Fluorinated ether compounds, coatings, lubricants for magnetic recording media, and magnetic recording media

By introducing fluoroether compounds with appropriately spaced alkylene chains and hydroxyl groups at both ends of the perfluoropolyether chain, the wear resistance and spin-off problems of thin lubricating layers are solved, achieving high durability and reliability of magnetic recording media.

CN123076580APending Publication Date: 2026-11-10RESONAC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202580025578.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-16
Filing Date
2025-04-16
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In magnetic recording and reproducing devices, the required lift of the magnetic head is smaller, and when the thickness of the lubricating layer is thin, the wear resistance is reduced, making it easy for the magnetic head to detach, which leads to a decrease in the durability of the magnetic recording medium.

Method used

Using fluorinated ether compounds with specific structures as lubricants, and introducing alkylene chains and hydroxyl groups at appropriate distances at both ends of the perfluoropolyether chain, the adhesion to the protective layer is improved, forming a lubricating layer with excellent wear resistance and spin-off resistance.

Benefits of technology

Even with a thin lubricating layer, it can effectively prevent film thickness reduction and improve the wear resistance and durability of magnetic recording media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076580A_ABST
    Figure CN123076580A_ABST
Patent Text Reader

Abstract

This fluorinated ether compound is produced by R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 [-CH2-R] 4 -CH2-R 3 ] x -CH2-O-(CH2) z -Y-R 5 -R 6 (x is 0 to 2; z is an integer from 2 to 10; Y is any one of 0, NH, and S; R) 3 It is a perfluoropolyether chain; R 4 It is a divalent linker with 1 to 3 hydroxyl groups and oxygen atoms at both ends; R 2 For equation (2-1) or (2-2); R 5 For equation (2-3) or (2-4); R 1 and R 6 (terminal group).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to fluorinated ether compounds, coatings, lubricants for magnetic recording media, and magnetic recording media.

[0002] This application asserts priority based on Japanese Patent Application No. 2024-066210 filed on April 16, 2024, the contents of which are incorporated herein by reference. Background Technology

[0003] Progress has been made in the development of magnetic recording media suitable for high recording density in order to increase the recording density in magnetic recording reproduction devices.

[0004] Traditionally, magnetic recording media consist of a recording layer formed on a substrate, upon which a protective layer, such as carbon, is formed. This protective layer protects the information recorded on the recording layer and improves the smoothness of the magnetic head. However, simply providing a protective layer on the recording layer is insufficient to achieve adequate durability of the magnetic recording medium. Therefore, generally, a lubricant is applied to the surface of the protective layer to form a lubricating layer.

[0005] As a lubricant used in forming a lubricating layer of a magnetic recording medium, for example, a substance containing a compound having polar groups such as hydroxyl or amino groups at the end of a fluorine-based polymer having a repeating structure containing -CF2- is proposed.

[0006] For example, patent documents 1, 3, and 4 disclose fluorinated ether compounds in which a linker combining an ether bond (-O-), a methylene group (-CH2-), and a methylene group with one hydrogen atom replaced by a hydroxyl group (-CH(OH)-) is configured between the perfluoropolyether chain and the two end groups.

[0007] Patent document 2 discloses a fluorinated ether compound having multiple hydroxyl groups at both ends.

[0008] Existing technical documents

[0009] Patent documents

[0010] Patent Document 1: International Publication No. 2021 / 251318

[0011] Patent Document 2: Japanese Patent No. 5334064

[0012] Patent Document 3: International Publication No. 2019 / 054148

[0013] Patent Document 4: International Publication No. 2021 / 090940 Summary of the Invention

[0014] The problem that the invention aims to solve

[0015] In magnetic recording playback devices, it is required to minimize the upward movement of the magnetic head. Therefore, it is necessary to reduce the thickness of the lubricating layer in the magnetic recording medium. However, generally speaking, a thinner lubricating layer tends to have reduced wear resistance. Reduced wear resistance of the lubricating layer increases the possibility of damage to the magnetic recording medium caused by contact with the magnetic head (head impact).

[0016] As a method to achieve a thin lubricating film while maintaining sufficient wear resistance, the use of lubricants formed from compounds with low number-average molecular weight is considered. However, lubricating layers formed using compounds with low number-average molecular weight are prone to spin-off.

[0017] Spin-off, also known as lubricant stripping, is the phenomenon where lubricant is dispersed or evaporated due to centrifugal force and heat generated by the rotation of the magnetic recording medium. In recent years, with the rapid increase in recording density and rotational speed of magnetic recording media, spin-off has become more likely to occur. If spin-off occurs, the thickness of the lubricant layer decreases, thus reducing its wear resistance and overall durability of the magnetic recording medium.

[0018] The present invention was made in view of the above circumstances, with the aim of providing a fluorinated ether compound suitable for use as a lubricant for magnetic recording media, which can form a lubricating layer that has excellent wear resistance even when the thickness is thin and is not prone to film thickness reduction caused by spin-off.

[0019] Furthermore, the present invention aims to provide a coating containing the fluorinated ether compound of the present invention, which can form a lubricating layer that has excellent wear resistance even when the thickness is thin and is not prone to film thickness reduction due to spin-off, as well as a lubricant for magnetic recording media.

[0020] Furthermore, the present invention aims to provide a magnetic recording medium having excellent reliability and durability, having a lubricating layer comprising the fluorinated ether compound of the present invention.

[0021] Methods for solving problems

[0022] This invention relates to the following matters.

[0023] [1] The fluorinated ether compound represented by the following formula (1).

[0024] R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 [-CH2-R] 4 -CH2-R 3 ] x -CH2-O-(CH2) z -YR 5-R 6 (1)

[0025] (In equation (1), x is 0 to 2; z is an integer from 2 to 10; Y is any one of 0, NH, and S; R 3 It is a perfluoropolyether chain. (x+1) R... 3 They can be partially or completely the same, or they can be different from each other; R 4 It is a divalent linker with 1 to 3 hydroxyl groups and oxygen atoms at both ends; when x is 2, the two R groups... 4 They can be the same or different; R 2 The connecting base is shown in equation (2-1) or equation (2-2) below; R 5 The connecting base is shown in equation (2-3) or equation (2-4) below; R 1 and R 6 To be with R 2 Or R 5 The terminal oxygen atom of R is bonded to a terminal group, which can be the same or different; 1 and R 6 Each is independently selected from terminal groups of hydrogen atoms, alkyl groups that may have substituents, and organogroups that have double or triple bonds and may have substituents.

[0026] (In equation (2-1), f1 represents an integer from 1 to 3. The oxygen atom at the left end of equation (2-1) and R) 1 (Combined.)

[0027] In equation (2-2), g1 represents an integer from 2 to 6. The oxygen atom at the left end of equation (2-2) and R 1 (Combined.)

[0028] In equation (2-3), f2 represents an integer from 1 to 3. The oxygen atom at the right end of equation (2-3) is related to R. 6 (Combined.)

[0029] In equation (2-4), g2 represents an integer from 2 to 6. The oxygen atom at the right end of equation (2-4) is related to R. 6 (Combined.)

[0030] [2] According to the fluorinated ether compound described in [1], z in the above formula (1) is each an integer from 2 to 6.

[0031] [3] According to the fluorinated ether compound described in [2], z in the above formula (1) is each an integer from 2 to 4.

[0032] [4] According to any one of [1] to [3], the Y in the above formula (1) is independently O or NH.

[0033] [5] According to the fluorinated ether compound described in [4], all Y in the above formula (1) is O.

[0034] [6] The fluorinated ether compound according to any one of [1] to [5], R 1 and R 6 The alkyl groups mentioned above that may have substituents are each independently an alkyl group having 1 to 8 carbon atoms that may have substituents.

[0035] [7] The fluorinated ether compound according to any one of [1] to [6], R 1 and R 6 The aforementioned organic groups having double or triple bonds and which may have substituents are each independently selected from at least one of aromatic hydrocarbon groups, unsaturated heterocyclic groups, alkenyl groups, and alkynyl groups that may have substituents.

[0036] [8] According to any one of [1] to [7], the x R in the above formula (1) 4 Each is independently any of the two-valent linkages shown in equations (2-5) to (2-8) below.

[0037]

[0038] (In equation (2-5), r represents an integer from 1 to 3.)

[0039] In equation (2-6), s represents an integer from 2 to 6. The oxygen atom at the left end of equation (2-6) is related to R. 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 The -CH2- atom on the left side of equation (2-7) binds to R. (In equation (2-7), t represents an integer from 2 to 6. The oxygen atom at the left end of equation (2-7) binds to R. 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 The -CH2- atom on the left side of equation (2-8) binds to the R atom. (In equation (2-8), u represents an integer from 1 to 6, and v represents an integer from 1 to 6. u and v are not both 1. The oxygen atom at the left end of equation (2-8) binds to R. 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 (Side-CH2- binding.)

[0040] [9] According to any one of [1] to [8], the (x+1) R in the above formula (1) 3 Each is independently represented by the following formula (Rf).

[0041] -(CF2) p1 -O-(CF2O) p2 -(CF2CF2O) p3 -(CF2CF2CF2O) p4 -(CF2CF2CF2CF2O) p5 -(CF2) p6 -(Rf)

[0042] (In equation (Rf), p2, p3, p4, and p5 represent the average degree of polymerization, each independently ranging from 0 to 20. Not all of p2, p3, p4, and p5 are simultaneously zero. p1 and p6 represent the average quantity of -CF2-, each independently ranging from 1 to 3. There are no particular restrictions on the order of (CF2O), (CF2CF2O), (CF2CF2CF2O), and (CF2CF2CF2CF2O) which are structural units in equation (Rf).)

[0043]

[10] According to any one of [1] to [9], the (x+1) R in the above formula (1) 3 Each is independently represented by the following equations (3-1) to (3-4).

[0044] -CF2-(OCF2CF2) h -(OCF2) i -OCF2- (3-1)

[0045] (In equation (3-1), h and i represent the average degree of polymerization, where h represents 1 to 20 and i represents 0 to 20.)

[0046] -CF2CF2-(OCF2CF2CF2) j -OCF2CF2- (3-2)

[0047] (In equation (3-2), j represents the average degree of polymerization, ranging from 1 to 15.)

[0048] -CF2CF2CF2-(OCF2CF2CF2CF2) k -OCF2CF2CF2- (3-3)

[0049] (In equation (3-3), k represents the average degree of polymerization, ranging from 1 to 10.)

[0050] -(CF2) w7 -O-(CF2CF2CF2O) w8 -(CF2CF2O) w9 -(CF2) w10 - (3-4)

[0051] (In equation (3-4), w8 and w9 represent the average degree of polymerization, each independently representing 1 to 20. w7 and w10 represent the average amount of CF2, each independently representing 1 to 2.)

[0052]

[11] The fluorinated ether compound according to any one of [1] to

[10] has a number average molecular weight in the range of 500 to 10,000.

[0053]

[12] A coating comprising any one of the fluorinated ether compounds described in [1] to

[11] .

[0054]

[13] A lubricant for magnetic recording media, comprising the coating described in

[12] .

[0055]

[14] A magnetic recording medium having at least a magnetic layer, a protective layer, and a lubricating layer disposed on a substrate. The above-mentioned lubricating layer contains any one of the fluorinated ether compounds described in [1] to

[11] .

[0056]

[15] According to the magnetic recording medium described in

[14] , the average film thickness of the above-mentioned lubricating layer is 0.5 nm to 2.0 nm.

[0057] The effects of the invention

[0058] The fluorinated ether compound of the present invention is the compound shown in formula (1) above, and is suitable as a material for a lubricant for magnetic recording media.

[0059] The coatings and lubricants for magnetic recording media of the present invention contain fluorinated ether compounds of the present invention, thus forming a lubricating layer that exhibits excellent wear resistance even when thin and is less prone to film thickness reduction due to spin-off.

[0060] The magnetic recording medium of the present invention has excellent reliability and durability because it is provided with a lubricating layer containing a fluorinated ether compound of the present invention, which has excellent wear resistance and spin-off resistance. Attached Figure Description

[0061] Figure 1 A schematic cross-sectional view illustrating an example of an embodiment of the magnetic recording medium of the present invention. Detailed Implementation

[0062] In order to solve the above-mentioned problems, the inventors have repeatedly conducted in-depth research as shown below.

[0063] Conventionally, as a material for a lubricant (hereinafter sometimes abbreviated as "lubricant") used as a magnetic recording medium coated on the surface of a protective layer, fluorinated ether compounds having end structures containing polar groups such as hydroxyl groups at one or both ends of the perfluoropolyether chain are preferred.

[0064] The polar groups contained in fluorinated ether compounds bind to the active sites on the protective layer, improving the adhesion between the lubricating layer and the protective layer. Among the polar groups, the hydrogen atoms of the hydroxyl groups, in particular, have a high positive charge, resulting in high adsorption to the protective layer. Therefore, as a method to improve the wear resistance of the lubricating layer, it is considered to configure multiple hydroxyl groups at the end of the fluorinated ether compound to enhance its adhesion to the protective layer.

[0065] However, the inventors conducted research and found that the hydroxyl group closest to the perfluoropolyether chain among the terminal hydroxyl groups in the fluoroether compound (hereinafter referred to as the first hydroxyl group) has low adsorption to the protective layer. It is presumed that this is because the interaction between the first hydroxyl group and the active sites on the protective layer is less likely to occur due to the influence of the perfluoropolyether chain, which exhibits strong electron-withdrawing properties and high steric hindrance.

[0066] Therefore, the inventors focused on the adsorption sites of the fluorinated ether compounds contained in the lubricating layer that can interact with the active sites on the protective layer. In order to realize a fluorinated ether compound in the lubricating layer that does not easily generate adsorption sites that do not participate in the interaction with the protective layer, they have repeatedly conducted in-depth research as shown below.

[0067] The results showed that by introducing an alkylene chain between the perfluoropolyether chain, which exhibits strong electron-withdrawing properties and high steric hindrance, and the first hydroxyl group in a fluorinated ether compound with hydroxyl-containing end structures at both ends of the perfluoropolyether chain, and maintaining the spacing between the two at an appropriate distance, the electron density of the first hydroxyl group can be increased, and the steric hindrance around the first hydroxyl group can be mitigated.

[0068] For such fluorinated ether compounds, the first hydroxyl group can interact with the active sites on the protective layer with sufficient strength, resulting in good adhesion between the first hydroxyl group and the protective layer. Therefore, it is presumed that the lubricating layer containing the above-mentioned fluorinated ether compound is less likely to generate adsorption sites that do not participate in the interaction with the protective layer, exhibits good adhesion with the protective layer, and possesses excellent wear resistance and anti-spreading properties even when thin.

[0069] Furthermore, the inventors discovered that by using a lubricant containing the aforementioned fluorinated ether compound to form a lubricating layer on the protective layer of a magnetic recording medium, a lubricating layer with excellent wear resistance and spin-off resistance can be formed even with a thin thickness, and thus conceived of the present invention.

[0070] The following describes in detail the fluorinated ether compounds, coatings, lubricants for magnetic recording media, and magnetic recording media of the present invention. It should be noted that the present invention is not limited to the embodiments shown below. Without departing from the spirit (technical requirements) of the present invention, additions, omissions, substitutions, and modifications can be made to the numbers, quantities, ratios, compositions, types, positions, materials, and structures. The term "polar group" in this specification does not include halogenated groups (-F, -Cl, -Br, etc.) and ether bonds (-O-).

[0071] [Fluoro-ether compounds]

[0072] The fluorinated ether compound in this embodiment is represented by the following formula (1).

[0073] R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 [-CH2-R] 4 -CH2-R 3 ] x -CH2-O-(CH2) z -YR 5 -R 6 (1)

[0074] (In equation (1), x is 0 to 2; z is an integer from 2 to 10; Y is any one of 0, NH, and S; R 3 It is a perfluoropolyether chain. (x+1) R... 3 They can be partially or completely the same, or they can be different from each other; R 4 It is a divalent linker with 1 to 3 hydroxyl groups and oxygen atoms at both ends; when x is 2, the two R groups... 4 They can be the same or different; R 2 The connecting base is shown in equation (2-1) or equation (2-2) below; R 5 The connecting base is shown in equation (2-3) or equation (2-4) below; R 1 and R 6 To be with R 2 Or R 5 The terminal groups bonded to the oxygen atoms at the ends of R can be the same or different; 1 and R 6 Each of these can be a terminal group selected from hydrogen atoms, alkyl groups that may have substituents, and organogroups that have double or triple bonds and may have substituents.

[0075] <-Y-(CH2) z ->

[0076] In equation (1), each of the two z's is an independent integer from 2 to 10. -(CH2) z -Make R 2 and R 5 The hydroxyl group it contains is the closest to R. 3 The first hydroxyl group of the perfluoropolyether chain shown is related to R. 3 The distance is appropriate. From the first hydroxyl group and R 3 For a more appropriate consideration, z is preferably an integer from 2 to 6, particularly preferably an integer from 2 to 4, and even more preferably 2.

[0077] Since z in equation (1) is greater than 2, therefore R 2 and R 5 The first hydroxyl group is not easily affected by the perfluoropolyether chain, which exhibits strong electron-withdrawing properties and large steric hindrance, and is more likely to interact with the active sites on the protective layer. Therefore, the lubricating layer containing the fluorinated ether compound shown in formula (1) is less likely to generate adsorption sites that do not participate in the interaction with the protective layer, has good adhesion to the protective layer, and has excellent wear resistance and spin-off resistance even when the thickness is thin.

[0078] Furthermore, since z in equation (1) is less than or equal to 10, therefore in R 2 The first hydroxyl group in R 5 The number of carbon atoms without hydroxyl groups present between the first hydroxyl group in the lubricant layer is not excessive. Therefore, it can prevent the fluorinated ether compounds contained in the lubricant layer from forming a backbone containing perfluoropolyether chains (-Y-(CH2)). z -O-CH2-R 3 [-CH2-R] 4 -CH2-R 3 ] x -CH2-O-(CH2) z It bends into an arc shape centered on the -Y-) axis. Therefore, it will not be subjected to a force away from the protective layer centered on the arc-shaped skeleton, thus preventing R from being affected. 2 The first hydroxyl group, R 5 The first hydroxyl group and the hydroxyl group in the skeleton (i.e., R when x is 1 or 2) 4 The interaction between the contained hydroxyl groups and the protective layer is reduced. Therefore, the fluorinated ether compound shown in formula (1) can form a lubricating layer with excellent wear resistance and spin-off resistance.

[0079] In equation (1), Y represents the relationship between R and R. 2 Or R 5 And with -(CH2) z- A divalent group is bonded. The two Ys in formula (1) are each independently any one of O, S, and NH. Since Y is any one of them, it becomes a fluorinated ether compound that achieves good adhesion to the protective layer through the interaction of the unpaired electrons of the heteroatom with the substrate. Among them, in order to become a fluorinated ether compound that exhibits good affinity with the protective layer of the magnetic recording medium, Y in formula (1) is preferably O or NH, and particularly preferably O.

[0080] <R 2 and R 5 The 2-valent linker shown >

[0081] R in the above formula (1) 2 The connecting base is shown in equation (2-1) or equation (2-2) below. R 5 The connecting base is shown in equation (2-3) or equation (2-4) below.

[0082]

[0083] In equation (2-1), f1 represents an integer from 1 to 3. The oxygen atom at the left end of equation (2-1) and R 1 (Combined.)

[0084] In equation (2-2), g1 represents an integer from 2 to 6. The oxygen atom at the left end of equation (2-2) is related to R. 1 (Combined.)

[0085] In equation (2-3), f2 represents an integer from 1 to 3. The oxygen atom at the right end of equation (2-3) is related to R. 6 (Combined.)

[0086] In equation (2-4), g2 represents an integer from 2 to 6. The oxygen atom at the right end of equation (2-4) is related to R. 6 (Combined.)

[0087] R 2 and R 5 As shown in formulas (2-1) to (2-4), these are divalent linkers containing hydroxyl groups. In formula (2-1), f1, and in formula (2-3), f2 are each integers from 1 to 3. Therefore, formulas (2-1) and (2-3) have 1 to 3 hydroxyl groups. Furthermore, formulas (2-2) and (2-4) have 1 hydroxyl group regardless of the values ​​of g1 and g2.

[0088] As shown in equations (2-1) to (2-4), R 2 and R 5 R in equation (1) is composed of -CH2-, -O- and -CH(OH)-. 1 Side or R 6The end configuration on the side -O-, in R 3 The end configuration on the side -CH2-, is configured in R 1 Side or R 6 One or more divalent linkers of a chain-like structure of -CH2- are configured between the -O- and -CH(OH)- at the end of the side. R 2 and R 5 Because it has divalent linkers in a chain structure composed of -CH2-, -O-, and -CH(OH)-, it possesses hydroxyl groups that help improve adhesion to the protective layer and exhibits moderate flexibility. Furthermore, R 2 and R 5 Because it is configured in R 1 Side or R 6 -CH2- is configured between -O- and -CH(OH)- at the end of the side and between -Y- and -CH(OH)- in equation (1), therefore it is related to R 2 Neutralize R 5 The interaction between the hydroxyl groups and the protective layer is achieved by being configured in R 1 Side or R 6 The interaction between the unpaired electrons of the -O- at the end of the side and the -Y- in equation (1) with the protective layer. Based on these conditions, R 2 and R 5 This improves the affinity between the lubricating layer and the protective layer containing the fluorinated ether compound of this embodiment. Therefore, the fluorinated ether compound of this embodiment can form a lubricating layer with excellent wear resistance and anti-spreading properties.

[0089] In equation (2-1) above, f1 and f2 in equation (2-3) are integers from 1 to 3, preferably 2. Furthermore, f1 and f2 are preferably the same integer value.

[0090] Since f1 is an integer greater than or equal to 1, therefore in R 2 In the case of the connection base shown in equation (2-1), R 2 It has one or more hydroxyl groups. Therefore, in R 2 In the case of the linker shown in formula (2-1), a lubricating layer is formed on the protective layer by using a lubricant containing a fluorinated ether compound of this embodiment, thereby obtaining the interaction between the hydroxyl groups in formula (2-1) and the protective layer. If f1 is an integer of 2 or more, then formula (2-1) has two or more hydroxyl groups. Therefore, the interaction between the hydroxyl groups in formula (2-1) and the protective layer becomes more significant.

[0091] Furthermore, since f2 is an integer greater than or equal to 1, therefore in R 5 In the case of the connection base shown in equation (2-3), R 5 It has one or more hydroxyl groups. Therefore, in R 5In the case of the linker shown in formula (2-3), a lubricating layer is formed on the protective layer by using a lubricant containing a fluorinated ether compound of this embodiment, thereby obtaining the interaction between the hydroxyl groups in formula (2-3) and the protective layer. If f2 is an integer of 2 or more, then formula (2-3) has two or more hydroxyl groups. Therefore, the interaction between the hydroxyl groups in formula (2-3) and the protective layer becomes more significant.

[0092] Since f1 and f2 are each integers of 3 or less, the number of hydroxyl groups in formulas (2-1) and (2-3) is three or less. Therefore, the polarity of the fluorinated ether compound will not become too high due to an excessive number of hydroxyl groups in formulas (2-1) and / or (2-3). Thus, the adhesion of the fluorinated ether compound to the magnetic head as a foreign object (stain) can be suppressed.

[0093] Formula (2-2) has one hydroxyl group, therefore in R 2 In the case of the connection base shown in equation (2-2), R 2 It has one hydroxyl group. Therefore, by using R... 2 A lubricant containing a fluorinated ether compound with a linker as shown in formula (2-2) forms a lubricating layer on the protective layer, thereby allowing a suitable interaction to occur between the hydroxyl group present in formula (2-2) and the protective layer.

[0094] Furthermore, formula (2-4) has one hydroxyl group, therefore in R 5 In the case of the connection base shown in equation (2-4), R 5 It has one hydroxyl group. Therefore, by using R... 5 A lubricant containing a fluorinated ether compound with a linker as shown in formula (2-4) forms a lubricating layer on the protective layer, thereby allowing a suitable interaction to occur between the hydroxyl group present in formula (2-4) and the protective layer.

[0095] Therefore, in R 2 In the case of the connecting base shown in equation (2-2) and / or R 5 In the case of the connecting base shown in Equation (2-4), a lubricating layer with excellent wear resistance is obtained.

[0096] Furthermore, g1 in formula (2-2) and g2 in formula (2-4) are each integers from 2 to 6. Since g1 in formula (2-2) and g2 in formula (2-4) are 2 or more, the hydroxyl groups in formulas (2-2) and (2-4) are related to R... 1 Or R 6The distance between the oxygen atoms becomes more appropriate. Therefore, the intramolecular interaction of the hydroxyl groups in formulas (2-2) and (2-4) does not become too strong, and the interaction between the fluorinated ether compound and the protective layer becomes stronger. Furthermore, since g1 and g2 are 6 or less, it is possible to prevent the fluorinated ether compound from bending into an arc shape with g1 or g2 methylene (-CH2-) as the center. Therefore, the interaction between the hydroxyl groups in formulas (2-2) and (2-4) and the protective layer is not reduced by bending into an arc shape with g1 or g2 methylene (-CH2-) as the center, and the hydroxyl groups in formulas (2-2) and (2-4) can help improve the adhesion to the protective layer. g1 and g2 are preferably 4 or less.

[0097] <R 1 and R 6 The terminal group shown is >

[0098] In the fluorinated ether compound shown in formula (1), R 1 To be with R 2 The terminal oxygen atom of R is bonded to a terminal group. 6 To be with R 5 The terminal oxygen atom of R is bonded to a terminal group. 1 and R 6 They can be the same or different. R 1 and R 6 Each is independently a terminal group selected from hydrogen atoms, alkyl groups that may have substituents, and organogroups that have double or triple bonds and may have substituents.

[0099] (Hydrogen atom)

[0100] In R 1 In the case of hydrogen atoms, with R 2 The terminal oxygen atom together forms a hydroxyl group. In R 6 In the case of hydrogen atoms, with R 5 The oxygen atom at the end of the radical forms a hydroxyl group.

[0101] (Alkyl groups may have substituents)

[0102] As R 1 and / or R 6 The alkyl group that can have substituents is preferably an alkyl group having 1 to 8 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms. Specifically, examples of alkyl groups that can have substituents include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, and octyl. The alkyl group can be straight-chain or branched.

[0103] Examples of substituents that can be used with alkyl groups include halogenated groups, alkoxy groups, hydroxyl groups, cyano groups, and mercapto groups. When an alkyl group has substituents selected from these groups, it becomes a fluorinated ether compound capable of forming a lubricating layer with superior wear resistance. To form a lubricating layer with better adhesion to the protective layer, the alkyl group that can have substituents is preferably an alkyl group having hydroxyl and / or mercapto groups. When an alkyl group has two or more substituents, the types of substituents can be the same or different.

[0104] The alkyl group having a halogenated group as a substituent is preferably an alkyl group having at least one fluorine group. Examples of alkyl groups having a fluorine group include trifluoromethyl, perfluoroethyl, perfluoropropyl, perfluorobutyl, perfluoropentyl, perfluorohexyl, octafluoropentyl, tridecafluorooctyl, etc.

[0105] The alkyl group having a hydroxyl group as a substituent is preferably an alkyl group having at least one primary hydroxyl group. The hydroxyl group is a polar group that achieves strong interaction with the protective layer. Furthermore, the primary hydroxyl group disposed at the end of the fluorinated ether compound is highly mobile and therefore readily interacts with the protective layer. Therefore, in R... 1 and / or R 6 When the alkyl group has at least one primary hydroxyl group, a lubricating layer with better adhesion to the protective layer can be formed. The alkyl group having at least one primary hydroxyl group preferably has 2 to 5 carbon atoms; specifically, examples include -CH2CH2OH, -CH2CH2CH2OH, -CH2CH2CH2CH2OH, -CH2CH2CH2CH2CH2OH, and -CH2CH(CH2OH)2, among which -CH2CH2OH or -CH2CH2CH2OH is preferred.

[0106] (Organic groups with double or triple bonds and may have substituents)

[0107] As R 1 and / or R 6 The organogroup having a double or triple bond and may have substituents (hereinafter simply referred to as "organogroup having a double or triple bond") is an organogroup having at least one double or triple bond, preferably an organogroup having 2 to 12 carbon atoms, more preferably an organogroup having 2 to 8 carbon atoms.

[0108] The double or triple bonds in an organogroup can be either alkene double bonds or aromatic double bonds. Because the carbon-carbon unsaturated bond sites in the organogroup possess delocalized charges, they exhibit adsorption capacity by interacting with sites on the protective layer where the charge distribution is expanded. Examples of organogroups with double or triple bonds include groups containing aromatic hydrocarbons (aromatic hydrocarbon groups), groups containing unsaturated heterocycles (unsaturated heterocyclic groups), alkenyl groups, and alkynyl groups.

[0109] Examples of substituents that can be used when an organic group having double or triple bonds has substituents include alkyl, alkoxy, hydroxy, mercapto, carboxyl, carbonyl, amino, cyano, and halogenated groups. Among these substituents, hydroxyl and / or mercapto groups are preferred to form a lubricating layer with better adhesion to the protective layer. When an organic group having double or triple bonds has two or more substituents, the types of substituents can be the same or different.

[0110] Specifically, examples of organic groups having double or triple bonds include phenyl, methoxyphenyl, fluorophenyl, naphthyl, phenethyl, methoxyphenylethyl, fluorophenylethyl, benzyl, methoxybenzyl, naphthylmethyl, methoxynaphthyl, pyrrole, pyrazolyl, methylpyrazolylmethyl, imidazolyl, furanyl, furfural, etc. azole group, iso Azolyl, thiophene, thiopheneylethyl, thiazolyl, methylthiazolylethyl, isothiazolyl, pyridyl, pyrimidinyl, pyrazinyl, dihydroindolyl, benzofuranyl, benzothiophene, benzimidazolyl, benzo[] Azolyl, benzothiazolyl, benzopyrazole, benzisocyanate Azolyl, benzisothiazolyl, quinolinyl, isoquinolinyl, quinazolinyl, quinoxalinyl, phthalazinyl, cyclolinyl, vinyl, allyl, butenyl, 1-propynyl, propynyl (2-propynyl), butynyl, methylbutynyl, penynyl, methylpentynyl, hexynyl.

[0111] As the organic group having double or triple bonds, the above-mentioned groups are particularly preferred to be any one of phenyl, methoxyphenyl, phenethyl, methoxyphenethyl, fluorophenethyl, thienylethyl, allyl, butenyl, and propargyl, and even more preferably any one of phenyl, thienylethyl, allyl, butenyl, and propargyl. When the organic group having double or triple bonds is any one of phenyl, thienylethyl, allyl, butenyl, and propargyl, it becomes a fluorinated ether compound capable of forming a lubricating layer with superior wear resistance.

[0112] <R 3 The perfluoropolyether chain shown >

[0113] The fluorinated ether compound shown in formula (1) has R3 The perfluoropolyether chain shown is sometimes abbreviated as "PFPE chain" below. The PFPE chain covers the surface of the protective layer in the lubricating layer containing the fluorinated ether compound of this embodiment, and imparts lubricity to the lubricating layer, thereby reducing the friction between the magnetic head and the protective layer.

[0114] (x+1) R 3 They can be partially or completely the same, or they can each be different. (x+1) R 3 Ideally, all should be identical. This is because the fluorinated ether compound results in a more uniform coating of the protective layer, leading to a lubricating layer with better adhesion.

[0115] When x is 1 or 2, the so-called (x+1) R... 3 Two or more of them R 3 Same means (x+1) R 3 The structural units containing two or more PFPE chains have the same structure, R 3 In the same R 3 It also includes PFPE chains with the same structural unit but different average degrees of polymerization.

[0116] R in equation (1) 3 There are no particular limitations; the appropriate choice can be made based on the required performance of the lubricant containing fluorinated ether compounds. Examples of PFPE chains include those formed from perfluoromethylene oxide polymers, perfluoroethyl oxide polymers, perfluoropropylene oxide polymers, perfluoroisopropylene oxide polymers, perfluorobutylene oxide polymers, and copolymers thereof.

[0117] R in equation (1) 3 Preferably, for example, a PFPE chain of the following formula (Rf) derived from a polymer or copolymer of perfluoroalkylene oxides.

[0118] -(CF2) p1 -O-(CF2O) p2 -(CF2CF2O) p3 -(CF2CF2CF2O) p4 -(CF2CF2CF2CF2O) p5 -(CF2) p6 -(Rf)

[0119] (In equation (Rf), p2, p3, p4, and p5 represent the average degree of polymerization, each independently representing 0 to 20. Not all of p2, p3, p4, and p5 are simultaneously 0. p1 and p6 are the average values ​​representing -CF2-, each independently representing 1 to 3. There are no particular restrictions on the order of (CF2O), (CF2CF2O), (CF2CF2CF2O), and (CF2CF2CF2CF2O) which are structural units in equation (Rf).)

[0120] In formula (Rf), p2, p3, p4, and p5 represent the average degree of polymerization, each independently representing 0 to 20, preferably 0 to 15, and more preferably 0 to 10.

[0121] In equation (Rf), p1 and p6 are the average values ​​of the numbers representing -CF2-, each independently representing 1 to 3. p1 and p6 are determined in the PFPE chain shown in equation (Rf) based on the structure of the structural units arranged at the ends of the chain structure.

[0122] In equation (Rf), (CF2O), (CF2CF2O), (CF2CF2CF2O), and (CF2CF2CF2CF2O) are structural units. There are no particular restrictions on the order in which the structural units in equation (Rf) are arranged. Furthermore, there are no particular restrictions on the number of different types of structural units in equation (Rf).

[0123] R in equation (1) 3 More preferably, it is any one of the following formulas (3-1) to (3-4).

[0124] -CF2-(OCF2CF2) h -(OCF2) i -OCF2- (3-1)

[0125] (In equation (3-1), h and i represent the average degree of polymerization, where h represents 1 to 20 and i represents 0 to 20.)

[0126] -CF2CF2-(OCF2CF2CF2) j -OCF2CF2- (3-2)

[0127] (In equation (3-2), j represents the average degree of polymerization, ranging from 1 to 15.)

[0128] -CF2CF2CF2-(OCF2CF2CF2CF2) k -OCF2CF2CF2- (3-3)

[0129] (In equation (3-3), k represents the average degree of polymerization, ranging from 1 to 10.)

[0130] -(CF2) w7 -O-(CF2CF2CF2O) w8 -(CF2CF2O) w9 -(CF2) w10 - (3-4)

[0131] (In equation (3-4), w8 and w9 represent the average degree of polymerization, each independently representing 1 to 20. w7 and w10 represent the average value of CF2, each independently representing 1 to 2.)

[0132] There are no particular restrictions on the order of (CF2CF2O) and (CF2O) as structural units in equation (3-1). In equation (3-1), the number h of (CF2CF2O) and the number i of (CF2O) can be the same or different. Equation (3-1) can include any of the following: random copolymers, block copolymers, and alternating copolymers composed of monomer units (CF2CF2O) and (CF2O).

[0133] There are no particular restrictions on the order of (CF2CF2CF2O) and (CF2CF2O) as structural units in Equation (3-4). In Equation (3-4), the number w8 of (CF2CF2CF2O) and the number w9 of (CF2CF2O) can be the same or different. Equation (3-4) can include any of the random copolymers, block copolymers, and alternating copolymers composed of monomer units (CF2CF2CF2O) and (CF2CF2O). In Equation (3-4), w7 and w10 are average values ​​representing the number of -CF2-, each independently representing 1 to 2. w7 and w10 in the PFPE chain shown in Equation (3-4) are determined according to the structure of the structural units arranged at the ends of the chain structure.

[0134] In formulas (3-1) to (3-4), h, j, k, w8, and w9 are each 1 or more, and if i is 0 or more, a lubricating layer with good adhesion is obtained. Furthermore, if h, i, w8, and w9 are each 20 or less, j is 15 or less, and k is 10 or less, the viscosity of the fluorinated ether compound will not become excessively high, and the lubricant containing the fluorinated ether compound is easy to apply. To obtain a fluorinated ether compound that easily wets and spreads on the protective layer and easily produces a lubricating layer with a uniform film thickness, h, i, w8, and w9, representing the average degree of polymerization, are preferably 1 to 15, more preferably 2 to 10, and even more preferably 3 to 8. j, representing the average degree of polymerization, is preferably 2 to 10, more preferably 3 to 8. k, representing the average degree of polymerization, is preferably 1 to 8, more preferably 1 to 6.

[0135] In equation (1) R 3When the fluorinated ether compound is any of formulas (3-1) to (3-4), its synthesis is readily possible and preferred. In R 3 In the case of formula (3-1), it is more preferable because the raw materials are readily available.

[0136] Furthermore, in R 3 In the case of any of formulas (3-1) to (3-4), the ratio of oxygen atoms (number of ether bonds (-O-)) to carbon atoms in the perfluoropolyether chain is appropriate. Therefore, it becomes a fluorinated ether compound with moderate hardness. Consequently, the fluorinated ether compound coated on the protective layer does not easily aggregate on the protective layer, and a thinner lubricating layer can be formed with sufficient coverage. As a result, in R... 3 When any of the formulas (3-1) to (3-4) are present, it becomes a fluorinated ether compound that provides a lubricating layer with good wear resistance and spin-off resistance.

[0137] <R 4 The 2-valent linker shown >

[0138] In the fluorinated ether compound shown in formula (1), R 4 When x is 1 or 2, it is configured in the adjacent R. 3 Between. x R 4 Each is independently a divalent linker having 1 to 3 hydroxyl groups and oxygen atoms at both ends. For the fluorinated ether compound shown in formula (1), when x is 1 or 2, due to being arranged in adjacent R 3 R between 4 Having 1 to 3 hydroxyl groups, when a lubricating layer is formed on the protective layer using a lubricant containing this fluorinated ether compound, the R contained in the lubricating layer... 4 The hydroxyl groups present interact appropriately with the protective layer. This prevents the fluorinated ether compound from bending into an arc shape around the backbone, thus forming a lubricating layer with excellent wear resistance and anti-spillage properties.

[0139] When x is 2, there are 2 R 4 They can be the same or different. R 4 Preferably, each of them is an independent bivalent linker as shown in equations (2-5) to (2-8). The reason is R 4 It has moderate softness, through R 4 The interaction between the hydroxyl groups and the protective layer can more effectively prevent fluorinated ether compounds from bending into an arc shape with the skeleton as the center.

[0140]

[0141] (In equation (2-5), r represents an integer from 1 to 3.)

[0142] In equation (2-6), s represents an integer from 2 to 6. The oxygen atom at the left end of equation (2-6) is related to R. 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 The -CH2- atom on the left side of equation (2-7) binds to R. (In equation (2-7), t represents an integer from 2 to 6. The oxygen atom at the left end of equation (2-7) binds to R. 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 The -CH2- atom on the left side of equation (2-8) binds to the R atom. (In equation (2-8), u represents an integer from 1 to 6, and v represents an integer from 1 to 6. u and v are not both 1. The oxygen atom at the left end of equation (2-8) binds to R. 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 (Side-CH2- binding.)

[0143] In R 4 In the case shown in equations (2-5) to (2-8), R 4 It is a divalent linker with 1 to 3 secondary hydroxyl groups and a chain-like structure with -O- at both ends, and is a linker that reacts with R. 1 The -CH2- group on the side combines with -O- and -CH(OH)- to form more than one -CH2- group, which is related to R. 6 The -CH2- on the side is linked by more than one divalent -CH2- linker between -O- and -CH(OH)-. Therefore, R 4 It contains hydroxyl groups that help improve adhesion to the protective layer and has moderate flexibility. Furthermore, due to its compatibility with R... 1 The -CH2- group on the side combines with -O- and -CH(OH)- to form more than one -CH2- group, which is related to R. 6 The -CH2- on the side combines with -O- and -CH(OH)- to form more than one -CH2-, therefore R 4 The hydroxyl groups contained are obtained through R 4 The methylene group (-CH2-) possesses moderate flexibility, making it less susceptible to steric hindrance from R. 3 The influence of these factors makes it easy for the active sites on the protective layer to interact. Based on these factors, for the fluorinated ether compounds of this embodiment, the backbone has 2 or 3 R... 3 In the case of being configured in adjacent R 3 R between 4 The interaction between the hydroxyl groups and the protective layer prevents bending into an arc shape centered on the skeleton. Therefore, it becomes a fluorinated ether compound capable of forming a lubricating layer with excellent wear resistance and anti-spreading properties.

[0144] The divalent linkers shown in formulas (2-5) to (2-8) all have oxygen atoms at both ends of the chain structure, and are bonded to R through ether bonds. 4 The divalent linker shown is methylene-bound. In formula (2-5), the number of carbon atoms between the oxygen atoms forming ether bonds in the chain structure of the divalent linker is 3. In formulas (2-6) and (2-7), the number of carbon atoms between the oxygen atoms forming ether bonds in the chain structure of the divalent linker is 4 to 8. In formula (2-8), the number of carbon atoms between adjacent oxygen atoms forming ether bonds in the chain structure of the divalent linker is 3 to 8. Therefore, the divalent linkers shown in formulas (2-5) to (2-8) have an appropriate number of carbon atoms and sufficient flexibility. Furthermore, the oxygen atoms in the chain structure of the divalent linkers shown in formulas (2-5) to (2-8) form ether bonds, imparting appropriate flexibility to the fluorinated ether compound shown in formula (1), thereby increasing the affinity of the hydroxyl groups of the divalent linkers shown in formulas (2-5) to (2-8) for the protective layer. Furthermore, the divalent linkers shown in formulas (2-5) to (2-8) possess sufficient flexibility, allowing them to move freely independently without being linked to the molecular motion of the adjacent perfluoropolyether chains on both sides. Therefore, the divalent linkers shown in formulas (2-5) to (2-8) are less susceptible to the influence of molecular motion caused by the perfluoropolyether chains bonded to their adjacent sides via methylene groups, and readily participate in interactions with the active sites on the protective layer.

[0145] In the fluorinated ether compound shown in formula (1), x ranges from 0 to 2. Therefore, the fluorinated ether compound shown in formula (1) has (x+1) R... 3 The PFPE chain shown. R 3 A compound with 1 x (a compound with x = 0) and R 3 Compared to two or more compounds, it is a fluorinated ether compound that is easier to synthesize. Furthermore, R... 3 Compounds consisting of 2 or 3 elements (compounds where x is 1 or 2) and R 3 For compounds that are different, in adjacent R 3 R is configured as a binary linker between them. 4 Therefore, with R 3 Compared to compounds with only one component, it is easier to obtain a lubricating layer with excellent adhesion to the protective layer. Furthermore, R... 3 Compounds consisting of 2 or 3 elements with R 3 Compared to compounds with a single molecular weight, it is easier to form compounds with a large number-average molecular weight, which can form a lubricating layer that is less prone to film thickness reduction caused by spin-deposition.

[0146] Furthermore, compared to compounds with four or more PFPE chains, the fluorinated ether compound shown in formula (1) does not have excessively large molecules and can move freely. Therefore, compared to compounds with four or more PFPE chains, the fluorinated ether compound shown in formula (1) is easier to wet and spread on the protective layer, and can form a lubricating layer with a thin and uniform film thickness.

[0147] In the fluorinated ether compound shown in formula (1), R 1 -R 2 -Y-(CH2) z - and -(CH2) z -YR 5 -R 6 They can be the same or different, but the same is preferred. The reason is to make them fluorinated ether compounds that are easy to synthesize.

[0148] In this specification, R refers to... 1 -R 2 -Y-(CH2) z - and -(CH2) z -YR 5 -R 6 The sameness refers to the fact that the atoms contained in both are relative to the -R atoms located at the center of the molecule. 3 [-CH2-R] 4 -CH2-R 3 ] x -and is symmetrically configured.

[0149] In equation (1), when x is 1 or 2, R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 They can be the same or different, but the same is preferred. The reason is that they become fluorinated ether compounds that are easy to synthesize.

[0150] In this specification, R refers to... 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 The sameness refers to the fact that the atoms contained in both are relative to the -CH2-R located in the center of the molecule. 4 -CH2- or -CH2-R4 -CH2-R 3 -CH2-R 4 -CH2- is configured symmetrically.

[0151] When x is 2 in equation (1), there are 2 R 4 They can be the same or different, but the same is preferred. If there are 2 Rs... 4 If the fluorinated ether compound has the same properties, the coating of the protective layer becomes more uniform, resulting in a lubricating layer with better adhesion. Furthermore, if the two R... 4 If they are the same, they become fluorinated ether compounds that can be easily manufactured, and are therefore preferred.

[0152] In this specification, the so-called 2 Rs 4 The sameness refers to the fact that the atoms contained in both are relative to the -CH2-R located in the center of the molecule. 3 -CH2- is configured symmetrically.

[0153] In the fluorinated ether compound shown in formula (1), R 1 -R 2 -The sum of the polar groups contained and -R 5 -R 6 The total number of polar groups contained is preferably 1 to 4, more preferably 2 to 3. This is because if the total number of each polar group is 1 or more, it becomes a fluorinated ether compound with good adsorption to the protective layer, capable of forming a lubricating layer exhibiting excellent wear resistance. Furthermore, if the total number of each polar group is 4 or less, the intramolecular interactions containing the polar groups will not become excessively strong, resulting in a fluorinated ether compound capable of forming a lubricating layer exhibiting excellent wear resistance.

[0154] In the fluorinated ether compound shown in formula (1), when x is 0 (in other words, when R is not present) 4 In the case of the divalent linker shown, the number of polar groups contained in one molecule is preferably 4 to 10, more preferably 4 to 8. Furthermore, when x is 1 or 2 (in other words, having 1 or 2 R groups), 4 In the case of the divalent linker shown, the number of polar groups contained in one molecule is preferably 6 to 12, more preferably 6 to 10.

[0155] If, when x is 0, a molecule contains 4 or more polar groups, or if, when x is 1 or 2, a molecule contains 6 or more polar groups, the overall adsorption of the molecule to the protective layer is good. Furthermore, if, when x is 0, a molecule contains 10 or fewer polar groups, or if, when x is 1 or 2, a molecule contains 12 or fewer polar groups, the intramolecular interactions containing polar groups do not become excessively strong, thus preventing the fluorinated ether compound from agglomerating on the protective layer. Therefore, the reduced spin resistance of the lubricating layer due to the agglomeration of the fluorinated ether compound on the protective layer can be suppressed.

[0156] The fluorinated ether compound represented by formula (1) is preferably any of the compounds represented by formulas (A) to (P) below.

[0157] In the compounds shown in formulas (A) to (P) below, Rf1 and Rf2, representing the PFPE chain, each have the following structure. That is, in the compounds shown in formulas (A) and (B) below, Rf1 is the PFPE chain shown in formula (3-1) below. In the compounds shown in formulas (C) to (P) below, Rf2 is the PFPE chain shown in formula (3-2) below. It should be noted that h and i in Rf1 and j in Rf2, representing the PFPE chain in formulas (A) to (P), are values ​​representing the average degree of polymerization, and therefore are not necessarily integers.

[0158]

[0159] The compounds shown in formulas (A) to (D) all have x = 0, and R in formula (1) 1 and R 6 For hydrogen atoms, R 2 As expressed by equation (2-1), f1 is 2, R 5 As can be expressed by equation (2-3), f2 is 2 and Y is 0.

[0160] The compounds shown in formulas (A) and (B) are in formula (1), R 3 For equation (3-1), z is 2.

[0161] The compound shown in formula (C) has R in formula (1). 3 For equation (3-2), z is 2.

[0162] The compound shown in formula (D) has R in formula (1). 3 For equation (3-2), z is 3.

[0163] The compounds shown in formulas (E) and (F) have R in formula (1) 1 and R 6 For hydrogen atoms, R 3 For equation (3-2), Y is 0 and z is 2.

[0164] The compound shown in formula (E) has R in formula (1). 2 As expressed by equation (2-1), f1 is 1, R 5 As can be expressed by equation (2-3), f2 is 2 and x is 0.

[0165] The compound shown in formula (F) has R in formula (1). 2 As expressed by equation (2-1), f1 is 1, R 5 As shown in equation (2-3), f2 is 1. For the compound represented by equation (F), x is 1, and R... 4 As shown in equation (2-8), u is 1 and v is 4.

[0166] The compounds represented by formulas (G) and (H) are all in formula (1), where x is 0 and R is 0. 1 and R 6 Y is a hydrogen atom, and R is an O atom. 3 As indicated by equation (3-2), z is 2.

[0167] The compound represented by formula (G) has R in formula (1). 2 As expressed by equation (2-1), f1 is 1, R 5 As indicated by equation (2-3), f2 is 1.

[0168] The compound represented by formula (H) has R in formula (1). 2 As expressed by equation (2-2), g1 is 2, R 5 As indicated by equation (2-4), g2 is 2.

[0169] The compounds shown in formulas (I) to (K) are all in formula (1), R 1 and R 6 For hydrogen atoms, R 2 As expressed by equation (2-1), f1 is 1, R 5 As expressed by equation (2-3), f2 is 1, Y is 0, and R... 3 As indicated by equation (3-2), z is 2.

[0170] The compound shown in formula (I) has x = 1 and R = 1 in formula (1). 4 As indicated by equation (2-5), r is 1.

[0171] The compound represented by formula (J) has x = 1 and R = 1 in formula (1). 4 As indicated by equation (2-5), r is 3.

[0172] The compound represented by formula (K) has x = 2 and R = 2 in formula (1). 4 As indicated by equation (2-5), r is 1.

[0173] The compounds represented by formulas (L) to (N) are all in formula (1), where x is 0 and R is 0. 2 As expressed by equation (2-1), f1 is 1, R 5 As expressed by equation (2-3), f2 is 1, Y is 0, and R... 3 As indicated by equation (3-2), z is 2.

[0174] The compound represented by formula (L) has R in formula (1). 1 and R 6 It is -CH2-CH2-OH.

[0175] The compound represented by formula (M) has R in formula (1). 1 and R 6 It is -CH2-CH2-CH=CH2(3-butenyl).

[0176] The compound represented by formula (N) has R in formula (1). 1 and R 6 It is a phenyl group.

[0177] The compounds represented by formulas (O) and (P) are all in formula (1), where x is 0 and R is 0. 1 and R 6 For hydrogen atoms, R 2 As expressed by equation (2-1), f1 is 1, R 5 As expressed by equation (2-3), f2 is 1, R 3 As indicated by equation (3-2), z is 2.

[0178] In the compound represented by formula (O), Y is NH in formula (1).

[0179] In formula (1), the compound represented by formula (P) has Y as S.

[0180]

[0181] (In Rf1 of equation (A), h and i represent the average degree of polymerization, where h represents 1 to 20 and i represents 1 to 20.)

[0182] (In Rf1 of equation (B), h and i represent the average degree of polymerization, where h represents 1 to 20 and i represents 0.)

[0183] (In equation (C), Rf2 represents the average degree of polymerization, where j ranges from 1 to 15.) (In equation (D), Rf2 represents the average degree of polymerization, where j ranges from 1 to 15.)

[0184] (In Rf2 of equation (E), j represents the average degree of polymerization, and j ranges from 1 to 15.) (In the two Rf2s of equation (F), j represents the average degree of polymerization, and j ranges from 1 to 15. The average degree of polymerization in the two Rf2s can be the same or different.)

[0185] (In Rf2 of equation (G), j represents the average degree of polymerization, and j represents 1 to 15.)

[0186] (In Rf2 of equation (H), j represents the average degree of polymerization, and j represents 1 to 15.)

[0187] (In Rf2 of equation (I), j represents the average degree of polymerization, and j represents 1 to 15.)

[0188] (In Rf2 of equation (J), j represents the average degree of polymerization, and j represents 1 to 15.)

[0189] (In Rf2 of equation (K), j represents the average degree of polymerization, and j represents 1 to 15.)

[0190] (In Rf2 of equation (L), j represents the average degree of polymerization, and j represents 1 to 15.)

[0191] (In Rf2 of formula (M), j represents the average degree of polymerization, and j represents 1 to 15.)

[0192] (In Rf2 of equation (N), j represents the average degree of polymerization, where j represents 1 to 15.)

[0193] (In Rf2 of equation (O), j represents the average degree of polymerization, and j represents 1 to 15.)

[0194] (In Rf2 of equation (P), j represents the average degree of polymerization, and j represents 1 to 15.)

[0195] If the compound shown in formula (1) is any of the compounds shown in formulas (A) to (F) above, the raw material is readily available and a lubricating layer with excellent wear resistance and anti-spinning properties can be formed even with a thin thickness, which is preferred.

[0196] The number-average molecular weight (Mn) of the fluorinated ether compound in this embodiment is preferably in the range of 500 to 10,000, more preferably in the range of 700 to 5,000, even more preferably in the range of 900 to 3,000, and particularly preferably in the range of 1,000 to 2,500. If the number-average molecular weight is 500 or higher, the lubricant containing the fluorinated ether compound of this embodiment is less prone to evaporation, and a lubricating layer that is less likely to experience film thickness reduction due to spin-off can be formed. Furthermore, if the number-average molecular weight is 500 or higher, lubricant evaporation and migration to the magnetic head can be prevented. The number-average molecular weight of the fluorinated ether compound is more preferably 900 or higher. Furthermore, if the number-average molecular weight is 10,000 or lower, the viscosity of the fluorinated ether compound is appropriate, and a thin lubricating layer can be easily formed by coating the lubricant containing the fluorinated ether compound. In order to achieve a viscosity that is easy to handle when used as a lubricant, the number-average molecular weight of the fluorinated ether compound is more preferably 3,000 or lower.

[0197] The number-average molecular weight (Mn) of fluorinated ether compounds is determined by using bleach. AVANCEIII400 made by バイオスピン Co., Ltd. 1 H-NMR and 19 The value is obtained by F-NMR. Specifically, it is obtained by... 1 H-NMR measurement or 19 The number-average molecular weight is calculated by taking the integrated intensity of each peak obtained from F-NMR determination and the number of hydrogen or fluorine atoms attributed to each peak. In NMR (nuclear magnetic resonance) determination, the sample is diluted in solvents such as hexafluorobenzene, d-acetone, and d-tetrahydrofuran, either alone or in mixtures, for determination. 19 The baseline for F-NMR chemical shift is set at -164.7 ppm for the peak of hexafluorobenzene. 1 The baseline for the H-NMR chemical shift is set at 2.2 ppm for the acetone peak.

[0198] "Manufacturing method"

[0199] The method for manufacturing the fluorinated ether compound in this embodiment is not particularly limited, and conventionally known manufacturing methods can be used. For example, the fluorinated ether compound in this embodiment can be manufactured using the manufacturing method shown below.

[0200] [First manufacturing method (when x is 0)]

[0201] First, prepare R in equation (1) 3 The two ends of the corresponding perfluoropolyether chain are respectively configured with fluorinated compounds containing hydroxymethyl (-CH2OH).

[0202] Next, the hydroxyl group of the hydroxymethyl group at one end of the above-mentioned fluorinated compound is reacted with R having the same properties as in formula (1). 1 -R 2 -Y-(CH2) z - The corresponding halogen or pseudohalogen compound reacts with the group (reaction 1). Thus, a compound is obtained in reaction with R... 3 One end of the corresponding perfluoropolyether chain has a property similar to R. 1 -R 2 -Y-(CH2) z - The intermediate compound 1-1 corresponding to the group.

[0203] For the first reaction, not only is it generated in relation to R 3 One end of the corresponding perfluoropolyether chain has a property similar to R. 1 -R 2 -Y-(CH2) z - The intermediate compound 1-1 corresponding to the group, and also generated in relation to R 3 The corresponding perfluoropolyether chain has R at both ends. 1 -R 2 -Y-(CH2) z -A compound corresponding to the group. In this embodiment, by adjusting the amount of solvent and raw materials used in the first reaction, the compounds having R at both ends can be controlled. 1 -R 2 -Y-(CH2) z - The amount of the corresponding group of the compound and the amount of intermediate compound 1-1 generated result in a higher proportion of intermediate compound 1-1 being generated. Furthermore, the above-mentioned compounds having R at both ends... 1 -R 2 -Y-(CH2) z Since the corresponding group of the compound and intermediate compound 1-1 have different polarities, intermediate compound 1-1, which is generated by only one terminal reaction, can be obtained efficiently by separating the product obtained from the first reaction using column chromatography or the like.

[0204] As having R in equation (1) 1 -R 2 -Y-(CH2) z - Halogenated or pseudohalogenated compounds with corresponding groups can be used, for example, compounds shown in formulas (4-1) to (4-3) below. In formulas (4-1) to (4-3) below, MOM represents methoxymethyl and Ts represents p-toluenesulfonyl.

[0205]

[0206] For example, when using the compound shown in formula (5-1) (described in formula (6-1) below) as having R in formula (1) 1 -R 2 -Y-(CH2) z In the case of halogenated compounds or pseudohalogenated compounds with corresponding groups, the following methods can be used to manufacture them.

[0207] First, as shown in equation (6-1) below, prepare an R with the same characteristics as in equation (1). 1 -R 2 - The alcohol corresponding to a portion of the terminal group shown (R in formula (6-1)).

[0208] Furthermore, a primary hydroxyl group and an epoxy group protected by a tetrahydropyran (THP) group are prepared, and a -R group is formed with respect to the group in formula (1). 2 -Y-(CH2) z -A compound corresponding to a portion of the structure.

[0209] Furthermore, it enables the R to have the characteristics described above. 1 -R 2 - Part of the corresponding structure of alcohols and having the above-mentioned -R 2 -Y-(CH2) z The reaction of a compound corresponding to a portion of the structure generates a secondary hydroxyl group that is protected with chloromethyl methyl ether (MOMCl). Then, the generated compound is reacted with an acid to selectively deprotect the THP group from the protected primary hydroxyl group, and the primary hydroxyl group is reacted with p-toluenesulfonyl chloride (TsCl).

[0210] By performing the above steps, the compound shown in formula (5-1) is obtained.

[0211] The number of methylene groups of the primary hydroxyl groups protected by the THP group in the compound used as a raw material is z in formula (1). Therefore, a1 in formula (6-1) is 1 to 9 (z-1 in formula (1)), determined according to the value of z in formula (1) of the synthesized compound.

[0212]

[0213] (In equation (6-1), R represents the same as R in equation (1) 1 -R 2 - The structure corresponding to a portion of the terminal group shown. a1 represents an integer from 1 to 9. In formula (6-1), THP represents tetrahydropyranyl, MOM represents methoxymethyl, and Ts represents p-toluenesulfonyl.

[0214] Furthermore, when using the compound shown in formula (5-2) (described in formula (6-2) below) as the above-mentioned compound having the same R as in formula (1), 1 -R 2 -Y-(CH2) z In the case of halogenated compounds or pseudohalogenated compounds with corresponding groups, the following methods can be used to manufacture them.

[0215] First, as shown in equation (6-2) below, prepare R with the same characteristics as in equation (1). 1 -R 2 - A compound corresponding to a portion of the terminal group shown (R in formula (6-2)) and a leaving group (Ts). Furthermore, a compound having the same structure as -Y-(CH2) in formula (1) is prepared. z - Part of the corresponding alkylene chain has hydroxyl groups bonded to both ends of the diol.

[0216] Furthermore, it enables the R to have the characteristics described above. 1 -R 2 Compounds with a structure corresponding to a portion of - and a leaving group, and compounds having the same -Y-(CH2) as described above. z The reaction of a portion of the diol corresponding to the structure of the compound causes the primary hydroxyl group of the resulting compound to react with p-toluenesulfonyl chloride (TsCl).

[0217] By performing the above steps, the compound shown in formula (5-2) is obtained.

[0218] In the diol used as a raw material, the number of methylene groups forming alkylene chains is z in formula (1). Therefore, a2 in formula (6-2) is 1 to 9 (z-1 in formula (1)), determined according to the value of z in the synthesized compound.

[0219]

[0220] (In equation (6-2), R represents the same as R in equation (1) 1 -R 2 - This represents a portion of the structure corresponding to the terminal group shown. a2 represents an integer from 1 to 9. Ts represents p-toluenesulfonyl group.

[0221] Next, the hydroxyl group of the hydroxymethyl group at the other end of the intermediate compound 1-1 obtained by the above method is reacted with a group having the same -(CH2) as in formula (1). z -YR 5 -R 6 The corresponding halogen or pseudohalogen compound reacts (reaction 2).

[0222] As used in the second reaction, it has -(CH2)z -YR 5 -R 6 Halogenated or pseudohalogenated compounds with corresponding groups can be used in the first reaction, having the same R group as those used in the first reaction. 1 -R 2 -Y-(CH2) z -The corresponding halogenated or pseudohalogenated compound is the same as the one containing the -(CH2) group. Therefore, as used in the second reaction, it has the same group as the halogenated or pseudohalogenated compound. z -YR 5 -R 6 Halogenated or pseudohalogenated compounds with corresponding groups can be, for example, compounds shown in formulas (4-1) to (4-3) above.

[0223] The first and second reactions can be carried out using conventionally known methods, based on R in equation (1). 1 -R 2 -Y-(CH2) z - and -(CH2) z -YR 5 -R 6 The type, etc., can be appropriately determined. Furthermore, any reaction between the first and second reactions can be carried out first. Additionally, in R... 1 -R 2 -Y-(CH2) z - and -(CH2) z -YR 5 -R 6 Under the same conditions, the first reaction and the second reaction can occur simultaneously.

[0224] After the above steps, a known method is used to carry out a deprotection reaction, thereby removing the protecting groups such as THP group, MOM group, and benzyl group to become hydroxyl groups, thereby producing a compound with x=0 in formula (1).

[0225] [Second manufacturing method (when x is 1)]

[0226] (R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 Different situations)

[0227] First, prepare for the meeting with R 1 -R 2 -Y-(CH2) z-R on the side 3 The corresponding perfluoropolyether chain has hydroxymethyl groups configured at both ends of a fluorinated compound. Furthermore, the hydroxyl group at one end of the fluorinated compound is combined with a fluorinated compound having the same R... 1 -R 2 -Y-(CH2) z - The corresponding halogen or pseudohalogen compound reacts to obtain intermediate compound 1a (reaction 1).

[0228] Next, we will prepare to work with -(CH2). z -YR 5 -R 6 Side R 3 The corresponding perfluoropolyether chain has hydroxymethyl groups configured at both ends of a fluorinated compound. Furthermore, one terminal hydroxyl group of the fluorinated compound is coupled with a group having the same -(CH2) composition as described above. z -YR 5 -R 6 The corresponding halogen or pseudohalogen compound reacts to obtain intermediate compound 1b (reaction 2).

[0229] Next, the terminal hydroxyl group of intermediate compound 1a is reacted with R in formula (1). 4 The corresponding chain structure has an epoxy group at one end and an alkenyl group at the other end. Then, the double bond of the resulting compound is oxidized to obtain intermediate compounds 1-2 (reaction 3).

[0230] As R in equation (1) 4 Compounds with an epoxy group at one end and an alkenyl group at the other end of the corresponding chain structure can be, for example, compounds shown in formulas (7-1) to (7-4) below.

[0231]

[0232] When using the compound shown in formula (7-1) or formula (7-2) as R 4 In the case of the corresponding compound, for example, it can be manufactured by the method shown below. That is, as shown in formula (8-1) or formula (8-2) below, a halogen compound having an alkenyl group, such as a bromine compound or a chlorine compound having an alkenyl group (in formulas (8-1) and (8-2), the halogen compound is a bromine compound) is reacted with an alcohol having an alkenyl group to obtain a compound having alkenyl groups at both ends. Then, it can be manufactured by reacting m-chloroperbenzoic acid (mCPBA) with the compound having alkenyl groups at both ends to oxidize one alkenyl group.

[0233]

[0234] As the compound shown in formula (7-3), commercially available products can be used (e.g., trade name: allyl glycidyl ether, manufactured by Tokyo Chemical Industry Co., Ltd.).

[0235] As the compound shown in formula (7-4), a commercially available product can be used (e.g., trade name: 2-[(3-buten-1-yloxy)methyl]ethylene oxide, manufactured by Aurora Fine Chemicals).

[0236] Next, the terminal hydroxyl group of intermediate compound 1b is reacted with the epoxy group of intermediate compound 1-2 obtained in the third reaction (reaction 4).

[0237] By performing a deprotection reaction using a known method after the above steps, it is possible to produce a product in formula (1) where x is 1 and R... 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 Different compounds.

[0238] [Third manufacturing method (when x is 1)]

[0239] (R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 (same situation)

[0240] Prepare to use R in equation (1) 3 The corresponding perfluoropolyether chain has hydroxymethyl groups configured at both ends of a fluorinated compound. Next, the hydroxyl group of the hydroxymethyl group configured at one end of the fluorinated compound is reacted with a compound having the same R... 1 -R 2 -Y-(CH2) z - Corresponding group (= and -(CH2)) z -YR 5 -R 6 The corresponding halogen compound or pseudohalogen compound reacts with R (reaction 1). Thus, a compound is obtained that reacts with R... 3 One end of the corresponding perfluoropolyether chain has a property similar to R. 1 -R 2-Y-(CH2) z - Corresponding group (= and -(CH2)) z -YR 5 -R 6 Intermediate compounds 1-3 (reaction 1) of the corresponding group.

[0241] Next, the terminal hydroxyl group of intermediate compounds 1-3 is reacted with R in formula (1). 4 The corresponding chain structure has epoxy groups at both ends of the compound reacts (reaction 2).

[0242] As in relation to R 4 Compounds with epoxy groups at both ends of the corresponding chain structure can be exemplified by compounds shown in formula (9-1) or formula (9-2) below.

[0243]

[0244] Using the compound shown in formula (9-1) as R in formula (1) 4 In the case of compounds with epoxy groups at both ends of the corresponding chain structure, for example, they can be manufactured using the method shown below. That is, as shown in the following reaction formula (10), a halogen compound having an alkenyl group, a chlorine compound having an alkenyl group, or a halogen compound having an alkenyl group (in reaction formula (10) the halogen compound is a bromine compound) is reacted with an alcohol having an alkenyl group to obtain a compound having alkenyl groups at both ends. Then, it can be manufactured by reacting m-chloroperbenzoic acid (mCPBA) with the compound having alkenyl groups at both ends to oxidize the two alkenyl groups.

[0245]

[0246] As the compound shown in formula (9-2), commercially available products can be used (e.g., trade name: 1,3-diglycidylglycerol ether, manufactured by Aurora Fine Chemicals).

[0247] By performing a deprotection reaction using a known method after the above steps, it is possible to manufacture a product in formula (1) where x is 1 and R... 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 The same compound.

[0248] [Fourth manufacturing method (when x is 2)]

[0249] (R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 Different situations)

[0250] First, the process is the same as the second manufacturing method, manufacturing in conjunction with R. 1 -R 2 -Y-(CH2) z -R on the side 3 One end of the corresponding perfluoropolyether chain has a property similar to R. 1 -R 2 -Y-(CH2) z - The intermediate compound 1a corresponding to the group (reaction 1).

[0251] Furthermore, the process is carried out in the same manner as the second manufacturing method, manufacturing with -(CH2) z -YR 5 -R 6 Side R 3 One end of the corresponding perfluoropolyether chain has a -(CH2) group. z -YR 5 -R 6 The intermediate compound 1b corresponding to the group (reaction 2).

[0252] Next, prepare R at the center of the molecule in equation (1). 3 The corresponding perfluoropolyether chain has fluorinated compounds with hydroxymethyl (-CH2OH) groups at both ends. Next, the hydroxyl groups of the hydroxymethyl groups at both ends of the fluorinated compounds are reacted with R in formula (1). 4 The above-mentioned compounds, whose corresponding chain structures have an epoxy group at one end and an alkenyl group at the other end, react (reaction 3).

[0253] As R in equation (1) 4 Compounds with an epoxy group at one end and an alkenyl group at the other end of the corresponding chain structure can be, for example, compounds shown in formulas (7-1) to (7-4) above.

[0254] Next, the alkenyl group is oxidized by reacting m-chloroperbenzoic acid (mCPBA) with the compound generated by the third reaction (reaction 4). This yields R at the center of the molecule in formula (1). 3 The two ends of the corresponding perfluoropolyether chain have the same R as in formula (1).4 The corresponding epoxy group intermediate compound 2-1. If the compound formed after the third reaction has a hydroxyl group, the fourth reaction can be carried out after the hydroxyl group has been appropriately protected by a known method.

[0255] Then, the hydroxyl group of the hydroxymethyl group at one end of intermediate compound 1a is reacted with the epoxy group at one end of intermediate compound 2-1 to obtain intermediate compound 2-2 (reaction 5).

[0256] Next, the hydroxyl group of the hydroxymethyl group at one end of intermediate compound 1b is reacted with the epoxy group of intermediate compound 2-2 obtained in reaction 5 (reaction 6).

[0257] By performing a deprotection reaction using a known method after the above steps, it is possible to manufacture a product in formula (1) where x is 2 and R... 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 Different compounds.

[0258] [Fifth manufacturing method (when x is 2)]

[0259] (R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 (same situation)

[0260] First, the process is the same as the third manufacturing method, manufacturing is carried out in conjunction with R. 1 -R 2 -Y-(CH2) z -R on the side 3 (=-(CH2) z -YR 5 -R 6 Side R 3 One end of the corresponding perfluoropolyether chain has a property similar to R. 1 -R 2 -Y-(CH2) z - Corresponding group (= and -(CH2)) z -YR 5 -R6 Intermediate compounds 1-3 (reaction 1) of the corresponding group.

[0261] Next, following the same procedure as in the fourth manufacturing method, R is manufactured at the center of the molecule in formula (1). 3 The two ends of the corresponding perfluoropolyether chain have the same R as in formula (1). 4 The corresponding epoxy group intermediate compound 2-1 (reaction 2).

[0262] Then, the hydroxyl group of the hydroxymethyl group at one end of intermediate compound 1-3 is reacted with the epoxy groups at both ends of intermediate compound 2-1 (reaction 3).

[0263] By performing a deprotection reaction using a known method after the above steps, it is possible to manufacture a product in formula (1) where x is 2 and R... 1 -R 2 -Y-(CH2) z -O-CH2-R 3 - and -R 3 -CH2-O-(CH2) z -YR 5 -R 6 The same compound.

[0264] [Sixth manufacturing method (for cases where x is 0)]

[0265] First, prepare R in equation (1) 3 The two ends of the corresponding perfluoropolyether chain are respectively configured with fluorinated compounds containing hydroxymethyl (-CH2OH).

[0266] Next, the hydroxyl group of the hydroxymethyl group at one end of the above-mentioned fluorinated compound is reacted with -R in formula (1). 2 -Y-(CH2) z - A compound with an alkenyl group at one end and a halogen or pseudohalogen group at the other end reacts (reaction 1). Thus, a compound is obtained in reaction with R... 3 One end of the corresponding perfluoropolyether chain has a -R 2 -Y-(CH2) z - The intermediate compound 3a corresponding to the group.

[0267] As in equation (1) -R 2 -Y-(CH2) z- Compounds with an alkenyl group at one end and a halogen or pseudohalogen group at the other end of the corresponding chain structure can be used, for example, compounds shown in formulas (11-1) to (11-4) below. In formulas (11-2) to (11-4) below, MOM represents methoxymethyl and Ts represents p-toluenesulfonyl.

[0268]

[0269] For example, when using the compound shown in formula (12-1) (described in formula (13-1) below) as -R in formula (1) 2 -Y-(CH2) z - In the case of a compound whose corresponding chain structure has an alkenyl group at one end and a halogen or pseudohalogen group at the other end, it can be manufactured using the method shown below.

[0270] First, as shown in formula (13-1) below, prepare an alcohol having an unsaturated bond, and a primary hydroxyl group and an epoxy group protected by a tetrahydropyranyl (THP) group and having the -R group in formula (1). 2 -Y-(CH2) z -A compound corresponding to a portion of the structure.

[0271] Furthermore, the above-mentioned allyl alcohol is reacted with the substance having the same -R 2 -Y-(CH2) z The compound corresponding to a portion of the structure is reacted, and the secondary hydroxyl group of the resulting compound is protected with chloromethyl methyl ether (MOMCl). Then, the resulting compound is reacted with an acid to selectively deprotect the THP group from the protected primary hydroxyl group, and the primary hydroxyl group is reacted with p-toluenesulfonyl chloride (TsCl). By performing the above steps, the compound shown in formula (12-1) is obtained.

[0272] The number of methylene groups of the primary hydroxyl groups protected by the THP group in the compound used as a raw material is z in formula (1). Therefore, a3 in formula (13-1) is 1 to 9 (z-1 in formula (1)), determined according to the value of z in formula (1) of the synthesized compound.

[0273]

[0274] (In formula (13-1), a3 represents an integer from 1 to 9, and a4 represents an integer from 1 to 4. In formula (13-1), THP represents tetrahydropyranyl, MOM represents methoxymethyl, and Ts represents p-toluenesulfonyl.)

[0275] As the compound shown in formula (11-1), a commercially available product can be used (e.g., trade name: 3-[(2-bromoethoxy)]-propene, manufactured by Aurora Fine Chemicals).

[0276] Next, the hydroxyl group of the hydroxymethyl group at the other end of the intermediate compound 3a obtained by the above method is reacted with -(CH2) in formula (1). z -YR 5 - A compound with an alkenyl group at one end and a halogen or pseudohalogen group at the other end reacts (reaction 2). Thus, a compound is obtained in reaction with R... 3 One end of the corresponding perfluoropolyether chain has a -R 2 -Y-(CH2) z - Corresponding group and having -(CH2) at another end. z -YR 5 - The intermediate compound 3b corresponding to the group.

[0277] As used in the second reaction with -(CH2) z -YR 5 - The corresponding chain structure has an alkenyl group at one end and a halogen or pseudohalogen group at the other end, and can be used with the compounds that can be used in the first reaction with -R 2 -Y-(CH2) z - The same compound as the one with an alkenyl group at one end and a halogen or pseudohalogen group at the other end of the corresponding chain structure. Therefore, as used in the second reaction with -(CH2) z -YR 5 - Compounds with an alkenyl group at one end and a halogen or pseudohalogen group at the other end of the corresponding chain structure can be used, for example, compounds shown in formulas (11-1) to (11-4) above.

[0278] The first and second reactions can be carried out using conventionally known methods, based on -R in equation (1). 2 -Y-(CH2) z - and -(CH2) z -YR 5 The type of - is determined appropriately. Furthermore, any reaction between the first and second reactions can be carried out first. Additionally, in -R 2 -Y-(CH2) z - and -(CH2) z -YR 5 - Under the same conditions, the first reaction and the second reaction can occur simultaneously.

[0279] Next, by oxidizing the double bonds in intermediate compound 3b and then subjecting it to acid treatment, R is obtained. 1 and R 6 The intermediate compound 3c (reaction 3) is a hydrogen atom.

[0280] After the above steps, a known method is used to carry out a deprotection reaction, thereby removing the protecting groups such as THP group, MOM group, and benzyl group and converting them into hydroxyl groups. The epoxy group is then hydrolyzed to become a diol, thereby producing a compound with x=0 in formula (1).

[0281] [Lubricant for magnetic recording media]

[0282] The lubricant (coating) for magnetic recording media in this embodiment includes a fluorinated ether compound as shown in formula (1).

[0283] Regarding the lubricant of this embodiment, any known materials used as lubricants may be mixed as needed, provided that the properties of the fluorinated ether compound represented by formula (1) are not impaired.

[0284] Specific examples of known materials include, for instance, FOMBLIN (registered trademark) ZDIAC, FOMBLINZDEAL, FOMBLIN AM-2001 (and above, manufactured by Solvay Solexis), Moresco A20H (manufactured by Moresco), etc. The known materials used in combination with the lubricant of this embodiment preferably have a number average molecular weight of 1000 to 10000.

[0285] When the lubricant of this embodiment contains materials other than the fluorinated ether compound shown in formula (1), the content of the fluorinated ether compound shown in formula (1) in the lubricant of this embodiment is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. The upper limit of the content of the fluorinated ether compound shown in formula (1) can be arbitrarily selected; for example, it can be 99% by mass or less, or 95% by mass or less.

[0286] The lubricant of this embodiment contains a fluorinated ether compound as shown in formula (1) above, and therefore can form a lubricating layer with excellent wear resistance and high spin-off inhibition effect.

[0287] In this embodiment, the use of the coating of the present invention as a lubricant for magnetic recording media is given as an example, but the application of the coating of the present invention is not limited to lubricants for magnetic recording media.

[0288] [Magnetic recording media]

[0289] In this embodiment, the magnetic recording medium has a magnetic layer, a protective layer, and a lubricating layer sequentially disposed on the substrate, starting from the substrate side.

[0290] For the magnetic recording medium of this embodiment, one or more base layers may be provided between the substrate and the magnetic layer as needed. Alternatively, an adhesion layer and / or a soft magnetic layer may be provided between the base layer and the substrate.

[0291] Figure 1 A schematic cross-sectional view showing one embodiment of the magnetic recording medium of the present invention.

[0292] In this embodiment, the magnetic recording medium 10 is formed on a substrate 11, and in sequence from the substrate 11 side, an adhesion layer 12, a soft magnetic layer 13, a first base layer 14, a second base layer 15, a magnetic layer 16, a protective layer 17, and a lubricating layer 18 are provided.

[0293] "Substrate"

[0294] The substrate 11 can be any type. Preferably, a non-magnetic substrate, for example, on a substrate formed of a metal or alloy such as Al or an Al alloy, on which a film formed of NiP or a NiP alloy is formed is used.

[0295] Furthermore, as substrate 11, a non-magnetic substrate formed of non-metallic materials such as glass, ceramic, silicon, silicon carbide, carbon, and resin can be used, or a non-magnetic substrate on which a film of NiP or NiP alloy is further formed on a substrate formed of these non-metallic materials can be used.

[0296] "Adhesion layer"

[0297] The adhesion layer 12 prevents corrosion of the substrate 11 when the substrate 11 is grounded to the soft magnetic layer 13 disposed on the adhesion layer 12.

[0298] The material of the adhesion layer 12 can be arbitrarily selected, for example, it can be appropriately selected from Cr, Cr alloy, Ti, Ti alloy, CrTi, NiAl, AlRu alloy, etc. The adhesion layer 12 can be formed, for example, by sputtering.

[0299] "Soft magnetic layer"

[0300] The soft magnetic layer 13 can be chosen arbitrarily, but preferably has a structure in which a first soft magnetic film, an intermediate layer made of Ru film, and a second soft magnetic film are stacked sequentially. That is, the soft magnetic layer 13 preferably has a structure in which the soft magnetic films above and below the intermediate layer are antiferroic coupled (AFC) by sandwiching an intermediate layer made of Ru film between the two soft magnetic films.

[0301] Examples of materials that can be used for the first and second soft magnetic films include CoZrTa alloys and CoFe alloys.

[0302] Preferably, any one of Zr, Ta, or Nb is added to the CoFe alloy used in the first and second soft magnetic films. This promotes the amorphization of the first and second soft magnetic films. As a result, the orientation of the first substrate layer (seed layer) can be improved, and the head lift can be reduced.

[0303] The soft magnetic layer 13 can be formed, for example, by sputtering.

[0304] "First basal layer"

[0305] The first base layer 14 is a layer that controls the orientation and crystal size of the second base layer 15 and the magnetic layer 16 disposed thereon.

[0306] Examples of first base layers 14 include layers composed of Cr, Ta, Ru, or CrMo alloy layers, CoW alloy layers, CrW alloy layers, CrV alloy layers, CrTi alloy layers, etc.

[0307] The first base layer 14 can be formed, for example, by sputtering.

[0308] "Second basal layer"

[0309] The second substrate layer 15 is a layer controlled in such a way that the orientation of the magnetic layer 16 becomes well. The second substrate layer 15 can be chosen arbitrarily, but is preferably a layer formed of Ru or a Ru alloy.

[0310] The second base layer 15 can be a single layer or multiple layers. If the second base layer 15 is composed of multiple layers, all layers can be made of the same material, or at least one layer can be made of a different material.

[0311] The second base layer 15 can be formed, for example, by sputtering.

[0312] "Magnetic layer"

[0313] The magnetic layer 16 is composed of a magnetic film whose easy magnetization axis is oriented vertically or horizontally relative to the substrate surface. The magnetic layer 16 can be arbitrarily selected, but is preferably a layer containing Co and Pt. To improve SNR characteristics, the magnetic layer 16 can be a layer containing oxides, Cr, B, Cu, Ta, Zr, etc.

[0314] Examples of oxides contained in the magnetic layer 16 include SiO2, SiO, Cr2O3, CoO, Ta2O3, and TiO2.

[0315] The magnetic layer 16 can consist of a single layer or multiple magnetic layers composed of different materials.

[0316] For example, when the magnetic layer 16 is composed of three layers—a first magnetic layer, a second magnetic layer, and a third magnetic layer—stacked sequentially from bottom to top, the first magnetic layer is preferably a granular structure formed of a material containing Co, Cr, and Pt, and further containing oxides. As the oxide contained in the first magnetic layer, oxides of, for example, Cr, Si, Ta, Al, Ti, Mg, and Co are preferred. In particular, TiO2, Cr2O3, and SiO2 are suitable. Furthermore, the first magnetic layer is preferably formed of a composite oxide containing two or more oxides. In particular, Cr2O3-SiO2, Cr2O3-TiO2, and SiO2-TiO2 are suitable. In addition to Co, Cr, Pt, and oxides, the first magnetic layer may also contain one or more elements selected from B, Ta, Mo, Cu, Nd, W, Nb, Sm, Tb, Ru, and Re.

[0317] The second magnetic layer can be made of the same material as the first magnetic layer. The second magnetic layer is preferably granular.

[0318] The third magnetic layer is preferably a non-granular structure formed of a material containing Co, Cr, and Pt, but not oxides. In addition to Co, Cr, and Pt, the third magnetic layer may also contain one or more elements selected from B, Ta, Mo, Cu, Nd, W, Nb, Sm, Tb, Ru, Re, and Mn.

[0319] When the magnetic layer 16 is formed of multiple magnetic layers, it is preferable to provide a non-magnetic layer between adjacent magnetic layers. When the magnetic layer 16 is composed of three layers: a first magnetic layer, a second magnetic layer, and a third magnetic layer, it is preferable to provide a non-magnetic layer between the first magnetic layer and the second magnetic layer, and between the second magnetic layer and the third magnetic layer.

[0320] The non-magnetic layer disposed between adjacent magnetic layers of magnetic layer 16 can be, for example, Ru, Ru alloy, CoCr alloy, CoCrX1 alloy (X1 represents one or more elements selected from Pt, Ta, Zr, Re, Ru, Cu, Nb, Ni, Mn, Ge, Si, O, N, W, Mo, Ti, V, B, etc.).

[0321] Preferably, an alloy material comprising oxides, metal nitrides, or metal carbides is used in the non-magnetic layer disposed between adjacent magnetic layers of the magnetic layer 16. Specifically, as oxides, examples include SiO2, Al2O3, Ta2O5, Cr2O3, MgO, Y2O3, TiO2, etc. As metal nitrides, examples include AlN, Si3N4, TaN, CrN, etc. As metal carbides, examples include TaC, BC, SiC, etc.

[0322] Non-magnetic layers can be formed, for example, by sputtering.

[0323] To achieve higher recording density, the magnetic layer 16 is preferably a magnetic layer for perpendicular magnetic recording with its easy magnetization axis oriented perpendicular to the substrate surface. The magnetic layer 16 may also be a magnetic layer for in-plane magnetic recording.

[0324] The magnetic layer 16 can be formed by any conventionally known method, such as vapor deposition, ion beam sputtering, or magnetron sputtering. The magnetic layer 16 is typically formed by sputtering.

[0325] "Protective layer"

[0326] The protective layer 17 protects the magnetic layer 16. The protective layer 17 can be composed of one layer or multiple layers. Examples of materials for the protective layer 17 include carbon, nitrogen-containing carbon, and silicon carbide. A carbon-based protective layer is preferred, and an amorphous carbon protective layer is particularly preferred. If the protective layer 17 is a carbon-based protective layer, the interaction with the polar groups (especially hydroxyl groups) contained in the fluorinated ether compound in the lubricating layer 18 is further enhanced, making it preferable.

[0327] The adhesion between the carbon-based protective layer and the lubricating layer 18 can be controlled by making the carbon-based protective layer hydrogenated carbon and / or nitrided carbon, and adjusting the hydrogen and / or nitrogen content in the carbon-based protective layer. The hydrogen content in the carbon-based protective layer is preferably 3 atomic% to 20 atomic% when measured by hydrogen forward scattering (HFS). Furthermore, the nitrogen content in the carbon-based protective layer is preferably 4 atomic% to 15 atomic% when measured by X-ray photoelectron spectroscopy (XPS).

[0328] The hydrogen and / or nitrogen contained in the carbon-based protective layer do not need to be uniformly contained throughout the entire carbon-based protective layer. For example, a tilted composition is suitable for the carbon-based protective layer 17, in which nitrogen is contained on the lubrication layer 18 side and hydrogen is contained on the magnetic layer 16 side. In this case, the adhesion between the magnetic layer 16 and the lubrication layer 18 and the carbon-based protective layer is further improved.

[0329] The thickness of the protective layer 17 is preferably 1 nm to 7 nm. If the thickness of the protective layer 17 is 1 nm or more, the performance of the protective layer 17 is fully obtained. If the thickness of the protective layer 17 is 7 nm or less, it is preferred from the viewpoint of thinning the protective layer 17.

[0330] The film formation method for the protective layer 17 can be a sputtering method using a carbon-containing target, a CVD (chemical vapor deposition) method using hydrocarbon raw materials such as ethylene and toluene, or an IBD (ion beam deposition) method.

[0331] When forming a carbon-based protective layer as protective layer 17, the film can be formed, for example, by DC magnetron sputtering. In particular, when forming a carbon-based protective layer as protective layer 17, it is preferable to form an amorphous carbon protective layer by plasma CVD. The amorphous carbon protective layer formed by plasma CVD has a uniform surface and low roughness.

[0332] "Lubrication layer"

[0333] The lubricating layer 18 prevents contamination of the magnetic recording medium 10. In addition, the lubricating layer 18 reduces the friction of the magnetic head of the magnetic recording and playback device that slides on the magnetic recording medium 10, thereby improving the durability of the magnetic recording medium 10.

[0334] Lubricating layer 18 Figure 1 As shown, the protective layer 17 is grounded. The lubricating layer 18 is formed by coating the protective layer 17 with the lubricant for magnetic recording media of the above embodiment. Therefore, the lubricating layer 18 contains the above-described fluorinated ether compound.

[0335] When the protective layer 17 disposed beneath the lubricating layer 18 is a carbon-based protective layer, the lubricating layer 18 is bonded to the protective layer 17 with a particularly high bonding force. As a result, it is easy to obtain a magnetic recording medium 10 in which the surface of the protective layer 17 is covered with a high coverage even if the thickness of the lubricating layer 18 is thin, and contamination of the surface of the magnetic recording medium 10 can be effectively prevented.

[0336] The average film thickness of the lubricating layer 18 can be arbitrarily selected, preferably 0.5 nm (5 Å) to 2.0 nm (20 Å), and more preferably 0.5 nm (5 Å) to 1.0 nm (10 Å). If the average film thickness of the lubricating layer 18 is 0.5 nm or more, the lubricating layer 18 will not become island-like or mesh-like, but will be formed with a uniform film thickness. Therefore, the surface of the protective layer 17 is covered with a high coverage rate through the lubricating layer 18, and the film thickness reduction caused by spin-off is less likely to occur. In addition, by making the average film thickness of the lubricating layer 18 2.0 nm or less, the lubricating layer 18 can be sufficiently thinned, and the rise of the magnetic head is sufficiently small.

[0337] "Methods for forming a lubricating layer"

[0338] As a method for forming the lubricating layer 18, for example, a magnetic recording medium in the manufacturing process in which layers up to the protective layer 17 are formed on the substrate 11 is prepared, a lubricating layer forming solution is applied to the protective layer 17, and then dried.

[0339] The lubricating layer forming solution is obtained by dispersing and dissolving the lubricant for the magnetic recording medium described in the above embodiment in a solvent as needed, to achieve a viscosity and concentration suitable for the coating method.

[0340] Solvents used in solutions for forming a lubricating layer include, for example, fluorinated solvents such as Bartel XF (trade name, manufactured by Mitsui Dupont Fluorokemica Co., Ltd.) and / or Asahieclein AE-3000 (trade name, manufactured by AGC Co., Ltd.).

[0341] There are no particular limitations on the application method of the solution for forming the lubricating layer; examples include spin coating, spray coating, paper coating, and impregnation.

[0342] When using the immersion method, a method as shown below can be used. First, a substrate 11, with layers up to the protective layer 17, is immersed in a lubricant layer forming solution added to the immersion tank of the immersion coating apparatus. Then, the substrate 11 is pulled out of the immersion tank at a predetermined speed. As a result, the lubricant layer forming solution is coated onto the surface of the protective layer 17 on the substrate 11.

[0343] By using the impregnation method, the lubricating layer forming solution can be uniformly coated on the surface of the protective layer 17, and the lubricating layer 18 can be formed on the protective layer 17 with a uniform film thickness.

[0344] In this embodiment, it is preferable to perform heat treatment on the substrate 11 on which the lubricating layer 18 is formed. By performing heat treatment, the adhesion between the lubricating layer 18 and the protective layer 17 is improved, and the bonding force between the lubricating layer 18 and the protective layer 17 is enhanced.

[0345] The heat treatment temperature is preferably 100°C to 180°C, more preferably 100°C to 160°C. If the heat treatment temperature is above 100°C, the effect of improving the adhesion between the lubricating layer 18 and the protective layer 17 is sufficiently achieved. Furthermore, by keeping the heat treatment temperature below 180°C, thermal decomposition of the lubricating layer 18 caused by heat treatment can be prevented. The heat treatment time can be appropriately adjusted according to the heat treatment temperature, and is preferably 10 minutes to 120 minutes.

[0346] In this embodiment, in order to further improve the adhesion of the lubricating layer 18 to the protective layer 17, the lubricating layer 18 can be treated with ultraviolet (UV) irradiation before or after heat treatment.

[0347] In this embodiment, the magnetic recording medium 10 has at least a magnetic layer 16, a protective layer 17, and a lubricating layer 18 sequentially disposed on a substrate 11. In this embodiment, a lubricating layer 18 comprising the aforementioned fluorinated ether compound is formed on the protective layer 17 in contact with the ground. This lubricating layer 18 covers the surface of the protective layer 17 with a high coverage even when it is thin.

[0348] Therefore, the lubricating layer 18 in the magnetic recording medium 10 of this embodiment has excellent wear resistance and spin-off resistance.

[0349] In summary, the magnetic recording medium 10 of this embodiment has excellent reliability and durability.

[0350] Example

[0351] The present invention will be further described in detail below through embodiments and comparative examples. It should be noted that the present invention is not limited to the following embodiments.

[0352] [Example 1]

[0353] The compound shown in formula (A) was obtained by the method described below.

[0354] Add HOCH2CF2O(CF2CF2O) to a 100mL round-bottom flask under a nitrogen atmosphere. h (CF2O) i 10 g of the compound represented by CF2CH2OH (where h represents the average degree of polymerization and i represents the average degree of polymerization, both being 4.5) (number average molecular weight 1000, molecular weight distribution 1.1), 9.41 g of the compound represented by formula (4-1) above, and 50 mL of dimethylformamide were stirred at room temperature until homogeneous to prepare a mixture. 11.9 g of cesium carbonate was added to this mixture, and the mixture was stirred at 50°C for 16 hours to allow the reaction to proceed.

[0355] The compound shown in formula (4-1) was synthesized by the following method. First, the hydroxyl group of ethylene glycol monoallyl ether was protected with dihydropyran, and the alkenyl group was oxidized with m-chloroperbenzoic acid to prepare a compound having a primary hydroxyl group and an epoxy group protected by a tetrahydropyran (THP) group. Then, acetone glycerol was reacted with the obtained compound to protect the secondary hydroxyl group of the resulting compound with chloromethyl methyl ether (MOMCl). Next, the resulting compound was reacted with an acid to selectively deprotect the THP group, and the primary hydroxyl group was reacted with p-toluenesulfonyl chloride (TsCl) to obtain the compound shown in formula (4-1).

[0356] The reaction solution was brought to room temperature, and 50 g of a 10% hydrogen chloride / methanol solution (hydrogen chloride-methanol reagent (5-10%) manufactured by Tokyo Chemical Industry Co., Ltd.) was added. The mixture was stirred at room temperature for 4 hours. Then, the reaction solution was transferred bit by bit to a separatory funnel containing 100 mL of saturated sodium bicarbonate solution and extracted twice with 200 mL of ethyl acetate. The organic layer was washed sequentially with 100 mL of saline, 100 mL of saturated sodium bicarbonate solution, and 100 mL of saline, and dehydrated with anhydrous sodium sulfate. After filtration with a drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain compound (A) (Rf1 in formula (A) is the PFPE chain shown in formula (3-1) above. In Rf1, h, representing the average degree of polymerization, represents 4.5, and i, representing the average degree of polymerization, represents 4.5.) 5.54 g.

[0357] The resulting compound (A) was subjected to... 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0358] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (34H), 4.13-4.30 (4H)

[0359] [Example 2]

[0360] The compound shown in formula (B) above was obtained by the method shown below.

[0361] Replace HOCH2CF2O(CF2CF2O) h (CF2O) i The compound shown is CF2CH2OH (where h represents the average degree of polymerization and i represents the average degree of polymerization, both of which are 4.5), with a number-average molecular weight of 1000 and a molecular weight distribution of 1.1, while HOCH2CF2O (CF2CF2O) was used. h (CF2O) i 9.86 g of the compound CF2CH2OH (where h represents the average degree of polymerization and i represents the average degree of polymerization as 8.5 and i represents the average degree of polymerization as 0.) (number average molecular weight 986, molecular weight distribution 1.1) was obtained. Otherwise, the same procedure as in Example 1 was performed to obtain 5.49 g of compound (B) (where Rf1 in formula (B) is the PFPE chain shown in formula (3-1) above. In Rf1, h represents the average degree of polymerization as 8.5 and i represents the average degree of polymerization as 0.)

[0362] The resulting compound (B) was subjected to... 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0363] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (34H), 4.13-4.30 (4H)

[0364] [Example 3]

[0365] The compound shown in formula (C) was obtained by the method described below.

[0366] Replace HOCH2CF2O(CF2CF2O) h (CF2O) i The compound shown in the formula CF2CH2OH (where h represents the average degree of polymerization and i represents the average degree of polymerization, both being 4.5) has a number-average molecular weight of 1000 and a molecular weight distribution of 1.1, while HOCH2CF2CF2O (CF2CF2CF2O) was used. j 10 g of the compound CF2CF2CH2OH (where j, representing the average degree of polymerization, is 4.5) (number average molecular weight 1000, molecular weight distribution 1.1) was obtained, and otherwise, the same procedure as in Example 1 was performed to obtain 5.54 g of compound (C) (where Rf2 in formula (C) is the PFPE chain shown in formula (3-2) above. In Rf2, j, representing the average degree of polymerization, is 4.5).

[0367] The resulting compound (C) was subjected to... 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0368] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (34H), 4.13-4.30 (4H)

[0369] [Example 4]

[0370] The compound shown in formula (D) was obtained by the method described below.

[0371] Instead of the compound shown in formula (4-1), 9.25 g of the compound shown in formula (4-2) was used, and the same procedure as in Example 3 was performed to obtain compound (D) (in formula (D), Rf2 is the PFPE chain shown in formula (4-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.) 5.66 g.

[0372] The compound shown in formula (4-2) was synthesized by the following method. First, after protecting the hydroxyl group of allyloxypropanol with dihydropyran, the alkenyl group was oxidized with m-chloroperbenzoic acid to prepare a compound having a primary hydroxyl group protected by a tetrahydropyran (THP) group and an epoxy group. Then, acetone glycerol was reacted with the obtained compound to protect the secondary hydroxyl group of the resulting compound with chloromethyl methyl ether (MOMCl). Next, the resulting compound was reacted with an acid to selectively deprotect the THP group, and the primary hydroxyl group was reacted with p-toluenesulfonyl chloride (TsCl) to obtain the compound shown in formula (4-2).

[0373] The resulting compound (D) was subjected to... 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0374] 1 ¹H-NMR (acetone-D6): δ [ppm] = 1.81-1.97 (4H), 3.44-3.91 (34H), 4.13-4.30 (4H)

[0375] [Example 5]

[0376] The compound shown in formula (E) was obtained by the method described below.

[0377] (Reaction 1)

[0378] Add HOCH2CF2CF2O(CF2CF2CF2O) to a 100mL round-bottom flask under a nitrogen atmosphere. j 10 g of the compound represented by CF2CF2CH2OH (where j represents the average degree of polymerization, which is 4.5) (number average molecular weight 1000, molecular weight distribution 1.1), 1.66 g of the compound represented by formula (4-3) above, and 20 mL of dimethylformamide were stirred at room temperature until homogeneous to prepare a mixture. 4.61 g of cesium carbonate was added to this mixture, and the mixture was stirred at 50°C for 16 hours to allow the reaction to proceed.

[0379] The compound shown in formula (4-3) was synthesized by the following method. First, the primary hydroxyl group of acetone glycerol was reacted with p-toluenesulfonyl chloride (TsCl). Then, ethylene glycol was reacted with the resulting compound. Furthermore, the primary hydroxyl group of the resulting compound was reacted with p-toluenesulfonyl chloride (TsCl) to obtain the compound shown in formula (4-3).

[0380] The reaction product obtained after the first reaction was cooled to 25°C and transferred to a separatory funnel containing 100 mL of water. It was extracted three times with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated with anhydrous sodium sulfate. After filtration with a drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 2.81 g of the compound represented by formula (11) as intermediate compound 1-1.

[0381]

[0382] (In equation (11), Rf2 represents the PFPE chain shown in equation (3-2) above. In Rf2, j, representing the average degree of polymerization, is 4.5.)

[0383] (Reaction 2)

[0384] In a 100 mL flask under a nitrogen atmosphere, 2.81 g of compound of formula (11), which is the intermediate compound 1-1 obtained above, 1.35 g of compound of formula (4-1), and 20 mL of dimethylformamide were added and stirred at room temperature until homogeneous to prepare a mixture. 1.78 g of cesium carbonate was added to this mixture, and the mixture was stirred at 50 °C for 16 hours to allow it to react.

[0385] The reaction solution was brought to room temperature, and 50 g of a 10% hydrogen chloride / methanol solution (hydrogen chloride-methanol reagent (5-10%) manufactured by Tokyo Chemical Industry Co., Ltd.) was added. The mixture was stirred at room temperature for 4 hours. Then, the reaction solution was transferred bit by bit to a separatory funnel containing 100 mL of saturated sodium bicarbonate solution and extracted twice with 200 mL of ethyl acetate. The organic layer was washed sequentially with 100 mL of saline, 100 mL of saturated sodium bicarbonate solution, and 100 mL of saline, and dehydrated with anhydrous sodium sulfate. After filtration with a drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 2.60 g of compound (E) (Rf2 in formula (E) is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5).

[0386] The resulting compound (E) was subjected to 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0387] 1 ¹H-NMR (acetone-D6): δ [ppm] = 3.44-3.91 (28H), 4.13-4.30 (4H)

[0388] [Example 6]

[0389] The compound shown in formula (F) was obtained by the method described below.

[0390] (Reaction 1)

[0391] The same procedure was followed as in the first reaction of Example 5, and compounds of formula (11) were obtained as intermediate compounds 1-3.

[0392] (Reaction 2)

[0393] Next, under a nitrogen atmosphere, 8.70 g of the compound represented by formula (11) of intermediate compounds 1-3 obtained above, 0.83 g of the compound represented by formula (9-1) above, and 20 mL of tert-butanol were added to a 100 mL flask, and stirred at room temperature until homogeneous to prepare a mixture. 0.23 g of potassium tert-butoxide was added to this mixture, and the mixture was stirred at 70 °C for 16 hours to allow it to react.

[0394] The reaction product obtained after the reaction was cooled to 25°C and transferred to a separatory funnel containing 100 mL of water. It was extracted three times with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated using anhydrous sodium sulfate. After filtration to separate the product from the drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain compound (F) (where Rf2 in formula (F) represents the PFPE chain shown in formula (3-2) above. In the two Rf2s, j, representing the average degree of polymerization, indicates 4.5). 6.05 g of compound (F) was obtained.

[0395] The resulting compound (F) was subjected to 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0396] 1 ¹H NMR (acetone-D6): δ [ppm] = 1.81-1.97 (6H), 3.44-3.91 (34H), 4.13-4.30 (8H)

[0397] [Example 7]

[0398] The compound shown in formula (G) was obtained by the method described below.

[0399] (Reaction 1)

[0400] Add HOCH2CF2CF2O(CF2CF2CF2O) to a 100mL round-bottom flask under a nitrogen atmosphere. j5 g of the compound represented by CF2CF2CH2OH (where j represents the average degree of polymerization, which is 4.5) (number average molecular weight 1000, molecular weight distribution 1.1), 1.73 g of the compound represented by formula (11-1) above, and 20 mL of dimethylformamide were stirred at room temperature until homogeneous to prepare a mixture. 2.30 g of cesium carbonate was added to this mixture, and the mixture was stirred at 50°C for 16 hours to allow the reaction to proceed.

[0401] The reaction product obtained after the first reaction was cooled to 25°C and transferred to a separatory funnel containing 100 mL of water. It was extracted three times with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated using anhydrous sodium sulfate. After filtration to separate the product with a drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 4.11 g of the compound represented by formula (16-1) as intermediate compound 3b.

[0402]

[0403] (In equation (16-1), Rf2 represents the PFPE chain shown in equation (3-2) above. In Rf2, j, representing the average degree of polymerization, is 4.5.)

[0404] (Reaction 2)

[0405] The double bond of the compound shown in formula (16-1) was oxidized with m-chloroperbenzoic acid (mCPBA). After the reaction, an aqueous solution of sodium thiosulfate was added, and the resulting reaction product was transferred to a separatory funnel containing 100 mL of water at 25 °C. The product was extracted three times with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated with anhydrous sodium sulfate. After filtration to separate the product using a drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography. 3.65 g of the compound shown in formula (16-2) was obtained as intermediate compound 3c.

[0406]

[0407] (Third reaction)

[0408] Finally, 31 g of a 10% hydrogen chloride / methanol solution (hydrogen chloride-methanol reagent (5-10%) manufactured by Tokyo Chemical Industry Co., Ltd.) was added to the compound shown in formula (16-2), and the mixture was stirred at room temperature for 2 hours. The reaction solution was transferred bit by bit to a separatory funnel containing 100 mL of saline solution and extracted three times with 200 mL of ethyl acetate. The organic layer was washed successively with 100 mL of saline solution, 100 mL of saturated sodium bicarbonate solution, and 100 mL of saline solution, and dehydrated with anhydrous sodium sulfate. After separation by filtration with a drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 3.87 g of compound (G) (Rf2 in formula (G) is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5).

[0409] The resulting compound (G) was subjected to 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0410] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (¹⁴H), 4.13-4.30 (⁴H)

[0411] [Example 8]

[0412] The compound represented by formula (H) above was obtained by the method shown below.

[0413] Instead of the compound shown in formula (11-1), 2.34 g of the compound shown in formula (15) was used, and otherwise the same operation as in Example 7 was performed to obtain 4.25 g of the compound (H) shown in formula (H) (Rf2 in formula (H) is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.)

[0414] The compound shown in formula (15) was synthesized by the following method. First, 3-buten-1-ol was reacted after protecting the primary hydroxyl group of ethylene oxide ethanol with dihydropyran. Next, ethylene glycol was reacted with a compound obtained by oxidizing the alkenyl group with m-chloroperbenzoic acid, and the primary hydroxyl group of the resulting compound was reacted with p-toluenesulfonyl chloride (TsCl) to obtain the compound shown in formula (15).

[0415]

[0416] The resulting compound (H) was subjected to... 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0417] 1¹H NMR (acetone-D6): δ [ppm] = 1.81-1.97 (8H), 3.44-3.91 (34H), 4.13-4.30 (4H)

[0418] [Example 9]

[0419] The compound shown in formula (I) above was obtained by the method shown below.

[0420] Instead of the compound shown in formula (9-1), 0.66 g of epibromoethanol was used, and otherwise the same operation as in Example 6 was performed to obtain compound (I) (in formula (I), Rf2 is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.) 5.45 g.

[0421] The resulting compound (I) was subjected to 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0422] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (29H), 4.13-4.30 (8H)

[0423] [Example 10]

[0424] The compound represented by formula (J) above was obtained by the method shown below.

[0425] Instead of the compound shown in formula (9-1), 0.99 g of the compound shown in formula (9-2) was used, and otherwise the same operation as in Example 6 was performed to obtain 6.32 g of compound (J) (in formula (J), Rf2 is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.)

[0426] The resulting compound (J) was subjected to 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0427] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (40H), 4.13-4.30 (8H)

[0428] [Example 11]

[0429] The compound represented by formula (K) above was obtained by the method shown below.

[0430] Instead of the compound shown in formula (9-1), 5.38 g of the compound shown in formula (17) was used, and otherwise the same operation as in Example 6 was performed to obtain 10.1 g of compound (K) (in formula (K), Rf2 is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.)

[0431] The compound shown in formula (17) is produced by making HOCH2CF2CF2O(CF2CF2CF2O). j The compound shown in CF2CF2CH2OH (where j represents the average degree of polymerization, which is 4.5) (number average molecular weight 1000, molecular weight distribution 1.1) was obtained by reacting epibromool with CF2CF2CH2OH.

[0432]

[0433] The resulting compound (K) was subjected to... 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0434] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (34H), 4.13-4.30 (12H)

[0435] [Example 12]

[0436] The compound represented by formula (L) above was obtained by the method shown below.

[0437] Instead of the compound shown in formula (4-1), 10.1 g of the compound shown in formula (18) was used, and otherwise the same operation as in Example 3 was performed to obtain compound (L) (in formula (L), Rf2 is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.) 5.72 g.

[0438] The compound shown in formula (18) was synthesized by the following method. First, after protecting the hydroxyl group of 2-allyloxyethanol with dihydropyran, the alkenyl group was oxidized with m-chloroperbenzoic acid to prepare a compound having a primary hydroxyl group and an epoxy group protected by a tetrahydropyran (THP) group. Then, ethylene glycol was reacted with the obtained compound to react the primary hydroxyl group of the resulting compound with p-toluenesulfonyl chloride (TsCl). Next, the secondary hydroxyl group of the resulting compound was protected with a tetrahydropyran (THP) group to obtain the compound shown in formula (18).

[0439]

[0440] The resulting compound (L) was subjected to1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0441] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (30H), 4.13-4.30 (4H)

[0442] [Example 13]

[0443] The compound represented by formula (M) above was obtained by the method shown below.

[0444] Instead of the compound shown in formula (4-1), 8.31 g of the compound shown in formula (19) was used, and otherwise the same operation as in Example 3 was performed to obtain compound (M) (in formula (M), Rf2 is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.) 5.08 g.

[0445] The compound shown in formula (19) was synthesized by the following method. First, ethylene glycol was reacted with 3-butenyl glycidyl ether, and the primary hydroxyl group of the resulting compound was reacted with p-toluenesulfonyl chloride (TsCl). Next, the secondary hydroxyl group of the resulting compound was protected with tetrahydropyranyl (THP) to obtain the compound shown in formula (19).

[0446]

[0447] The resulting compound (M) was subjected to... 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0448] 1 ¹H-NMR (acetone-D6): δ [ppm] = 3.44–3.91 (28H), 4.13–4.30 (4H), 5.1–5.2 (1H), 5.2–5.3 (1H), 5.8–6.0 (1H)

[0449] [Example 14]

[0450] The compound represented by formula (N) above was obtained by the method shown below.

[0451] Instead of the compound shown in formula (4-1), 9.01 g of the compound shown in formula (20) was used, and otherwise the same operation as in Example 3 was performed to obtain compound (N) (Rf2 in formula (N) is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.) 5.51 g.

[0452] The compound represented by formula (20) was synthesized by the following method. First, ethylene glycol was reacted with glycidyl phenyl ether, and the primary hydroxyl group of the resulting compound was reacted with p-toluenesulfonyl chloride (TsCl). Next, the secondary hydroxyl group of the resulting compound was protected with tetrahydropyranyl (THP) to obtain the compound represented by formula (20).

[0453]

[0454] The resulting compound (N) was subjected to 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0455] 1 ¹H-NMR (acetone-D6): δ [ppm] = 3.44–3.91 (28H), 4.13–4.30 (4H), 5.1–5.2 (1H), 5.2–5.3 (1H), 5.8–6.0 (1H)

[0456] [Example 15]

[0457] The compound represented by formula (O) above was obtained by the method shown below.

[0458] Instead of the compound shown in formula (4-1), 9.01 g of the compound shown in formula (21) was used, and the same procedure as in Example 3 was performed to obtain 7.74 g of compound (O) (Rf2 in formula (O) is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.)

[0459] The compound shown in formula (21) was synthesized by reacting 2-bromoethanol with a compound obtained by reacting (2,2-dimethyl-1,3-dioxolane-4-yl)methaneamine with di-tert-butyl dicarbonate in methanol, and then reacting the resulting compound with p-toluenesulfonyl chloride (TsCl).

[0460]

[0461] The resulting compound (O) was subjected to 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0462] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (¹⁶H), 4.13-4.30 (¹⁴H)

[0463] [Example 16]

[0464] The compound shown in formula (P) was obtained by the method described below.

[0465] Instead of the compound shown in formula (4-1), 9.01 g of the compound shown in formula (22) was used, and otherwise the same operation as in Example 3 was performed to obtain compound (P) (in formula (P), Rf2 is the PFPE chain shown in formula (3-2) above. In Rf2, j, which represents the average degree of polymerization, means 4.5.) 7.92 g.

[0466] The compound shown in formula (22) was synthesized by reacting (2,2-dimethyl-1,3-dioxolane-4-yl)methanethiol with 2-bromoethanol, and then reacting the resulting compound with p-toluenesulfonyl chloride (TsCl).

[0467]

[0468] The resulting compound (P) was subjected to... 1 The structure was identified by H-NMR measurements, and the following results were obtained.

[0469] 1 ¹H NMR (acetone-D6): δ [ppm] = 3.44-3.91 (¹⁴H), 4.13-4.30 (⁴H)

[0470] Substituting the compounds (A) to (F) of Examples 1 to 16 obtained in this manner into Equation (1) yields the values ​​of x and R. 1 R 2 R 3 R 4 R 5 R 6 The structure of Y, the elements of Y, and the value of z are shown in Table 1.

[0471] [Table 1]

[0472] Comparative Example 1

[0473] The compound represented by the following formula (AA) was synthesized by the method described in Patent Document 1.

[0474]

[0475] (In equation (AA), Rf2 represents the average degree of polymerization, and j represents 4.5.)

[0476] [Comparative Example 2]

[0477] The compound shown in formula (AB) was synthesized by the method described in Patent Document 2.

[0478]

[0479] (In Rf1 of equation (AB), h and i represent the average degree of polymerization, where h represents 4.5 and i represents 4.5.)

[0480] Comparative Example 3

[0481] The compound represented by the following formula (AC) was synthesized by the method described in Patent Document 3.

[0482]

[0483] (In Rf1 of equation (AC), h and i represent the average degree of polymerization, where h represents 4.5 and i represents 4.5.)

[0484] Comparative Example 4

[0485] The compound shown in formula (AD) was synthesized by the method described in Patent Document 4.

[0486]

[0487] (In Rf2 of equation (AD), j represents the average degree of polymerization, and j represents 4.5.)

[0488] Next, a lubricant layer forming solution was prepared using the compounds obtained in Examples 1-16 and Comparative Examples 1-4, according to the method shown below. Then, using the obtained lubricant layer forming solution, a lubricant layer of the magnetic recording medium was formed using the method shown below, thus obtaining the magnetic recording media of Examples 1-16 and Comparative Examples 1-4.

[0489] "Solution for forming a lubricating layer"

[0490] The compounds obtained in Examples 1-16 and Comparative Examples 1-4 were dissolved in Virtue XF (trade name, manufactured by Mitsui Dupont Fluorokemica Co., Ltd.), a fluorinated solvent, and diluted with Virtue to a film thickness of 0.8 nm (8 Å) to 0.9 nm (9 Å) when coated on a protective layer, thus preparing a solution for forming a lubricating layer.

[0491] "Magnetic recording medium"

[0492] A magnetic recording medium was prepared, on which an adhesion layer, a soft magnetic layer, a first base layer, a second base layer, a magnetic layer, and a protective layer were sequentially disposed on a substrate with a diameter of 65 mm. The protective layer was formed of carbon.

[0493] The lubricating layer forming solutions of Examples 1-16 and Comparative Examples 1-4 were applied to the protective layers of magnetic recording media that had formed layers up to the protective layer by an impregnation method. It should be noted that the impregnation method was performed under the conditions of an impregnation speed of 10 mm / sec, an impregnation time of 30 sec, and a pull-out speed of 1.2 mm / sec.

[0494] Then, by adding the magnetic recording medium coated with the lubricant layer forming solution into a constant temperature bath, and performing a heat treatment at 120°C for 10 minutes to remove the solvent from the lubricant layer forming solution and improve the adhesion between the protective layer and the lubricant layer, a lubricant layer is formed on the protective layer, thereby obtaining the magnetic recording medium.

[0495] The film thickness of the lubricating layer of the magnetic recording media of Examples 1-16 and Comparative Examples 1-4 obtained by this operation was measured using a Fourier transform infrared spectrophotometer (FT-IR, trade name: Nicolet iS50, manufactured by Thermo Fisher Scientific). The results are shown in Table 2.

[0496] Next, the magnetic recording media of Examples 1-16 and Comparative Examples 1-4 were subjected to the following abrasion resistance test and spin-off characteristic test.

[0497] [Abrasion Resistance Test]

[0498] Using a pin-disc type tribometer, an alumina ball with a diameter of 2 mm, serving as the contact element, was slid across the lubricating layer of a magnetic recording medium under a load of 40 gf and a sliding speed of 0.25 m / sec. The surface friction coefficient of the lubricating layer was measured. Furthermore, the sliding time until the surface friction coefficient of the lubricating layer increased sharply was measured. The sliding time until the friction coefficient increased sharply was measured four times for each lubricating layer of the magnetic recording medium, and the average value (time) was used as an index of the wear resistance of the lubricant coating. The results for magnetic recording media using the compounds of Examples 1-16 and Comparative Examples 1-4 are shown in Table 2. The evaluation of the friction coefficient increase time is described below.

[0499] A: Over 850 seconds

[0500] B: 750 seconds or more but less than 850 seconds

[0501] C: 650 seconds or more but less than 750 seconds

[0502] D: Less than 650 seconds

[0503] It should be noted that the time until the coefficient of friction increases sharply can be used as an indicator of the wear resistance of the lubricating layer for the following reasons. This is because the lubricating layer of the magnetic recording medium wears down through the use of the medium. If the lubricating layer disappears due to wear, the contact element comes into direct contact with the protective layer, and the coefficient of friction increases sharply. Therefore, the time until this coefficient of friction increases sharply can be considered relevant to friction tests.

[0504] [Spin-off property test]

[0505] A magnetic recording medium was mounted on a spin-support and rotated at 10,000 rpm for 72 hours at 80°C. Before and after this operation, the film thickness of the lubricating layer at a radius of 20 mm from the center of the magnetic recording medium was measured using FT-IR, and the reduction rate of the lubricating layer film thickness before and after the test was calculated. The spin-desolvation characteristics were evaluated using the calculated film thickness reduction rate according to the evaluation criteria shown below. The results for magnetic recording media using the compounds of Examples 1-16 and Comparative Examples 1-4 are shown in Table 2.

[0506] Evaluation Criteria for Spin-Desiccation Properties

[0507] A: Film thickness reduction rate less than 2%

[0508] B: Film thickness reduction rate exceeding 2% but less than 3%

[0509] C: Film thickness reduction rate exceeding 3% and below 9%

[0510] D: Film thickness reduction rate exceeds 9%

[0511] The results of the wear resistance test and spin-off characteristic test were comprehensively evaluated using the evaluation criteria shown below.

[0512] "Overall Evaluation"

[0513] A: The evaluations for both the wear resistance test and the spin-off characteristic test are all A.

[0514] B: The evaluation of the wear resistance test and the spin-off characteristic test is A or B, and more than one of them is B.

[0515] C: C is awarded for one or more of the evaluations in the wear resistance test and spin-off characteristic test; D is not awarded.

[0516] D: One or more of the evaluations in the wear resistance test and spin-off characteristic test are rated as D.

[0517] [Table 2]

[0518] As shown in Table 2, the magnetic recording media of Examples 1 to 16, which formed a lubricating layer using the fluorinated ether compound shown in Formula (1), were all rated A in the wear resistance test and spin-off characteristic test, and the overall rating was A.

[0519] In contrast, for compounds that do not possess the -(CH2) group in fluorinated ether compounds as shown in formula (1) z The magnetic recording media of Comparative Examples 1 to 4 showed poor results in all evaluations of wear resistance and spin-off characteristics compared to the magnetic recording media of Examples 1 to 16.

[0520] Industry availability

[0521] The fluorinated ether compound of this embodiment is suitable for use as a lubricant for magnetic recording media.

[0522] Explanation of symbols

[0523] 10 Magnetic recording media, 11 substrate, 12 Adhesion layer, 13 Soft magnetic layer, 14 First basal layer, 15 2nd basal layer, 16 Magnetic layer, 17 Protective layer, 18 Lubricating layer.

Claims

1. The fluorinated ether compound represented by formula (1) below, R 1 -R 2 -Y-(CH2) z -O-CH2-R 3 [-CH2-R 4 -CH2-R 3 ] x -CH2-O-(CH2) z -Y-R 5 -R 6 (1) In equation (1), x is 0 to 2; z is an integer from 2 to 10; Y is any one of 0, NH, and S; R 3 It is a perfluoropolyether chain; (x+1) R 3 They can be partially or completely the same, or they can be different from each other; R 4 It is a divalent linker with 1 to 3 hydroxyl groups and oxygen atoms at both ends; when x is 2, the two R groups... 4 They can be the same or different; R 2 The connecting base is shown in equation (2-1) or equation (2-2) below; R 5 The connecting base is shown in equation (2-3) or equation (2-4) below; R 1 and R 6 To be with R 2 Or R 5 The terminal oxygen atom of R is bonded to a terminal group, which can be the same or different; 1 and R 6 Each is independently a terminal group selected from hydrogen atoms, alkyl groups that may have substituents, and organogroups that have double or triple bonds and may have substituents; In equation (2-1), f1 represents an integer from 1 to 3; the oxygen atom at the left end of equation (2-1) and R 1 Combine; In equation (2-2), g1 represents an integer from 2 to 6; the oxygen atom at the left end of equation (2-2) and R 1 Combine; In equation (2-3), f2 represents an integer from 1 to 3; the oxygen atom at the right end of equation (2-3) and R 6 Combine; In equation (2-4), g2 represents an integer from 2 to 6; the oxygen atom at the right end of equation (2-4) and R 6 Combine.

2. The fluorinated ether compound according to claim 1, wherein each z in formula (1) is an integer from 2 to 6.

3. The fluorinated ether compound according to claim 2, wherein each z in formula (1) is an integer from 2 to 4.

4. The fluorinated ether compound according to claim 1, wherein each of the Y in formula (1) is independently O or NH.

5. The fluorinated ether compound according to claim 4, wherein all Y in formula (1) is O.

6. The fluorinated ether compound according to claim 1, R 1 and R 6 The alkyl groups described herein are each independently an alkyl group having 1 to 8 carbon atoms that may have substituents.

7. The fluorinated ether compound according to claim 1, R 1 and R 6 The organic groups having double or triple bonds and which may have substituents are each independently selected from at least one of aromatic hydrocarbon groups, unsaturated heterocyclic groups, alkenyl groups and alkynyl groups that may have substituents.

8. The fluorinated ether compound according to claim 1, wherein the x R's in formula (1) 4 Each is independently any of the two-valent linkers shown in equations (2-5) to (2-8) below; In equation (2-5), r represents an integer from 1 to 3; In equation (2-6), s represents an integer from 2 to 6; the oxygen atom at the left end of equation (2-6) and R 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 The -CH2- atom on the side is bonded; in equation (2-7), t represents an integer from 2 to 6; the oxygen atom at the left end of equation (2-7) binds to R. 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 The -CH2- atom on the side is bonded; in equation (2-8), u represents an integer from 1 to 6, and v represents an integer from 1 to 6; u and v are not both 1; the oxygen atom at the left end of equation (2-8) binds to R. 1 The -CH2- atom on the right side is bonded, and the oxygen atom at the right end is bonded to R. 6 Side-CH2- binding.

9. The fluorinated ether compound according to claim 1, wherein the (x+1) R in formula (1) 3 Each is independently represented by the following formula (Rf); -(CF2) p1 -O-(CF2O) p2 -(CF2CF2O) p3 -(CF2CF2CF2O) p4 -(CF2CF2CF2CF2O) p5 -(CF2) p6 - (Rf) In equation (Rf), p2, p3, p4, and p5 represent the average degree of polymerization, each independently representing 0–20; where, p2, p3, p4, and p5 are not all simultaneously zero; p1 and p6 represent the average number of -CF2-, each independently representing 1 to 3; there are no special restrictions on the order of (CF2O), (CF2CF2O), (CF2CF2CF2O), and (CF2CF2CF2CF2O) which are structural units in equation (Rf).

10. The fluorinated ether compound according to claim 1, wherein the (x+1) R in formula (1) 3 Each is independently represented by the following equations (3-1) to (3-4). -CF2-(OCF2CF2) h -(OCF2) i -OCF2- (3-1) In equation (3-1), h and i represent the average degree of polymerization, where h represents 1 to 20 and i represents 0 to 20; -CF2CF2-(OCF2CF2CF2) j -OCF2CF2- (3-2) In equation (3-2), j represents the average degree of polymerization, which ranges from 1 to 15; -CF2CF2CF2-(OCF2CF2CF2CF2) k -OCF2CF2CF2- (3-3) In equation (3-3), k represents the average degree of polymerization, which ranges from 1 to 10; -(CF2) w7 -O-(CF2CF2CF2O) w8 -(CF2CF2O) w9 -(CF2) w10 - (3-4) In equation (3-4), w8 and w9 represent the average degree of polymerization, each independently representing 1 to 20; w7 and w10 represent the average amount of CF2, each independently representing 1 to 2.

11. The fluorinated ether compound according to claim 1, wherein the number average molecular weight is in the range of 500 to 10,000.

12. A coating comprising any one of the fluorinated ether compounds according to claims 1 to 11.

13. A lubricant for magnetic recording media, comprising the coating as described in claim 12.

14. A magnetic recording medium having at least a magnetic layer, a protective layer, and a lubricating layer disposed on a substrate. The lubricating layer comprises any one of the fluorinated ether compounds according to claims 1 to 11.

15. The magnetic recording medium according to claim 14, wherein the average film thickness of the lubricating layer is 0.5 nm to 2.0 nm.

Citation Information

Patent Citations

  • Master cylinder

    JP1978034064A

  • Ventilator

    JP2024066210A

  • Fluorine-containing ether compound, lubricant for magnetic recording media, and magnetic recording medium

    WO2019054148A1

  • Fluorine-containing ether compound, lubricant for magnetic recording medium, and magnetic recording medium

    WO2021090940A1

  • Fluorine-containing ether compound, lubricant for magnetic recording medium, and magnetic recording medium

    WO2021251318A1