Stress detection method for single crystal layers of bonded wafers

By adjusting the sample stage angle to make the incident light parallel to the C-axis of the crystal, the background stripes of the 4H-SiC single crystal material are eliminated, solving the problem of stress detection signal being submerged in the existing technology and realizing high-confidence full-field stress detection.

CN123076216APending Publication Date: 2026-11-10DONGGUAN TIANYU SEMICON TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611323449.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively remove the complex interference fringe background caused by strong optical anisotropy and cutting methods in 4H-SiC single crystal materials, resulting in the stress detection signal being submerged or misread, and failing to meet the requirements for high confidence and full-field stress screening.

Method used

By constructing a polarization optical path and adjusting the pitch angle of the sample stage, the incident light is made parallel to the C-axis of the crystal, eliminating the inherent background fringes introduced by off-axis cutting. Polarization image information is obtained using an image detection component, and stress information is obtained through data processing.

Benefits of technology

It achieves full-field non-destructive, high-confidence stress detection of single-crystal layers on bonded wafers, eliminating strong background fringe interference and improving the accuracy and reliability of stress detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076216A_ABST
    Figure CN123076216A_ABST
Patent Text Reader

Abstract

This invention discloses a method for stress detection of a single-crystal layer in a bonded wafer. The bonded wafer includes an off-axis single-crystal layer, and the surface normal of the off-axis single-crystal layer forms an off-axis angle with its crystal C-axis. The stress detection method includes the following steps: constructing a polarization optical path, which includes a light source, a polarizer, a mirror, a sample stage, an analyzer, and an image detection component arranged sequentially. The bonded wafer is placed on the sample stage, which is horizontally positioned. The transmission axis of the polarizer and the transmission axis of the analyzer are perpendicular to each other, and the light is incident perpendicularly on the sample stage after passing through the mirror; rotating the sample stage along a first direction so that the rotation angle of the sample stage is equal to the off-axis angle, and the sample stage is positioned at a first position after rotation, where the first direction is the direction from the crystal C-axis toward the surface normal of the off-axis single-crystal layer; and using the image detection component to obtain polarization image information of the sample stage when it is in the first position to obtain stress information of the off-axis single-crystal layer. This invention can remove strong background stripes caused by off-axis cutting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductors, and more particularly to a method for stress detection of a single crystal layer on a bonded wafer. Background Technology

[0002] In the manufacturing of third-generation semiconductors (such as 4H-SiC) and advanced semiconductor packaging, wafer bonding and subsequent cleaving and annealing processes, due to thermal expansion coefficient mismatch and mechanical constraints, easily introduce residual stress into the bonded wafer single-crystal substrate and device layers, inducing bonding interface delamination, edge cleaving, and warpage failure. Therefore, a stress detection method capable of performing full-field, non-destructive evaluation of bonded wafer single-crystal layers is needed. In existing technologies, birefringence imaging based on photoelasticity provides an intuitive full-field stress distribution and has been widely studied and applied. By using orthogonal polarized light paths, the refractive index change caused by stress is converted into phase retardation fringes for interpretation, while supplemented by point measurements such as Raman spectroscopy, X-ray diffraction (XRD), or wafer curvature methods for microscopic or local verification. However, when the aforementioned birefringence imaging technology is directly applied to single-crystal materials with strong optical anisotropy, such as 4H-SiC, it faces severe challenges: the inherent uniaxial crystal structure of 4H-SiC endows it with significant natural birefringence (Δn0). In addition, the commonly used 4° off-cut method, wafer bowl, and polishing wedge effect in the industry will produce complex strong interference fringe backgrounds in orthogonal polarization images, even if there is no stress inside the material. Existing technologies lack effective suppression mechanisms for such inherent backgrounds of single crystals, which leads to the weak birefringence signal (δn_σ) induced by stress being submerged or misread as stress distribution, failing to meet the bonding process's requirement for high confidence and full-field stress screening. Summary of the Invention

[0003] The purpose of this invention is to provide a stress detection method for a single crystal layer of a bonded wafer, so as to solve the problem of strong interference fringe background in the prior art.

[0004] To achieve the above objectives, the present invention provides a stress detection method for a single crystal layer of a bonded wafer. The bonded wafer includes a first bonding layer and an off-axis single crystal layer bonded to the first bonding layer. The surface normal of the off-axis single crystal layer forms an off-axis angle with its crystal C-axis. The stress detection method includes the following steps: S1, constructing a polarization optical path, the polarization optical path including a light source, a polarizer, a mirror, a sample stage, an analyzer, and an image detection component arranged sequentially along the optical path. The sample stage, the analyzer, and the image detection component are all located below the light source, the polarizer, and the mirror. The bonded wafer is disposed on the sample stage. The sample stage is horizontally positioned, with the transmission axis of the polarizer and the transmission axis of the analyzer perpendicular to each other. Light emitted from the light source passes through the polarizer and the reflector and is incident perpendicularly on the sample stage. S2, the sample stage is rotated along a first direction, with the rotation angle equal to the off-axis angle. After rotation, the sample stage is positioned at a first position, where the first direction is the direction from the C-axis of the crystal towards the surface normal of the off-axis single crystal layer. S3, the polarization image information of the sample stage at the first position is acquired using the image detection component. S4, the polarization image information is processed to obtain the stress information of the off-axis single crystal layer.

[0005] Preferably, the step of processing the polarization image information to obtain the stress information of the off-axis single crystal layer includes: processing the polarization image information and converting the polarization image information into a first phase delay field; obtaining a second phase delay field induced by bonding stress between the first bonding layer and the off-axis single crystal layer based on the first phase delay field; and obtaining the principal stress difference to obtain the stress information of the off-axis single crystal layer based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer.

[0006] Preferably, the formula for calculating the second phase delay field δσ(x,y) is: δσ(x,y)=δ(x,y), where δ(x,y) is the first phase delay field; the linear relationship between the second phase delay field and the principal stress difference is: δσ(x,y)=4π·C eff (x,y)·(σ1 σ2)(x,y)·d eff (x,y) / λ; where (σ1) σ²)(x,y) is the principal stress difference, C eff (x,y) represents the effective stress optical coefficient of the off-axis single crystal layer in a specific crystal orientation, d eff (x,y) represents the equivalent depth of the stress-active layer, and λ is the wavelength of the light emitted by the light source.

[0007] Preferably, based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer, the formula for obtaining the principal stress difference is: (σ1 σ²)(x,y)=K·δ(x,y); where K is the proportionality constant, K=λ / (4π·C eff (x,y)·d eff (x,y)).

[0008] Preferably, the step of obtaining the principal stress difference to obtain the stress information of the off-axis single crystal layer based on the linear relationship between the second phase delay field and the principal stress difference includes: obtaining the principal stress difference based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer; obtaining the value of the actual principal stress difference at a specific point based on micro-area Raman spectroscopy or a finite element simulation model, and then back-calculating the scaling factor K, wherein the scaling factor K is calculated using the formula: K = (σ1) / (σ1) σ2) ref / δ ref ; where, (σ1 σ2) ref δ is the value of the actual principal stress difference at the specific point. ref The value of the actual first phase delay field at the specific point; substitute the obtained K value into (σ1) In the formula σ2)(x,y)=K·δ(x,y), we obtain (σ1) The value of σ²)(x,y).

[0009] Preferably, after processing the polarization image information to obtain the stress information of the off-axis single crystal layer, the method further includes: providing a preset threshold, obtaining a first region where the value of the principal stress difference is greater than or equal to the preset threshold, and marking the first region as a potential absence or crack region.

[0010] Preferably, the step of rotating the sample stage along the first direction and making the rotation angle of the sample stage equal to the off-axis angle, and the sample stage being located in the first position after rotation, includes: selecting a flat area on the sample stage not covered by the bonding wafer as a reference area; rotating the sample stage along the first direction and monitoring the average gray value of the reference area in real time, and finding the gray value minimum point as θ_center; obtaining the angle of θ_center; if θ_center is the same as the off-axis angle, then locking the sample stage and the sample stage being located in the first position; if θ_center is inconsistent with the off-axis angle, then verifying the levelness of the sample stage, finding the gray value minimum point again, and comparing θ_center with the off-axis angle.

[0011] Preferably, the transmission axis of the analyzer is a rotatable structure. The step of acquiring polarization image information when the sample stage is in the first position using the image detection component includes: acquiring polarization image information when the sample stage is in the first position and the angle between the transmission axis of the analyzer and the transmission axis of the polarizer is 0°, 90°, 180°, and 270° respectively; and the step of converting the polarization image information into a first phase delay field includes: converting the polarization image information into a continuous first phase delay field using a four-step phase shift method.

[0012] Preferably, a collimating beam expander is provided between the light source and the polarizer, and a quarter-wave plate is provided between the polarizer and the reflector.

[0013] Preferably, the first bonding layer is a 3C-SiC layer, the off-axis single crystal layer is a 4H-SiC layer, and the off-axis angle is 4°.

[0014] Compared with the prior art, the present invention adjusts the pitch angle of the sample stage so that the propagation direction of the light incident on the off-axis single crystal layer is parallel to the C-axis direction of the crystal, thereby removing strong background fringes caused by off-axis cutting and overcoming the inherent defect of "fringes even without stress" in traditional birefringence detection. Attached Figure Description

[0015] Figure 1 This is a structural diagram of the polarization optical path for stress detection of the single crystal layer of the bonded wafer in an embodiment of the present invention.

[0016] Figure 2 This is a structural diagram of the off-axis single crystal layer in an embodiment of the present invention.

[0017] Explanation of reference numerals in the attached diagram: 1. Light source; 2. Polarizer; 3. Mirror; 4. Sample stage; 5. Analyzer; 6. Image detection component; 7. Bonded wafer; 71. First bonding layer; 72. Off-axis single crystal layer; 721. Surface normal; 722. Crystal C-axis; 8. Collimating beam expander; 9. Quarter-wave plate; 10. Imaging lens. Detailed Implementation

[0018] To illustrate the technical content, structural features, and effects of the present invention in detail, the following description is provided in conjunction with the embodiments and accompanying drawings.

[0019] like Figures 1 to 2 As shown, this embodiment of the invention provides a stress detection method for a single crystal layer of a bonded wafer. The bonded wafer 7 includes a first bonding layer 71 and an off-axis single crystal layer 72 bonded to the first bonding layer 71. An off-axis angle θ is formed between the surface normal 721 of the off-axis single crystal layer 72 and its crystal C-axis 722. The stress detection method includes the following steps: S1. Construct a polarization optical path. The polarization optical path includes a light source 1, a polarizer 2, a reflector 3, a sample stage 4, an analyzer 5, and an image detection component 6 arranged sequentially along the optical path. The sample stage 4, analyzer 5, and image detection component 6 are all located below the light source 1, polarizer 2, and reflector 3. The bonding wafer 7 is confined on the sample stage 4. The sample stage 4 is horizontally positioned. The transmission axis of the polarizer 2 and the transmission axis of the analyzer 5 are perpendicular to each other. The light emitted from the light source 1 passes through the polarizer 2 and the reflector 3 and is perpendicularly incident on the sample stage 4. Specifically, the first bonding layer 71 is a 3C-SiC layer, and the off-axis single crystal layer 72 is a 4H-SiC layer. The off-axis angle θ is 4°. The off-axis single crystal layer 72 exhibits significant optical anisotropy. The light source 1 is an LED light source with a wavelength in the near-infrared band. The light emitted from the light source 1 passes sequentially through the polarizer 2, reflector 3, bonding wafer 7, and analyzer 5 before illuminating the image detection component 6. The image detection component 6 can be a CCD camera. In this embodiment, the sample stage 4 is horizontally positioned, i.e., the bonding wafer 7 is horizontally positioned. The light reflected by the reflector 3 is perpendicularly incident on the bonding wafer 7. The transmission axis of the polarizer 2 and the transmission axis of the analyzer 5 are perpendicular to each other so that the polarizer 2 and the analyzer 5 are in an orthogonal extinction state. It should be noted that in some other specific embodiments, the off-axis single crystal layer 72 can also be a 6H-SiC layer, etc., and the off-axis angle θ is determined according to the specific wafer cutting process.

[0020] S2, rotate the sample stage 4 along the first direction so that the rotation angle of the sample stage 4 is equal to the off-axis angle θ. After rotation, the sample stage 4 is in the first position, and the first direction is the direction from the crystal C-axis 722 toward the surface normal 721 of the off-axis single crystal layer 72. Specifically, the sample stage 4 has a five-axis adjustment function and can be adjusted for pitch. By rotating the sample stage 4 to the first position, the crystal C-axis 722 can be made parallel to the propagation direction of light incident on the off-axis single crystal layer 72, that is, the incident light propagates along the crystal C-axis 722. When the light propagates along the crystal C-axis 722, the ordinary refractive index n o With the extraordinary refractive index n e Equally, the inherent birefringence effect introduced by off-axis cutting is completely eliminated (Δn=0). Therefore, the first phase delay field δ(x,y) does not contain any inherent birefringence background noise and directly corresponds to the birefringence signal induced only by bonding stress.

[0021] S3, the polarization image information of the sample stage 4 when it is in the first position is obtained by the image detection component 6; specifically, when the sample stage 4 is in the first position, the bonding wafer 7 set on it is also tilted at the same angle.

[0022] S4, perform data processing on the polarization image information to obtain stress information of the off-axis single crystal layer 72.

[0023] This invention adjusts the pitch angle of the sample stage 4 so that the propagation direction of light incident on the off-axis single crystal layer 72 is parallel to the direction of the crystal C-axis 722, thereby removing strong background fringes caused by off-axis cutting and overcoming the inherent defect of "fringes even without stress" in traditional birefringence detection.

[0024] In this embodiment of the invention, step S2, rotating the sample stage 4 along the first direction and making the rotation angle of the sample stage 4 equal to the off-axis angle θ, and then positioning the sample stage 4 at the first position after rotation, includes: S21. Select a flat area on the sample stage 4 that is not covered by the bonding wafer 7 as the reference area.

[0025] S22. Rotate the sample stage 4 along the first direction and monitor the average gray value of the reference area in real time to find the gray value minimum point as θ_center; the gray value minimum point corresponds to the position where the incident light is closest to the C-axis 722 of the crystal, at which time the inherent birefringence background is the weakest.

[0026] S23. Obtain the angle θ_center. If θ_center is the same as the off-axis angle θ, lock the sample stage 4 and place the sample stage 4 in the first position. If θ_center is not the same as the off-axis angle θ, check the levelness of the sample stage 4, find the grayscale minimum point again, and compare θ_center with the off-axis angle θ. Specifically, in this embodiment of the invention, the off-axis angle θ is 4°, so the angle θ_center is also 4°.

[0027] In this embodiment of the invention, step S4, which involves processing the polarization image information to obtain the stress information of the off-axis single crystal layer 72, includes: S41. Perform data processing on the polarization image information and convert the polarization image information into a first phase delay field, specifically the first phase delay field is δ(x,y).

[0028] S42. Based on the first phase delay field, obtain the second phase delay field induced by the bonding stress between the first bonding layer 71 and the off-axis single crystal layer 72; specifically, the calculation formula for the second phase delay field δσ(x,y) is the first formula, which is: δσ(x,y)=δ(x,y).

[0029] S43. Based on the linear relationship between the second phase retardation field and the principal stress difference of the off-axis single-crystal layer 72, obtain the principal stress difference to acquire stress information of the off-axis single-crystal layer 72. Specifically, the linear relationship between the second phase retardation field and the principal stress difference is given by the second formula, which is: δσ(x,y)=4π·C eff (x,y)·(σ1 σ2)(x,y)·d eff (x,y) / λ; Among them, (σ1) σ²)(x,y) represents the principal stress difference, and C eff (x,y) represents the effective stress optical coefficient of the off-axis single crystal layer 72 in a specific crystal orientation, d eff (x,y) represents the equivalent depth of the stress-active layer, and λ is the wavelength of the light emitted by light source 1.

[0030] Further, in step S43 of this embodiment of the invention, based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer 72, the formula for obtaining the principal stress difference is the third formula, which is: (σ1 σ²)(x,y)=K·δ(x,y); Where K is the proportionality coefficient, K=λ / (4π·C) eff (x,y)·d eff (x,y)). The third formula can be obtained from the first and second formulas in the embodiments of this invention.

[0031] Further, in step S43 of this embodiment of the invention, the step of obtaining the stress information of the off-axis single crystal layer 72 by obtaining the principal stress difference based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer 72 includes: S431. Obtain the principal stress difference based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer 72.

[0032] S432. Based on the micro-area Raman spectroscopy or finite element simulation model, obtain the actual principal stress difference value at a specific point, and then deduce the scaling factor K. The formula for calculating the scaling factor K is the fourth formula, which is: K=(σ1 σ2) ref / δ ref ; Among them, (σ1) σ2) ref δ represents the actual principal stress difference at a specific point. ref This represents the actual first phase delay field value at a specific point. It should be noted that the actual principal stress difference values ​​obtained from micro-area Raman spectroscopy or finite element simulation models at specific points correspond to the values ​​obtained when sample stage 4 is in the first position.

[0033] S433, Substitute the obtained K value into (σ1) In the formula σ2)(x,y)=K·δ(x,y), we obtain (σ1) The values ​​of σ²)(x,y) are obtained, thus yielding the principal stress difference distribution.

[0034] In this embodiment of the invention, after step S4, which involves processing the polarization image information to obtain the stress information of the off-axis single crystal layer 72, the method further includes: S5 provides a preset threshold, identifies a first region where the principal stress difference is greater than or equal to the preset threshold, and marks the first region as a potential absence or crack region. Specifically, the first region can be correlated with bonding process parameters, such as bonding pressure, temperature gradient, and annealing curve, to output process optimization and adjustment instructions, thereby reducing the stress failure risk of subsequent batches of bonded wafers 7. Of course, in some other specific embodiments, if only qualitative screening of stress concentration risk is required, |Δδ(x,y)| can be directly used as the stress concentration index to generate a pseudo-color thermal map, which visually displays high-risk areas.

[0035] In this embodiment of the invention, the transmission axis of the analyzer 5 is a rotatable structure. Step S3, acquiring polarization image information of the sample stage 4 when it is in the first position using the image detection component 6, includes: S41. The image detection component 6 is used to acquire polarization image information when the sample stage 4 is in the first position and the angle between the transmission axis of the analyzer 5 and the transmission axis of the polarizer 2 is 0°, 90°, 180° and 270° respectively. That is, the four-step phase shift method is used to acquire multiple frames of images to eliminate the interference of light source 1 fluctuation and environmental noise.

[0036] In this embodiment of the invention, step S41, converting polarization image information into a first phase delay field, includes: S411. A four-step phase-shifting method is used to convert polarization image information into a continuous first phase delay field.

[0037] In this embodiment of the invention, a collimating beam expander 8 is provided between the light source 1 and the polarizer 2, and a quarter-wave plate 9 is provided between the polarizer 2 and the reflector 3. Specifically, by setting the collimating beam expander 8, the light emitted by the light source 1 can be converted into parallel light, and by setting the quarter-wave plate 9, the light can be converted into the desired polarized light. In addition, an imaging lens 10 is also provided between the analyzer 5 and the image detection component 6 to focus the light and increase the intensity of the light entering the image detection component 6.

[0038] The above-disclosed examples are merely preferred embodiments of the present invention and should not be construed as limiting the scope of the present invention. Therefore, any equivalent variations made in accordance with the claims of the present invention shall still fall within the scope of the present invention.

Claims

1. A method for stress detection of a single crystal layer in a bonded wafer, characterized in that: The bonded wafer includes a first bonding layer and an off-axis single-crystal layer bonded to the first bonding layer. The surface normal of the off-axis single-crystal layer forms an off-axis angle with its crystal C-axis. The stress detection method includes the following steps: S1, Construct a polarization optical path, which includes a light source, a polarizer, a mirror, a sample stage, an analyzer, and an image detection component arranged sequentially along the optical path. The sample stage, the analyzer, and the image detection component are all located below the light source, the polarizer, and the mirror. The bonding wafer is disposed on the sample stage, which is horizontally positioned. The transmission axis of the polarizer and the transmission axis of the analyzer are perpendicular to each other. The light emitted by the light source passes through the polarizer and the mirror and then is perpendicularly incident on the sample stage. S2, rotate the sample stage along the first direction and make the rotation angle of the sample stage equal to the off-axis angle. After the sample stage is rotated, it is located in the first position. The first direction is the direction of the crystal C-axis toward the surface normal of the off-axis single crystal layer. S3, using the image detection component to obtain polarization image information when the sample stage is in the first position; S4, perform data processing on the polarization image information to obtain the stress information of the off-axis single crystal layer.

2. The stress detection method for the single crystal layer of a bonded wafer as described in claim 1, characterized in that: The steps of processing the polarization image information to obtain the stress information of the off-axis single crystal layer include: The polarization image information is processed and converted into a first phase delay field; Based on the first phase delay field, a second phase delay field induced by bonding stress between the first bonding layer and the off-axis single crystal layer is obtained; Based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer, the principal stress difference is obtained to obtain the stress information of the off-axis single crystal layer.

3. The stress detection method for the single crystal layer of a bonded wafer as described in claim 2, characterized in that: The formula for calculating the second phase delay field δσ(x,y) is as follows: δσ(x,y)=δ(x,y), where δ(x,y) is the first phase delay field; The linear relationship between the second phase delay field and the principal stress difference is as follows: δσ(x,y)=4π·C eff (x,y)·(σ1 σ2)(x,y)·d eff (x,y) / λ; Among them, (σ1) σ²)(x,y) is the principal stress difference, C eff (x,y) represents the effective stress optical coefficient of the off-axis single crystal layer in a specific crystal orientation, d eff (x,y) represents the equivalent depth of the stress-active layer, and λ is the wavelength of the light emitted by the light source.

4. The stress detection method for the single crystal layer of a bonded wafer as described in claim 3, characterized in that: Based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer, the formula for obtaining the principal stress difference is as follows: (σ1 σ2)(x,y)=K·δ(x,y); Where K is the proportionality coefficient, K=λ / (4π·C) eff (x,y)·d eff (x,y)).

5. The stress detection method for the single crystal layer of a bonded wafer as described in claim 4, characterized in that: The step of obtaining the stress information of the off-axis single crystal layer by acquiring the principal stress difference based on the linear relationship between the second phase delay field and the principal stress difference includes: The principal stress difference is obtained based on the linear relationship between the second phase delay field and the principal stress difference of the off-axis single crystal layer; Based on the micro-area Raman spectroscopy or finite element simulation model, the actual principal stress difference at a specific point is obtained, and the scaling factor K is derived by reverse calculation. The formula for calculating the scaling factor K is as follows: K=(σ1 p2) ref / d ref ; Among them, (σ1) σ2) ref δ is the value of the actual principal stress difference at the specific point. ref The value of the actual first phase delay field at the specific point; Substitute the obtained K value into (σ1) In the formula σ2)(x,y)=K·δ(x,y), we obtain (σ1) The value of σ²)(x,y).

6. The stress detection method for the single crystal layer of a bonded wafer as described in claim 5, characterized in that: After processing the polarization image information to obtain the stress information of the off-axis single crystal layer, the method further includes: A preset threshold is provided to obtain a first region where the value of the principal stress difference is greater than or equal to the preset threshold, and the first region is marked as a potential absence or crack region.

7. The stress detection method for the single crystal layer of a bonded wafer as described in claim 1, characterized in that: The step of rotating the sample stage along the first direction and making the rotation angle of the sample stage equal to the off-axis angle, so that the sample stage is located in the first position after rotation, includes: A flat area on the sample stage that is not covered by the bonding wafer is selected as a reference area; Rotate the sample stage along the first direction and monitor the average gray value of the reference area in real time to find the gray value minimum point as θ_center; Obtain the angle θ_center. If θ_center is the same as the off-axis angle, lock the sample stage and place it in the first position. If θ_center is not the same as the off-axis angle, check the levelness of the sample stage, find the grayscale minimum point again, and compare θ_center with the off-axis angle.

8. The stress detection method for the single crystal layer of a bonded wafer as described in claim 5, characterized in that: The transmittance axis of the analyzer is a rotatable structure. The step of acquiring polarization image information when the sample stage is in the first position using the image detection component includes: The image detection component acquires polarization image information when the sample stage is in a first position and the angles between the transmission axis of the analyzer and the transmission axis of the polarizer are 0°, 90°, 180°, and 270°, respectively; and... The step of converting the polarization image information into a first phase delay field includes: The polarization image information is converted into a continuous first phase delay field using a four-step phase shifting method.

9. The stress detection method for the single crystal layer of a bonded wafer as described in claim 1, characterized in that: A collimating beam expander is provided between the light source and the polarizer, and a quarter-wave plate is provided between the polarizer and the reflector.

10. The stress detection method for the single crystal layer of a bonded wafer as described in claim 1, characterized in that: The first bonding layer is a 3C-SiC layer, the off-axis single crystal layer is a 4H-SiC layer, and the off-axis angle is 4°.