A TOPCon battery coating method
By using remote plasma pre-oxidation and low-temperature thermal oxidation technologies to prepare the tunneling oxide layer and polycrystalline silicon layer of TOPCon batteries in the same vacuum chamber, the problems of uneven nucleation, doped atom penetration and interface defects in the existing technology are solved, and the uniformity and thermal stability of the film layer are improved, thereby improving battery performance and mass production adaptability.
Patent Information
- Application Number
- CN202611254533.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies for preparing the tunneling oxide layer of TOPCon batteries suffer from problems such as uneven nucleation, doped atom penetration, numerous interface defects, unstable film quality, and poor large-size compatibility, which limit the improvement of battery performance.
Remote plasma pre-oxidation is used to form an oxide crystal nucleus layer. Combined with low-temperature thermal oxidation technology, tunneling SiOx layer and polycrystalline silicon layer are prepared in the same vacuum chamber. This avoids damage caused by high-energy ion bombardment and high-temperature oxidation, and ensures the uniformity and thermal stability of the film.
It significantly reduces interface defects, improves film uniformity and thermal stability, increases the open-circuit voltage and photoelectric conversion efficiency of the battery, adapts to the production of large-size silicon wafers, simplifies mass production processes, and reduces production costs.
Smart Images

Figure CN123076044A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of TOPCon battery technology, and more particularly to a TOPCon battery coating method. Background Technology
[0002] TOPCon cells are currently one of the mainstream technologies in the photovoltaic industry. Their core advantage lies in the passivated contact structure on the back, which consists of an ultra-thin tunneling oxide layer (SiO2). x The TOPCon battery consists of a tunneling oxide layer and a heavily doped polycrystalline silicon layer (Poly-Si). The quality of the tunneling oxide layer directly determines the level of interface passivation of the battery and is a key factor affecting the open-circuit voltage (Voc) and final conversion efficiency. However, the mainstream technologies currently used in industrial applications to prepare tunneling oxide layers generally have insurmountable drawbacks, limiting further improvements in TOPCon battery performance.
[0003] Currently, there are three main technical solutions for preparing tunneling oxide layers in the industry: 1. Pure high-temperature thermal oxidation Technical Description: Silicon wafers are placed in a high-temperature (typically >700℃) oxygen or nitrous oxide atmosphere, causing the silicon wafer surface to naturally oxidize and form SiO₂. x film.
[0004] The disadvantages are: ① Uneven nucleation: The oxidation process involves random nucleation, resulting in poor uniformity of film thickness and making it easy to form local thin spots at defects on the silicon wafer surface.
[0005] ② Dopant atom penetration: During the subsequent high-temperature annealing process, dopant atoms (such as phosphorus) in the polycrystalline silicon layer can easily penetrate these local thin spots and enter the silicon substrate, causing severe carrier recombination and reducing battery performance.
[0006] ③ Poor compatibility with large sizes: It is extremely difficult to achieve uniform high-temperature thermal oxidation for large silicon wafers such as 210mm.
[0007] 2. One-step plasma oxidation (PECVD) Technical Description: In a plasma-enhanced chemical vapor deposition (PECVD) system, plasma is used to excite an oxidizing gas (such as N2O), causing it to react with the silicon wafer surface to form SiO2. x film.
[0008] shortcoming: ① Ion bombardment damage: During conventional PECVD, high-energy ions directly bombard the silicon wafer surface, destroying the silicon lattice and introducing a large number of interface defects (such as dangling bonds), resulting in an increase in the interface density of states (Dit) and a deterioration in the passivation effect.
[0009] ② Unstable film quality: The instability of plasma may lead to pinholes or uneven regions in the film.
[0010] 3. Wet chemical oxidation Technical description: The silicon wafer surface is oxidized using chemical solutions such as dilute nitric acid.
[0011] shortcoming: ① Poor process stability: This method is extremely sensitive to parameters such as solution concentration, temperature, and processing time, and has poor batch-to-batch repeatability, making it difficult to achieve large-scale stable mass production.
[0012] ② Insufficient thermal stability: The oxide layer formed by wet oxidation is relatively loose, which is prone to pinholes during subsequent high-temperature annealing, leading to passivation failure.
[0013] Therefore, it is necessary to develop a TOPCon battery coating method to solve the above problems. Summary of the Invention
[0014] The purpose of this invention is to design a TOPCon battery coating method to solve the above problems.
[0015] The present invention achieves the above objectives through the following technical solutions: A TOPCon battery coating method, comprising: S1. Load the N-type crystalline silicon wafer that has been alkaline polished on the back into the tubular PECVD oxidation chamber, seal and evacuate, introduce H2 gas, turn on the remote plasma, and use hydrogen free radicals to remove the natural oxide layer and organic contaminants on the surface of the silicon wafer. After the process is completed, maintain the vacuum state. S2. Maintain a vacuum, introduce N2O gas, and use substrate-free biased remote plasma for excitation to decompose N2O and generate oxygen free radicals, which will form an ultrathin oxide nucleus layer on the silicon wafer surface.
[0016] S3. Maintain vacuum, turn off the plasma radio frequency power supply, introduce N2O as an oxidation atmosphere, and raise the chamber temperature to 520-620℃ for low-temperature thermal oxidation, relying on the uniform growth of oxide crystal nuclei to form complete tunneled SiO. x layer; S4. The gas source is directly switched inside the same vacuum chamber, and a mixture of SiH4 and PH3 gas is introduced to deposit a phosphorus-doped amorphous silicon layer in situ. Subsequently, an n⁺ polycrystalline silicon layer is formed by annealing and crystallization, thus completing the continuous coating of the tunneling oxide layer and the Poly-Si composite structure in the same cavity.
[0017] Preferably, in step S2, the thickness of the oxide nucleus layer is 0.2 to 0.5 nm.
[0018] Preferably, in step S3, tunneling SiO xThe final total thickness of the layer is 0.8–1.4 nm.
[0019] The beneficial effects of this invention are as follows: Significantly reduces interface defects and ensures Si / SiO x A clean and intact interface: On the one hand, the remote plasma pre-oxidation adopts a substrate-free bias design, relying solely on oxygen free radical diffusion to complete the oxidation reaction. There is no high-energy ion bombardment throughout the process, preventing silicon lattice damage at its source and protecting the integrity of the interface structure. On the other hand, the entire process maintains a sealed cavity to prevent vacuum breakage, completely avoiding the risk of the silicon wafer coming into contact with air during process transfer and regenerating the natural oxide layer, ensuring a clean and impurity-free interface. Simultaneously, the low-temperature thermal oxidation process of 520–620℃ significantly reduces the thermal stress between silicon and the oxide layer compared to traditional high-temperature thermal oxidation, further reducing the formation of interface defects. The synergistic effect of these three factors effectively reduces the Si / SiO ratio. x The density of states at the interface (Dit) lays the foundation for excellent passivation performance.
[0020] To improve the uniformity and density of the film and eliminate local thin spots, a nucleus-guided growth mechanism is employed: First, a uniformly distributed oxide nucleus is formed across the entire silicon wafer through remote plasma pre-oxidation, providing a regular nucleation template for subsequent oxidation growth and resolving the uneven film formation and local thin spots caused by random nucleation in pure thermal oxidation. Subsequent low-temperature thermal oxidation allows for directional and synchronous growth along the predetermined nucleus sites, ultimately forming a continuous, dense, and pore-free tunneling SiO₂. x The thickness of the layer is controlled between 0.8 and 1.4 nm, which can still maintain excellent film thickness uniformity and structural consistency on large-size silicon wafers.
[0021] Enhanced thermal stability of the film layer and effective blocking of dopant atom penetration: The tunneling oxide layer prepared by nucleus-guided growth has a dense structure and low porosity, which can effectively suppress the generation of pinhole defects in the subsequent n⁺ polycrystalline silicon high-temperature annealing and crystallization process; at the same time, the dense oxide layer can stably block the diffusion and penetration of phosphorus atoms into the silicon substrate, avoid interface failure and device performance degradation caused by dopant atom penetration, ensure the functional integrity of the composite structure after high-temperature processing, and effectively reduce the battery saturation dark current J0.
[0022] Comprehensive improvement of TOPCon cell photoelectric performance: Relying on the tunneling oxide / polycrystalline silicon composite structure with low interface defects, high uniformity and density, and high thermal stability, the passivation effect of the cell surface is significantly optimized: carrier recombination loss is greatly reduced, saturated dark current (J0) is effectively reduced, and implicit open circuit voltage (iVoc) is significantly improved, ultimately achieving a steady increase in the photoelectric conversion efficiency of TOPCon cells.
[0023] Compatible with mass production equipment and easy to quickly industrialize: The entire process is based on the existing tubular PECVD / LPCVD mass production equipment architecture. It can be achieved simply by adjusting the process gas source, temperature parameters and plasma working mode. There is no need to modify the equipment hardware or reconstruct the production line. The process introduction cost is low, the adaptability is strong, and it can be quickly applied to large-scale photovoltaic cell production lines. Attached Figure Description
[0024] Figure 1 This is a flowchart illustrating the process of this application. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.
[0026] Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the invention.
[0027] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0028] In the description of this invention, it should be understood that the terms "upper," "lower," "inner," "outer," "left," "right," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product of this invention is in use, or the orientation or positional relationship commonly understood by those skilled in the art. They are only used to facilitate the description of this invention and to simplify the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0029] Furthermore, the terms "first," "second," etc., are used only to distinguish descriptions and should not be interpreted as indicating or implying relative importance.
[0030] In the description of this invention, it should also be noted that, unless otherwise explicitly specified and limited, terms such as "set" and "connection" should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be a connection within two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0031] The specific embodiments of the present invention will now be described in detail with reference to the accompanying drawings.
[0032] like Figure 1 As shown, a TOPCon battery coating method includes: S1: In-situ hydrogen plasma cleaning of silicon wafers: The N-type crystalline silicon wafer, after back-side alkaline polishing, is loaded into a tubular PECVD oxidation chamber and sealed under vacuum. H2 gas is introduced, and remote plasma is activated. Hydrogen free radicals are used to remove the natural oxide layer and organic contaminants on the silicon wafer surface. The temperature is 420℃, the pressure is 40Pa, the H2 flow rate is 8000sccm, the power is 3500W, and the treatment time is 90s. After treatment, the vacuum state is maintained.
[0033] S2: Remote Plasma Pre-oxidation: A vacuum is maintained while N2O gas is introduced. A substrate-free, remote plasma is used for excitation, causing N2O to decompose and generate oxygen free radicals. The temperature is 420℃, the pressure is 60Pa, the N2O flow rate is 6000 sccm, the RF power is 4000W, and the time is 100s. These active oxygen groups diffuse to the silicon wafer surface and react with silicon to form an ultrathin, uniform oxide nucleus layer with a thickness of 0.35nm. This process avoids high-energy ion bombardment, thus preventing damage to the silicon substrate.
[0034] S3: Mild Thermal Oxidation Thickening: Without opening the cavity or breaking the vacuum, and with the plasma RF power supply turned off, N2O is introduced as an oxidation atmosphere to raise the cavity temperature to 520–620°C for low-temperature thermal oxidation. The temperature is 580°C, the pressure is 120 Pa, and the N2O atmosphere is maintained for 420 seconds. During the oxidation process, the oxide crystals will grow uniformly along the pre-formed oxide nuclei in step S2, ultimately forming a complete tunneled SiO with a total thickness of 1.1 nm. x layer.
[0035] S4: In-situ deposition of doped amorphous silicon: After the oxidation process, the gas source in the cavity is directly switched to introduce SiH4 (silane) and PH3 (phosphine) to deposit a phosphorus-doped amorphous silicon layer in situ under the same vacuum environment. Subsequently, after annealing and crystallization, n⁺ polycrystalline silicon is formed, thus fully realizing the continuous deposition of tunnel oxide layer + Poly-Si in the same cavity.
[0036] Test results of this embodiment: Interface state density Dit = 6.2 × 10 10 cm -2 ·eV -1 .
[0037] The implicit open-circuit voltage of the symmetrical sample is iVoc = 724mV.
[0038] Saturated dark current J O =12.6fA / cm².
[0039] Comparative Example 1: Using the traditional single high-temperature thermal oxidation method Process: 1.1nm SiO2 is prepared using pure thermal oxidation at 680℃ on silicon wafers of the same specifications. x The remaining deposition conditions were the same as in Example 1.
[0040] Test results: Interface state density Dit = 1.3 × 10 11 cm -2 ·eV -1 .
[0041] The implicit open-circuit voltage of the symmetrical sample is iVoc = 716mV.
[0042] Saturated dark current J O =21.3fA / cm².
[0043] Comparative Example 2: Using the conventional one-step plasma oxidation method Process: The tunneling layer of the same thickness was prepared by conventional substrate biased PECVD one-step oxidation, and the other conditions were the same as in Example 1.
[0044] Test results: Interface state density Dit = 1.15 × 10 11 cm -2 ·eV -1 .
[0045] The implicit open-circuit voltage of the symmetrical sample is iVoc = 718mV.
[0046] Saturated dark current J O =18.5fA / cm².
[0047] Conclusion: This application employs a two-step composite oxidation process: remote plasma pre-oxidation (uniform nucleation) + mild thermal oxidation (520-620℃, nucleus-guided growth). Compared to Comparative Example 1, this application exhibits better uniformity: nucleus-guided growth solves the problem of localized thin spots caused by random nucleation, significantly improving film thickness uniformity. It also demonstrates stronger thermal stability: the dense film structure effectively blocks dopant atoms from penetrating.
[0048] This application employs a two-step composite oxidation process: the first step uses unbiased remote plasma (without ion bombardment), and the second step is thermal oxidation. Compared with Comparative Example 2, the interface damage is smaller: it completely avoids the bombardment damage of high-energy ions to the silicon substrate, resulting in a lower interface state density (Dit), better passivation effect, and higher film quality: it combines the uniformity of plasma oxidation with the density of thermal oxidation.
[0049] This application adopts a continuous vacuum process without breaking the cavity: all steps are completed continuously in the same cavity. Compared with the traditional cavity process, the interface is purer: the formation of the regenerated natural oxide layer is avoided during the silicon wafer transfer process, additional interface defects are eliminated, and passivation performance is further improved; production efficiency is higher: the process flow is simplified and the production cycle is shortened.
[0050] Furthermore, experimental data show that the two-step composite oxidation method of the present invention is significantly superior to the traditional single thermal oxidation and one-step plasma oxidation methods in terms of reducing interface state density, increasing implicit open-circuit voltage, and reducing saturation dark current.
[0051] The above are merely preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A TOPCon battery coating method, characterized in that, include: S1. Load the N-type crystalline silicon wafer that has been alkaline polished on the back into the tubular PECVD oxidation chamber, seal and evacuate, introduce H2 gas, turn on the remote plasma, and use hydrogen free radicals to remove the natural oxide layer and organic contaminants on the surface of the silicon wafer. After the process is completed, maintain the vacuum state. S2. Maintain a vacuum, introduce N2O gas, and use substrate-free biased remote plasma for excitation to decompose N2O and generate oxygen free radicals, thereby generating an ultrathin oxide nucleus layer on the silicon wafer surface. S3. Maintain vacuum, turn off the plasma radio frequency power supply, introduce N2O as an oxidation atmosphere, and raise the chamber temperature to 520-620℃ for low-temperature thermal oxidation, relying on the uniform growth of oxide crystal nuclei to form complete tunneled SiO. x layer; S4. The gas source is directly switched inside the same vacuum chamber, and a mixture of SiH4 and PH3 gas is introduced to deposit a phosphorus-doped amorphous silicon layer in situ. Subsequently, an n⁺ polycrystalline silicon layer is formed by annealing and crystallization, thus completing the continuous coating of the tunneling oxide layer and the Poly-Si composite structure in the same cavity.
2. The TOPCon battery coating method according to claim 1, characterized in that, In step S2, the thickness of the oxide nucleus layer is 0.2–0.5 nm.
3. The TOPCon battery coating method according to claim 1, characterized in that, In step S3, tunneling SiO x The final total thickness of the layer is 0.8–1.4 nm.