A board-level fan-out package structure and a packaging process

By mounting and encapsulating a metal block on the back of the chip before molding, the synergistic effect of the metal block and molding compound solves the problems of warpage control and high heat dissipation in board-level fan-out packaging, achieving low warpage and high heat dissipation, and simplifying the manufacturing process.

CN123076296APending Publication Date: 2026-11-10JIANGSU PANGU SEMICONDUCTOR TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611520950.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Traditional board-level fan-out packaging struggles to simultaneously address warpage control and high heat dissipation requirements, especially in the field of large-size, high-computing-power and high-power chips. Existing technologies suffer from mismatches between warpage control and heat dissipation structures, as well as high interface thermal resistance.

Method used

Before molding, a metal block is mounted on the back of the chip and covered by the molding layer. After grinding, it is exposed. The high CTE of the metal block and the molding material are used to balance the warpage introduced by the redistribution layer stack, while building a low thermal resistance heat dissipation channel.

Benefits of technology

It achieves both low warpage and high heat dissipation in board-level fan-out packaging, meeting the heat dissipation requirements of large-size high-power chips, and simplifies the manufacturing process, improving packaging yield and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076296A_ABST
    Figure CN123076296A_ABST
Patent Text Reader

Abstract

This invention discloses a board-level fan-out packaging structure and packaging process. The packaging structure includes: a redistribution layer stack, the redistribution layer stack including multiple metal wiring layers and a passivation insulating layer covering the metal wiring layers; a chip flip-chip mounted on the redistribution layer stack via metal pillars; an underfill filling between the chip and the redistribution layer stack; a metal block mounted on the back side of the chip via a conductive and thermally conductive adhesive layer; and a molding compound layer covering the chip, the underfill, the conductive and thermally conductive adhesive layer, and the metal block; the top surface of the metal block is exposed from the molding compound layer by grinding. This invention achieves both low warpage and high heat dissipation in a board-level fan-out packaging by mounting the metal block on the back side of the chip before molding and exposing it by being covered by the molding compound layer and then grinding it. The high CTE of the metal block and the molding compound work together to balance the warpage introduced by the redistribution layer stack, while simultaneously constructing a low thermal resistance heat dissipation channel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor packaging technology, specifically relating to a board-level fan-out packaging structure and packaging process. Background Technology

[0002] Traditional FCBGA, FCCSP, and FCLGA packaging are primarily based on two major process frameworks: wafer-level bumping and substrate mounting. They are widely used in large-size, high-performance chips and high-power heat dissipation devices. In recent years, with the rapid development of applications such as 5G communication, artificial intelligence, and high-performance computing, the computing power density and power density of chips have continued to rise, placing higher demands on the electrical performance, heat dissipation capabilities, and reliability of packaging structures. However, limited substrate production capacity and their highly customized nature make it difficult for traditional packaging solutions to meet the ever-increasing demands for computing power and heat dissipation.

[0003] Fan-out board-level packaging (FOPLP), with its excellent packaging efficiency and flexible wiring design, has significantly alleviated the pain point of insufficient substrate production capacity while improving packaging performance, and has become an important development direction in the field of advanced packaging. However, these high-performance and high-power chips typically have two main characteristics: first, they are relatively large in size, especially FCBGA products, whose package dimensions are generally larger than 10×10mm; second, they have strong heat dissipation requirements, and the heat generated during chip operation needs to be efficiently dissipated. This places high technical demands on fan-out board-level packaging.

[0004] Specifically, board-level fan-out packaging faces a technical bottleneck in simultaneously achieving warpage control and heat dissipation performance. On the one hand, the coefficients of thermal expansion (CTE) of materials such as the chip, molding compound, redistribution layer, and substrate in the package structure differ, generating thermal stress during temperature changes and causing the package to warp. The large area of ​​board-level packages exacerbates the absolute deformation and in-plane non-uniformity of warpage, severely impacting subsequent mounting and reliability. On the other hand, large-size, high-power chips have long heat dissipation paths. Relying solely on molding compound and redistribution layers for heat conduction results in high thermal resistance, making it difficult to meet high heat dissipation requirements. While existing technologies have attempted to place heat sinks or metal blocks on the back of the chip, these often suffer from problems such as mismatch between the heat dissipation structure and the molding process sequence, high interface thermal resistance, and mutual constraints between warpage control and heat dissipation function, making it difficult to simultaneously achieve good warpage control and high heat dissipation performance at the board-level.

[0005] Therefore, board-level fan-out packaging has not yet achieved significant breakthroughs in the aforementioned high-computing-power and high-power chip fields, and there is an urgent need for a board-level fan-out packaging structure and process that can simultaneously address warp control and high heat dissipation requirements. Summary of the Invention

[0006] To address the aforementioned technical problems, the present invention aims to provide a board-level fan-out packaging structure and packaging process. The present invention involves mounting a metal block onto the back of the chip before molding, encapsulating it with a molding layer, and then exposing it after grinding. The high CTE of the metal block, in conjunction with the molding compound, balances the warpage introduced by the redistribution layer stack, while simultaneously constructing a low thermal resistance heat dissipation channel. This achieves both low warpage and high heat dissipation in the board-level fan-out packaging.

[0007] To achieve the above-mentioned technical objectives and effects, the present invention is implemented through the following technical solution: This invention provides a board-level fan-out packaging structure, comprising: A redistribution layer stack, the redistribution layer stack comprising multiple metal wiring layers and a passivation insulating layer covering the metal wiring layers; A chip flip-chip mounted on the redistribution layer using metal protrusions; Underfill adhesive between the chip and the redistribution layer stack; A metal block is attached to the back of the chip via a conductive and thermally conductive adhesive layer; And a molding compound covering the chip, the underfill, the conductive and thermally conductive adhesive layer, and the metal block; The top surface of the metal block is exposed from the plastic sealant by grinding.

[0008] Furthermore, the planar dimensions of the metal block satisfy: 0.9 times X 芯片 ≤X 金属块 ≤X 重布线层叠层 0.9 times Y 芯片 ≤Y 金属块 ≤Y 重布线层叠层 , where X 重布线层叠层 Y 重布线层叠层 These are the dimensions of the rewiring layer stack in the X and Y directions, respectively. 芯片 Y 芯片 These are the dimensions of the chip in the X and Y directions, respectively. 金属块 Y 金属块 These are the dimensions of the metal block in the X and Y directions, respectively.

[0009] Furthermore, the top surface of the metal block is flush with the top surface of the plastic encapsulation layer, and the top surface of the metal block is a flat surface that has been ground, for welding to the external heat sink.

[0010] Furthermore, the underfill, the conductive and thermally conductive adhesive layer, and the molding compound form a continuous organic material system. The metal protrusions and the metal blocks are located on the front and back sides of the chip, respectively, and together apply stress compensation to the chip during the curing process of the molding compound.

[0011] Furthermore, the packaging structure includes multiple chips, each with an independently disposed metal block on its back. The thickness and / or planar dimensions of the metal blocks for different chips are set differently according to their positions to achieve uniform compensation for in-plane warping.

[0012] Another aspect of the present invention provides a board-level fan-out packaging process, comprising the following steps: A temporary carrier plate is provided, and a temporary bonding layer is formed on the temporary carrier plate; A redistribution layer stack is formed on the temporary bonding layer, the redistribution layer stack comprising multiple metal wiring layers and a passivation insulating layer covering the metal wiring layers; The chip is flip-chip bonded to the redistribution layer using metal protrusions; An underfill is filled between the chip and the redistribution layer stack; A metal block is attached to the back of the chip using a conductive and thermally conductive adhesive layer. The chip, the underfill, the conductive and thermally conductive adhesive layer, and the metal block are encapsulated to form an encapsulation layer covering the metal block; The molding layer is ground to expose the top surface of the metal block; Remove the temporary carrier and the temporary bonding layer.

[0013] Furthermore, the process of forming the redistribution layer stack is as follows: a metal wiring layer is formed on the temporary bonding layer by a patterned metal deposition process, a passivation insulating layer is formed on the metal wiring layer, and an opening is made in the passivation insulating layer to expose the metal wiring layer. The above steps are repeated to form a multilayer redistribution layer stack.

[0014] Furthermore, before mounting the metal block, the underfill adhesive has been filled and cured, and the size of the conductive and thermally conductive adhesive layer is slightly smaller than the back surface size of the chip to prevent adhesive overflow from affecting the uniformity of subsequent molding.

[0015] Furthermore, the molding material used for molding is a liquid or powder with an adjustable coefficient of thermal expansion and modulus, so that the coefficient of thermal expansion of the composite consisting of the molding layer, the underfill, the chip, and the metal block after molding matches the coefficient of thermal expansion of the composite consisting of the redistribution layer.

[0016] Furthermore, the chip is a chip with a pre-processed structure, the pre-processed structure including metal protrusions formed on the front side of the chip body, and the chip is flip-chip bonded to the redistribution layer through the metal protrusions of the pre-processed structure.

[0017] The beneficial effects of this invention are as follows: This invention mounts a metal block onto the back of the chip before molding, so that the metal block is covered by the molding layer and then exposed by grinding. The high CTE of the metal block and the molding material work together to balance the warpage introduced by the redistribution layer stack, while building a low thermal resistance heat dissipation channel, thereby achieving both low warpage and high heat dissipation in a board-level fan-out package.

[0018] Specifically, the metal block is mounted on the back of the chip via a conductive and thermally conductive adhesive layer and is encapsulated by a molding compound. During the curing and shrinkage process of the molding compound, the metal block, molding compound, underfill, and chip together form a composite. The high CTE of the metal block generates a bending moment opposite to the stacking direction of the redistribution layers. This bending moment begins to act during the molding curing stage, interacting with the shrinkage stress of the molding compound at the same stage, rather than being passively added after molding is completed. This reduces the warpage of the package after cooling to room temperature.

[0019] Meanwhile, the metal protrusions are located on the front side of the chip, and the metal block is located on the back side. Both are rigid metal structures, forming a continuous organic material system with the underfill, conductive and thermally conductive adhesive layer, and molding layer, respectively. During the curing process of the molding layer, the metal protrusions and the metal block jointly apply stress compensation to the chip, and the bending moments on both sides of the chip tend to be balanced, avoiding the introduction of new warping modes due to the rigid structure on one side.

[0020] The top surface of the metal block is exposed from the molding compound through grinding, making direct contact with the outside environment. Heat from the chip is conducted through the chip body to the conductive and thermally conductive adhesive layer, then to the metal block, and finally dissipated through the top surface of the metal block. This heat dissipation path has lower thermal resistance than paths relying solely on the molding compound and redistribution layers, meeting the heat dissipation requirements of large-size, high-power chips. The exposed, flat metal surface also facilitates subsequent soldering of external heat sinks.

[0021] At the process level, the metal block mounting step is placed before the molding process, ensuring the metal block is in place while the molding compound is curing and shrinking. After the molding compound encapsulates the metal block, the two form an integrated composite. The thermal expansion behavior of the metal block and the curing and shrinkage of the molding compound interact in the same stage, achieving in-situ stress control during the molding process. The grinding step to expose the metal block is performed directly after molding, compatible with board-level grinding processes, eliminating the need for additional mounting or windowing processes. Compared to the scheme of molding first and then mounting the heat sink, it eliminates the alignment and fixing steps of secondary mounting after molding, resulting in a shorter process chain. After removing the temporary carrier and temporary bonding layer, a complete package structure is obtained, with the redistribution layer as the wiring basis, the chip flipped on it, and the metal block placed on the back of the chip with the top surface exposed. This process sequence is compatible with existing equipment and process frameworks for board-level fan-out packaging. Metal block mounting can be performed using surface mounting, bonding, and other methods without significant changes to the production line configuration, which helps improve the yield and production efficiency of board-level packaging. Attached Figure Description

[0022] Figure 1This is a schematic diagram of steps one and two of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0023] Figure 2 This is a schematic diagram of step three of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0024] Figure 3 This is a schematic diagram of step four of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0025] Figure 4 This is a schematic diagram of step five of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0026] Figure 5 This is a schematic diagram of step six of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0027] Figure 6 This is a schematic diagram of step seven of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0028] Figure 7 This is a schematic diagram of step eight of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0029] Figure 8 This is a schematic diagram of step nine of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0030] Figure 9 This is a schematic diagram of step ten of the board-level fan-out packaging process in Embodiment 1 of the present invention.

[0031] Figure 10 This is a schematic diagram of the board-level fan-out packaging structure of Embodiment 2 of the present invention.

[0032] In the diagram, 100: Temporary carrier; 200: Temporary bonding layer; 300: Redistribution layer stack; 310: Metallic wiring layer; 320: Passivation insulating layer; 330: Window; 400: Chip; 410: Chip body; 420: Solder cap; 430: Metal protrusion; 500: Underfill; 600: Conductive and thermally conductive adhesive layer; 700: Metal block; 800: Molding layer; 900: Solder ball. Detailed Implementation

[0033] The technical solutions of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] Reference Figure 9 and Figure 10As shown, the present invention provides a board-level fan-out packaging structure. Exemplarily, the packaging structure includes a redistribution layer 300, a chip 400, an underfill 500, a metal block 700, and a molding compound 800.

[0035] The redistribution layer stack 300 includes multiple metal wiring layers 310 and a passivation insulating layer 320 covering the metal wiring layers 310. Preferably, the metal wiring layers 310 are made of copper, and the passivation insulating layer 320 is made of insulating dry film or photosensitive insulating material. The number of layers in the redistribution layer stack 300 can be determined according to the integrated circuit product design, for example, 2, 3, 4 or more layers.

[0036] The chip 400 is a chip with a pre-processed structure. The pre-processed structure includes metal protrusions 430 formed on the front side of the chip body 410, and solder caps 420 disposed on the top of the metal protrusions 430. The chip 400 is flip-chip bonded to the redistribution layer 300 through the metal protrusions 430 and the solder caps 420. For example, the metal protrusions 430 are copper metal protrusions.

[0037] The underfill adhesive 500 fills the gap between the chip 400 and the redistribution layer 300 to cover the metal protrusion 430 and enhance connection reliability.

[0038] The metal block 700 is attached to the back side of the chip 400 via a conductive and thermally conductive adhesive layer 600. For example, the metal block 700 is a copper block, and the conductive and thermally conductive adhesive layer 600 is a conductive adhesive, conductive silver paste, or conductive DAF. Preferably, the size of the conductive and thermally conductive adhesive layer 600 is slightly smaller than the back side size of the chip 400 to prevent adhesive overflow from affecting the uniformity of subsequent molding.

[0039] The molding compound 800 encapsulates the chip 400, the underfill 500, the conductive and thermally conductive adhesive layer 600, and the metal block 700. The top surface of the metal block 700 is exposed from the molding compound 800 by grinding. Exemplarily, the top surface of the metal block 700 is flush with the top surface of the molding compound 800, and the top surface of the metal block 700 is a smooth, ground surface for soldering to an external heat sink.

[0040] Preferably, the planar dimensions of the metal block 700 satisfy: 0.9 × X 芯片 ≤X 金属块 ≤X 重布线层叠层 0.9×Y 芯片 ≤Y 金属块 ≤Y 重布线层叠层 , where X 重布线层叠层 Y 重布线层叠层The dimensions of the redistribution layer stack 300 in the X and Y directions are respectively, and the dimensions of the chip 400 in the X and Y directions are respectively. 金属块 Y 金属块 These are the dimensions of the metal block 700 in the X and Y directions, respectively.

[0041] For example, the underfill 500, the conductive and thermally conductive adhesive layer 600 and the molding compound 800 form a continuous organic material system, and the metal protrusion 430 and the metal block 700 are located on the front side and the back side of the chip 400, respectively, and together apply stress compensation to the chip 400 during the curing process of the molding compound 800.

[0042] Preferably, the packaging structure includes multiple chips 400, each chip 400 having an independently disposed metal block 700 on its back side. The thickness and / or planar dimensions of the metal blocks 700 on different chips 400 are differentiated according to their positions on the redistribution layer stack to achieve uniform warpage compensation. For example, chips 400 located at the edge region of the redistribution layer stack may be configured with thicker or larger metal blocks 700, while chips 400 located in the central region of the redistribution layer stack may be configured with thinner or smaller metal blocks 700.

[0043] Reference Figures 1 to 10 As shown, the present invention provides a board-level fan-out packaging process. Exemplarily, the process includes the following steps: Step 1: Provide a temporary carrier board 100.

[0044] For example, the temporary carrier plate 100 is made of metal, glass, or composite material.

[0045] Step 2: Form a temporary bonding layer 200 on the temporary carrier plate 100.

[0046] For example, the temporary bonding layer 200 includes, but is not limited to, a pyrolytic temporary bonding film, a temporary bonding adhesive, a separable copper foil, or a separable double-sided adhesive.

[0047] Step 3: Form a redistribution layer stack 300 on the temporary bonding layer 200.

[0048] The redistribution stack 300 includes multiple metal wiring layers 310 and a passivation insulating layer 320 covering the metal wiring layers 310. Exemplarily, the redistribution stack 300 is formed as follows: a metal wiring layer 310 is formed on the temporary bonding layer 200 using a patterned metal deposition process; a passivation insulating layer 320 is formed on the metal wiring layer 310; and an opening 330 is formed in the passivation insulating layer 320 to expose the metal wiring layer 310. These steps are repeated to form the multiple redistribution stack 300.

[0049] Preferably, the patterned metal deposition process includes sequentially performing seed layer metallization, film lamination, exposure, development, electroplating, film removal, and seed layer removal. The passivation insulating layer 320 is formed by methods including, but not limited to, vacuum lamination or slot coating, and the window 330 is formed by laser drilling or exposure and development.

[0050] Step 4: The chip 400 is flip-chip soldered onto the redistribution layer 300 using metal protrusions 430.

[0051] For example, the chip 400 is a chip with a pre-processed structure, which includes metal protrusions 430 formed on the front side of the chip body 410 and solder caps 420 disposed on the top of the metal protrusions 430. For example, the metal protrusions 430 are copper metal protrusions. The chip 400 is flip-chip bonded onto the redistribution layer 300 using this pre-processed structure.

[0052] Step 5: Fill the space between the chip 400 and the redistribution layer 300 with underfill adhesive 500.

[0053] For example, an underfill adhesive 500 is filled into the gap between the chip 400 and the redistribution layer 300 using a dispensing machine.

[0054] Step 6: Mount the metal block 700 on the back of the chip 400 using a conductive and thermally conductive adhesive layer 600.

[0055] For example, a conductive and thermally conductive adhesive layer 600 is formed on the back side of the chip 400. The conductive and thermally conductive adhesive layer 600 includes, but is not limited to, conductive adhesive, conductive silver paste, or conductive DAF. The formation method can be dispensing or stencil or screen printing. For process design, the size of the conductive and thermally conductive adhesive layer 600 is slightly smaller than the back side size of the chip 400.

[0056] A pre-prepared metal block 700 is bonded to the conductive and thermally conductive adhesive layer 600. The metal block 700 can be configured with different thicknesses according to product requirements. Preferably, the planar dimensions of the metal block 700 satisfy: 0.9 × X 芯片 ≤X 金属块 ≤X 重布线层叠层 0.9×Y 芯片 ≤Y 金属块 ≤Y 重布线层叠层 .

[0057] Preferably, the underfill adhesive 500 has been filled and cured before the metal block 700 is mounted, so as to prevent the underfill adhesive 500 from flowing in subsequent processes and affecting the mounting accuracy of the metal block 700.

[0058] Step 7: Encapsulate the chip 400, the underfill 500, the conductive and thermally conductive adhesive layer 600, and the metal block 700.

[0059] For example, the chip 400, the underfill 500, the conductive and thermally conductive adhesive layer 600, and the metal block 700 are encapsulated by compression molding to form a molding compound 800 covering the metal block 700. The molding compound material can be liquid or powder, and its coefficient of thermal expansion and modulus are adjustable. It is combined with the conductive and thermally conductive adhesive layer 600, the underfill 500, and the chip 400 to form a whole. The composite coefficient of thermal expansion of this whole should be close to the composite coefficient of thermal expansion of the redistribution layer stack 300.

[0060] Step 8: Grind the molding layer 800 to expose the top surface of the metal block 700.

[0061] For example, the top surface of the metal block 700 is exposed by plate-level grinding technology, so that the top surface of the metal block 700 is flush with the top surface of the molding layer 800, and the top surface of the metal block 700 is a flat surface that has been ground, which facilitates subsequent welding with external heat sinks.

[0062] Step 9: Remove the temporary carrier 100 and the temporary bonding layer 200.

[0063] For example, depending on the type of temporary bonding material used in step two, the corresponding debonding method is used to release the bonding effect of the temporary bonding layer 200 and remove the temporary carrier plate 100.

[0064] Step 10: Form solder balls 900 for external soldering.

[0065] For example, board-level balling technology is used to form solder balls 900 for external soldering. Alternatively, depending on the product type, the structure after removing the temporary carrier board 100 can be retained directly.

[0066] Example 1

[0067] Reference Figures 1 to 9 As shown, this embodiment provides a board-level fan-out packaging structure and its packaging process.

[0068] The packaging structure includes a redistribution layer 300, a chip 400, an underfill 500, a metal block 700, and a molding compound 800. The redistribution layer 300 includes four metal wiring layers 310 and a passivation insulating layer 320 covering each metal wiring layer 310. The metal wiring layers 310 are made of copper with a single-layer thickness of 5 μm, and the passivation insulating layer 320 is made of insulating dry film with a single-layer thickness of 10 μm. The overall planar dimensions of the redistribution layer 300 are 12 mm × 12 mm. The chip 400 is a silicon-based chip with a planar dimension of 6 mm × 6 mm, flip-chip mounted on the redistribution layer 300 via metal protrusions 430. The underfill 500 is an epoxy-based underfill, filling the space between the chip 400 and the redistribution layer 300, and covering the metal protrusions 430. The metal block 700 is a copper block with a planar dimension of 8mm × 8mm. It is mounted on the back of the chip 400 via a conductive and thermally conductive adhesive layer 600. The conductive and thermally conductive adhesive layer 600 is a conductive silver paste with a printed size of 5.5mm × 5.5mm, slightly smaller than the chip's back dimension of 6mm × 6mm. The molding compound 800 encapsulates the chip 400, the underfill 500, the conductive and thermally conductive adhesive layer 600, and the metal block 700. The molding compound is epoxy molding compound, and its coefficient of thermal expansion and modulus are adjusted by adding silica filler. This results in a composite material with a coefficient of thermal expansion of approximately 9.5ppm / ℃, matching the composite material with a redistribution layer stack 300 (approximately 10ppm / ℃). The top surface of the metal block 700 is exposed from the molding compound 800 through grinding and is flush with the top surface of the molding compound 800.

[0069] The packaging process in this embodiment includes the following steps: Step 1: Provide a glass carrier plate as a temporary carrier plate 100.

[0070] Step 2: A pyrolytic temporary bonding film is formed on the temporary carrier plate 100 as a temporary bonding layer 200, such as... Figure 1 As shown.

[0071] Step 3: As Figure 2 As shown, a redistribution layer stack 300 is formed on the temporary bonding layer 200. Specifically, a first metal wiring layer 310, made of copper and 5 μm thick, is formed on the temporary bonding layer 200 using a patterned metal deposition process. A passivation insulating layer 320, made of insulating dry film and 10 μm thick, is formed on the first metal wiring layer 310, and an opening 330 is formed in the passivation insulating layer 320 to expose the first metal wiring layer 310. The above steps are repeated to form four metal wiring layers 310 and corresponding passivation insulating layers 320, resulting in a redistribution layer stack 300 with an overall planar dimension of 12 mm × 12 mm.

[0072] Step Four: As Figure 3 As shown, a chip 400 with a pre-processed structure is flip-chip bonded to a redistribution layer 300. The pre-processed structure includes metal protrusions 430 (copper pillars) and solder caps 420 formed on the front side of the chip body 410. The chip 400 is flip-chip bonded to the redistribution layer 300 using this pre-processed structure. The chip 400 has a planar dimension of 6mm × 6mm.

[0073] Step 5: As Figure 4 As shown, an underfill 500 is filled between the chip 400 and the redistribution layer 300 and then cured.

[0074] Step Six: As Figure 5 As shown, a metal block 700 is mounted on the back of chip 400 using a conductive and thermally conductive adhesive layer 600. The conductive and thermally conductive adhesive layer 600 is made of conductive silver paste and has a printing size of 5.5mm × 5.5mm. The metal block 700 is made of copper and has a planar size of 8mm × 8mm.

[0075] Step Seven: As Figure 6 As shown, the chip 400, the underfill 500, the conductive and thermally conductive adhesive layer 600 and the metal block 700 are encapsulated to form an encapsulation layer 800 covering the metal block 700.

[0076] Step 8: As Figure 7 As shown, the molding layer 800 is ground to expose the top surface of the metal block 700. After grinding, the top surface of the metal block 700 is flush with the top surface of the molding layer 800.

[0077] Step Nine: Figure 8 As shown, the temporary carrier 100 and the temporary bonding layer 200 are removed.

[0078] Step 10: As Figure 9 As shown, solder balls 900 are formed on the side of the redistribution layer stack 300 away from the chip 400.

[0079] Example 2

[0080] like Figure 10 As shown, this embodiment 2 provides another board-level fan-out packaging structure. The difference from embodiment 1 is that: the planar dimensions of the metal block 700 are consistent with the planar dimensions of the chip 400; the chip 400 is a GaN or SiC power device chip; and the thickness of the metal block 700 is ≥150μm.

[0081] In this embodiment, the planar dimensions of the metal block 700 are the same as those of the chip 400, i.e., X 金属块 =X 芯片 Y 金属块 =Y 芯片For example, if chip 400 is a GaN power device chip with a planar dimension of 5mm × 5mm, then the planar dimension of metal block 700 is also 5mm × 5mm. Metal block 700 is a copper block with a thickness of 200μm to meet the high heat capacity requirements generated by chip 400 during instantaneous operation. Due to the larger thickness of metal block 700, its heat capacity is correspondingly increased, allowing it to absorb more heat during the instantaneous high-power operation of chip 400, thus reducing chip temperature rise.

[0082] The remaining structures, including the redistribution layer 300, the underfill 500, the conductive and thermally conductive adhesive layer 600, the molding compound 800, their positional relationships and materials, and the packaging process steps, are the same as in Example 1 and will not be described again. In this example, the metal block thickness is ≥150μm, and the planar dimensions are consistent with the chip, making it suitable for board-level fan-out packaging of GaN, SiC, and other power device chips 400.

[0083] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

[0084] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A board-level fan-out packaging structure, characterized in that, include: A redistribution layer stack, the redistribution layer stack comprising multiple metal wiring layers and a passivation insulating layer covering the metal wiring layers; A chip flip-chip mounted on the redistribution layer using metal protrusions; Underfill adhesive between the chip and the redistribution layer stack; A metal block is attached to the back of the chip via a conductive and thermally conductive adhesive layer; And a molding compound covering the chip, the underfill, the conductive and thermally conductive adhesive layer, and the metal block; The top surface of the metal block is exposed from the plastic sealant by grinding.

2. The board-level fan-out packaging structure according to claim 1, characterized in that, The planar dimensions of the metal block satisfy: 0.9 times X 芯片 ≤X 金属块 ≤X 重布线层叠层 0.9 times Y 芯片 ≤Y 金属块 ≤Y 重布线层叠层 , where X 重布线层叠层 Y 重布线层叠层 These are the dimensions of the rewiring layer stack in the X and Y directions, respectively. 芯片 Y 芯片 These are the dimensions of the chip in the X and Y directions, respectively. 金属块 Y 金属块 These are the dimensions of the metal block in the X and Y directions, respectively.

3. The board-level fan-out packaging structure according to claim 1, characterized in that, The top surface of the metal block is flush with the top surface of the plastic encapsulation layer, and the top surface of the metal block is a flat surface that has been ground, for welding to the external heat sink.

4. The board-level fan-out packaging structure according to claim 1, characterized in that, The underfill, the conductive and thermally conductive adhesive layer, and the molding compound form a continuous organic material system. The metal protrusions and the metal blocks are located on the front and back sides of the chip, respectively, and together apply stress compensation to the chip during the curing process of the molding compound.

5. The board-level fan-out packaging structure according to claim 1, characterized in that, It includes multiple chips, each with an independently placed metal block on its back. The thickness and / or planar dimensions of the metal blocks for different chips are set differently according to their positions to achieve uniform compensation for in-plane warping.

6. A board-level fan-out packaging process, characterized in that, Includes the following steps: A temporary carrier plate is provided, and a temporary bonding layer is formed on the temporary carrier plate; A redistribution layer stack is formed on the temporary bonding layer, the redistribution layer stack comprising multiple metal wiring layers and a passivation insulating layer covering the metal wiring layers; The chip is flip-chip bonded to the redistribution layer using metal protrusions; An underfill is filled between the chip and the redistribution layer stack; A metal block is attached to the back of the chip using a conductive and thermally conductive adhesive layer. The chip, the underfill, the conductive and thermally conductive adhesive layer, and the metal block are encapsulated to form an encapsulation layer covering the metal block; The molding layer is ground to expose the top surface of the metal block; Remove the temporary carrier and the temporary bonding layer.

7. The board-level fan-out packaging process according to claim 6, characterized in that, The process of forming the redistribution layer stack is as follows: a metal wiring layer is formed on the temporary bonding layer by a patterned metal deposition process, a passivation insulating layer is formed on the metal wiring layer, and an opening is made in the passivation insulating layer to expose the metal wiring layer. The above steps are repeated to form the redistribution layer stack.

8. The board-level fan-out packaging process according to claim 6, characterized in that, Before mounting the metal block, the underfill adhesive has been filled and cured, and the size of the conductive and thermally conductive adhesive layer is slightly smaller than the back surface size of the chip.

9. The board-level fan-out packaging process according to claim 6, characterized in that, The molding material used is a liquid or powder with adjustable coefficient of thermal expansion and modulus, so that the coefficient of thermal expansion of the composite consisting of the molding layer, the underfill, the chip and the metal block after molding matches the coefficient of thermal expansion of the composite consisting of the redistribution layer.

10. The board-level fan-out packaging process according to claim 6, characterized in that, The chip is a chip with a pre-processed structure. The pre-processed structure includes metal protrusions formed on the front side of the chip body. The chip is flip-chip bonded to the redistribution layer through the metal protrusions of the pre-processed structure.