Polyethylene and films containing the same
By controlling the thermal tack window range and molecular weight distribution of polyethylene, the problem of insufficient sealing properties of linear low-density polyethylene film under low-temperature conditions is solved, achieving stable sealing and thermal tack over a wide temperature range. It is suitable for various film applications and meets the requirements of D4R design and PPWR.
Patent Information
- Application Number
- CN202580027751.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-06-05
- Filing Date
- 2025-06-05
- Publication Date
- 2026-11-10
AI Technical Summary
Existing linear low-density polyethylene films suffer from process instability and insufficient sealing properties during preparation, especially at low temperatures where their sealing properties and thermal adhesion strength are inadequate, making it difficult to meet the requirements of high-speed packaging and high reliability.
A polyethylene is provided having a first hot-tack window ranging from 15 to 35°C and a second hot-tack window ranging from 40 to 55°C, meeting the sealing strength measurement requirements of ASTM F 1921. It is prepared by a hybrid supported metallocene catalyst, controlling the molecular weight distribution and crystal structure to ensure excellent low-temperature sealing and hot-tack properties over a wide temperature range.
It achieves stable sealing and thermal adhesion over a wide temperature range, reduces energy consumption, improves the film's impact resistance and processability, is suitable for a variety of film applications, meets D4R design and PPWR requirements, and is suitable for high-reliability packaging such as food and pharmaceuticals.
Smart Images

Figure CN123076618A_ABST
Abstract
Description
Cross-references to related applications
[0001] This application claims priority to Korean Patent Application No. 10-2024-0073747, filed on June 5, 2024, and Korean Patent Application No. 10-2025-0073542, filed on June 5, 2025, and all disclosures in the aforementioned Korean patent applications are incorporated herein by reference. Technical Field
[0002] This invention relates to polyethylene with excellent low-temperature sealing properties, sealing stability and process reliability, and to films containing the same. Background Technology
[0003] Linear low-density polyethylene (LLDPE) is produced by copolymerizing ethylene and α-olefins under low pressure using a polymerization catalyst. It is a resin with a narrow molecular weight distribution and short-chain branches of constant length without long-chain branches.
[0004] In addition to the characteristics of ordinary polyethylene, linear low-density polyethylene film also has high tensile strength and elongation, excellent film processability and transparency, as well as excellent tear strength and dart impact resistance. Therefore, its use is increasing in industrial films where it is difficult to apply traditional low-density polyethylene or high-density polyethylene (such as food packaging and industrial composite (laminated) films, heavy-duty packaging films, stretch wrap films, etc.).
[0005] It is well known that for linear low-density polyethylene (LDPE), the lower the density, the higher the dart impact resistance. However, if a large amount of comonomer is used to produce LDPE, the frequency of scaling during slurry polymerization increases, and several problems arise when preparing films containing this LDPE. For example, the amount of anti-sticking agent needs to be increased due to stickiness. Furthermore, issues such as process instability or deterioration of the resulting polyethylene morphology can occur, leading to a decrease in bulk density.
[0006] In recent years, due to the market trends of sustainability and D4R (Design for Recycling), the demand for down-gauging (D / G) has been growing, and therefore the demand for linear low-density polyethylene with excellent molding processability and dart impact resistance is also increasing.
[0007] Before the COVID-19 pandemic, D / G focused on reducing the thickness of the polyethylene layer in multilayer films from a cost perspective; however, after the COVID-19 pandemic, with increased attention to environmental issues, the demand for thinning from a recycling perspective has also increased, and the issue of energy consumption to reduce carbon emissions has also emerged.
[0008] Furthermore, D4R design from a recycling perspective to promote and activate the transition to a circular economy is gaining attention, and the need to improve the sealing properties of the sealing layer during the co-extrusion or lamination process is also increasing in the preparation of BOPE (biaxially oriented polyethylene) films and MDO (mechanically oriented) films applied to single-material all-polyethylene (All-PE) films.
[0009] In sealing properties, heat tack strength is very important. It is a key physical property for reducing defect rates in high-speed packaging processes (such as high-speed FFS) or hot-fill processes (for heavy packaged items or those requiring sterilization / pasteurization). Summary of the Invention
[0010] [Technical Issues] In order to address the problems of the prior art, the present invention aims to provide a polyethylene with excellent low-temperature sealing properties, sealing stability and process reliability.
[0011] Furthermore, the present invention aims to provide a film comprising the aforementioned polyethylene.
[0012] [Technical Solution] According to the present invention, a polyethylene is provided in which, when the seal strength is measured simultaneously with varying temperatures according to ASTM F 1921, the first hot-tight window ranges from 15 to 35°C, wherein the first hot-tight window range refers to the temperature at which a seal strength of 3 N / 25.4 mm (heat seal strength) is first achieved (HT-SIT). 3N The initial temperature of the heat-sealed seal (unit: °C) and the temperature at which the seal strength of 3 N / 25.4 mm was finally achieved (HTHT) 3N The temperature difference between the high-temperature hot-sticking temperature (unit: °C) and the high-temperature hot-sticking temperature (HTHT) 3N – HT-SIT 3N ).
[0013] Furthermore, according to the present invention, a film comprising the polyethylene is also provided.
[0014] [Beneficial Effects] The polyethylene according to the present invention exhibits excellent low-temperature sealing and hot-adhesion properties. Furthermore, the polyethylene also exhibits excellent dart impact resistance and stiffness, as well as improved molding processability. Therefore, thinner films can be achieved when using this polyethylene for film preparation, which is beneficial for D4R applications.
[0015] Furthermore, because it maintains its thermal adhesion strength above a certain level over a wide temperature range, it exhibits consistent adhesion performance, unaffected by variations in ambient temperature around the packaging machine, production speed, or localized changes in film thickness and composition that cause uneven temperature distribution in the sealing strip. It also maintains consistent adhesion performance regardless of weight variations in the packaged items or for packaging heavy items.
[0016] The polyethylene can be used as a film for a variety of purposes, such as food film, agricultural film, general industrial film or stretch film, and can be used as a sealing layer in the preparation of BOPE (biaxially oriented polyethylene) film and MDO (mechanically oriented) film applied to single-material all-polyethylene (All-PE) film, in the process of co-extrusion or lamination.
[0017] Furthermore, because it does not contain PFAS (per- and polyfluoroalkyl substances) which are subject to the Packaging and Packaging Waste Regulation (PPWR) implemented by the European Union (EU), it is also beneficial in addressing PPWR. Attached Figure Description
[0018] Figure 1 A diagram showing the first and second thermal bonding window ranges of the embodiment.
[0019] Figure 2 A diagram showing the comparative ranges of the first and second thermally bonded window areas. Detailed Implementation
[0020] In this invention, terms such as first, second, etc. are used to describe different components, and the terms are used only to distinguish one component from another.
[0021] Furthermore, the terminology used in this specification is for describing exemplary embodiments only and is not intended to limit the invention. Unless the context clearly specifies otherwise, the singular form includes the plural form. In this specification, terms such as "comprising," "having," etc., are intended to indicate the presence of the implemented features, quantities, steps, components, or combinations thereof, and should be understood to not exclude the possibility of the presence or addition of one or more other features, quantities, steps, components, or combinations thereof.
[0022] Furthermore, the term "to" used in this specification to describe numerical ranges includes both the upper and lower limits. For example, "1 to 3" means above 1 and below 3.
[0023] While the present invention can be modified and substituted in many ways, only specific embodiments are described herein, and will be described in detail. However, it should be understood that this is not intended to limit the invention to the specific forms disclosed; on the contrary, the invention is intended to cover all modifications, equivalents, and substitutions that fall within the spirit and scope of the invention.
[0024] The polyethylene of the present invention and the film comprising the polyethylene will now be described in detail.
[0025] According to one embodiment of the present invention, the polyethylene satisfies the following: when measuring the seal strength according to ASTM F 1921 while varying the temperature, the first hot-tight window ranges from 15 to 35°C, where the first hot-tight window range refers to the temperature at which the seal strength (heat seal strength) of 3 N / 25.4 mm is first achieved (HT-SIT). 3N The initial temperature of the heat-sealed seal (unit: °C) and the temperature at which the seal strength of 3 N / 25.4 mm was finally achieved (HTHT) 3N The temperature difference between (HTHT3N – HT-SIT) and (unit: °C) high-temperature hot-tack temperature (HT-SIT) 3N ).
[0026] Furthermore, when measuring seal strength while varying the temperature according to ASTM F 1921, the second hot-tight window range is 40 to 55°C. This second hot-tight window range refers to the temperature at which the seal strength (2 N / 25.4 mm) is first achieved (HT-SIT). 2N The initial temperature of the heat-sealed seal (unit: °C) and the temperature at which the seal strength of 2 N / 25.4 mm was finally achieved (HTHT) 2N The temperature difference between the high-temperature hot-sticking temperature (unit: °C) and the high-temperature hot-sticking temperature (HTHT) 2N – HT-SIT 2N ).
[0027] The term “hot-tack window range” as used in this specification is defined as the temperature difference (HTHT – HT-SIT, hot-tack seal initiation temperature) (in °C) between the temperature at which a predetermined reference seal strength (hot-tack strength) is first reached (HT-SIT, hot-tack seal initiation temperature) (in °C) and the temperature at which the same reference seal strength is last reached (HTHT, high-temperature hot-tack temperature) (in °C) as measured under specific conditions by varying the applied temperature according to ASTM F 1921.
[0028] Hot tack strength refers to the adhesive strength exceeding a certain level when sealing a film containing a heat-sealable resin layer using a heat-sealing process, before the film immediately cures (short cooling time). A specific standard hot tack strength refers to the weight of the packaged item, while HT-SIT refers to the sealing temperature exceeding that specific standard strength. On the other hand, HTHT (High Temperature Hot Tack Temperature) refers to the upper limit of the sealing temperature at which the strength of the heat-sealable resin decreases due to high temperatures and falls below the standard strength. Therefore, the temperature range between HT-HT and HT-SIT that meets the standard strength is called the hot tack window. Since the temperature of the packaging machine's heating element can fluctuate by ±5°C, ±10°C, or more due to the ambient environment, a wider hot tack window results in higher sealing stability. Furthermore, if the hot tack window shifts towards the lower temperature side, sealing can be performed even at lower sealing temperatures, thereby reducing energy consumption and allowing for the safe packaging of temperature-sensitive items.
[0029] Therefore, the heat-tack window range reflects the process window within which the film can maintain stable adhesive strength under various heat-sealing conditions. During the production of sealing films, various factors, such as changes in the temperature of the sealing strip, variations in production line speed, and inhomogeneities in film thickness or structure, can affect the consistency of sealing performance. A wide heat-tack window range ensures excellent sealing stability and process reliability even under such varying process conditions. This is especially true in vertical form-fill-seal (VFFS) and horizontal form-fill-seal (HFFS) processes, where product weight is immediately transferred to the packaging after sealing, or the sealed portion is subjected to opening forces. Therefore, the sealing portion needs to withstand these forces without damage. Thus, the heat-tack window range is a crucial technical indicator for assessing the commercial viability and practicality of packaging materials.
[0030] When measuring seal strength while varying the temperature according to ASTM F 1921, polyethylene according to one embodiment of the invention may have a first hot-tight window range of 15 to 35°C, the first hot-tight window range referring to the temperature at which a seal strength of 3 N / 25.4 mm (heat seal strength) is first achieved (HT-SIT). 3N The initial temperature of the heat-sealed seal (unit: °C) and the temperature at which the seal strength of 3 N / 25.4 mm was finally achieved (HTHT) 3N The temperature difference between the high-temperature hot-sticking temperature (unit: °C) and the high-temperature hot-sticking temperature (HTHT) 3N – HT-SIT 3N ).
[0031] More specifically, the first hot-bonding window range can be above 15°C, or above 16°C, or above 16.5°C, or above 17°C, or above 18°C, or above 19°C, or above 20°C, and below 35°C, or below 34°C, or below 33°C, or below 32°C, or below 31°C, or below 30°C.
[0032] Therefore, the polyethylene according to one embodiment of the present invention has a wide temperature range and can maintain a seal even at a high thermal tack strength of 3N. Thus, it can exhibit consistent adhesive properties without being affected by factors such as uneven sealing strip temperature, changes in production speed, local variations in film thickness and composition.
[0033] Furthermore, in the polyethylene according to one embodiment of the present invention, when the sealing strength is measured simultaneously with temperature variation according to ASTM F 1921, the temperature at which the sealing strength (heat seal strength) of 3 N / 25.4 mm is first achieved is HT-SIT. 3N It can be below 94℃. More specifically, HT-SIT 3N It can be below 94℃, or below 93.5℃, or below 93.0℃, or below 92.5℃, or below 92℃, or below 91.5℃, or below 91℃, and above 80℃, or above 81℃, or above 81.5℃, or above 82℃, or above 83℃, or above 84℃. Therefore, due to HT-SIT 3N It has a low temperature value (below 94℃) and exhibits low-temperature sealing properties even at a strength of 3N, thereby reducing energy consumption.
[0034] Furthermore, the polyethylene according to one embodiment of the invention can be designed to have a hot-tack window range of 40 to 55°C at a sealing strength standard of 2 N / 25.4 mm. Specifically, in the polyethylene according to one embodiment of the invention, when measuring the sealing strength while varying the temperature according to ASTM F 1921, a second hot-tack window range can be 40 to 55°C, where the second hot-tack window range refers to the temperature (HT-SIT) at which the sealing strength (heat seal strength) is first achieved at 2 N / 25.4 mm. 2N The initial temperature of the heat-sealed seal (unit: °C) and the temperature at which the seal strength of 2 N / 25.4 mm was finally achieved (HTHT) 2N The temperature difference between the high-temperature hot-sticking temperature (unit: °C) and the high-temperature hot-sticking temperature (HTHT) 2N – HT-SIT 2N ).
[0035] More specifically, the second heat-bonding window range can be above 40°C, or above 41°C, or above 42°C, or above 43°C, or above 43.5°C, or above 44°C, and below 55°C, or below 54°C, or below 53°C, or below 52°C, or below 51°C, or below 50°C, or below 49°C, or below 48°C, or below 47°C, or below 46°C.
[0036] Furthermore, in the polyethylene according to one embodiment of the present invention, the temperature at which the sealing strength is first reached at 2 N / 25.4 mm (heat seal strength) when the sealing strength is measured simultaneously with temperature changes according to ASTM F 1921 is HT-SIT. 2N It can be kept below 85℃. More specifically, HT-SIT 2N It can be below 85℃, or below 84.5℃, or below 84℃, or below 83.5℃, or below 83℃, and above 60℃, or above 61℃, or above 62℃, or above 63℃, or above 64℃, or above 65℃, or above 66℃, or above 67℃, or above 68℃, or above 69℃, or above 70℃, or above 71℃, or above 72℃, or above 73℃. Therefore, due to HT-SIT 2N It exhibits low values below 85°C, demonstrating low-temperature sealing properties even at a strength of 2N, thereby reducing energy consumption.
[0037] HT-SIT 3N HTHT 3N HT-SIT 2N and HTHT 2N The values are measured according to ASTM F 1921 (sealing time 0.5 seconds, sealing pressure 0.3 MPa, delay time 0.1 seconds, stretching speed 200 mm / s, J&B 5000 sealing machine) after producing a single-layer film with a thickness of 45 to 55 μm or 48 to 52 μm, more specifically 50 μm, based on a polyethylene content of 95 wt%, 96 wt%, 97 wt%, 98 wt%, 99 wt%, or 99.9 wt% or more in total composition using a blown film extruder (120 mm die diameter, 2.0 mm die gap, BUR2.5, dual air-ring system).
[0038] Therefore, since the polyethylene film according to one embodiment of the present invention has a wide temperature range in which its thermal adhesion strength can be maintained above a certain level, it can exhibit consistent adhesive performance and is not affected by factors such as uneven temperature of the sealing strip, changes in production speed, film thickness and local differences in composition.
[0039] In the case of films with a narrow heat-bonding window, defects can easily occur even with a slight error in the sealing temperature setting. However, this invention can significantly reduce the defect rate by achieving a stable seal over a wide temperature range.
[0040] Therefore, even in processes where the sealing portion is loaded immediately after product filling, such as vertical forming-fill-seal (VFFS) machines, the film maintains sufficient thermal tack strength before cooling, thus providing excellent protection against packaging breakage on high-speed production lines.
[0041] Therefore, it can be used as a highly reliable packaging material for food, medicine, disposable products, etc., and is especially suitable for harsh environments such as excessive product load, high-speed automatic packaging, and uneven sealing conditions.
[0042] Furthermore, the polyethylene according to one embodiment of the present invention has a strength of 0.900 to 0.925 g / cm³ as measured according to ASTM D 1505 standard. 3 The density.
[0043] If the density of polyethylene is too low, it is difficult to guarantee the stability of the slurry polymerization process. Furthermore, there is a trade-off between density and dart resistance, and between density and low-temperature sealing properties. If the density of polyethylene is too high, it becomes difficult to thin the film during production due to the decrease in dart resistance and low-temperature sealing properties. More specifically, the polyethylene according to the present invention has a density of 0.900 g / cm³. 3 Above, or 0.901 g / cm 3 Above, or 0.902 g / cm 3 Above, or 0.903 g / cm 3 Above, or 0.904 g / cm 3 Above, or 0.905 g / cm 3 Above, or 0.906 g / cm 3 Above, or 0.907 g / cm 3 Above, or 0.908 g / cm 3 Above, or 0.909 g / cm 3 Above, or 0.910 g / cm 3 Above, or 0.911 g / cm 3 Above, or 0.912 g / cm 3 Above, or 0.913 g / cm 3 Above, or 0.914 g / cm 3 Above, or 0.915 g / cm 3 The above, and 0.925 g / cm³ 3 Below, or 0.924 g / cm 3Below, or 0.923 g / cm 3 Below, or 0.922 g / cm 3 Below, or 0.921 g / cm 3 Below, or 0.920 g / cm 3 Below, or 0.919 g / cm 3 Below, or 0.918 g / cm 3 the following.
[0044] The polyethylene according to one embodiment of the present invention has a significantly lower sealing initiation temperature compared to conventional polyethylene of similar density, thus exhibiting excellent low-temperature sealing properties and improved stiffness. As a product with a balance of sealing properties and stiffness, when using a low-density product to improve the low-temperature sealing properties of conventional polyethylene, the waste of unused resources caused by adhesion problems that occur in practical applications of laminated roll packaging can be avoided, and the use of additives such as anti-blocking agents used to reduce the coefficient of friction can be reduced.
[0045] Furthermore, according to one embodiment of the present invention, polyethylene in the temperature-elution fractionation (TREF) process of cross-fractional chromatography (CFC) can display a specific fraction content distribution according to the elution temperature range.
[0046] For example, according to one embodiment of the present invention, the polyethylene satisfies the following condition: during the temperature elution fractionation process of cross-fractional chromatography, based on the total weight of polyethylene, the content of the polymer fraction eluted at an elution temperature of 30°C or higher and less than 60°C (30°C ≤ Te < 60°C) is 18.0 to 38.0 wt%. More specifically, the content of the polymer fraction eluted at an elution temperature of 30°C or higher and less than 60°C can be 18.0 wt% or higher, or 19.0 wt% or higher, or 20.0 wt% or higher, or 21.0 wt% or higher, or 22.0 wt% or higher, or 23.0 wt% or higher, or 24.0 wt% or higher, or 25.0 wt% or higher, and is less than 38.0 wt%, or less than 37.0 wt%, or less than 36.0 wt%, or less than 35.0 wt%, or less than 34.0 wt%, or less than 33.0 wt%.
[0047] Polymer fractions eluted within a temperature range above 30°C and below 60°C can delay secondary crystallization between the die and the frost line during blown film forming, resulting in smaller lamellar sizes and thus improved low-temperature sealing and hot-tack properties. However, if the content of this fraction is below 18.0 wt%, the increased crystallization rate leads to an increase in lamellar size, which may degrade the low-temperature sealing and hot-tack properties. On the other hand, if the content of this fraction exceeds 38.0 wt%, the relatively increased content of low crystallinity, which affects mechanical strength, may degrade the stiffness during film preparation.
[0048] Furthermore, according to one embodiment of the present invention, the polyethylene satisfies the following condition: during the temperature elution fractionation process of cross-fractional chromatography, the content of the polymer fraction eluted at an elution temperature below 35°C (Te≤35°C) based on the total weight of the polyethylene is 5.0 to 30.0 wt%. More specifically, the content of the polymer fraction eluted at an elution temperature below 35°C can be 5.0 wt% or more, or 6.0 wt% or more, or 7.0 wt% or more, or 8.0 wt% or more, or 9.0 wt% or more, or 10.0 wt% or more, or 11.0 wt% or more, or 12.0 wt% or more, and is below 30.0 wt%, or 29.0 wt%, or 28.0 wt%, or 27.0 wt%, or 26.0 wt%, or 25.0 wt%, or 24.0 wt%, or 23.0 wt%, or 22.0 wt%, or 21.0 wt%, or 20.0 wt%, or 19.0 wt%, or 18.0 wt%, or 17.0 wt%, or 16.0 wt%, or 15.0 wt%.
[0049] The polymer fraction eluted at elution temperatures below 35°C refers to a molecular structure that has ultra-low crystallinity and a high proportion of amorphous states due to the high SCB content in the polymer, or has low crystallinity and a high SCB content in the polymer. The polyethylene according to the present invention exhibits excellent low-temperature sealing properties and hot-adhesion characteristics due to this molecular structure.
[0050] Furthermore, according to one embodiment of the present invention, the polyethylene satisfies the following condition: during the temperature-elution fractionation process of cross-fractional chromatography, based on the total weight of polyethylene, the content of the polymer fraction eluted at an elution temperature of 60°C or higher and below 80°C (60°C ≤ Te < 80°C) is 20.0 to 50.0 wt%. More specifically, the content of the polymer fraction eluted at an elution temperature of 60°C or higher and below 80°C may be 20.0 wt% or higher, or 21.0 wt% or higher, or 22.0 wt% or higher, or 23.0 wt% or higher, or 24.0 wt% or higher, and is less than 30.0 wt%, or less than 29.0 wt%, or less than 28.0 wt%, or less than 27.0 wt%, or less than 26.0 wt%.
[0051] The elution temperature range above 60°C and below 80°C is the main range that determines the density and molecular weight (MI) of polyethylene. Typically, linear low-density polyethylene (LLDPE) exhibits a high crystallinity distribution within this elution temperature range. In contrast, the polyethylene according to the present invention has a low density and contains this fraction within the aforementioned content range, thereby exhibiting excellent low-temperature sealing properties and hot-tack characteristics.
[0052] Furthermore, according to one embodiment of the present invention, the polyethylene satisfies the following condition: during the temperature elution fractionation process of cross-fractional chromatography, the content of the polymer fraction eluted at an elution temperature of 80°C or higher (Te≥80°C) is 30.0 to 60.0 wt%. More specifically, the content of the polymer fraction eluted at an elution temperature above 80°C can be 30.0 wt% or more, or 31.0 wt% or more, or 32.0 wt% or more, or 33.0 wt% or more, or 34.0 wt% or more, or 35.0 wt% or more, or 36.0 wt% or more, or 37.0 wt% or more, or 38.0 wt% or more, or 39.0 wt% or more, or 40.0 wt% or more, and is below 60.0 wt%, or below 59.0 wt%, or below 58.0 wt%, or below 57.0 wt%, or below 56.0 wt%, or below 55.0 wt%, or below 54.0 wt%, or below 53.0 wt%, or below 52.0 wt%, or below 51.0 wt%, or below 50.0 wt%.
[0053] Polymer fractions eluted at elution temperatures above 80°C can affect stiffness during polyethylene film production, and the lower the content of this fraction, the lower the stiffness. On the other hand, if the content of this fraction is too high, the low-temperature sealing properties of polyethylene may be degraded. The polyethylene according to the present invention, by including polymer fractions eluted at temperatures above 80°C within the above-mentioned content range, can exhibit excellent stiffness.
[0054] Meanwhile, in this invention, temperature-elution fractionation (TREF) analysis by cross-fractional chromatography (CFC) can be performed as follows: polyethylene is dissolved in trichlorobenzene solvent, stabilized, cooled to crystallize, and then, while measuring the eluted polymer content, the crystallized polyethylene sample is heated to the fractionation temperature at a constant heating rate. More detailed measurement methods are described in the examples below.
[0055] Furthermore, according to one embodiment of the present invention, the molecular weight distribution (MWD, Mw / Mn) of the polyethylene is 2.0 to 5.0.
[0056] If the molecular weight distribution is narrow, less than 2.0, mechanical properties such as toughness are excellent, but there is a concern that molding processability may be degraded. If the molecular weight distribution exceeds 5.0, molding processability is excellent, but there is a concern that mechanical properties may be degraded. More specifically, the molecular weight distribution (MWD) of polyethylene can be: 2.0 or more, or 2.1 or more, or 2.2 or more, or 2.3 or more, or 2.4 or more, or 2.5 or more, or 2.6 or more, or 2.7 or more, or 2.8 or more, or 2.9 or more, or 3.0 or more, or 3.1 or more, or 3.2 or more, or 3.3 or more, or 3.4 or more, or 3.5 or more, or 3.6 or more, or 3.65 or more, or 3.7 or more, or 3.8 or more, and below 5.0, or below 4.9, or below 4.8, or below 4.7, or below 4.6, or below 4.5, or below 4.4, or below 4.3, or below 4.25, or below 4.2, or below 4.15, or below 4.1, or below 4.0, or below 3.9. The polyethylene according to the present invention, by satisfying the above molecular weight distribution conditions, can exhibit well-balanced and improved molding processability and mechanical properties.
[0057] In this invention, after measuring the weight-average molecular weight (Mw) and number-average molecular weight (Mn) of polyethylene using gel permeation chromatography (GPC), the molecular weight distribution is calculated using the ratio of weight-average molecular weight to number-average molecular weight (Mw / Mn). In this case, both weight-average molecular weight (Mw) and number-average molecular weight (Mn) are equivalent molecular weights of polystyrene obtained through GPC analysis.
[0058] Specifically, the PolymerChar GPC-IR chromatogram equipped with a Polymer Laboratories PLgel MIX-B 300mm long column was used. ®The instrument was used to evaluate polyethylene samples. The evaluation temperature was 160 °C, 1,2,4-trichlorobenzene was used as the solvent, and measurements were performed at a flow rate of 1 mL / min. Polyethylene samples were prepared to a concentration of 16 mg / 8 mL and then injected in 200 μL volumes. Mw and Mn values were measured using calibration curves plotted with polystyrene standards. The polystyrene standards used had nine molecular weights: 2,000 / 10,000 / 30,000 / 70,000 / 200,000 / 700,000 / 2,000,000 / 4,000,000 / 10,000,000.
[0059] Furthermore, the melt index (MI) of polyethylene according to one embodiment of the present invention was measured at a temperature of 190°C and a load of 2.16 kg according to ASTM D 1238 standard. 2.16The concentration is 0.5 to 5.0 g / 10 min. More specifically, it can be 0.5 g / 10min or more, or 0.6 g / 10min or more, or 0.7 g / 10min or more, or 0.8 g / 10min or more, or 0.9 g / 10min or more, or 1.0 g / min or more, or 1.1 g / 10min or more, or 1.2 g / min or more, or 1.3 g / min or more, or 1.4 g / min or more, or 1.5 g / min or more, and below 5.0 g / 10min, or below 4.9 g / 10min, or below 4.8 g / 10min, or below 4.7 g / 10min, or below 4.6 g / 10min, or below 4.5 g / 10min, or below 4.4 g / 10min, or below 4.3 g / 10min, or below 4.2 g / 10min, or below 4.1 g / 10min, or 4.0 g / 10min. Below 3.9 g / 10 min, or below 3.8 g / 10 min, or below 3.7 g / 10 min, or below 3.6 g / 10 min, or below 3.5 g / 10 min, or below 3.4 g / 10 min, or below 3.3 g / 10 min, or below 3.2 g / 10 min, or below 3.1 g / 10 min, or below 3.0 g / 10 min, or below 2.9 g / 10 min, or below 2.8 g / 10 min, or below 2.7 g / 10 min, or below 2.6 g / 10 min, or below 2.5 g / 10 min, or below 2.4 g / 10 min, or below 2.3 g / 10 min, or below 2.2 g / 10 min, or below 2.1 g / 10 min, or below 2.0 g / 10 min, or below 1.9 g / 10 min, or below 1.8 g / 10 min. Below 1.7 g / 10 min, or below 1.6 g / 10 min.
[0060] Thus, by satisfying the conditions of low density and optimized molecular weight distribution range and melt index, in addition to the aforementioned crystallization distribution characteristics and molecular weight distribution characteristics, the polyethylene according to the present invention can exhibit excellent sealing properties and dart impact resistance, as well as improved molding and processing properties and mechanical properties.
[0061] Furthermore, according to one embodiment of the present invention, the polyethylene may be a copolymer of a single type of ethylene and α-olefin, specifically comprising ethylene repeating units and α-olefin repeating units derived from α-olefin monomers.
[0062] The α-olefin monomer may specifically be an α-olefin monomer containing 3 to 20 carbon atoms. Specific examples include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, etc., and more preferably 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, or 1-octene. Preferably, the polyethylene according to one embodiment of the present invention may be a copolymer of a single type of ethylene and 1-hexene, rather than a mixture with other polyethylenes.
[0063] Polyethylene possessing these physical properties can be prepared, for example, by a preparation method comprising the following steps: polymerizing ethylene monomers and α-olefin monomers in the presence of a hybrid supported metallocene catalyst comprising a first transition metal compound represented by Chemical Formula 1 and a second transition metal compound represented by Chemical Formula 2. This preparation method is merely one example of implementing polyethylene according to the invention, and the polyethylene of the invention is not limited to this preparation method.
[0064] [Chemical Formula 1]
[0065] In the above chemical formula 1, M1 is a group 4 transition metal. X 11 and X 12 Each independently is C 1-20 Alkyl or halogen, A1 is carbon, silicon, or germanium. Q 11 and Q 12 Each is independently hydrogen, halogen, C 1-20 Alkyl or C 2-20 Alkoxyalkyl, and R 11 To R 15 Each is independently hydrogen or C 1-20 alkyl, [Chemical Formula 2]
[0066] In the above chemical formula 2, M2 is a group 4 transition metal. X 21 and X 22 Each independently is C 1-20 Alkyl or halogen, R 21 To R 25 Each independently is C 1-20 alkyl, R26 Is it hydrogen or C? 1-20 Alkyl, and R 27 It is hydrogen, C 1-20 Alkyl, C 2-20 Alkoxy or C 2-20 Alkoxyalkyl.
[0067] In this invention, the substituents of the chemical formula can be described more specifically as follows.
[0068] Halogens can be fluorine (F), chlorine (Cl), bromine (Br), or iodine (I).
[0069] C 1-20 Alkyl groups can be straight-chain, branched, or cyclic. Specifically, C 1-20 The alkyl group can be a straight-chain alkyl group having 1 to 20 carbon atoms; a straight-chain alkyl group having 1 to 10 carbon atoms; a straight-chain alkyl group having 1 to 5 carbon atoms; a branched or cyclic alkyl group having 3 to 20 carbon atoms; a branched or cyclic alkyl group having 3 to 15 carbon atoms; or a branched or cyclic alkyl group having 3 to 10 carbon atoms. More specifically, the alkyl group having 1 to 20 carbon atoms can be methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, or cyclohexyl, etc.
[0070] C 2-20 The alkenyl group can be straight-chain, branched, or cyclic. Specifically, C 2-20 The alkenyl group can be a straight-chain alkenyl group containing 2 to 20 carbon atoms, a straight-chain alkenyl group containing 2 to 10 carbon atoms, a straight-chain alkenyl group containing 2 to 5 carbon atoms, a branched alkenyl group containing 3 to 20 carbon atoms, a branched alkenyl group containing 3 to 15 carbon atoms, a branched alkenyl group containing 3 to 10 carbon atoms, a cyclic alkenyl group containing 5 to 20 carbon atoms, or a cyclic alkenyl group containing 5 to 10 carbon atoms. More specifically, C 2-20 The alkenyl group can be vinyl, propenyl, butenyl, pentenyl, or cyclohexenyl, etc.
[0071] C 1-20 Alkoxy groups can be straight-chain, branched, or cyclic. Specifically, C 1-20 The alkoxy group can be a straight-chain alkoxy group having 1 to 20 carbon atoms; a straight-chain alkoxy group having 1 to 10 carbon atoms; a straight-chain alkoxy group having 1 to 5 carbon atoms; a branched or cyclic alkoxy group having 3 to 20 carbon atoms; a branched or cyclic alkoxy group having 3 to 15 carbon atoms; or a branched or cyclic alkoxy group having 3 to 10 carbon atoms. More specifically, the alkoxy group having 1 to 20 carbon atoms can be methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, tert-butoxy, n-pentoxy, isopentoxy, neopentoxy, or cyclohexyloxy, etc.
[0072] C 2-20 Alkoxyalkyl groups may contain -R y -OR z Substituents in the structure, wherein the alkyl group (-R) y One or more hydrogen atoms on the ) are bonded by alkoxy groups (-OR) z The C2 to C20 alkoxyalkyl group can be methoxymethyl, methoxyethyl, ethoxymethyl, isopropoxymethyl, isopropoxyethyl, isopropoxyhexyl, tert-butoxymethyl, tert-butoxyethyl, or tert-butoxyhexyl, etc.
[0073] In addition, Group 4 transition metals can be titanium, zirconium, hafnium, etc.
[0074] The hybrid supported metallocene catalyst used in the production of polyethylene according to the present invention is a hybrid catalyst comprising a first transition metal compound having a high molecular weight and high copolymerization ability and a second transition metal compound having a low molecular weight and low copolymerization ability.
[0075] Specifically, the first transition metal compound represented by Formula 1 facilitates the production of high molecular weight copolymers with high SCB content, while the second transition metal compound represented by Formula 2 facilitates the production of low molecular weight copolymers with low SCB content. Therefore, the hybrid supported metallocene catalyst exhibits high copolymerization ability in the high molecular weight region of polyethylene through the first transition metal compound, and low copolymerization ability in the low molecular weight region of polyethylene through the action of the second transition metal compound. Thus, by using the hybrid supported metallocene catalyst, strong low crystallinity is exhibited in the high molecular weight region of polyethylene, thereby enabling molecule formation and, consequently, readily manufacturing polyethylene that meets the aforementioned physical property requirements.
[0076] Specifically, in the hybrid supported metallocene catalyst, the first transition metal compound represented by Formula 1 facilitates the production of high molecular weight copolymers and exhibits a relatively higher comonomer incorporation rate compared to the second transition metal compound.
[0077] Specifically, in chemical formula 1, M1 can be zirconium (Zr) or titanium (Ti).
[0078] In addition, X 11 and X 12 Each can be a halogen, or more specifically, chlorine.
[0079] Furthermore, in chemical formula 1, Al is silicon, and Q... 11 and Q 12 Each is independently hydrogen, halogen, C 1-20 Alkyl or C2-20 Alkoxyalkyl, condition Q 11 and Q 12 One of them can be C 2-20 The tether group of an alkoxyalkyl group. More specifically, Q 11 and Q 12 Any one of them can be C 2-20 alkoxyalkyl, the other can be C 1-20 alkyl.
[0080] Thus, when Q 11 and Q 12 One of them contains C 2-20 When alkoxyalkyl groups are used as bridging groups connecting two ligands, their atomic size becomes larger, and the available angles are also increased compared to carbon bridges in conventional metallocene compounds, resulting in excellent catalytic activity during polymerization due to their easy access to the monomer. Furthermore, leaching of the catalyst precursor during polymerization is prevented, thereby preventing scaling caused by the reaction of the leached catalyst precursor with the co-catalyst. When Q 11 and Q 12 One of them is -(CH2) n R b (where R) b C 1-6 Alkoxy, more specifically C 1-6 Straight-chain alkoxy or C 3-6 Branched alkoxy groups, or more specifically, C-type alkoxy groups such as tert-butoxy groups. 3-6 Branched alkoxy groups (n is an integer from 2 to 10 or 3 to 9), the other is C. 1-4 This effect can be further enhanced with alkyl groups. More specifically, Q 11 and Q 12 One of them can be tert-butoxyhexyl, and the other can be methyl.
[0081] Furthermore, in chemical formula 1, R 11 To R 14 Each can be independently C 1-10 Alkyl, more specifically C 1-4 Alkyl groups, or more specifically methyl groups. Thus, by using R... 11 To R 14 Replacing the cyclopentadienyl ligand in Formula 1, it exhibits superior catalytic activity due to the inductive effect of providing sufficient electrons.
[0082] Furthermore, in chemical formula 1, R 15 It can be C 1-6 Alkyl, more specifically C 1-4 Straight-chain alkyl or C 3-6Branched alkyl groups, or more specifically tert-butyl groups.
[0083] As specific examples of first transition metal compounds represented by Formula 1, compounds with the following structures may be mentioned, but the invention is not limited thereto.
[0084]
[0085] The first transition metal compound represented by chemical formula 1 can be synthesized by applying known reactions; more detailed synthesis methods can be found in the examples.
[0086] Meanwhile, in the hybrid supported metallocene catalyst, the second transition metal compound represented by Formula 2 has a non-bridged structure, wherein the hydride indene ligand (specifically, the 4,5,6,7-tetrahydro-1-indene ligand) and the cyclopentadiene ligand are not bridged. Therefore, the electronic / space environment around the transition metal can be easily controlled, thereby easily adjusting the chemical structure, molecular weight distribution, and mechanical properties of the synthesized polyethylene.
[0087] Specifically, in Formula 2, M2 can be zirconium (Zr). When a second transition metal compound contains Zr as the central metal, it has more orbitals that accept electrons compared to compounds containing other Group 14 elements (such as Hf), thus enabling it to bind to monomers more readily with higher affinity and thereby exhibit a superior effect in improving catalytic activity.
[0088] In addition, X 21 and X 22 Each can be a halogen on its own; more specifically, it can be chlorine.
[0089] Furthermore, in chemical formula 2, R 21 To R 25 Each can be independently represented as C. 1-10 Alkyl, more specifically C 1-4 Alkyl groups, or more specifically methyl groups. Therefore, by using R... 21 To R 25 The cyclopentadienyl ligand in Formula 2, by replacing it, exhibits superior catalytic activity due to the inductive effect of providing sufficient electrons. Furthermore, by combining it with the first transition metal compound represented by Formula 1, the distribution of the comonomer in the produced polyethylene is appropriately controlled, thereby enabling the easy production of polyethylene that meets the aforementioned physical property requirements.
[0090] Furthermore, since the second transition metal compound contains a hydride indene ligand, specifically 4,5,6,7-tetrahydro-1-indene ligand, it exhibits better hydrogen reactivity compared to compounds containing conventional indene groups. Therefore, during the polymerization process, the amount of hydrogen input and wax formation can be reduced, thereby improving process stability. Moreover, by combining it with the first transition metal compound represented by Formula 1, the distribution of the comonomer in the final polyethylene is concentrated towards the high molecular weight side, thereby significantly improving the impact strength properties of the polyethylene.
[0091] Furthermore, the 1 and 3 positions of the 4,5,6,7-tetrahydro-1-indene ligand can be unsubstituted, or can be substituted by R, respectively. 26 and R 27 Replacement. Specifically, R 26 It is hydrogen or C 1-20 Alkyl, R 27 It can be hydrogen, C 1-20 Alkyl, C 2-20 Alkoxy or C 2-20 Alkoxyalkyl. More specifically, R 26 It is hydrogen or C 1-6 Alkyl, R 27 It can be hydrogen, C 1-6 Alkyl or -(CH2) n -R b alkoxyalkyl (where R b C 1-6 Alkoxy, more specifically C 1-6 Straight-chain alkoxy or C 3-6 Branched alkoxy groups, and n is an integer from 2 to 10). Furthermore, in -(CH2) n -R b In the middle, R b It can be C 3-6 Branched alkoxy groups, more specifically, such as tert-butoxy groups, have a C12-C ... 3-6 Branched alkoxy groups, where n can be an integer from 3 to 9. Even more specifically, R... 26 It can be hydrogen or methyl, R 27 It can be hydrogen, methyl, ethyl or tert-butoxyhexyl.
[0092] As specific examples of second transition metal compounds represented by chemical formula 2, compounds with the following structures may be mentioned, but the present invention is not limited thereto.
[0093] .
[0094] The second transition metal compound represented by chemical formula 2 can be synthesized by applying known reactions; more detailed synthesis methods can be found in the examples.
[0095] Furthermore, by controlling the molar ratio of the first and second transition metal compounds, the hybrid supported metallocene catalyst can improve catalyst activity and more easily achieve the physical properties of the produced polymer.
[0096] For example, the hybrid supported metallocene catalyst may contain first and second transition metal compounds in a molar ratio of 1:1 to 10:1. When the above mixing ratio conditions are met, the catalyst activity remains excellent, and the high and low copolymerization capabilities of polyethylene produced by this hybrid supported catalyst are optimized, thereby further improving sealing properties, dart impact resistance, stiffness, and molding processability. More specifically, the molar ratio of the first and second transition metal compounds may be 2:1 to 8:1, or 2:1 to 5:1.
[0097] In addition, the hybrid supported metallocene catalyst may include a co-catalyst.
[0098] When the hybrid supported metallocene catalyst contains a co-catalyst, it exhibits high catalyst activity and improved process stability.
[0099] Specifically, the co-catalyst may include one or more compounds represented by the following chemical formula 3.
[0100] [Chemical Formula 3] -[Al(R 41 )-O] a - In the above chemical formula 3, R 41 It is a halogen; or a C that is either unsubstituted or halogenated. 1-20 Hydrocarbon group; and a is an integer greater than 2.
[0101] In this specification, a hydrocarbon group refers to a monovalent functional group formed by removing one hydrogen atom from a hydrocarbon, and may include alkyl, alkenyl, alkynyl, aryl, aralkyl, aryl-alkenyl, arylynyl, alkylaryl, alkenylaryl, and alkynylaryl, etc. Furthermore, a hydrocarbon group having 1 to 20 carbon atoms may have 1 to 15 carbon atoms or 1 to 10 carbon atoms. Specifically, a hydrocarbon group having 1 to 20 carbon atoms may be linear, branched, or cyclic alkyl, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, cyclohexyl, etc.; or aryl, such as phenyl, naphthyl, or anthracene, etc.
[0102] Examples of compounds represented by Formula 3 include alkylaluminoxane-based compounds, such as methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, or butylaluminoxane, any one or a mixture of two or more of these may be used. In these compounds, the co-catalyst may more specifically be methylaluminoxane.
[0103] The alkylaluminoxane-based cocatalyst stabilizes the first and second transition metal compounds by acting as a Lewis acid, and further enhances the catalyst activity by including a metal element that can form a bond with the functional group introduced into the bridging group of the first transition metal compound through Lewis acid-base interactions.
[0104] Furthermore, the amount of co-catalyst can be appropriately adjusted according to the desired catalyst and the physical properties or effects of polyethylene. For example, when silica is used as a support as described below, the loading of co-catalyst can be more than 100g, or more than 1000g, or more than 2000g, and less than 6000g, or less than 5500g, or less than 5400g, based on the weight of the support per 1000g of silica.
[0105] Furthermore, the hybrid supported metallocene catalyst may include a support. When the hybrid supported metallocene catalyst includes a support, the first and second transition metal compounds are used in the form of a supported catalyst on the support.
[0106] As a support, a support with highly active hydroxyl, silanol, or siloxane groups on its surface can be used. For this purpose, a support that has been surface-modified by calcination or a support from which moisture has been removed by drying can be used. For example, silica prepared by calcining silica gel, or silica (e.g., silica dried at high temperature), silica-alumina, and silica-magnesium oxide can be used, and these supports typically contain oxide, carbonate, sulfate, and nitrate components, such as Na2O, K2CO3, BaSO4, and Mg(NO3)2.
[0107] When used as a supported catalyst, the produced polymer exhibits excellent particle shape and bulk density, and it is suitable for conventional slurry polymerization, bulk polymerization, and gas-phase polymerization processes. Furthermore, among various supports, in the case of silica supports, due to the chemical bonding and support of the functional groups of transition metal compounds, almost no catalyst detachment from the support surface occurs during ethylene polymerization. Therefore, when producing polyethylene via slurry polymerization or gas-phase polymerization, scaling caused by reactor walls or polymer particles adhering together can be minimized.
[0108] The support can be a support with an average particle size (D50) of 20 to 40 μm. When the particle size is as described above, transition metal compounds can be loaded with better efficiency, thereby improving catalyst activity. More specifically, the average particle size of the support can be greater than 20 μm, or greater than 25 μm and less than 40 μm, or less than 30 μm.
[0109] In this invention, the average particle size (D50) of the carrier refers to the particle size at the 50% point of the cumulative distribution based on the number of particles of that size (particle diameter). D50 can be measured using laser diffraction. Specifically, the carrier to be measured is dispersed in a dispersion medium such as deionized water and then introduced into a commercially available laser diffraction particle size analyzer (e.g., Microtrac S3500). The diffraction pattern of the particles as they pass through the laser beam is measured to change with particle size, thereby calculating the particle size distribution. The particle size at the 50% point of the cumulative distribution based on particle size is calculated and used as the average particle size.
[0110] Furthermore, when loaded onto a support, the loading amounts of the first and second transition metal compounds can be, for example, based on 1000 g of silica support, 1 mmol or more, or 1.5 mmol or more, or 2 mmol or more, and less than 100 mmol, or less than 50 mmol, or less than 30 mmol, or less than 10 mmol, or less than 5 mmol. When loaded within the above-mentioned content ranges, it can exhibit appropriate supported catalyst activity, offering advantages in maintaining catalyst activity and economic efficiency.
[0111] The hybrid supported metallocene catalyst with the above configuration can be prepared by a method including the following steps: loading a cocatalyst compound on a support, and loading first and second transition metal compounds on a support. The loading order of the cocatalyst compound and the first and second transition metal compounds can be changed as needed, and the loading order of the first and second transition metal compounds can also be changed as needed. The first and second transition metal compounds can be loaded simultaneously. Considering the influence of the supported catalyst structure determined by the loading order, loading the cocatalyst compound on the support followed by the sequential loading of the first and second transition metal compounds allows the prepared supported catalyst to achieve high catalytic activity and better process stability in polyethylene production.
[0112] Furthermore, in the polymerization reaction, specific examples of α-olefin monomers, as described above, include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, etc., and two or more of these may be used. More specifically, the α-olefin monomer may be 1-hexene.
[0113] The amount of α-olefin monomer added can be determined according to the physical properties of the polyethylene to be produced. For example, considering the physical properties of the polyethylene to be achieved by the present invention, the amount of α-olefin monomer added can be 4 to 30 wt%, more specifically, 4 wt% or more, or 8 wt% or more, or 10 wt% or more, or 12 wt% or more, and less than 30 wt%, or less than 25 wt%, or less than 20 wt%.
[0114] Furthermore, the polymerization reaction is carried out under conditions where hydrogen is introduced.
[0115] Specifically, based on the total weight of the monomers, including ethylene monomers and α-olefin monomers, the amount of hydrogen added can be from 10 to 50 ppm, more specifically, above 10 ppm, or above 15 ppm, or above 20 ppm, or above 25 ppm, and below 50 ppm, or below 45 ppm, or below 40 ppm, or below 38 ppm, or below 35 ppm. When added within the above ranges, it is easier to achieve the aforementioned physical properties of polyethylene. If the polymerization reaction is carried out under conditions without hydrogen input, the melt index (MI) of the produced polyethylene may be significantly reduced.
[0116] In addition, polymerization can be carried out as slurry polymerization.
[0117] In solution polymerization, the catalyst is activated by a high-temperature, high-pressure reaction, which promotes catalyst decomposition and chain transfer, resulting in a resin composition with a narrow molecular weight distribution and low high molecular weight tail content. Consequently, when using resin compositions produced by solution polymerization to manufacture films, they exhibit poor processability. However, in the slurry polymerization process of the present invention, because polymerization is carried out at a relatively low temperature, a molecular structure with a wide molecular weight distribution (MWD) and a large number of high molecular weight tail chains can be ensured, which is exactly what is needed for polyethylene resin compositions used to produce transparent films. Therefore, excellent processability can be exhibited.
[0118] The slurry polymerization reaction can be carried out using a continuous slurry polymerization reactor or a loop slurry reactor.
[0119] Furthermore, during the slurry polymerization reaction, a hybrid supported catalyst can be injected by dissolving or diluting the hybrid supported catalyst in an aliphatic hydrocarbon solvent having 4 to 12 carbon atoms (e.g., isobutane, pentane, hexane, heptane, nonane, decane, and their isomers), an aromatic hydrocarbon solvent (e.g., toluene and benzene), or a hydrocarbon solvent with chlorine atoms substituted (e.g., dichloromethane and chlorobenzene). Preferably, a solvent in which a small amount of alkylaluminum has been treated to remove trace amounts of water or air as catalyst poisons is used, and this can also be achieved through further treatment with a co-catalyst.
[0120] Furthermore, the polymerization reaction can be carried out at temperatures above 40°C, or above 60°C, or above 80°C and below 110°C, or below 100°C, or below 90°C. Moreover, if the pressure conditions during the polymerization process are further controlled, it can be carried out at pressures above 5 bar, or above 10 bar, or above 20 bar, or above 30 bar and below 50 bar, or below 45 bar, or below 40 bar. When the polymerization reaction is carried out at such temperatures and pressures, the desired physical properties of polyethylene can be achieved more easily.
[0121] The polyethylene produced by the above preparation method possesses the aforementioned crystallinity distribution characteristics, molecular weight distribution characteristics, rheological properties, and processing properties. Therefore, this polyethylene exhibits excellent low-temperature sealing properties and hot-tack characteristics, as well as excellent dart impact resistance and stiffness, while also possessing a good balance and improved molding processability. Thus, thinner films can be produced using this polyethylene, and it is advantageous for D4R applications. Furthermore, this polyethylene can be usefully used in films for various applications, such as food films, agricultural films, general industrial films, or stretch films, and is particularly suitable for use as a sealing layer in all-polyethylene (All-PE) films.
[0122] Therefore, the present invention provides a resin composition comprising the polyethylene, and more particularly, a composition for forming a film.
[0123] Furthermore, the present invention also provides a membrane produced using the polyethylene or the resin composition.
[0124] In addition to using the polyethylene described above, the membrane can be produced using conventional membrane production methods. For example, the membrane can be produced according to the expansion process, in which a film composition is prepared by containing only the polyethylene described above, or by optionally mixing additives such as antioxidants and processing aids, and then extruded into a film shape using an extruder.
[0125] More specifically, the resin composition containing the polyethylene can be used as a sealing layer and co-extruded with a composition for forming another film layer, or extruded using a blown film extruder or a cast film extruder, or the film can be prepared separately using the resin composition containing the polyethylene on a substrate such as paper via extrusion coating, and then the prepared film can be laminated with another film. However, the invention is not limited thereto, and it can be produced into various films by applying any known production method.
[0126] Because the membrane contains the polyethylene, it exhibits excellent low-temperature sealing properties, sealing stability, and process reliability.
[0127] Specifically, when the membrane is a single-layer membrane with a thickness of 45 to 55 μm, or 48 to 52 μm, more specifically 50 μm, its seal initiation temperature (SIT) as measured according to ASTM F 1921 is below 80.0 °C. The seal initiation temperature is below 80.0 °C, or below 79.5 °C, or below 79.0 °C, or below 78.5 °C, or below 78.0 °C, or below 77.5 °C, or below 77.0 °C, or below 76.5 °C, or below 76.0 °C, or below 75.5 °C, or below 75.0 °C, or below 74.5 °C, or below 74.0 °C. Since the lower the initial sealing temperature, the better the low-temperature sealing properties and sealing strength, there is no particular restriction on its lower limit. For example, it can be above 60.0℃, or above 61.0℃, or above 62.0℃, or above 63.0℃, or above 64.0℃, or above 65.0℃, or above 66.0℃, or above 67.0℃, or above 68.0℃, or above 69.0℃, or above 70.0℃, or above 71.0℃, or above 72.0℃, or above 73.0℃.
[0128] For reference, the sealing onset temperature refers to the temperature at which the heat seal strength reaches 2 N / 25.4 mm when the membrane is a single-layer membrane with a thickness of 45 to 55 μm, or 48 to 52 μm, more specifically 50 μm, as measured according to ASTM F 1921 (sealing time 0.5 seconds, sealing pressure 0.3 MPa, delay time 30.0 seconds, tensile speed 200 mm / s, J&B 5000).
[0129] In addition to exhibiting the aforementioned sealing properties, the polyethylene film also exhibits improved dart impact resistance.
[0130] Specifically, when the membrane is a single-layer membrane with a thickness of 45 to 55 μm, or 48 to 52 μm, more specifically 50 μm, the dart impact resistance measured according to ASTM D 1709 [Method A] is greater than 1,200 gf, or greater than 1,250 gf, or greater than 1,300 gf, or greater than 1,350 gf. Since the higher the impact resistance of the dart, the better, there is no particular limit to the upper limit. For example, it can be below 3,000gf, or below 2,900gf, or below 2,800gf, or below 2,700gf, or below 2,600gf, or below 2,500gf, or below 2,400gf, or below 2,300gf, or below 2,200gf, or below 2,100gf, or below 2,000gf, or below 1,900gf, or below 1,800gf, or below 1,700gf.
[0131] Furthermore, when the membrane is a single-layer membrane with a thickness of 45 to 55 μm, or 48 to 52 μm, more specifically 50 μm, the 1% secant modulus of the membrane in the MD direction, measured using a Universal Testing Machine (UTM) according to ASTM D 882, is 1,500 kg / cm². 2 Above, or 1,600 kg / cm 2 Above, or 1,700 kg / cm 2 Above, or 1,800 kg / cm 2 The above; the 1% secant modulus in the TD direction is 1,800 kg / cm². 2 Above, or 1,900 kg / cm 2 Above, or 2,000 kg / cm 2 Above, or 2,100 kg / cm 2 above.
[0132] The secant modulus, as defined in ASTM D 882, represents the stiffness of the film. The secant modulus is density-dependent; higher density generally results in higher secant modulus and stiffness. Furthermore, a higher secant modulus leads to better openability, gloss, and coefficient of friction (COF). Therefore, there is no specific upper limit to the secant modulus; however, for example, 1% secant modulus in the MD and TD directions of the film can be 3,000 kg / cm². 2 Below, or 2,900 kg / cm 2 Below, or 2,800 kg / cm 2 Below, or 2,700 kg / cm 2 Below, or 2,600 kg / cm 2 Below, or 2,500 kg / cm 2 Below, or 2,400 kg / cm 2 the following.
[0133] For reference, the sealing initiation temperature, dart impact resistance, and secant modulus were measured on films formed by producing monolayer films of thickness 45 to 55 μm, or 48 to 52 μm, more specifically 50 μm, from a composition comprising 95 wt%, 96 wt%, 97 wt%, 98 wt%, 99 wt%, or 99.9 wt% or more of the polyethylene of the present invention based on the total composition.
[0134] The following preferred embodiments are provided to aid in understanding the present invention. However, the following embodiments are provided only to aid in understanding the present invention, and the scope of the present invention is not limited thereto.
[0135] In this instruction manual, room temperature refers to 23±2℃.
[0136] <Preparation of Transition Metal Compounds> Synthesis example 1
[0137] Preparation of ligands TMCp (tetramethylcyclopentadiene, 1 equivalent) was dissolved in THF (0.3 M), and n-BuLi (1.05 equivalent) was slowly added dropwise at -25 °C, followed by stirring at room temperature for 3 hours. t-BuOHexSiMeCl2 (1.00 equivalent) was added to the resulting reaction mixture at -10 °C, followed by stirring at room temperature overnight. The solvent was completely removed by vacuum drying, and tBuNH2 (10 equivalent) was added, followed by stirring at room temperature overnight. Afterwards, post-treatment with water was performed, followed by drying to obtain the ligand.
[0138] Preparation of transition metal compounds The ligand prepared above was dissolved in toluene (0.3 M), and n-BuLi (2.05 equivalents) was added at -25 °C, followed by stirring at room temperature for 3 hours. In a glove box, TiCl4(THF)2 (titanium tetrachloride tetrahydrofuran adduct, 1 equivalent) was prepared in another flask and added using a sleeve to the ligand-lithium flask at -25 °C, after washing with toluene (1.0 M) and adding.
[0139] After the reaction was complete, the solvent was removed by vacuum drying, DCM was added, LiCl was removed by filtration, and the filtrate was dried under vacuum to obtain a liquid transition metal compound (Cat 1).
[0140] 1 H NMR (500 MHz, CDCl3) δ 3.34 (t, 2H), 2.24 (d, J = 1.7 Hz, 6H), 2.13 (d, J = 3.2 Hz, 6H), 1.57 - 1.45 (m, 6H), 1.42 (s, 9H), 1.32 - 1.22 (m,4H), 1.18 (s, 9H), 0.67 (s, 3H).
[0141] Synthesis example 2-1 (Cat 2-1) Indene (1 equivalent) was dissolved in THF (0.3 M), and n-BuLi (1.05 equivalent) was slowly added dropwise at -25 °C, followed by stirring at room temperature for 3 hours. Then, CH3-I (1.05 equivalent) was added at -10 °C, and the mixture was stirred overnight at room temperature. After post-treatment with water and drying, 3-methylindene was obtained. The synthesized 3-methylindene (1 equivalent) was dissolved in THF (0.3 M), and n-BuLi (1.05 equivalent) was slowly added dropwise at -25 °C, followed by stirring at room temperature for 3 hours. Then, CH3-I (1.05 equivalent) was added at -10 °C, and the mixture was stirred overnight at room temperature. After post-treatment with water and drying, 1,3-dimethylindene was obtained.
[0142] Preparation of transition metal compounds The ligand prepared above was dissolved in diethyl ether (0.3 M), and n-BuLi (1.05 equivalents) was added at -25 °C, followed by stirring at room temperature for 3 hours. In a glove box, PMCpZrCl3 (pentamethylcyclopentadienyl zirconium trichloride) (1 equivalent) was prepared in another flask and added through a sleeve to the ligand-lithium flask at -25 °C, after washing with diethyl ether (1.0 M) and adding.
[0143] After the reaction was complete, the solvent was removed by vacuum drying, then DCM was added, and LiCl was removed by filtration. The filtrate was then dried under vacuum and slurryed with hexane. The resulting solid was then filtered and dried under vacuum to obtain a solid metallocene intermediate.
[0144] In a glove box, the metallocene intermediate was placed in a mini Parr reactor, and 5 mol% Pd / C (10 wt%) was added. A magnetic stir bar was added, and the reactor was removed from the glove box as a closed system. DCM (0.5 M) was added to the Parr reactor, and hydrogen gas (10 barg) was introduced. The venting-charge process was repeated three times, and then the reactor was placed in a 40°C oil bath with stirring. When the pressure inside the Parr reactor dropped to less than 5 barg, the venting process was repeated, and the reaction continued until no more hydrogen was consumed. After the reaction was complete, the remaining hydrogen was vented and replaced with argon. After cooling to room temperature, the filtrate was filtered through a sleeve and dried under vacuum. The dried filtrate was slurried with hexane and then filtered to obtain a solid transition metal compound (Cat 2-1).
[0145] 1H NMR (500 MHz, CDCl3) δ 5.60 (s, 1H), 2.90 (dt, J = 16.4, 6.3 Hz, 2H), 2.32 (dt, J = 16.3, 6.0 Hz, 2H), 2.04 (s, 15H), 1.79 - 1.66 (m, 2H), 1.67 (s, 6H), 1.64 - 1.54 (m, 2H).
[0146] Synthesis example 2-2 (Cat 2-2) Preparation of ligands Indene (1 equivalent) was dissolved in THF (0.3 M), and n-BuLi (1.05 equivalent) was slowly added dropwise at -25 °C, followed by stirring at room temperature for 3 hours. Then, CH3-CH2-I (1.05 equivalent) was added at -10 °C, followed by stirring at room temperature overnight, post-treatment with water, and drying to obtain 3-ethylindene.
[0147] Preparation of transition metal compounds The ligand prepared above was dissolved in diethyl ether (0.3 M), and n-BuLi (1.05 equivalents) was added at -25 °C, followed by stirring at room temperature for 3 hours. In a glove box, PMCpZrCl3 (pentamethylcyclopentadienyl zirconium trichloride) (1 equivalent) was prepared in another flask and added through a sleeve to the ligand-lithium flask at -25 °C, followed by washing with diethyl ether (1.0 M) and adding.
[0148] After the reaction was complete, the solvent was removed by vacuum drying, then DCM was added, and LiCl was removed by filtration. The filtrate was then dried under vacuum and slurryed with hexane. The resulting solid was then filtered and dried under vacuum to obtain a solid metallocene intermediate.
[0149] In a glove box, the metallocene intermediate was placed in a mini Palermo reactor, and 5 mol% Pd / C (10 wt%) was added. A magnetic stir bar was added, and the reactor was removed from the glove box as a closed system. DCM (0.5 M) was added to the Palermo reactor, and hydrogen gas (10 barg) was introduced. The purging-purging process was repeated three times, and then the reactor was placed in a 40°C oil bath with stirring. When the pressure inside the Palermo reactor dropped to less than 5 barg, the previous purging process was repeated, and the reaction continued until no more hydrogen was consumed. After the reaction was complete, the remaining hydrogen gas was purged and replaced with argon gas. After cooling to room temperature, the filtrate was filtered through a sleeve and dried under vacuum. The dried filtrate was slurried with hexane and then filtered to obtain a solid transition metal compound (Cat 2-2).
[0150] 1H NMR (500 MHz, CDCl3) δ 5.60 (d, J = 2.7 Hz, 2H), 5.20 (d, J = 2.7Hz, 2H), 2.83 - 2.71 (m, 2H), 2.49 - 2.36 (m, 3H), 2.21 (dd, J = 15.1, 7.6Hz, 1H), 2.01 (s, 15H), 1.98 - 1.80 (m, 2H), 1.66 - 1.51 (m, 2H), 1.03 (t, J= 7.6 Hz, 3H).
[0151] <Catalyst Preparation> Preparation Example 1 In a 20L stainless steel (SUS) high-pressure reactor, 2.0 kg of toluene and 1000 g of silica (SP2410, purchased from Grace Davision) were added, and the reactor was heated to 40°C while stirring. Then, 5.4 kg of methylaluminoxane (10 wt% toluene solution, purchased from Albemarle) was added, and the mixture was heated to 70°C and stirred at approximately 200 rpm for about 12 hours. Afterward, the reactor temperature was lowered to 40°C and stirring was stopped. The reaction product was then allowed to stand for about 10 minutes, followed by decantation. Another 2.0 kg of toluene was added to the reaction product, and the mixture was stirred for about 10 minutes. Stirring was then stopped, and the mixture was allowed to stand for about 30 minutes, followed by decantation.
[0152] 2.0 kg of toluene was added to the reactor, followed by the compound (Cat 1) (15 mmol) prepared in Synthesis Example 1 as the first transition metal compound, the compound (Cat 2-1) (10 mmol) prepared in Synthesis Example 2-1 as the second transition metal compound, and 1000 mL of toluene. The reactor temperature was raised to 85 °C and stirred for about 90 minutes.
[0153] Subsequently, the reactor temperature was lowered to room temperature, stirring was stopped, and the reaction product was allowed to stand for about 30 minutes before being decanted. Next, 3 kg of hexane was added to the reactor, and the hexane slurry was transferred to a 20 L filter dryer for filtration. The solution was then dried under reduced pressure at 50 °C for about 4 hours to obtain 1.5 kg of mixed metallocene catalyst.
[0154] (Cat 1) (Cat 2-1) Preparation Examples 2 to 3 Except for changing the types of the first and second transition metal compounds as described in Table 1 below, the hybrid supported metallocene catalyst was prepared in the same manner as in Preparation Example 1.
[0155] Table 1
[0156] <Preparation of Polyethylene> Examples 1-1 to 3-1 A 140L continuous polymerization reactor capable of performing an isobutylene slurry circulation process and operating at a reaction flow rate of approximately 7 m / s was prepared. The reactants required for polyethylene polymerization were then continuously added to the reactor as described in Table 2. The catalyst used in each polymerization reaction was the catalyst prepared in the preparation example described in Table 1, and was added by mixing the catalyst into the isobutylene slurry. The polymerization reactions were carried out at a pressure of approximately 40 bar and a temperature of approximately 85°C; other key polymerization reaction conditions are shown in Table 2 below.
[0157] Comparative Example 1-1 The ethylene-1-hexene copolymer HP1018 from LG Chem was used.
[0158] Comparative Example 2-1 The ethylene and 1-hexene copolymer EP2010 from LG Chem was used.
[0159] Comparative Example 3-1 The ethylene-1-octene copolymer LF100A from LG Chem was used.
[0160] Table 2
[0161] In Table 2, the activity (kg PE / kg SiO2·hr) is calculated as follows: based on the ratio of the weight of polymer produced per unit time (hour) (kg PE) to the weight of catalyst used (kg).
[0162] In addition, the 1-hexene feed rate (wt%) is calculated as a percentage of the 1-hexene feed relative to the total weight of monomers including ethylene and 1-hexene, and the hydrogen feed rate (ppm) is based on the total weight of monomers including ethylene and 1-hexene.
[0163] <Membrane Preparation> Films were prepared using the polyethylene prepared in the examples and comparative examples using the following methods.
[0164] Examples 1-2 to 3-2, Comparative Examples 1-2 to 3-2 Based on the total weight of polyethylene prepared in the above examples or comparative examples, 1200 ppm of antioxidant (Songnox 1076 (Songwon) : Songnox 1680 (Songwon) = 1:2 by weight) was added and mixed. The mixture was then extruded using a twin-screw extruder (TEK 30 MHS, purchased from SMPLATECH, diameter 32phi, L / D=40) at an extrusion temperature of 190°C and an extrusion rate of 35 kg / h to prepare approximately 18 kg of granular film-forming composition.
[0165] A film is prepared by expanding the film-forming composition prepared above under the following film extrusion conditions.
[0166] <Film formation conditions> Single-screw extruder (Yoojin Engineering's single-screw extruder, blown film machine (Blown FilmM / C), 50phi, L / D=32) Melt temperature (or extrusion temperature): 185℃ Die head clearance: 2.0mm Die head diameter: 120mm Inflation ratio: 2.5 The height of the frost line should be maintained at 200~250mm. Sample extrusion rate: 300~500 g / min Cooling: Dual air rings are used Film thickness: 50μm.
[0167] Experimental Example 1 The physical properties of the polyethylene prepared in the above examples and comparative examples were measured as follows, and the results are shown in Tables 3 and 5 below.
[0168] (1) Melt index (MI) 2.16 ): Measured according to ASTM D1238 (Condition E, 190°C, 2.16 kg load).
[0169] (2) Density: Measured according to ASTM D1505 standard.
[0170] (3) Molecular weight distribution (MWD) For the polyethylene according to the examples and comparative examples, the weight-average molecular weight (Mw, g / mol) and number-average molecular weight (Mn, g / mol) were measured by gel permeation chromatography (GPC), and the molecular weight distribution (MWD, Mw / Mn) was obtained by dividing the weight-average molecular weight measured above by the number-average molecular weight.
[0171] Specifically, PolymerChar GPC-IR is used. ®The instrument was a gel permeation chromatography (GPC) system, using a Polymer Laboratories PLgel MIX-B 300 mm column. The measurement temperature was 160 °C, 1,2,4-trichlorobenzene was used as the solvent, and the flow rate was 1 mL / min. Each polyethylene sample prepared in the examples and comparative examples was analyzed using a PolymerChar GPC-IR analyzer. ® Pretreatment was performed by dissolving 1,2,4-trichlorobenzene containing 0.03% BHT at 160°C for 2 hours, followed by preparation at a concentration of 16 mg / 8 mL, and injection at a volume of 200 μL. The values of Mw and Mn were calculated using a calibration curve formed from polystyrene standard samples. Nine polystyrene standard samples with weight-average molecular weights of 2000 g / mol, 10000 g / mol, 30000 g / mol, 70000 g / mol, 200000 g / mol, 700000 g / mol, 2000000 g / mol, 4000000 g / mol, and 10000000 g / mol were used.
[0172] (4) Analysis of crystallization distribution and molecular weight distribution Cross-fractional chromatography (CFC) analysis was performed on the polyethylene prepared in the examples and comparative examples using the following method.
[0173] [Cross-grading chromatographic measurement conditions (including TREF and GPC analysis)] - Analysis equipment: Polymer Char CFC-7890B (G3440D) (Detector: Integrated detector IR5 MCT) - Sample preparation and injection: Place 32 mg of polyethylene prepared in the examples or comparative examples into a 10 mL sample vial, insert it into an autosampler, add 8 mL of 1,2,4-trichlorobenzene (TCB), dissolve at 160 °C for 90 min, and then stabilize at 140 °C for 20 min. After purging with nitrogen, extract and load the sample into a temperature elution fractionation column (TREF column).
[0174] - Crystallization: Set the temperature of the sample previously loaded into the TREF column to 140°C, then cool it from 140°C to 35°C at a rate of 0.5°C / min and hold for 15 minutes.
[0175] The detailed conditions for stabilization and crystallization are as follows:
[0176] - Temperature Rising Elution Fractionation (TREF) analysis: Heat the previously crystallized sample from 30°C to 120°C at a rate of 1°C / min until the specified fractionation temperature is reached, then hold this temperature for 5 minutes while measuring the concentration of the fraction eluted at this temperature. A TREF analysis plot is drawn based on these concentration measurements.
[0177] From the TREF plot, based on the total weight of all eluted fractions, the content ratio of the polymer fraction eluted in the region where the elution temperature is below 35°C (Te≤35°C), the content ratio of the polymer fraction eluted in the region where the elution temperature is above 30°C and less than 60°C (30°C≤Te<60°C), the content ratio of the polymer fraction eluted in the region where the elution temperature is above 60°C and less than 80°C (60°C≤Te<80°C), and the content ratio (wt%) of the polymer fraction eluted in the region where the elution temperature is above 80°C (80°C≤Te) are calculated respectively.
[0178] <Fractionation temperature> 30°C / 35°C / 40°C / 43°C / 46°C / 49°C / 52°C / 55°C / 58°C / 61°C / 64°C / 67°C / 70°C / 73°C / 76°C / 79°C / 82°C / 85°C / 88°C / 91°C / 94°C / 97°C / 100°C / 105°C / 120°C <Measurement conditions>
[0179] - GPC analysis: Transfer the fractions eluted in each temperature range from the previous TREF analysis to the GPC chromatographic column equipped in the GPC apparatus (PolymerChar GPC-IR ® ), and then perform GPC analysis under the following conditions.
[0180] <Sample preparation> The polyethylene fraction is pretreated by dissolving it in 1,2,4-trichlorobenzene at 160°C for 10 hours to prepare a concentration of 10mg / 10mL, and then injected in an amount of 200μL.
[0181] <GPC analysis conditions> GPC apparatus: PolymerChar GPC-IR ® GPC chromatographic column: Polymer Laboratories PLgel MIX-B 300mm long chromatographic column Measurement temperature: 160°C Solvent: 1,2,4-trichlorobenzene Flow rate: 1mL / min Standard sample: Polystyrene standard sample (Weight-average molecular weights of polystyrene standard samples: nine types, 2000 g / mol, 10000 g / mol, 30000 g / mol, 70000 g / mol, 200000 g / mol, 700000 g / mol, 2000000 g / mol, 4000000 g / mol, 10000000 g / mol) <Measurement Conditions>
[0182] Experiment Example 2 The physical properties of the membranes prepared in the following examples and comparative examples were measured, and the results are shown in Tables 4 and 6 below.
[0183] (1) Impact resistance of darts For the membranes of the above-prepared examples and comparative examples, the dart impact resistance was measured according to ASTM D1709 [Method A] standard. Each membrane sample was measured in 5 groups (20 times / group) or more, and the average value was taken.
[0184] (2) Sealing start temperature (SIT) According to ASTM F 1921 standard, using a J&B hot tack tester (Hot tacker 5000), the seal strength was measured at 5°C intervals between 60°C and 130°C under the following conditions: sealing time of 0.5 seconds, sealing pressure of 0.3 MPa, delay time of 30.0 seconds, and tensile speed of 200 mm / s. The temperature at which the heat seal strength reaches 2 N / 25.4 mm was taken as the seal initiation temperature (SIT).
[0185] In the unit N / 25.4mm, "25.4mm" is the width of the membrane sample being measured in the sealing test.
[0186] (3) Thermal bonding window range According to ASTM F 1921, using a J&B hot tack tester (Hot Tacker 5000), the seal strength was measured at 5°C intervals between 60°C and 145°C under the following conditions: sealing time of 0.5 seconds, sealing pressure of 0.3 MPa, delay time of 0.1 seconds, and tensile speed of 200 mm / s. The temperature at which the seal strength (heat seal strength) first reached 3 N / 25.4 mm was measured (HT-SIT). 3N The initial temperature of the heat-sealed seal (unit: °C) and the temperature at which the seal strength of 3 N / 25.4 mm was finally achieved (HTHT). 3NHigh temperature hot-sticking temperature (unit: °C), and the temperature difference (HTHT) 3N – HT-SIT 3N The range is calculated as the first thermal adhesion window.
[0187] Under the same sealing conditions, the temperature at which the first 2 N / 25.4 mm seal strength (heat seal strength) is achieved is measured (HT-SIT). 2N The initial temperature of the heat-melt seal (unit: °C) and the temperature at which the final seal strength of 2 N / 25.4 mm was achieved (HTHT). 2N High-temperature hot melt temperature (unit: °C), and the temperature difference (HTHT) 2N – HT-SIT 2N The range is calculated as the second thermal adhesion window.
[0188] In the unit N / 25.4 mm, "25.4 mm" indicates the width of the membrane sample being measured in a sealed manner.
[0189] Figure 1 The first and second thermal bonding window ranges in the embodiments are shown in the figure.
[0190] also, Figure 2 The first and second thermal adhesion window ranges are shown in the comparative example.
[0191] (4) Secant modulus For the membranes of the examples and comparative examples, the 1% secant modulus in the machine direction (MD) and transverse direction (TD) of the membrane was measured using an Instron UTM (General Purpose Testing Machine) in accordance with ASTM D 882.
[0192] Table 3
[0193] Table 4
[0194] Table 5
[0195] Table 6
[0196] ( In comparative examples 2-2 and 3-2, due to HT-SIT 3N and HTHT 3N (The temperature could not be measured, therefore the temperature is not listed.) See Tables 3 to 6 and Figures 1 to 2The polyethylene of Examples 1 to 3 of the present invention has a wide first hot-tack window range of 29.5°C, 16.5°C, and 21°C, and a wide second hot-tack window range of 47°C, 44.5°C, and 44.5°C, respectively. This means that for the polyethylene of the present invention, the temperature range in which its hot-tack strength remains above a certain level is wide, thus it can exhibit consistent adhesive performance, unaffected by uneven sealing strip temperature, changes in production speed, or local variations in film thickness and composition, thereby achieving stable sealing over a wide temperature range.
[0197] In contrast, the first heat-sealing window range of Comparative Example 1, which is conventional polyethylene, is 4°C, which is very narrow; Comparative Examples 2 and 3 cannot maintain a seal at a sealing strength of 3 N / 25.4 mm. The second heat-sealing window ranges of Comparative Examples 1 to 3 are 37.5°C, 14.5°C, and 37.5°C, respectively, which are also narrower than those of the examples, confirming their low sealing stability.
[0198] Furthermore, the HT-SIT of the polyethylene in Examples 1 to 3 can be determined. 2N The temperature is low, and compared to Comparative Examples 1 to 3, the curve of its hot tack strength as a function of temperature shifts to the left (low temperature). Therefore, compared to conventional polyethylene, it can reduce energy consumption due to its excellent low-temperature sealing properties.
Claims
1. A type of polyethylene, wherein, When measuring seal strength while varying the temperature according to ASTM F 1921, the first hot-tight window range is 15 to 35°C. This first hot-tight window range refers to the temperature at which a seal strength of 3 N / 25.4 mm (heat seal strength) is first achieved (HT-SIT). 3N The initial temperature of the heat-sealed seal (unit: °C) and the temperature at which the seal strength of 3 N / 25.4 mm was finally achieved (HTHT) 3N The temperature difference between the high-temperature hot-sticking temperature (unit: °C) and the high-temperature hot-sticking temperature (HTHT) 3N – HT-SIT 3N ).
2. The polyethylene according to claim 1, in, HT-SIT 3N It is below 94℃.
3. The polyethylene according to claim 1, in, When measuring seal strength while varying the temperature according to ASTM F 1921, the second hot-tight window range is 40 to 55°C. This second hot-tight window range refers to the temperature at which the seal strength (heat seal strength) of 2 N / 25.4 mm is first achieved (HT-SIT). 2N The initial temperature of the heat-sealed seal (unit: °C) and the temperature at which the seal strength of 2 N / 25.4 mm was finally achieved (HTHT) 2N The temperature difference between the high-temperature hot-sticking temperature (unit: °C) and the high-temperature hot-sticking temperature (HTHT) 2N – HT-SIT 2N ).
4. The polyethylene according to claim 3, in, HT-SIT 2N The temperature is below 85℃.
5. The polyethylene according to claim 1, in, In the temperature elution fractionation process of cross-fractional chromatography, based on the total weight of polyethylene, the content of the polymer fraction eluted at an elution temperature above 30°C and below 60°C meets the requirement of 18.0 to 38.0 wt%.
6. The polyethylene according to claim 1, in, in, In the temperature-elution fractionation process of cross-fractional chromatography, based on the total weight of polyethylene, the content of polymer fractions eluted at elution temperatures below 35°C meets the requirement of 5.0 to 30.0 wt%.
7. The polyethylene according to claim 1, in, In the temperature elution fractionation process of cross-fractional chromatography, based on the total weight of polyethylene, the content of the polymer fraction eluted at an elution temperature above 60°C and below 80°C is satisfied to be 20.0 to 50.0 wt%.
8. The polyethylene according to claim 1, in, In the temperature elution fractionation process of cross-fractional chromatography, based on the total weight of polyethylene, the content of the polymer fraction eluted at an elution temperature above 80°C is 30.0 to 60.0 wt%.
9. The polyethylene according to claim 1, in, The density, measured according to ASTM D1505, is 0.900 to 0.925 g / cm³. 3 .
10. The polyethylene according to claim 1, in, The molecular weight distribution (MWD) ranges from 2.0 to 5.
0.
11. The polyethylene according to claim 1, in, The polyethylene, measured according to ASTM D1238 at a temperature of 190°C and a load of 2.16 kg, has a melt index of 0.5 to 5.0 g / 10 min.
12. The polyethylene according to claim 1, in, The polyethylene is a copolymer of a single type of ethylene and α-olefin.
13. The polyethylene according to claim 12, in, The α-olefin is 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, or 1-octene.
14. A membrane comprising the polyethylene according to claim 1.
15. The membrane according to claim 14, in, When the film thickness is 45 to 55 μm, the seal initiation temperature (SIT) measured according to ASTM F 1921 is below 80°C.
16. The membrane according to claim 14, in, When the film thickness is 45 to 55 μm, the dart impact resistance measured according to ASTM D 1709 is above 1,200 gf.
17. The membrane according to claim 14, in, When the film thickness is 45 to 55 μm, the 1% secant modulus in the MD direction, measured according to ASTM D 882, is 1,500 kg / cm². 2 The 1% secant modulus in the TD direction is 1,800 kg / cm². 2 above.
Citation Information
Patent Citations
Method of processing image data and Electronic device for performing the Method
KR1020240073747A
Substituted 1,2-dihydro-3h-pyrazolo[3,4-d]pyrimidin-3-ones
KR1020250073542A