technology, specifically relating to a fully finned GaN-based P-type multichannel device with high conduction current and its fabrication method. Background Technology

[0002] Gallium nitride (GaN), a wide-bandgap semiconductor material, has been widely used in power switches and power electronic devices due to its advantages such as large bandgap, high critical breakdown electric field, and high electron saturation velocity. In digital circuit applications, using GaN-based CMOS technology as a logic control module can effectively reduce system power consumption and improve operating efficiency. This structure consists of logic-complementary N-channel and P-channel devices. However, currently, the driving capability of P-channel devices in GaN-based CMOS technology is far lower than that of N-channel devices, severely limiting the overall performance of GaN-based CMOS circuits.

[0003] In high-power, high-frequency applications, GaN HEMTs, as core components, require peripheral circuitry to implement functions such as driving, control, sensing, and protection. Existing technologies primarily employ three logic control schemes for GaN devices: heterogeneous packaging with silicon-based CMOS, GaN E (enhancement-mode) / D (depletion-mode) integration using all N-channel devices, and GaN-based CMOS solutions. Among these, the heterogeneous packaging with silicon-based CMOS suffers from significant parasitic effects between modules, making it difficult to fully leverage the performance advantages of GaN devices. The GaN E / D integration scheme exhibits high static power consumption due to its non-complementary logic. Therefore, GaN-based CMOS technology, with its low power consumption and low parasitic characteristics, shows great application potential in the logic control of GaN HEMTs.

[0004] Due to technical challenges such as low intrinsic hole mobility, high magnesium acceptor activation energy, and difficulty in forming effective ohmic contacts, the driving capability of GaN-based P-channel devices has consistently lagged behind that of N-channel devices. Current methods for increasing P-channel current density mainly involve increasing the thickness of the P-type material, using epitaxial structures with strong polarization effects (such as P-GaN / AlN and P-InGaN / P-GaN), and multi-channel structures. However, when increasing the hole density by increasing the P-type material thickness and enhancing the heterojunction polarization effect, the already extremely low hole mobility further decreases with increasing hole density, thus offsetting the improvement in the conduction current of P-channel devices. While multi-channel structures can decouple hole density and mobility by distributing two-dimensional hole gas in multiple channels, offering a potentially effective solution for high current density P-channel devices, existing research struggles to achieve efficient ohmic contacts with multiple channels simultaneously, limiting the full realization of the advantages of P-type multi-channel structures in improving conduction current. Furthermore, the requirements of GaN-based CMOS structures for enhancement-mode operation place higher demands on gate control of P-type multi-channel devices. The gate control capability and switching characteristics of multi-channel devices in existing research still need to be further improved.

[0005] Due to the high activation energy of magnesium impurities and the difficulty in finding metals with sufficiently high work functions to form an anti-blocking layer, P-type GaN has consistently struggled to form effective ohmic contacts. This has become one of the key bottlenecks restricting the development of high-current P-type channel devices. Furthermore, to reduce power consumption in applications, gate control capability often faces greater challenges for P-type channel devices with high current. Currently, to achieve a matching of driving capabilities between N-type and P-type channel devices in GaN-based complementary logic, the layout area of ​​the P-type channel device needs to be much larger than that of the N-type channel device, leading to increased chip area and cost. Summary of the Invention

[0006] To address the aforementioned problems in the prior art, this invention provides a fully finned GaN-based P-type multichannel device with high on-current and its fabrication method. In a first aspect, embodiments of the present invention provide a fully finned GaN-based P-type multichannel device with high on-current, the fully finned GaN-based P-type multichannel device comprising: Substrate, and a buffer layer located on the substrate; The P-type multi-channel epitaxial structure is located on the buffer layer. The P-type multi-channel epitaxial structure is composed of N P-type barrier layers and N P-type channel layers stacked alternately from bottom to top, where N≥2. A two-dimensional cavitation channel is formed between each P-type channel layer and the adjacent P-type barrier layer. The full-fin array structure extends through the source, gate, and drain regions of the P-type multi-channel epitaxial structure, all the way to the bottom barrier layer of the P-type multi-channel epitaxial structure, in order to divide the P-type multi-channel epitaxial structure into multiple sub-P-type multi-channel epitaxial structures. The N-type heavily doped layer is located on the surface and sidewalls of each sub-P-type multichannel epitaxial structure in the source and drain regions, as well as on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures; the N-type heavily doped layer and the P-type channel layer form a tunnel junction. The source electrode and drain electrode are located on the heavily doped N-type layers in the source region and drain region, respectively. The gate dielectric layer, the surface and sidewalls of each sub-P-type multichannel epitaxial structure between the source and drain regions, and the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures; The gate electrode is located on the gate dielectric layer in the gate region; In the full fin array structure, the width of the fin structure in the source and drain regions is greater than the width of the fin structure in the gate region.

[0007] In one embodiment of the present invention, each P-type barrier layer is made of a group III nitride material, has a thickness of 5 nm to 20 nm, is doped with Mg, and has a doping concentration of 5 × 10¹. 8 cm -3 ~5×10¹ 9 cm -3 .

[0008] In one embodiment of the present invention, each P-type channel layer is made of a group III nitride material with a band gap smaller than that of the P-type barrier layer, has a thickness of 3 nm to 20 nm, is doped with Mg, and has a doping concentration of 5 × 10¹. 8 cm -3 ~5×10¹ 9 cm -3 .

[0009] In one embodiment of the present invention, the N-type heavily doped layer is made of either InGaN or GaN, has a thickness of 10 nm to 30 nm, is doped with Si, and has a doping concentration of 5 × 10¹. 9 cm -3 ~5×10² 0 cm -3 .

[0010] In one embodiment of the present invention, the width of the fin structure in the source region and the drain region is 300nm~500nm.

[0011] In one embodiment of the present invention, the width of the fin structure in the gate region is 10nm~200nm.

[0012] In one embodiment of the present invention, the all-fin GaN-based P-type multichannel device further includes: An N-type channel epitaxial structure is located between a buffer layer and a P-type multi-channel epitaxial structure, used for co-integration of GaN-based N-type channel devices. The N-type channel epitaxial structure is composed of M N-type channel layers and M N-type barrier layers stacked alternately from bottom to top, where M≥1.

[0013] In one embodiment of the present invention, each N-type channel layer is made of unintentionally doped GaN material with a thickness of 10 nm to 300 nm.

[0014] In one embodiment of the present invention, each N-type barrier layer material is one of unintentionally doped AlGaN, InAlN, and AlN, with a thickness of 5nm to 20nm.

[0015] Secondly, embodiments of the present invention provide a method for fabricating a fully finned GaN-based P-type multi-channel device with high conduction current, used for fabricating any of the fully finned GaN-based P-type multi-channel devices with high conduction current described in the first aspect, the corresponding fabrication method including: Obtain a substrate and grow a buffer layer on the substrate; A P-type multi-channel epitaxial structure is grown on a buffer layer. The P-type multi-channel epitaxial structure is composed of N P-type barrier layers and N P-type channel layers stacked alternately from bottom to top, where N≥2. A two-dimensional hole gas channel is formed between each P-type channel layer and the adjacent P-type barrier layer. Etch the P-type multi-channel epitaxial structure until it reaches the bottom barrier layer of the P-type multi-channel epitaxial structure, divide the P-type multi-channel epitaxial structure into multiple sub-P-type multi-channel epitaxial structures, and form a full fin array structure that runs through the source region, gate region and drain region. N-type heavily doped layers are grown on the surface and sidewalls of each sub-P-type multichannel epitaxial structure, as well as on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures. The N-type heavily doped layer on the surface of each sub-P-type multi-channel epitaxial structure in the gate region and the barrier layer surface between adjacent sub-P-type multi-channel epitaxial structures is etched away, and the etching of each sub-P-type multi-channel epitaxial structure in the gate region continues until the bottom barrier layer is reached, so that in the full fin array structure, the width of the fin structure in the gate region is smaller than the width of the fin structure in the source region and the drain region; wherein, during the etching of the fin structure in the gate region, the N-type heavily doped layer on the sidewall of each sub-P-type multi-channel epitaxial structure is simultaneously etched away. Ohmic metal is deposited on the N-type heavily doped layers in the source and drain regions to form the source and drain electrodes. A gate dielectric layer is grown on the surface and sidewalls of each sub-P-type multichannel epitaxial structure between the source and drain regions, and on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures. Gate metal is deposited on the gate dielectric layer in the gate region to form the gate electrode.

[0016] The beneficial effects of this invention are: This invention proposes a fully finned GaN-based P-type multi-channel device with high on-current. It employs a high-conductivity P-type multi-channel structure, distributing the hole density across multiple two-dimensional hole gas channels. This removes the mutual constraint between hole mobility and hole density, significantly improving the on-current of the P-type channel device. The heavily N-type doped layers in the source / drain regions form a tunnel junction with the P-type channel layer of the P-type channel device itself, transforming the ohmic contact of the P-type material into a contact with the tunnel junction. This solves the problem of finding metals with sufficiently high work functions in the ohmic contact of P-type materials. Simultaneously, the fully finned array structure allows the ohmic metal to simultaneously achieve sidewall contact with multiple two-dimensional hole gas channels, further improving ohmic contact efficiency. By controlling the width of the finned structure in the gate region, this invention enables both the top gate and sidewall gate to simultaneously deplete the holes in the finned structure, thereby improving the device's gate control capability and achieving enhancement-mode operation of the gallium nitride-based P-type multi-channel device. Because the P-type multi-channel device provided by this invention has high on-current characteristics, it can promote the matching of driving capabilities between P-type and N-type devices in gallium nitride-based complementary logic applications, significantly reducing the layout area of ​​P-type channel devices, thereby reducing circuit area and cost. The tunneling junction ohmic contact process in this invention is compatible with the ohmic contact process of N-type channel devices in gallium nitride-based complementary metal-oxide-semiconductor technology, which can reduce manufacturing costs and process complexity, and facilitate the monolithic integration of P-type and N-type channel devices.

[0017] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of the structure of a fully finned GaN-based P-type multichannel device with high on-current provided in an embodiment of the present invention; Figure 2 This is a schematic flowchart of a method for fabricating a fully finned GaN-based P-type multichannel device with high on-current provided in an embodiment of the present invention. Figures 3(a)~3(k) This is a schematic diagram of the fabrication process of a fully finned GaN-based P-type multichannel device with high conduction current provided in an embodiment of the present invention. Detailed Implementation

[0019] The present invention will be further described in detail below with reference to specific embodiments, but the implementation of the present invention is not limited thereto.

[0020] Firstly, please see Figure 1 This invention provides a fully finned GaN-based P-type multichannel device with high on-current, the fully finned GaN-based P-type multichannel device comprising: Substrate, and a buffer layer located on the substrate; The P-type multi-channel epitaxial structure is located on the buffer layer. The P-type multi-channel epitaxial structure is composed of N P-type barrier layers and N P-type channel layers stacked alternately from bottom to top, where N≥2. A two-dimensional cavitation channel is formed between each P-type channel layer and the adjacent P-type barrier layer. The full-fin array structure extends through the source, gate, and drain regions of the P-type multi-channel epitaxial structure, all the way to the bottom barrier layer of the P-type multi-channel epitaxial structure, in order to divide the P-type multi-channel epitaxial structure into multiple sub-P-type multi-channel epitaxial structures. The N-type heavily doped layer is located on the surface and sidewalls of each sub-P-type multichannel epitaxial structure in the source and drain regions, as well as on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures; the N-type heavily doped layer and the P-type channel layer form a tunnel junction. The source electrode and drain electrode are located on the heavily doped N-type layers in the source region and drain region, respectively. The gate dielectric layer, the surface and sidewalls of each sub-P-type multichannel epitaxial structure between the source and drain regions, and the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures; The gate electrode is located on the gate dielectric layer in the gate region; In the full fin array structure, the width of the fin structure in the source and drain regions is greater than the width of the fin structure in the gate region.

[0021] In this embodiment of the invention, the substrate is one of Si, SiC, GaN, or sapphire.

[0022] The buffer layer in this embodiment of the invention is made of GaN and has a thickness of 100nm~300nm, which is used to alleviate the lattice mismatch between the substrate and the P-type multi-channel epitaxial structure.

[0023] The P-type multi-channel epitaxial structure of this invention is composed of N P-type barrier layers and N P-type channel layers stacked alternately, where N ≥ 2. In this embodiment, N is preferably 3 to 5. For example, when N is 3, it includes three P-type barrier layers and three P-type channel layers. Each P-type barrier layer forms a two-dimensional hole-gas channel 2DHG with the adjacent P-type channel layer. Therefore, this P-type multi-channel epitaxial structure has three two-dimensional hole-gas channels as conductive channels.

[0024] All P-type barrier layers in the embodiments of this invention have the same material composition and thickness range; for example, each P-type barrier layer is made of a group III nitride material, has a thickness of 5 nm to 20 nm, is doped with Mg, and has a doping concentration of 5 × 10¹. 8 cm -3 ~5×10¹ 9 cm -3 Group III nitride materials are GaN, InN, AlN, or multi-component compounds formed therefrom.

[0025] All P-type channel layers in the embodiments of this invention have the same material composition and thickness range; for example, each P-type channel layer is made of a group III nitride material, has a thickness of 3nm~20nm, is doped with Mg, and has a doping concentration of 5×10¹. 8 cm -3 ~5×10¹ 9 cm -3 The bandgap of the P-type channel layer is smaller than that of the P-type barrier layer to ensure the formation of two-dimensional cavitation channels at the interface.

[0026] In this embodiment of the invention, the N-type heavily doped layer is made of either InGaN or GaN, has a thickness of 10 nm to 30 nm, is doped with Si, and has a doping concentration of 5 × 10¹. 9 cm -3 ~5×10² 0 cm -3 The N-type heavily doped layer is used to form a tunnel junction with the P-type channel layer in the P-type multi-channel epitaxial structure, further improving the ohmic contact performance.

[0027] In this embodiment of the invention, the full-fin array structure extends through the source region, gate region, and drain region, forming a three-dimensional structure.

[0028] In this embodiment of the invention, the width of the fin structure in the source and drain regions is 300nm~500nm.

[0029] In this embodiment of the invention, the width of the fin structure in the gate region is 10nm~200nm.

[0030] The gate dielectric layer in this embodiment of the invention is made of one or more of Al2O3, SiO2, SiN, and HfO2, and has a thickness of 10nm~20nm.

[0031] In this embodiment of the invention, the source electrode and drain electrode adopt a metal stack structure consisting of four metal layers, Ti, Al, Ni and Au, arranged sequentially from bottom to top, with metal thicknesses of 20 nm, 160 nm, 55 nm and 45 nm, respectively.

[0032] In this embodiment of the invention, the gate electrode adopts a metal stack structure composed of two layers of metal, Ni and Au, from bottom to top, with metal thicknesses of 45 nm and 200 nm, respectively.

[0033] The fully finned GaN-based P-type multichannel device with high on-current provided in this embodiment of the invention further includes: an undoped InGaN layer located on the surface of the P-type multichannel epitaxial structure. An N-type heavily doped layer is formed on the undoped InGaN layer, and the resulting polarized tunneling junction can further improve tunneling efficiency and enhance ohmic contact performance compared to a structure with only an N-type heavily doped layer.

[0034] The fully finned GaN-based P-type multi-channel device with high conduction current provided in this invention further includes: an N-type channel epitaxial structure located between the buffer layer and the P-type multi-channel epitaxial structure for co-integration of GaN-based N-type channel devices; wherein the N-type channel epitaxial structure is composed of M N-type channel layers and M N-type barrier layers stacked alternately from bottom to top, where M≥1. This invention grows N-type channel layers and N-type barrier layers between the buffer layer and the P-type multi-channel epitaxial structure, achieving monolithic integration of P-type and N-type channel devices, further simplifying the circuit structure and reducing parasitic effects.

[0035] In this embodiment of the invention, each N-type channel layer is made of unintentionally doped GaN material with a thickness of 10 nm to 300 nm; each N-type barrier layer is made of one of unintentionally doped AlGaN, InAlN, and AlN with a thickness of 5 nm to 20 nm.

[0036] In summary, the fully finned GaN-based P-type multi-channel device with high on-current provided by this invention employs a P-type multi-channel structure with high conduction capability, distributing the hole density across multiple two-dimensional hole gas channels. This removes the mutual constraint between hole mobility and hole density, significantly improving the on-current of the P-type channel device. The heavily N-type doped layers in the source / drain regions of this invention form a tunnel junction structure with the P-type channel layer of the P-type channel device itself, transforming the ohmic contact of the P-type material into a contact with the tunnel junction. This solves the problem of finding metals with sufficiently high work functions in the ohmic contact of P-type materials. Simultaneously, the fully finned array structure allows the ohmic metal to simultaneously achieve sidewall contact with multiple two-dimensional hole gas channels, further improving ohmic contact efficiency. By controlling the width of the finned structure in the gate region, this invention enables both the top gate and sidewall gate to simultaneously deplete the holes in the finned structure, thereby improving the gate control capability of the device and achieving enhancement-mode operation of the gallium nitride-based P-type multi-channel device. Because the P-type multi-channel device provided by this invention has high on-current characteristics, it can promote the matching of driving capabilities between P-type and N-type devices in gallium nitride-based complementary logic applications, significantly reducing the layout area of ​​P-type channel devices, thereby reducing circuit area and cost. The tunneling junction ohmic contact process in this invention is compatible with the ohmic contact process of N-type channel devices in gallium nitride-based complementary metal-oxide-semiconductor technology, which can reduce manufacturing costs and process complexity, and facilitate the monolithic integration of P-type and N-type channel devices.

[0037] Secondly, please see Figure 2 This invention provides a method for fabricating a fully finned GaN-based P-type multichannel device with high conduction current, used for fabricating any of the fully finned GaN-based P-type multichannel devices with high conduction current as described in the first aspect. The corresponding fabrication method includes: S10. Obtain the substrate and grow a buffer layer on the substrate.

[0038] In this embodiment of the invention, a buffer layer of GaN material with a thickness of 100nm~300nm is grown on a sapphire / Si / SiC substrate using MOCVD (Metal-Organic Chemical Vapor Deposition) process, as shown in Figure 3(a).

[0039] S20. A P-type multi-channel epitaxial structure is grown on the buffer layer. The P-type multi-channel epitaxial structure is composed of N P-type barrier layers and N P-type channel layers stacked alternately from bottom to top, where N≥2. A two-dimensional cavitation channel is formed between each P-type channel layer and the adjacent P-type barrier layer.

[0040] This invention employs MOCVD technology to grow a P-type multi-channel epitaxial structure on a buffer layer, as shown in Figure 3(b). The specific details of this P-type multi-channel epitaxial structure are shown in Figure 3(c): it consists of N P-type barrier layers and N P-type channel layers stacked alternately from bottom to top. Each P-type channel layer forms a two-dimensional hole gas channel with its adjacent P-type barrier layer. Each P-type barrier layer is made of a group III nitride material, has a thickness of 5 nm to 20 nm, is doped with Mg, and has a doping concentration of 5 × 10¹. 8 cm -3 ~5×10¹ 9 cm -3 Each P-type channel layer is made of a group III nitride material, with a thickness of 3 nm to 20 nm, and is doped with Mg at a doping concentration of 5 × 10¹. 8 ~5×10¹ 9 cm -3 .

[0041] S30. Etch the P-type multi-channel epitaxial structure until it reaches the bottom barrier layer of the P-type multi-channel epitaxial structure, dividing the P-type multi-channel epitaxial structure into multiple sub-P-type multi-channel epitaxial structures, and forming a full-fin array structure that runs through the source region, gate region and drain region.

[0042] In this embodiment of the invention, fin array lithography is first performed. Specifically: the sample obtained in S20 is baked on a hot plate at 200 ℃ for 5 min; then, photoresist is applied and spun at a spin speed of 3500 r / min, and the sample is baked on a hot plate at 90 ℃ for 1 min; next, fin array lithography is performed on the entire active region of the device, as shown in the top view in Figure 3(d). The width of each fin structure in the fin array structure is 300nm~500nm, and the duty cycle between the fin structure and the etched area is 1:1, that is, the width of the fin area and the gap area are the same. The sample is placed in a lithography machine to expose the photoresist in the etched area. Finally, the exposed sample is placed in a developing solution to remove the photoresist in the etched area, and then rinsed with ultrapure water and dried with nitrogen.

[0043] Next, the fin array structure is etched. Specifically, the sample is baked on a hot plate at 100°C for 1 min to complete the hard mold. Then, the fin array structure of the entire active region of the device is formed using ICP (Inductively Coupled Plasma Etching) etching process. The etching conditions are: the reaction gases are BCl3 and Cl2, the reaction chamber pressure is 5 mTorr, and the RF power of the upper and lower electrodes is 50 W and 15 W, respectively. The etching depth of the etched area needs to reach the bottom P-type barrier layer as shown in Figure 3(e), or penetrate the bottom P-type barrier layer to reach the buffer layer (not shown). Then, the sample is sequentially immersed in acetone solution, stripping solution, acetone solution and ethanol solution for cleaning to remove the photoresist on the sample surface.

[0044] S40. An N-type heavily doped layer is grown on the surface and sidewalls of each sub-P-type multichannel epitaxial structure, and on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures.

[0045] In this embodiment of the invention, an N-type heavily doped layer is grown on the sample surface using MBE (Molecular Beam Epitaxy), as shown in Figure 3(f). The N-type heavily doped layer is made of either InGaN or GaN, has a thickness of 10 nm to 30 nm, is doped with Si, and has a doping concentration of 5 × 10¹. 9 cm -3 ~5×10² 0 cm -3 With N + Taking a heavily doped GaN layer as an example, the specific growth conditions are as follows: trimethylgallium and ammonia are used as Ga and N sources, respectively, the carrier gas is H2 or N2, and the heavy silicon doping concentration is 5 × 10⁻⁶. 19 cm -3 ~5×10 20 cm -3 The growth thickness is 10nm~30nm. Based on N + - A heavily doped GaN layer, with N-type N-type doped sources and drain regions respectively. + -GaN / P + -GaN tunnel junction structure.

[0046] S50. Etch away the N-type heavily doped layer on the surface of each sub-P-type multi-channel epitaxial structure in the gate region and the barrier layer surface between adjacent sub-P-type multi-channel epitaxial structures, and continue to etch away each sub-P-type multi-channel epitaxial structure in the gate region until the bottom barrier layer is reached, so that in the full fin array structure, the width of the fin structure in the gate region is smaller than the width of the fin structure in the source region and the drain region; wherein, during the etching of the fin structure in the gate region, the N-type heavily doped layer on the sidewall of each sub-P-type multi-channel epitaxial structure is etched away simultaneously.

[0047] In this embodiment of the invention, the gate region is first lithographically ...

[0048] Next, excess N-type heavily doped layers were etched onto the surface of each sub-P-type multi-channel epitaxial structure in the gate region and onto the surface of the barrier layer between adjacent sub-P-type multi-channel epitaxial structures, as shown in Figure 3(g). Specifically: First, the sample was baked on a hot plate at 100°C for 1 min to complete the hard mold process; then, a low-power ICP etching process was used to remove excess N-type heavily doped layers under the gate. The etching conditions were: the reaction gases were BCl3 and Cl2, the reaction chamber pressure was 5 mTorr, the RF power of the upper and lower electrodes was 20 W and 5 W, respectively, and the etching depth was the thickness of the N-type heavily doped layer.

[0049] The under-gate fin structure photolithography continues. Specifically: First, the sample is baked on a hot plate at 200 °C for 5 minutes; then, electron beam photoresist is applied and spun off, and the sample is baked on the hot plate again; next, a second fin array photolithography is performed on the device gate region. Using an electron beam lithography machine, the fin width of the gate region is further reduced from the original 300nm~500nm, defining the fin structure width of the gate region as 10nm~200nm. The sample is placed in the lithography machine to expose the etched area; finally, the exposed sample is placed in the developer to remove the photoresist in the etched area, and then rinsed with ultrapure water and dried with nitrogen.

[0050] Next, the under-gate fin structure is etched. Specifically: First, the sample is baked on a hot plate at 100 °C for 1 min to complete the hard mold. Then, the width of the under-gate fin structure is defined using ICP etching. The etching conditions are: the reaction gases are BCl3 and Cl2, the reaction chamber pressure is 5 mTorr, the RF power of the upper and lower electrodes is 50 W and 15 W, respectively, and the etching depth of the etched area is the same as that of the first fin array, that is, it needs to reach the bottom P-type barrier layer, or penetrate the bottom P-type barrier layer to reach the buffer layer. At this time, the N-type heavily doped layer on the fin sidewall of the gate region is also removed. The structure after the second fin array etching of the gate region is shown in Figure 3(h). The width of the fin structure in the gate region is smaller than the width of the fin structures in the source and drain regions.

[0051] S60. Ohmic metal is deposited on the N-type heavily doped layers in the source and drain regions to form the source and drain electrodes.

[0052] In this embodiment of the invention, ohmic patterns are first lithographically patterned on the heavily doped N-type layers in the source and drain regions. Specifically: First, the sample is baked on a hot plate at 200 °C for 5 min; then, a release agent is coated and spin-spinned onto the sample surface to a thickness of 0.35 μm, and the sample is baked on a hot plate at 200 °C for 5 min; next, photoresist is coated and spin-spinned onto the release agent to a thickness of 0.77 μm, and the sample is baked on a hot plate at 90 °C for 1 min; subsequently, the sample with the coating and spin-spinned photoresist is placed in a lithography machine to expose the photoresist in the source and drain regions; finally, the exposed sample is placed in a developing solution to remove the photoresist and release agent in the source and drain regions, and then rinsed with ultrapure water and dried with nitrogen.

[0053] Next, ohmic metal evaporation is performed. Unlike traditional P-type channel devices that use a Ni and Au metal stack as the ohmic contact, the ohmic contact in this invention is based on a tunnel junction structure of an N-type heavily doped layer / P-type channel layer, allowing the metal to make ohmic contact with the N-type material. The ohmic metal is a metal stack structure composed of four layers of metal from bottom to top: Ti, Al, Ni, and Au, with evaporation metal thicknesses of 20 nm, 160 nm, 55 nm, and 45 nm, respectively. Due to the full-fin array structure of the P-type multi-channel device, the source and drain electrodes also exhibit corresponding fin structures. Utilizing the tunnel junction structure of the N-type heavily doped layer / P-type channel layer, this fin structure reduces contact resistance and achieves efficient ohmic contact with multiple two-dimensional hole gas channels simultaneously. The specific process is as follows: First, the sample with the gate photolithography pattern is placed in a plasma resist remover for bottom film treatment, which takes 5 minutes; then, the sample is placed in an electron beam evaporation stage, and the vacuum level in the reaction chamber of the electron beam evaporation stage reaches 2 × 10⁻⁶.-6 After the torsion process, the ohmic metal is evaporated. This ohmic metal is a metal stack structure consisting of four layers of metal, Ti, Al, Ni and Au, arranged from bottom to top. Next, the sample after the ohmic metal evaporation is completed is stripped to remove the ohmic metal, photoresist and release adhesive outside the source and drain regions. Finally, the sample is rinsed with ultrapure water and dried with nitrogen.

[0054] Finally, ohmic metal annealing is performed. Specifically, the sample after ohmic metal evaporation and stripping is placed in a rapid thermal annealing furnace for annealing, thereby forming an ohmic contact between the ohmic metal and the tunnel junction structure based on the N-type heavily doped layer / P-type channel layer. The annealing process conditions are: annealing atmosphere of N2, annealing temperature of 830 ℃, and annealing time of 30 s. At this time, both the source and drain regions are formed based on the tunnel junction ohmic contact of the N-type heavily doped layer, and the device structure is shown in Figure 3(i).

[0055] S70. A gate dielectric layer is grown on the surface and sidewalls of each sub-P-type multichannel epitaxial structure between the source and drain regions, and on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures.

[0056] In this embodiment of the invention, a gate dielectric layer is first grown as shown in Figure 3(j). The gate dielectric layer material is one or more of Al2O3, SiO2, SiN, and HfO2, with a thickness of 10nm~20nm. Taking the growth of an Al2O3 dielectric layer as an example, at 300℃, an Al2O3 layer of 10nm~20nm is deposited on the sample surface using ALD (Atomic Layer Deposition) technology as the gate dielectric of the P-type channel device to reduce the leakage current level of the device.

[0057] Next, ohmic region aperture photolithography was performed. Specifically: First, the sample was baked on a hot plate at 200 °C for 5 min; then, photoresist was applied and spun at a speed of 3500 r / min, and the sample was baked on a hot plate at 90 °C for 1 min; the sample was then placed in a photolithography machine to expose the ohmic region, and subsequently immersed in a developing solution to remove the photoresist from the ohmic region, while the gate region was protected by the photoresist. Finally, the sample was rinsed with ultrapure water and dried with nitrogen.

[0058] Next, ohmic region opening etching is performed. Specifically: First, the sample is baked on a hot plate at 100°C for 1 minute to complete the hard mold. Then, ohmic region opening is performed using ICP etching. The etching conditions are: CF4 gas is used for etching, the reaction chamber pressure is 10 mTorr, and the RF power of the upper and lower electrodes is 150 W and 35 W, respectively. The Al2O3 thickness is over-etched by 50% to ensure that all Al2O3 above the source and drain electrodes is etched.

[0059] S80. Deposit gate metal on the gate dielectric layer in the gate region to form a gate electrode.

[0060] In this embodiment of the invention, the gate region is first lithographically etched. Specifically: First, the sample is baked on a hot plate at 200 °C for 5 min; then, a stripping agent is applied and spun to a thickness of 0.35 μm, and the sample is baked on a hot plate at 200 °C for 5 min; next, photoresist is applied and spun to the stripping agent to a thickness of 0.77 μm, and the sample is baked on a hot plate at 90 °C for 1 min; after that, the sample with the completed coating and spun toggle is placed in a lithography machine to expose the photoresist in the gate region; finally, the exposed sample is placed in a developing solution to remove the photoresist and stripping agent in the gate region, and then rinsed with ultrapure water and dried with nitrogen.

[0061] Next, the gate metal is evaporated as shown in Figure 3(k). Specifically: First, the sample with the photolithographic pattern of the gate electrode is placed in a plasma resist remover for bottom film treatment, which takes 5 minutes; then, the sample is placed in an electron beam evaporation stage, and the vacuum degree of the reaction chamber of the electron beam evaporation stage reaches 2 × 10⁻⁶. -6 After Torr, gate metal is evaporated onto the photoresist inside and outside the gate region. The gate metal is a metal stack structure consisting of two layers of metal, Ni and Au, with thicknesses of 45 nm and 200 nm, respectively, from bottom to top. Next, the sample with the gate metal evaporated is stripped to remove the gate metal, photoresist, and release adhesive outside the gate region. Finally, the sample is rinsed with ultrapure water and dried with nitrogen.

[0062] As for the second aspect of the preparation method embodiment, since it is basically similar to the first aspect of the device structure embodiment, the description is relatively simple. For relevant details, please refer to the description of the first aspect of the device structure embodiment.

[0063] In the description of this invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0064] Although the invention has been described herein in conjunction with various embodiments, those skilled in the art, by reviewing the specification and accompanying drawings, will understand and implement other variations of the disclosed embodiments in carrying out the claimed invention. In the specification, the word "comprising" does not exclude other components or steps, and "a" or "an" does not exclude a plurality. While certain measures are described in different embodiments, this does not mean that these measures cannot be combined to produce good results.

[0065] The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention.

Claims

1. A fully finned GaN-based P-type multichannel device with high on-current, characterized in that, The fully finned GaN-based P-type multichannel device includes: Substrate, and a buffer layer located on the substrate; The P-type multi-channel epitaxial structure is located on the buffer layer. The P-type multi-channel epitaxial structure is composed of N P-type barrier layers and N P-type channel layers stacked alternately from bottom to top, where N≥2. A two-dimensional cavitation channel is formed between each P-type channel layer and the adjacent P-type barrier layer. The full-fin array structure extends through the source, gate, and drain regions of the P-type multi-channel epitaxial structure, all the way to the bottom barrier layer of the P-type multi-channel epitaxial structure, in order to divide the P-type multi-channel epitaxial structure into multiple sub-P-type multi-channel epitaxial structures. The N-type heavily doped layer is located on the surface and sidewalls of each sub-P-type multichannel epitaxial structure in the source and drain regions, as well as on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures; the N-type heavily doped layer and the P-type channel layer form a tunnel junction. The source electrode and drain electrode are located on the heavily doped N-type layers in the source region and drain region, respectively. The gate dielectric layer, the surface and sidewalls of each sub-P-type multichannel epitaxial structure between the source and drain regions, and the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures; The gate electrode is located on the gate dielectric layer in the gate region; In the full fin array structure, the width of the fin structure in the source and drain regions is greater than the width of the fin structure in the gate region.

2. The all-fin GaN-based P-type multichannel device with high on-current as described in claim 1, characterized in that, Each p-type barrier layer is made of a group III nitride material, with a thickness of 5 nm to 20 nm, and is doped with Mg at a doping concentration of 5 × 10¹. 8 cm -3 ~5×10¹ 9 cm -3 .

3. The all-fin GaN-based P-type multichannel device with high on-current as described in claim 1, characterized in that, Each P-type channel layer is made of a group III nitride material with a band gap smaller than that of the P-type barrier layer, has a thickness of 3 nm to 20 nm, is doped with Mg, and has a doping concentration of 5 × 10¹. 8 cm -3 ~5×10¹ 9 cm -3 .

4. The all-fin GaN-based P-type multichannel device with high on-current as described in claim 1, characterized in that, The N-type heavily doped layer is made of either InGaN or GaN, has a thickness of 10 nm to 30 nm, is doped with Si, and has a doping concentration of 5 × 10¹. 9 cm -3 ~5×10² 0 cm -3 .

5. The all-fin GaN-based P-type multichannel device with high on-current as described in claim 1, characterized in that, The width of the fin structure in the source and drain regions is 300nm~500nm.

6. The all-fin GaN-based P-type multichannel device with high on-current as described in claim 1, characterized in that, The width of the fin structure in the gate region is 10nm~200nm.

7. The all-fin GaN-based P-type multichannel device with high on-current as described in claim 1, characterized in that, The fully finned GaN-based P-type multichannel device also includes: An N-type channel epitaxial structure is located between a buffer layer and a P-type multi-channel epitaxial structure, used for co-integration of GaN-based N-type channel devices. The N-type channel epitaxial structure is composed of M N-type channel layers and M N-type barrier layers stacked alternately from bottom to top, where M≥1.

8. The all-fin GaN-based P-type multichannel device with high on-current as described in claim 7, characterized in that, Each N-type channel layer is made of unintentionally doped GaN material with a thickness of 10nm~300nm.

9. The all-fin GaN-based P-type multichannel device with high on-current as described in claim 7, characterized in that, Each N-type barrier layer material is one of the following: unintentionally doped AlGaN, InAlN, or AlN, with a thickness of 5 nm to 20 nm.

10. A method for fabricating a fully finned GaN-based p-type multichannel device with high on-current, characterized in that, The fabrication method for the fully finned GaN-based P-type multichannel device with high conduction current as described in any one of claims 1 to 9 includes: Obtain a substrate and grow a buffer layer on the substrate; A P-type multi-channel epitaxial structure is grown on a buffer layer. The P-type multi-channel epitaxial structure is composed of N P-type barrier layers and N P-type channel layers stacked alternately from bottom to top, where N≥2. A two-dimensional hole gas channel is formed between each P-type channel layer and the adjacent P-type barrier layer. Etch the P-type multi-channel epitaxial structure until it reaches the bottom barrier layer of the P-type multi-channel epitaxial structure, divide the P-type multi-channel epitaxial structure into multiple sub-P-type multi-channel epitaxial structures, and form a full fin array structure that runs through the source region, gate region and drain region. N-type heavily doped layers are grown on the surface and sidewalls of each sub-P-type multichannel epitaxial structure, as well as on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures. The N-type heavily doped layer on the surface of each sub-P-type multi-channel epitaxial structure in the gate region and the barrier layer surface between adjacent sub-P-type multi-channel epitaxial structures is etched away, and the etching of each sub-P-type multi-channel epitaxial structure in the gate region continues until the bottom barrier layer is reached, so that in the full fin array structure, the width of the fin structure in the gate region is smaller than the width of the fin structure in the source region and the drain region; wherein, during the etching of the fin structure in the gate region, the N-type heavily doped layer on the sidewall of each sub-P-type multi-channel epitaxial structure is simultaneously etched away. Ohmic metal is deposited on the N-type heavily doped layers in the source and drain regions to form the source and drain electrodes. A gate dielectric layer is grown on the surface and sidewalls of each sub-P-type multichannel epitaxial structure between the source and drain regions, and on the surface of the barrier layer between adjacent sub-P-type multichannel epitaxial structures. Gate metal is deposited on the gate dielectric layer in the gate region to form the gate electrode.