Thermo-detachable two-component polyurethane adhesive composition

By utilizing a heat-detachable two-component polyurethane adhesive composition with a specific OH/NCO ratio and thermal activation, the problem of difficult detangle of existing adhesives is solved, achieving effective detangle in electric vehicles and consumer electronics while protecting the substrate.

CN123076624APending Publication Date: 2026-11-10HENKEL KGAA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580026835.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-11
Filing Date
2025-03-11
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing adhesives are difficult to use effectively for debonding in electric vehicles and consumer electronics, and traditional methods may damage the substrate or are complicated to operate, especially when debonding at high temperatures, which can easily damage the substrate.

Method used

A heat-detachable two-component polyurethane adhesive composition is used, comprising a first component and a second component, which are respectively polymeric polyol and isocyanate-terminated compounds. The components are mixed by a specific OH/NCO equivalent ratio and detangled by applying heat at 60 to 200°C.

Benefits of technology

It effectively reduces bond strength while maintaining adhesion and mechanical properties, facilitates debonding, and protects the substrate from heat. It is suitable for various substrates such as metal, electro-coated metal, PET, and pretreated PP.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The present invention relates to the use of a heat-detachable two-component polyurethane adhesive composition or cured product according to the present invention in an adhesive structure, wherein the adhesive structure is, for example, an electric mobility-related component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a heat-release two-component polyurethane adhesive composition, which is particularly suitable for use in electric mobility-related components. Background Technology

[0002] Adhesive bonding and polymer coatings are commonly used in the assembly and finishing of manufactured goods. They are used to replace mechanical fasteners such as screws, bolts, and rivets to provide adhesion with reduced processing costs and greater adaptability during manufacturing. Adhesive bonding distributes stress evenly, reduces the likelihood of fatigue, and seals joints to protect against corrosive substances.

[0003] While adhesive bonding offers many advantages over mechanical fasteners, disassembling adhesively bonded objects is often difficult when required in practical applications. Removing the adhesive mechanically—such as by sandblasting or wire brushing—is generally impossible, partly because the adhesive is situated between the substrates and is therefore either inaccessible or difficult to abrade without damaging the substrate surface. Disassembly by applying chemicals and / or high temperatures may be effective, but can be time-consuming and complex; furthermore, the required corrosive chemicals and / or harsh conditions may damage the separated substrates, rendering them unsuitable for subsequent applications.

[0004] As an example, it is obviously desirable to remove, replace, and / or recycle components from the automotive industry, such as electric vehicle battery cells and helmets that have been attached to devices using adhesives. However, such adhesives are typically strong, as they are designed to remain adhered during drop or impact events and under a wide range of operating temperatures and other environmental conditions. If not handled carefully, adhesive-bonded device components can be damaged or destroyed when removed by mechanical methods or by applying chemicals.

[0005] Some authors have sought to develop release adhesive compositions in which applied heat is used to break the bond at the adhesive-substrate interface. The problem with heat release is that, if not handled carefully, the high temperature can damage the substrate.

[0006] Noting these issues, some authors have also sought to develop debonded adhesive compositions in which an electric current is passed through the cured composition to break the bond at the adhesive-substrate interface.

[0007] Water-based systems and UV-activated acrylates have been used as release adhesive layers in the past. However, despite good release efficiency, the adhesive strength at room temperature, poor adhesion to substrates such as PP, PET, or electrocoated steel, and poor compatibility with thermally conductive polyurethane adhesives have been found to be unsatisfactory.

[0008] Therefore, there remains a need in the art to provide a means to effectively debond bonded substrates, particularly bonded structures in electric vehicle batteries and consumer electronics, while maintaining the optimal adhesive and mechanical properties of the adhesive. Summary of the Invention

[0009] This invention relates to a heat-detachable two-component polyurethane adhesive composition comprising a first component comprising two or more polymeric polyols having an average hydroxyl functionality of at least 1.8, wherein the average hydroxyl functionality is measured according to ASTM D4274; and heat-expandable thermoplastic microspheres; and a second component comprising at least one isocyanate-terminated compound; wherein the first component and the second component are mixed at an OH / NCO equivalent ratio of 1:0.7 to 1:1.1.

[0010] The present invention also relates to a cured, heat-detachable, two-component polyurethane composition according to the present invention.

[0011] This invention covers the use of the thermally debonded two-component polyurethane compositions or cured products according to the invention in bonded structures.

[0012] The present invention also covers an adhesive structure comprising: a first substrate; a second substrate; a thermally removable two-component polyurethane composition layer or cured product layer according to the present invention; and an adhesive layer, wherein the thermally removable two-component polyurethane composition is disposed on the surface of the first substrate and / or the surface of the second substrate, and wherein the adhesive layer is disposed on top of the thermally removable two-component polyurethane composition layer, wherein the adhesive layer is preferably formed of an adhesive selected from: epoxy adhesives, acrylic adhesives, polyurethane adhesives, cyanoacrylate adhesives, silicone adhesives, polyimide adhesives, silane-modified polymers, butyl rubber, hot melt adhesives, and mixtures thereof.

[0013] Furthermore, the present invention relates to a method for debonding the adhesive structure according to the present invention, the method comprising the steps of: i) applying heat; and ii) debonding the surface, wherein the temperature applied in step i) is preferably 60 to 200°C, and preferably applied for a duration of 15 seconds to 60 minutes. Attached Figure Description

[0014] Figure 1 The bonding structure and debonding method are shown.

[0015] Figure 2 The tensile lap shear strength results of LOCTITE TLB9150ABS combined with Examples 1-6 on Al3003 substrate are shown.

[0016] Figure 3The tensile lap shear strength results of thermally conductive epoxy adhesive (from Henkel) combined with the composition layer according to the invention on an Al3003 substrate are shown.

[0017] Figure 4 The tensile lap shear strength of LOCTITE TLB9150ABS combined with the composition according to the invention on an Al3003 substrate is shown as a function of temperature.

[0018] Figure 5 The tensile lap shear strength results of LOCTITE TLB9150ABS combined with the composition layer according to the invention on electrocoated steel are shown.

[0019] Figure 6 and 7 The tensile lap shear strength results of LOCTITE TLB9150ABS combined with the composition layer according to the invention on Al3003 / PET-Al3003 and PP are shown.

[0020] Figure 8 The test setup for a preliminary debonding test using an empty battery casing is shown, and the temperature during debonding is monitored.

[0021] Figure 9 The development of battery cell temperature profiles during thermal debonding using thermally conductive adhesive (LOCTITE TLB9150ABS) and the composition layer according to the invention is shown. Detailed Implementation

[0022] The invention is described in more detail in the following paragraphs. Each aspect thus described may be combined with any other one or more aspects unless the contrary is explicitly stated. In particular, any feature indicated as preferred or advantageous may be combined with or in combination with any other feature indicated as preferred or advantageous.

[0023] In the context of this invention, unless the context otherwise requires, the terminology used shall be interpreted in accordance with the following definitions.

[0024] As used herein, the singular forms “a,” “an,” and “one” include both singular and plural referents, unless the context clearly specifies otherwise.

[0025] As used herein, the term “comprising” is synonymous with “including” or “containing” and is inclusive or open-ended, not excluding additional, unlisted members, elements or method steps.

[0026] As used herein, the term “composed of” excludes any unspecified element, ingredient, member, or method step.

[0027] The terms “preferred,” “ideally,” “desirably,” and “particularly” are frequently used herein to refer to embodiments of this disclosure that may provide particular benefits in certain circumstances. However, the description of one or more preferred, preferred, desired, or particular embodiments does not imply that other embodiments are not useful, and is not intended to exclude those other embodiments from the scope of this disclosure.

[0028] As used throughout this application, the word “may” is used in a permissive sense—that is, meaning having potential—rather than in a mandatory sense.

[0029] The description of numerical endpoints includes all numbers and fractions contained within the corresponding range, as well as the described endpoints.

[0030] All percentages, portions, proportions, etc. mentioned in this article are based on weight unless otherwise indicated.

[0031] When quantities, concentrations, or other values ​​or parameters are expressed in the form of ranges, preferred ranges, or preferred upper and lower limits, it should be understood that any range obtained by combining any upper or preferred value with any lower or preferred value is specifically disclosed, regardless of whether the obtained range is explicitly mentioned in the context.

[0032] As used herein, the term "one-component (1K) composition" refers to a composition in which all the components of the composition are mixed together during the storage period of the composition, but the properties of the composition, including viscosity, remain sufficiently consistent during the storage period to allow the composition to be used successfully thereafter.

[0033] A “two-component (2K) composition” should be understood as a composition in which the first component / part and the second component / part must be stored in separate containers due to their (high) reactivity. The two components / parts are mixed only shortly before application and then react, typically without additional activation, with bond formation and thus the formation of a polymer network. Higher temperatures may be applied here to accelerate the crosslinking reaction.

[0034] As used herein, room temperature is 23°C ± 2°C. As used herein, “ambient conditions” means the temperature and pressure of the surrounding environment in which the composition is located or the coating or the substrate of the coating is located.

[0035] As used herein, the term "detachable" means that after the adhesive has cured, the bond strength may decrease by at least 50% after being subjected to a temperature of 60 to 200 °C for a duration of 15 seconds to 60 minutes. The bond strength was measured by a tensile lap shear (TLS) test performed at room temperature and based on EN 1465:2009 (German version) "Adhesives – Determination of tensile lap shear strength of bonded components".

[0036] The viscosity of the compositions described herein, unless otherwise specified, was measured using an Anton Paar viscometer, model MCR 301, under standard conditions of 25°C and 50% relative humidity (RH). The viscometer was calibrated annually and inspected by the service department. Calibration was performed using standard liquids with known viscosities from 1 to 50,000 cps (parallel plate PP20, shear rate 1 s⁻¹ at 23°C). -1 The composition according to the invention was measured using parallel plates PP20 at different shear rates from 1.5 to 100 s. -1 The following will proceed.

[0037] As used herein, the terms “polymer” and “polymerized” refer to prepolymers as well as homopolymers and copolymers.

[0038] As used herein, the terms “oligomer” and “oligomeric” refer to molecules having only a few repeating units, such as about 2 to about 20 repeating units.

[0039] As used herein, the term "prepolymer" refers to a polymer precursor that can be further reacted or polymerized by one or more reactive groups to form a higher molecular weight or cross-linked state. As used herein, the prefix "polymer" refers to two or more.

[0040] Polyols should be understood as compounds containing more than one hydroxyl (-OH) group in their molecules. Polyols may also have other functional groups on their molecules. The term "polyol" encompasses a single polyol or a mixture of two or more polyols.

[0041] The average hydroxyl (-OH) functionality refers to the average number of reactive hydroxyl groups contained in a molecule of polyol.

[0042] All references cited in this specification are incorporated herein by reference in their entirety.

[0043] Unless otherwise defined, all terms used in disclosing this invention, including technical and scientific terms, have the meanings commonly understood by one of ordinary skill in the art to which this invention pertains. As further guidance, terminology definitions are included to better understand the teachings of this invention.

[0044] This invention relates to a heat-detachable two-component polyurethane adhesive composition comprising a first component comprising two or more polymeric polyols having an average hydroxyl functionality of at least 1.8, wherein the average hydroxyl functionality is measured according to ASTM D4274; and heat-expandable thermoplastic microspheres; and a second component comprising at least one isocyanate-terminated compound; wherein the first component and the second component are mixed at an OH / NCO equivalent ratio of 1:0.7 to 1:1.1.

[0045] The applicant has discovered that the compositions according to the invention have optimized activation temperatures for battery applications without adversely affecting battery performance. The compositions according to the invention exhibit good adhesion to a variety of substrates such as metals, electroplated metals, PET, and pretreated PP, and also good adhesion to other adhesives such as thermally conductive polyurethane adhesives. Furthermore, the adhesive strength of the compositions according to the invention decreases significantly after thermal activation, thus facilitating debonding and cleaning of the debonded parts. Finally, the compositions according to the invention also provide a thermal insulation effect, thus protecting the substrate to be debonded from heat during debonding.

[0046] The first component and the second component are mixed in an OH / NCO equivalent ratio of 1:0.7 to 1:1.1, preferably in an equivalent ratio of 1:1.1.

[0047] These ratios are preferred because a higher ratio may cause the NCO groups to act as plasticizers and soften the matrix, while a lower ratio may cause the matrix to be too soft and the bond strength to decrease.

[0048] The first component of the heat-release two-component polyurethane adhesive composition according to the present invention comprises two or more polymeric polyols having an average hydroxyl functionality of at least 1.8, wherein the average hydroxyl functionality is preferably 1.8 to 6.0, more preferably 1.8 to 4.0, as measured according to ASTM D4274.

[0049] The polymeric polyol may have a weight-average molecular weight of 400 to 10,000 g / mol. Unless otherwise stated, “molecular weight” here refers to weight-average molecular weight. The number-average molecular weight Mn and weight-average molecular weight Mw are determined according to the present invention by gel permeation chromatography (GPC, also known as SEC) at 23°C using styrene standards in accordance with DIN EN ISO 16014-5:2012-10.

[0050] The polymeric polyol may also have a hydroxyl value of 10 to 500 mg KOH / g, preferably 20 to 400 mg KOH / g, more preferably 50 to 350 mg KOH / g, as measured according to DIN EN ISO 4629.

[0051] Some suitable polyols include the reaction products of low molecular weight polyols with olefinic oxygen, i.e., so-called polyether polyols. The olefinic oxygen preferably contains 2 to 4 carbon atoms. Some reaction products of this type include, for example, ethylene glycol, propylene glycol, isobutanediol, hexanediol, or 4,4'-dihydroxydiphenylpropane with ethylene oxide, propylene oxide, or butane oxide, or mixtures thereof. It is also suitable to react polyols, such as glycerol, trimethylolethane or trimethylolpropane, pentaerythritol, or sugar alcohols, or mixtures thereof, with the aforementioned olefinic oxygen to form polyether polyols. Therefore, depending on the desired molecular weight, products can be obtained by adding only a few moles of ethylene oxide and / or propylene oxide or more than one hundred moles of ethylene oxide and / or propylene oxide to a low molecular weight polyol. Other polyether polyols can be obtained by, for example, the condensation and elimination of water from glycerol or pentaerythritol. Some suitable polyols include those that can be obtained by the polymerization of tetrahydrofuran.

[0052] The polyether polyol is prepared in a known manner by reacting a starting compound containing reactive hydrogen atoms with an olefinic oxygen, such as ethylene oxide, propylene oxide, butane oxide, styrene oxide, tetrahydrofuran, or epichlorohydrin, or a mixture of two or more thereof.

[0053] Suitable starting compounds are, for example, water, ethylene glycol, 1,2- or 1,3-propanediol, 1,4- or 1,3-butanediol, hexane-1,6-diol, octane-1,8-diol, neopentyl glycol, 1,4-hydroxymethylcyclohexane, 2-methylpropane-1,3-diol, glycerol, trimethylolpropane, hexane-1,2,6-triol, butane-1,2,4-triol, trimethylolethane, pentaerythritol. Mannitol, sorbitol, methyl glycosides, sugars, phenol, isononylphenol, resorcinol, hydroquinone, 1,2,2- or 1,1,2-tri-(hydroxyphenyl)-ethane, ammonia, methylamine, ethylenediamine, tetra- or hexamethylenediamine, triethanolamine, aniline, phenylenediamine, 2,4- and 2,6-diaminotoluene, and polyphenyl polymethylene polyamines, which can be obtained by aniline / formaldehyde condensation, or mixtures of two or more thereof.

[0054] Some suitable polymeric polyols include glycol EO / PO (ethylene oxide / propylene oxide) block copolymers, EO-terminated polypropylene glycol, or alkoxylated bisphenol A.

[0055] Some suitable polymerizable polyols include polyether polyols modified with vinyl polymers. These polyols can be obtained, for example, by polymerizing styrene or acrylonitrile or mixtures thereof in the presence of polyether polyols.

[0056] Commercially available examples of polyether polyols include the Arcol series of polyols from Covestro, such as Arcol PPG 425 and Arcol PPG 2025; the Dianol series of polyols from Arkema, such as Dianol 330; and the Pluracol series of polyols from BASF, such as P-2010.

[0057] Some suitable polymerizable polyols include polyester polyols. For example, polyester polyols can be obtained by reacting low molecular weight alcohols, more particularly ethylene glycol, diethylene glycol, neopentyl glycol, hexanediol, butanediol, propylene glycol, glycerol, or trimethylolpropane with caprolactone. Other suitable polyols for producing polyester polyols are 1,4-hydroxymethylcyclohexane, 2-methylpropane-1,3-diol, butane-1,2,4-triol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, dibutylene glycol, and polybutanediol.

[0058] Some suitable polymerizable polyols include polyester polyols obtained by polycondensation. Therefore, diols and / or triols can be condensed with less than stoichiometric amounts of dicarboxylic acids and / or tricarboxylic acids or their reactive derivatives to form polyester polyols. Suitable dicarboxylic acids are, for example, adipic acid or succinic acid and their higher homologues containing up to 16 carbon atoms, unsaturated dicarboxylic acids such as maleic acid or fumaric acid, cyclohexanedicarboxylic acid (CHDA), and aromatic dicarboxylic acids, more particularly isophthalic acids such as phthalic acid, isophthalic acid, or terephthalic acid. Citric acid and trimellitic acid, for example, are also suitable tricarboxylic acids. The mentioned acids can be used alone or as mixtures of two or more of them. At least one of the mentioned dicarboxylic acids is suitable with a polyester polyol containing glycerol and a residual OH group content. Suitable alcohols include, but are not limited to, propylene glycol, butanediol, pentanediol, hexanediol, ethylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, cyclohexanediol (CHDM), 2-methyl-1,3-propanediol (MPDiol), or neopentyl glycol, or their isomers or derivatives, or mixtures of two or more thereof. High molecular weight polyester polyols can be used in the second synthesis stage and include, for example, reaction products of poly(preferably di) alcohols (optionally with a small amount of triol) and poly(preferably di) carboxylic acids. Instead of free polycarboxylic acids, corresponding polycarboxylic anhydrides or esters of the corresponding polycarboxylic acids with alcohols preferably containing 1 to 3 carbon atoms (where possible) can also be used. The polycarboxylic acids can be aliphatic, cycloaliphatic, aromatic, or heterocyclic, or both. They can optionally be substituted, for example, with alkyl, alkenyl, ether, or halogen groups. Suitable polycarboxylic acids are, for example, succinic acid, adipic acid, octanoic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, tetrachlorophthalic anhydride, methylenetetrahydrophthalic anhydride, glutaric anhydride, maleic acid, maleic anhydride, fumaric acid, dimer fatty acids, or trimer fatty acids, or mixtures of two or more thereof. A small amount of monofunctional fatty acids may optionally be present in the reaction mixture.

[0059] The polyester polyol may optionally contain a small amount of terminal carboxyl groups. Polyesters that can be obtained from lactones (e.g., those based on ε-caprolactone (also known as "polycaprolactone")) or hydroxycarboxylic acids (e.g., ω-hydroxyhexanoic acid) may also be used.

[0060] Oil-derived polyester polyols may also be used. Oil-derived polyester polyols can be obtained, for example, by the complete ring-opening of an epoxidized triglyceride containing at least a portion of an olefinically unsaturated fatty acid mixture with one or more alcohols containing 1 to 12 carbon atoms, followed by partial transesterification of the triglyceride derivative to form an alkyl ester polyol having 1 to 12 carbon atoms in the alkyl group.

[0061] Some suitable polymeric polyols include C36 dimer diols and their derivatives. Some suitable polymeric polyols include castor oil and its derivatives. Some suitable polymeric polyols include fatty polyols, such as hydroxylated products of unsaturated or polyunsaturated natural oils, hydrogenated products of unsaturated and polyunsaturated polyhydroxy natural oils, polyhydroxy esters of alkyl hydroxy fatty acids, polymerized natural oils, soybean polyols, and alkyl hydroxylated amides of fatty acids. Some suitable polyols include hydroxyl-functionalized polybutadiene (polybutadiene polyols, such as Krasol LBH 2000 from Cray Valley). Some suitable polymeric polyols include polyisobutylene polyols. Some suitable polymeric polyols include polyacetal polyols. Polyacetal polyols should be understood as compounds that can be obtained by reacting diols, such as diethylene glycol or hexanediol, or mixtures thereof, with formaldehyde. Polyacetal polyols can also be obtained by polymerizing cyclic acetals. Some suitable polymeric polyols include polycarbonate polyols. Polycarbonate polyols can be obtained, for example, by reacting diols such as propylene glycol, butane-1,4-diol or hexane-1,6-diol, diethylene glycol, triethylene glycol or tetraethylene glycol or mixtures thereof with diaryl carbonates, such as diphenyl carbonate, or phosgene. Some suitable polymerizable polyols include polyamide polyols.

[0062] Some suitable polymeric polyols include polyacrylates containing OH groups. These polyacrylates can be obtained, for example, by polymerizing olefinically unsaturated monomers with OH groups. Such monomers can be obtained, for example, by esterification of olefinically unsaturated carboxylic acids with diols, typically in a slight excess. Suitable olefinically unsaturated carboxylic acids for this purpose are, for example, acrylic acid, methacrylic acid, crotonic acid, or maleic acid. The corresponding OH-functionalized esters are, for example, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, or 3-hydroxypropyl methacrylate, or mixtures of two or more thereof.

[0063] Some suitable polymerizable polyols include those based on cashew nut shell liquid. Cashew nut shell liquid is derived from the layer between the cashew kernel and the shell. This intermediate layer mainly contains ascorbic acid (2-carboxy-3-pentadecanediol) and related acids with varying double bond contents, as well as cashew diol (m-pentadecanediol). The liquid is extracted from the intermediate layer by heating, during which the acids are decarboxylated. The resulting products include cashew nut shell liquid, cashew diol, and related compounds with varying double bond numbers. Cashew nut shell liquid is ultimately separated from CNSL by distillation. The side chains, which are saturated or cis-unsaturated, can undergo further reactions, such as polymerization, to form compounds with higher molecular weights.

[0064] Preferably, the cashew nutshell polyol is selected from cashew nutshell polyether polyols, cashew nutshell polyester polyols, cashew nutshell Mannich polyols, and combinations thereof. Suitable cashew nutshell polyols include, but are not limited to, Polycard polyols from Chemical Technical Services Inc. (e.g., Polycard XFN-50, Polycard XFN-53, and Polycard 425M), polyols from Cardolite Corp. (e.g., GX-9201, GX9203, NX-9001, NX-9001LV, NX-9004, NX-9007, NX-9008, NX-5285, GX-9005, GX-9006, GX-9007, GX-9101, GX-9102, GX-9103, GX-9104), and polyols from BioBased Technologies (e.g., Agrol Platinum).

[0065] Preferably, the polymeric polyol is selected from polyether polyols, polyester polyols, polybutadiene polyols and mixtures thereof, and preferably the polymeric polyol is a mixture of trifunctional polypropylene ether polyol and castor oil.

[0066] These polymeric polyols are preferred because their short chains can help increase adhesive strength and provide the required stiffness to the matrix.

[0067] Two or more polymeric polyols may be present in an amount of 15% to 75%, preferably 28% to 65%, or even more preferably 35% to 58% of the total weight of the first component of the composition.

[0068] These amounts are preferred and considered ideal for the overall function of the composition. Excessive amounts may result in too little amount of thermally expandable thermoplastic microspheres, thus negatively affecting the debinding properties and the stability of the composition, while excessive amounts may negatively affect the application of the composition.

[0069] The first component of the thermally detackible two-component polyurethane adhesive composition according to the present invention may include at least one monofunctional alcohol. The monofunctional alcohol acts as a rheology modifier for the polymerized polyol, and when added at the desired application temperature, produces significantly lower viscosity of the polyol component and significantly better flow rate of the overall thermally conductive adhesive composition mixture.

[0070] In a highly preferred embodiment, the first component of the thermally detangleable two-component polyurethane adhesive composition according to the invention comprises at least one monofunctional alcohol.

[0071] The monofunctional alcohol may be a monofunctional alkyl alcohol, preferably having 1 to 20 carbon atoms, more preferably having 4 to 18 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 8 to 18 carbon atoms.

[0072] The monofunctional alcohol is selected from methanol, ethanol, propanol, isopropanol, butanol, 2-butanol, isobutanol, pentanol, hexanol, heptanol, octanol, nonanol, 1-decanol, undecylol, dodecanol, tridecanol, tetradecanol, pentadecylol, hexadecylol, heptadecanol, octadecylol, nonadecanol, eicosanol and mixtures thereof, with 1-decylol being the preferred monofunctional alcohol.

[0073] In a highly preferred embodiment, the monofunctional alcohol is 1-decyl alcohol.

[0074] 1-Decanol is a preferred monofunctional alcohol because it affects the softening point of the adhesive composition and produces thermoplastic polyurethane behavior, and further has a positive effect on the debonding properties.

[0075] Suitable commercially available monofunctional alcohols applicable to this invention include, but are not limited to, 1-decyl alcohol from Thermo Scientific.

[0076] The monofunctional alcohol may be present in an amount of 0.5 to 20%, preferably 0.5 to 15%, more preferably 0.6 to 10% of the total weight of the first component of the composition.

[0077] These amounts are preferred because they provide the desired performance for the compositions according to the invention. Too low an amount, below 0.5%, may not provide the desired technical effect, while too high an amount may fail to improve the desired technical effect without negatively impacting other properties.

[0078] The first component of the thermally detangleable two-component polyurethane adhesive composition according to the present invention comprises thermally expandable thermoplastic microspheres.

[0079] Suitable thermoplastic microspheres have a core-shell structure, wherein the shell is formed of a cross-linked polymer and the core is composed of a foaming agent.

[0080] Suitable crosslinked polymers can be prepared by (co)polymerization of any suitable monomer or comonomer. Suitable monomers that can be used to prepare said polymers include nonionic olefinic unsaturated monomers.

[0081] Suitable nonionic olefinic unsaturated monomers applicable to the present invention may be selected from styrene, vinyltoluene, ethylene, butadiene, vinyl acetate, vinyl chloride, vinylidene chloride, acrylonitrile, acrylamide, methacrylamide, C1-C20 alkyl esters or C2-C20 alkenyl esters of acrylic acid or methacrylic acid, methacrylates, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, benzyl acrylate, benzyl methacrylate, lauryl acrylate, lauryl methacrylate, oleic acid esters, oleic acid esters, palmitic acid esters, palmitic acid esters, stearic acid esters, stearic acid esters, hydroxyl-containing monomers, especially C1-C10 hydroxyalkyl (meth)acrylates, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glycidyl (meth)acrylate, preferably methyl methacrylate and mixtures thereof.

[0082] Suitable polymers can also be copolymers prepared by copolymerizing two or more of the monomers mentioned above. Preferred monomer combinations include acrylonitrile / (meth)acrylate, styrene / (meth)acrylate, acrylamide / (meth)acrylate, and acrylonitrile / (meth)hydroxyethyl acrylate. A more preferred combination is acrylonitrile / methyl methacrylate.

[0083] Suitable crosslinking agents for polymer crosslinking applicable to the present invention are compounds having two or more olefinically unsaturated groups, such as diacrylates or dimethacrylates of at least a dibasic alcohol, such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,2-propanediol diacrylate, 1,2-propanediol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, hexanediol diacrylate, hexanediol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 3-methylpentyl glycol diacrylate, and 3-methylpentyl glycol dimethacrylate. Another class of crosslinking agents includes diacrylates or dimethacrylates of polyethylene glycol or polypropylene glycol, each with a molecular weight of 200 to 9000. The polyethylene glycol and / or polypropylene glycol used to prepare the diacrylates or dimethacrylates preferably each have a molecular weight of 400 to 2000. Not only homopolymers of ethylene oxide and / or propylene oxide can be used, but also block copolymers of ethylene oxide and propylene oxide, or random copolymers of ethylene oxide and propylene oxide comprising a random distribution of ethylene oxide and propylene oxide units. Similarly, oligomers of ethylene oxide and / or propylene oxide can be used to prepare crosslinking agents, examples of which are diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, and / or tetraethylene glycol dimethacrylate.

[0084] The crosslinking agent is preferably used in an amount of 0.1 to 30% based on the monomer to be polymerized in any stage.

[0085] The core is preferably composed of a physical blowing agent. Suitable physical blowing agents include alkanes and / or cycloalkanes having at least 4 carbon atoms, dialkyl ethers, esters, ketones, acetals, fluoroalkanes having 1 to 8 carbon atoms, and tetraalkylsilanes having 1 to 3 carbon atoms in the alkyl chain, particularly tetramethylsilane.

[0086] Examples of suitable blowing agents that can be used according to the invention include propane, n-butane, isobutane and cyclobutane, n-pentane, isopentane and cyclopentane, cyclohexane, dimethyl ether, methyl ethyl ether, methyl butyl ether, methyl formate and acetone, as well as fluoroalkanes that can degrade in the troposphere and are therefore ozone-free, such as trifluoromethane, difluoromethane, 1,1,1,3,3-pentafluorobutane, 1,1,1,3,3-pentafluoropropane, 1,1,1,2-tetrafluoroethane, difluoroethane and 1,1,1,2,3,3,3-heptafluoropropane, and perfluoroalkanes such as C3F8, C4F8, etc. 10 C5F 12 C6F 14 and C7F 16 The foaming agents can be used alone or in any combination of each other.

[0087] In addition, hydrofluoroolefins, such as 1,3,3,3-tetrafluoropropylene, or hydrochlorofluoroolefins, such as 1-chloro-3,3,3-trifluoropropylene, can be used as blowing agents.

[0088] In a preferred embodiment, the physical blowing agent is a hydrocarbon, preferably selected from alkanes and / or cycloalkanes having at least four carbon atoms. In particular, pentane is used, with isopentane and cyclopentane being preferred. Cyclopentane is preferred when rigid foam is used as an insulating material in cooling equipment. The hydrocarbon can be mixed with water.

[0089] The thermally expandable microspheres can be prepared by seeding swelling of cross-linked polymers and encapsulation with foaming agents.

[0090] The thermally expandable thermoplastic microspheres have a particle size of 5 to 100 µm, preferably 8 to 75 µm, preferably 9 to 50 µm, more preferably 10 to 30 µm, more preferably 12 to 20 µm, and even more preferably 13 to 19 µm, wherein the particle size is measured by laser diffraction (low-angle laser light scattering LALLS).

[0091] The particle size range defined above refers to the size before expansion.

[0092] The thermally expandable thermoplastic microspheres expand when exposed to heat, preferably at 60 to 200°C, more preferably at 80 to 160°C, and even more preferably at 80 to 120°C.

[0093] The heat source can be, for example, a heat source, an ultrasonic processing probe, or an electromagnetic source.

[0094] The thermo-expandable thermoplastic microspheres may be present in the thermo-detachable two-component polyurethane adhesive composition according to the invention in an amount of 15 to 50%, preferably 20 to 40%, more preferably 27 to 37% based on the total weight of the first component of the composition.

[0095] The above-defined and preferred ranges are ideal for breaking the bond line while maintaining a low solids content in the composition. Too low a amount, less than 15%, may not result in complete bond failure, while too high a amount, more than 50%, may increase the solids content excessively without providing any additional technical benefit.

[0096] The first component of the heat-release two-component polyurethane adhesive composition according to the present invention may optionally include a tackifier. A tackifier can be added to the composition to improve the adhesion of the polyurethane resin to the substrate. The tackifier functions by forming a new layer at the interface that is firmly bonded to both the substrate and the coating. The resulting interface area is also more resistant to environmental chemical attack.

[0097] The choice of tackifier can be determined by the type of surface to which the composition will be applied. Nevertheless, the most common commercial tackifiers are organosilanes, such as epoxy-functionalized organosilanes. Suitable organosilanes for use in this invention are, but are not limited to, glycidoxypropyltrimethoxysilane. Other types of tackifiers for which uses can be found herein include: organometallic compounds such as titanates and zirconates, specific examples of which include isopropyltris(N-ethylaminoethylamino)titanate, tetraisopropyl di(dioctyl phosphate)titanate, neoalkoxytrinedecyl zirconate, and zirconium propionate; diphenolic compounds such as catechol and thiodiol; hydroxylamines such as tris(hydroxymethyl)aminomethane; polyphenols such as pyrogallol, gallic acid, or tannic acid; and plastisols, which are suspensions of polyvinyl chloride particles in a plasticizer.

[0098] Suitable commercially available adhesives for use in this invention include, but are not limited to, Dynasylan GLYMO from Evonic.

[0099] The adhesive aid may be present in the heat-detachable two-component polyurethane adhesive composition according to the invention in an amount of 0.1 to 10% by weight, preferably 1 to 9% by weight, more preferably 2.5 to 8% by weight, based on the total weight of the first component of the composition.

[0100] The above-defined and preferred range of tackifier dosages is ideal, providing an appropriate increase in adhesive strength without adversely affecting other properties.

[0101] The heat-release two-component polyurethane adhesive composition according to the present invention is characterized in that both components contain fillers. The composition of the fillers in each component is determined independently, and therefore can be the same or different for each component.

[0102] In a broad sense, there is no particular intention to limit the shape of the particles used; needle-like, spherical, ellipsoidal, cylindrical, bead-like, cubic, or flake-like particles can be used alone or in combination. Furthermore, it is conceivable to use agglomerates of more than one particle type.

[0103] Preferably, the filler is selected from calcium carbonate, calcium oxide, calcium hydroxide (lime powder), precipitated and / or pyrolytic silica, zeolite, bentonite, wollastonite, magnesium carbonate, diatomaceous earth, barium sulfate, alumina, clay, talc, sand, quartz, flint, mica, glass beads, glass powder, paramagnetic nanoparticles, alumina-based thermally conductive fillers, and other abrasive minerals. Short fibers such as glass fiber, glass filament, polyacrylonitrile, carbon fiber, or polyethylene fiber may also be added.

[0104] The pyrolysis and / or precipitation of silica advantageously has a concentration of 10 to 90 m. 2 / g BET surface area. When used, they do not cause any additional increase in viscosity of the compositions according to the invention, but do help to enhance the cured composition.

[0105] Similarly, it is conceivable to use surfaces with a higher BET area, advantageously 100 to 250 m². 2 / g of pyrolytic and / or precipitated silica as filler: Due to the larger BET surface area, the effect of enhancing the cured composition is achieved with a smaller weight ratio of silica.

[0106] Furthermore, hollow spheres with mineral or plastic shells are suitable as non-conductive fillers. These can be, for example, hollow glass spheres commercially available under the trade name Glass Bubbles®. Plastic-based hollow spheres, such as Expancel® or Dualite®, and described in EP 0 520 426 B1, can also be used: they are composed of inorganic or organic materials and each has a diameter of 1 mm or less, preferably 500 µm or less, more preferably 100 to 200 µm.

[0107] Non-conductive fillers that impart thixotropic properties to a composition may be preferred for many applications: such fillers are also described as rheology modifiers, such as hydrogenated castor oil, fatty acid amides, or swellable plastics such as PVC.

[0108] In a highly preferred embodiment, the filler is the same in the first and second components and is a mixture of calcium carbonate and zeolite powder.

[0109] Suitable commercially available fillers for use in this invention include, but are not limited to, Omya BH from Omya, UOP-L powder from Azelis, and WINNOFIL SPM and Extra M 100 from Imerys.

[0110] The filler may be present in an amount of 2 to 20%, preferably 5 to 15%, more preferably 6 to 13% of the total weight of the first component of the composition.

[0111] The filler may be present in an amount of 20 to 50%, preferably 25 to 40%, more preferably 27 to 33% of the total weight of the second component of the composition.

[0112] The second component of the heat-detachable two-component polyurethane adhesive composition according to the present invention comprises an isocyanate-terminated compound.

[0113] The isocyanate-terminated compound can be any compound having an average of two, three, or more isocyanate groups. As used herein, the term "isocyanate-terminated compound" encompasses diisocyanates, polymeric isocyanates, and isocyanate-terminated oligomers and polymers. Such isocyanate-terminated compounds can be used alone or in combination. In one embodiment, the isocyanate-terminated compound is selected from aromatic polyisocyanates, alicyclic polyisocyanates, aliphatic polyisocyanates, and mixtures thereof, and preferably one or more aliphatic polyisocyanates. The isocyanate-terminated compound preferably has an NCO content of 20 to 30%. The viscosity of the isocyanate-terminated compound preferably does not exceed 5000 mPa·s.

[0114] Some advantageous isocyanate-terminated compounds have the general formula O=C=NXN=C=O, where X is an aliphatic, alicyclic, or aromatic group, preferably an aliphatic or alicyclic group containing 4 to 18 carbon atoms.

[0115] Some suitable isocyanates include 1,5-naphthylene diisocyanate, diphenylmethane diisocyanate (MDI) including 2,2'-, 2,4'- and 4,4'- isomers, polymeric MDI (pMDI), hydrogenated MDI (HMDI), phenylene diisocyanate (XDI), tetramethylphenylene diisocyanate (TMXDI), di- and tetraalkylene diphenylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, isomers of toluene diisocyanate (TDI), 1-methyl-2,4-diisocyanocyclohexane, 1,6-diisocyano-2,2,4-trimethylhexane, 1,6-diisocyano-2,4,4'-diisocyano-2,4,4'-diisocyanate, and so on. - Trimethylhexane, 1-isocyanomethyl-3-isocyano-1,5,5-trimethylcyclohexane (IPDI), chlorinated and brominated diisocyanates, phosphorus-containing diisocyanates, 4,4'-diisocyanophenyl perfluoroethane, tetramethoxybutane-1,4-diisocyanate, butane-1,4-diisocyanate, hexane-1,6-diisocyanate (HDI), dicyclohexylmethane diisocyanate, cyclohexane-1,4-diisocyanate, ethylene diisocyanate, phthalic acid-bis-isocyanoethyl ester; diisocyanates containing reactive halogen atoms, such as 1-chloromethylphenyl-2,4-diisocyanate, 1-bromomethylphenyl-2,6-diisocyanate, or 3,3-bis-chloromethyl ether-4,4'-diphenyl diisocyanate. Aromatic polyisocyanates are preferred, with diphenylmethane diisocyanate (MDI) and its isomers and polymeric MDI (pMDI) being more preferred as part or all of the polyisocyanates used in the synthesis of prepolymers.

[0116] Some suitable isocyanates include isocyanate-functionalized prepolymers. Such prepolymers are formed by reacting an excess of polyisocyanate with a polyol, polyamine, polythiol, or a combination thereof. "Excess" should be understood to mean that, during the reaction to form the prepolymer, the equivalent number of isocyanate functional groups from the polyisocyanate compound is greater than the equivalent number of hydroxyl functional groups from the polyol. In this disclosure, it should be understood that the terms polyisocyanate prepolymer or prepolymer or isocyanate-functionalized prepolymer apply to any compound prepared according to the foregoing description, i.e., provided that the compound is prepared with at least a stoichiometric excess of isocyanate groups relative to isocyanate reactive groups, it is referred to herein as a polyisocyanate prepolymer or prepolymer or isocyanate-functionalized prepolymer.

[0117] Sulfur-containing polyisocyanates are obtained, for example, by reacting 2 moles of hexamethylene diisocyanate with 1 mole of thiodiglycol or dihydroxydihexyl sulfide. Other suitable diisocyanates are, for example, trimethylhexamethylene diisocyanate, 1,4-diisocyanobutane, 1,12-diisocyanododecane, and dimer fatty acid diisocyanates. Suitable diisocyanates are tetramethylene diisocyanate, hexamethylene diisocyanate, undecane diisocyanate, dodecane diisocyanate, 2,2,4-trimethylhexane-2,3,3-trimethylhexamethylene diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, 1,3- and 1,4-tetramethylphenyldimethyl diisocyanate, isophorone, 4,4-dicyclohexylmethane, tetramethylphenyldimethyl (TMXDI), and lysine ester diisocyanate.

[0118] Aliphatic polyisocyanates with two or more isocyanate functionalities formed by biuret bonds, diuret bonds, urethane bonds and / or trimerization are suitable.

[0119] Suitable at least trifunctional isocyanates are polyisocyanates formed by the trimerization or oligomerization of diisocyanates or by the reaction of diisocyanates with polyfunctional compounds containing hydroxyl or amino groups. The isocyanates suitable for producing trimers are the aforementioned diisocyanates, with trimers of HDI, MDI, TDI, or IPDI being preferred.

[0120] End-capped, reversibly end-capped polyisocyanates, such as 1,3,5-tris-[6-(1-methylpropyleneaminooxycarbonylamino)-hexyl]-2,4,6-trioxahexahydro-1,3,5-triazine, are also suitable. Polymeric isocyanates, for example, formed as residues from diisocyanate distillation, are also suitable. The isocyanate-end-capping compounds encompass single compounds or mixtures of two or more compounds.

[0121] The isocyanate-terminated compound is preferably selected from aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, aromatic polyisocyanates, alicyclic polyisocyanates, aliphatic polyisocyanates, and mixtures thereof, and preferably the at least one isocyanate-terminated compound is methylene diphenyl diisocyanate.

[0122] In a highly preferred embodiment, the isocyanate-terminated compound is methylene diphenyl diisocyanate.

[0123] Methylene diphenyl diisocyanate is preferred because of its ideal reaction rate.

[0124] Suitable commercially available isocyanate-terminated compounds for use in this invention include, but are not limited to, Desmodur VK10, Desmodur VK5 and Desmodur VK20 from Covestro.

[0125] The isocyanate-terminated compound may be present at 35 to 70%, preferably 40 to 65%, more preferably 45 to 60%, and even more preferably 48 to 58% based on the total weight of the second component of the composition.

[0126] The above amounts are preferred because excessive amounts (above 70%) may cause the composition to age and become unstable, while excessive amounts (mainly less than 35%) may cause the composition to become too viscous and difficult to dispense.

[0127] The ratio of isocyanate groups in the isocyanate-terminated compound to OH groups in the polyol is generally within the equivalence range, and it is advantageous if a slight excess of isocyanate groups relative to humidity is present on the surface. According to the invention, the NCO / OH ratio is between 0.90:1 and 1.5:1, particularly between 1.0:1 and 1.3:1. According to the invention, the polyol component and the isocyanate component can be mixed in a weight ratio of 1:10 to 10:1, preferably 1:5 to 5:1, more preferably 1:2 to 2:1, depending on the selection of the polyol and the isocyanate-terminated compound.

[0128] The second component of the heat-release two-component polyurethane adhesive composition according to the present invention may further include a plasticizer. The plasticizer improves the flexibility of the composition according to the present invention.

[0129] The plasticizer is preferably selected from ethers of monofunctional, linear, or branched C4-C16 alcohols; esters of rosin acid, butyric acid, thiobutyric acid, and propionic acid esters; esters based on nitrocellulose and polyvinyl acetate; dicarboxylic acid esters; glycolates; benzoates; phosphate esters; sulfonates; trimellitates; end-capped polyethylene, polypropylene glycol, difunctional polyether polyols, and mixtures thereof, preferably alkyl sulfonates of phenol.

[0130] Suitable commercially available plasticizers applicable to this invention include, but are not limited to, Lupronol 1000 / 1 from BASF, Caradol ED 56-300 from Shell, Arcol PPG 2000 from Covestro, Voranol 2000 L from Dow, Jeffol PPG 2000 from Huntsman, and Mesamoll from LANXESS.

[0131] According to the thermally removable two-component polyurethane adhesive composition of the present invention, the plasticizer may be present in an amount of 5 to 25%, preferably 10 to 20%, more preferably 13 to 19% by weight of the second component of the composition.

[0132] These amounts are preferred because too low an amount, less than 5%, may not have a technical effect, while too high an amount, more than 25%, may reduce the adhesion performance and initial strength of the bonded structure.

[0133] This invention relates to a cured, heat-detachable two-component polyurethane composition according to the present invention.

[0134] The composition according to the invention can be cured in about 10 to 360 minutes at a temperature ranging from about 40°C to about 90°C. When cured, the cured product exhibits good adhesion.

[0135] This invention relates to the use of the heat-debonded two-component polyurethane composition or cured product according to the present invention in bonded structures.

[0136] This invention relates to an adhesive structure comprising: a first substrate; a second substrate; a thermally removable two-component polyurethane composition layer or cured product layer according to the invention; and an adhesive layer, wherein the thermally removable two-component polyurethane composition is disposed on the surface of the first substrate and / or the surface of the second substrate, and wherein the adhesive layer is disposed on top of the thermally removable two-component polyurethane composition layer, wherein the adhesive layer is preferably formed of an adhesive selected from the group consisting of: epoxy adhesives, acrylic adhesives, polyurethane adhesives, cyanoacrylate adhesives, silicone adhesives, polyimide adhesives, silane-modified polymers, butyl rubber, hot melt adhesives, and mixtures thereof.

[0137] The first and second substrates may be the same or different, and are not limited to any particular substrate material. However, a suitable substrate should have temperature stability below the debonding temperature and a melting point above 100°C.

[0138] Suitable substrates for this invention include, but are not limited to, aluminum, aluminum alloys, electrocoated steel, and PET-coated aluminum.

[0139] The adhesive layer of the bonding structure according to the invention can be formed from any type of adhesive suitable for adhesion to the selected substrate. Suitable adhesives can be one-component (1k) compositions or two-component (2k) compositions. Suitable adhesives can be selected from epoxy adhesives, acrylic adhesives, polyurethane adhesives, cyanoacrylate adhesives, silicone adhesives, polyimide adhesives, silane-modified polymers, butyl rubber, hot melt adhesives, and mixtures thereof.

[0140] Suitable commercially available adhesives applicable to this invention include, but are not limited to, Teroson EP 5065, LOCTITE TLB9150APS and Teroson MS 939 from Henkel Group.

[0141] Examples of bonded structures are automotive components such as batteries, helmets, and interior trim. Specific, non-limiting examples of electric mobility components include battery covers, battery cells (cell-to-cell, cell-to-module, cell-to-body), battery modules, inverters, converters, and various structural adhesive applications and various thermal conductive applications.

[0142] The present invention relates to a method for debonding the adhesive structure according to the invention, the method comprising the steps of: i) applying heat; and ii) debonding the surface, wherein the temperature applied in step i) is preferably 60 to 200°C, and preferably applied for a duration of 15 seconds to 60 minutes.

[0143] The heat source can be a heat source, an ultrasonic processing probe, or an electromagnetic source.

[0144] Figure 1 A bonding structure and a debonding method using a combination of a thermally debondable two-component polyurethane composition and a thermally conductive adhesive according to the present invention are shown.

[0145] Example The examples described below illustrate the performance of compositions according to embodiments of the present invention. Unless otherwise indicated, all parts and percentages in the following examples and throughout the description are parts by weight or weight percentages. The examples are included for illustrative purposes so that the present disclosure can be more readily understood, and are not intended to limit the scope of the present disclosure unless otherwise specifically indicated.

[0146] Tensile shear strength was measured according to DIN EN 1465:2009-07.

[0147] The tensile lap shear strength was measured according to DIN EN 1465:2009-07.

[0148] The thermally conductive polyurethane adhesive (PU TCA) LOCTITE TLB9150APS is from Henkel. Thermally conductive epoxy adhesive (from Henkel, with a thermal conductivity of 2 W / mK and high lap shear strength (e.g., 9.8 MPa on Al3003 = structural adhesive). It cures at room temperature and has a high elongation of 10%). Two-component polyurethane adhesive (Loctite UK 2073 from Henkel) Expancel 031DU40 (Nouryon, LKJBHK6556) Rubber gasket (d = 1.6 mm) Bonderite M-NT 1455 W wipes (from Henkel).

[0149] Substrate: The electrocoated steel (Rocholl E-COATED STEEL Stahlprüfkörper #50725) has the following dimensions: 100mm x 25mm x 1.8mm. Aluminum 3003 (Al3003, Rocholl Aluminiumprüfkörper #77467) has the following dimensions: 100 mm x 25 mm x 2.0 mm. The manually wrapped aluminum 3003 (Al3003 / PET) in PET adhesive foil has the following dimensions: 100 mm x 25 mm x 2.2 mm. The polypropylene sample PP (InnoTech, PRÜF10106PP) has the following dimensions: 100 mm x 25 mm x 3.0 mm.

[0150] The substrate is pretreated as follows: The substrate was wiped with a piece of paper impregnated with iPrOH and allowed to dry.

[0151] For Al3003, an additional wiping step is performed using a Bonderite M-NT 1455 W wiping cloth to create a good adhesive base for the removable coating.

[0152] The PP substrate was first wiped with a paper sheet impregnated with iPrOH, and then flame-treated with a flame treatment machine at a speed of 48 m / min and a flame distance of 6 cm.

[0153] Al3003 encased in PET was first wiped with paper soaked in iPrOH, and then pretreated with atmospheric plasma at a distance of 16 mm.

[0154] The heat-detachable two-component polyurethane adhesive compositions and comparative examples according to the present invention were prepared according to Tables 1 and 2 below.

[0155] Mix parts A and B in the desired A:B ratio in a speed mixer cup at 1500 rpm for 15 seconds.

[0156] Table 1

[0157] Table 2

[0158] Substrate preparation for lap shear measurement After pretreating the substrate as described above, the substrate is assembled using the following procedure.

[0159] Half of the substrate was bar-coated with the composition according to the invention (Examples 1-6) according to the desired final thickness. The coated substrate was cured in an oven at 60 °C for 2 hours. Once the samples were cured, the resulting coating thickness was between 100 and 200 µm, depending on the experiment.

[0160] Before applying the adhesive, apply 1.6 mm rubber pads on top of the layers of Examples 1-6, with adjacent pads spaced 10 mm apart. This is necessary to provide an adhesive line of uniform thickness.

[0161] Apply the adhesive (LOCTITE TLB9150APS or Loctite UK 2073) between the rubber pads using a manual glue applicator via a static mixer, with a total adhesive line area of ​​2.5 cm x 1 cm.

[0162] Mount the second substrate (uncoated and cleaned) opposite the first substrate containing the adhesive. After removing excess adhesive, clamp it to ensure good adhesion of the adhesive on the top surface.

[0163] After repeating the procedure on all substrates, the substrates were cured in an oven at 60°C for 3 days (Loctite UK2073) and at 60°C for 2 days (LOCTITE TLB9150APS).

[0164] The tensile lap shear strength of LOCTITE TLB9150 ABS combined with the heat-detachable two-component polyurethane adhesive composition according to the present invention on Al3003 The lap shear strength of LOCTITE TLB9150 ABS combined with different thermally removable two-component polyurethane adhesive compositions according to the present invention (Examples 1-6, with an average thickness of 180 µm) was measured before and after debonding (at 100°C for 1 hour). The results are shown in Figure 2 middle.

[0165] The effect of crosslinking density on the lap shear strength before and after debonding was investigated (Examples 1 and 2). The layers in Example 1 and Example 2 differed only in the NCO / OH ratio, which was 1.1 and 0.7, respectively. The NCO / OH ratio (also expressed as crosslinking density) strongly affected the lap tensile shear strength at 23°C (the sample with lower crosslinking density was approximately 3.3 MPa lower), but also affected the debonding efficiency (the sample with higher crosslinking density was approximately 13% lower). Figure 1 As shown.

[0166] The different results can be explained by considering the strength of the debonded adhesive layer. The sample with higher strength (Example 1 layer) did not allow the expandable microspheres to fully expand, resulting in lower debonding efficiency. To improve debonding efficiency, a monofunctional alcohol was added to the formulation to achieve full crosslinking density, but with side-attached polymer chains that help increase the flexibility of the debonded layer. Example 6 showed the most favorable results, maintaining an lap shear strength of approximately 7 MPa at 23°C; however, the debonding efficiency was approximately 86%.

[0167] In addition, the combination of thermally conductive epoxy adhesive (from Henkel) with Example 6 (thickness 212 ± 50 µm) on an Al3003 substrate was tested. Tensile lap shear strength results are shown in... Figure 3 As can be seen from this, the composition according to the present invention is also effective when used in conjunction with thermally conductive epoxy adhesive, and maintains a high debonding efficiency of about 95%.

[0168] The tensile shear strength of LOCTITE TLB9150 ABS combined with the layer combination of Example 6 on Al3003 as a function of temperature The lap shear strength of LOCTITE TLB9150 ABS combined with a layer (thickness 212 ± 50 µm) from Example 6 on Al3003 was measured within a temperature range of -40°C to 100°C. The test results are shown below. Figure 4 From. Figure 4 As can be seen, the thickness of the release layer affects the strength at 23°C. Furthermore, the tensile shear strength decreases to 1.14 MPa above 80°C, possibly due to the weakening strength of both the adhesive and the release layer above these temperatures.

[0169] However, at temperatures above 100°C, a 99% reduction in strength was recorded, which can be explained by the destruction of the adhesive lines caused by the expandable microspheres contained in the release layer.

[0170] The tensile lap shear strength of LOCTITE TLB9150 ABS combined with the composition layer according to the invention on electrocoated steel The lap shear strength of LOCTITE TLB9150 ABS combined with layers from Examples 1-6 was measured to evaluate its effectiveness on electrocoated steel. The results are shown in... Figure 5 As can be seen, the results are very close to those obtained using Al3003, confirming that the composition according to the present invention works well on different metal substrates.

[0171] LOCTITE TLB9150ABS and the tensile lap shear strength of the layer combination of Example 6 on Al3003 / PET-Al3003 and PP The lap shear strength of the LOCTITE TLB9150 ABS combined with the layer of Example 6 was measured to evaluate the effectiveness of the LOCTITE UK 2073 / 2173 layer of Example 6 in the Al3003 / PET encapsulation on a PP substrate. The composition of Example 6 was applied as a rod to the substrate. The results are shown below. Figure 6 and 7 middle.

[0172] The composition of Example 6 exhibited very good adhesion to PET, with the failure rate before debonding actually falling between PET and Al3003. After debonding the substrate at 100°C for 1 hour, the failure rate was recorded in the debonded layer, with a debonding efficiency of almost 96%. The composition of Example 6 also exhibited very good adhesion to PP, with the failure rate before debonding actually falling between PP and Al3003. After debonding the substrate at 100°C for 1 hour, the failure rate was recorded in the debonded layer, with a debonding efficiency of approximately 64%.

[0173] Assessment of temperature propagation in battery cells during debinding For safety reasons, it is important that the temperature of the car battery does not exceed 65°C to avoid dangerous electrolyte leakage. Therefore, it is crucial that the temperature of the battery cells does not exceed 65°C during the cell debonding process. For this reason, an initial debonding test was conducted using an empty battery casing, and the temperature was monitored during the debonding process.

[0174] The device used is shown Figure 8 In the diagram, T1 is the temperature of the heating element, T2 is the temperature of layer 6 (Example 6), T3 is the temperature of the adhesive layer, and T4 is the temperature of the battery cell. The T1 mark at the bottom indicates the heating element used to heat the thermally desiccant two-component polyurethane composition layer and the battery cell. Next is a 1 mm thick aluminum plate on which Formulation 1 layer (marked T2) needs to be applied. On top of Formulation 1 layer is LOCTITE TLB9150ABS (marked T3), with a thickness of 1.6 mm. On top of all components is an aluminum empty battery cell with a thickness of 0.5 mm.

[0175] Figure 9 The development of the battery cell temperature profile during thermal debonding using thermally conductive adhesive (LOCTITE TLB9150ABS) and the layer of Example 6 is shown. It is clearly visible that once the layer of Example 6 expands due to the expansion of the expandable microsphere filler, the temperature of the battery cell casing remains below 65°C, and easy debonding of the battery casing is also achieved.

Claims

1. A heat-release two-component polyurethane adhesive composition, comprising: The first component, the first component comprising Two or more polymeric polyols having an average hydroxyl functionality of at least 1.8, wherein the average hydroxyl functionality is measured according to ASTM D4274; and Thermally expandable thermoplastic microspheres; as well as The second component, the second component includes At least one isocyanate-terminated compound; The first component and the second component are mixed at an OH / NCO equivalent ratio of 1:0.7 to 1:1.

1.

2. The heat-detachable two-component polyurethane adhesive composition according to claim 1, wherein the first component and the second component are mixed in an equivalent ratio of 1:1.

1.

3. The heat-release two-component polyurethane adhesive composition according to claim 1 or 2, wherein the polymeric polyol is selected from polyether polyols, polyester polyols, polybutadiene polyols and mixtures thereof, preferably the polymeric polyol is a mixture of trifunctional polypropylene ether polyol and castor oil.

4. The heat-detachable two-component polyurethane adhesive composition according to claim 1 or 3, wherein the two or more polymeric polyols are present in an amount of 15% to 75% by weight, preferably 28% to 65% by weight, or even more preferably 35% to 58% by weight of the total weight of the first component of the composition.

5. The heat-release two-component polyurethane adhesive composition according to any one of claims 1 to 4, wherein the first component of the composition further comprises at least one monofunctional alcohol, wherein the at least one monofunctional alcohol is preferably selected from methanol, ethanol, propanol, isopropanol, butanol, 2-butanol, isobutanol, pentanol, hexanol, heptanol, octanol, nonanol, 1-decanol, undecylol, dodecanol, tridecanol, tetradecanol, pentadecylol, hexadecylol, heptadecanol, octadecylol, nonadecanol, eicosaneol and mixtures thereof, preferably 1-decanol.

6. The heat-detachable two-component polyurethane adhesive composition according to claim 5, wherein the at least one monofunctional alcohol is present in an amount of 0.5 to 20% by weight, preferably 0.5 to 15%, more preferably 0.6 to 10% of the total weight of the first component of the composition.

7. The thermo-detachable two-component polyurethane adhesive composition according to any one of claims 1 to 6, wherein the thermo-expandable thermoplastic microspheres have a core-shell structure, and wherein the shell is formed of a crosslinked polymer and the core is composed of a foaming agent.

8. The heat-detachable two-component polyurethane adhesive composition according to any one of claims 1 to 7, wherein the heat-expandable thermoplastic microspheres expand when exposed to heat, preferably at 60 to 200°C, more preferably at 80 to 160°C, and even more preferably at 80 to 120°C.

9. The thermo-detachable two-component polyurethane adhesive composition according to any one of claims 1 to 8, wherein the thermo-expandable thermoplastic microspheres have a particle size of 5 to 100 µm, preferably 8 to 75 µm, preferably 9 to 50 µm, more preferably 10 to 30 µm, more preferably 12 to 20 µm, and even more preferably 13 to 19 µm, wherein the particle size is measured by laser diffraction (low-angle laser light scattering LALLS).

10. The thermally detangleable two-component polyurethane adhesive composition according to any one of claims 1 to 9, wherein the thermally expandable thermoplastic microspheres are present in 15 to 50% by weight, preferably 20 to 40% by weight, more preferably 27 to 37% by weight, based on the total weight of the first component of the composition.

11. The heat-detachable two-component polyurethane adhesive composition according to any one of claims 1 to 10, wherein the at least one isocyanate-terminated compound is selected from aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, aromatic polyisocyanates, alicyclic polyisocyanates, aliphatic polyisocyanates, and mixtures thereof, preferably the at least one isocyanate-terminated compound is methylene diphenyl diisocyanate.

12. The heat-detachable two-component polyurethane adhesive composition according to any one of claims 1 to 11, wherein the at least one isocyanate-terminated compound is present at 35 to 70% by weight, preferably 40 to 65%, more preferably 45 to 60%, and even more preferably 48 to 58% based on the total weight of the second component of the composition.

13. Cured heat-detachable two-component polyurethane composition according to any one of claims 1 to 12.

14. Use of the heat-debonded two-component polyurethane composition according to any one of claims 1 to 12 or the cured product according to claim 13 in an adhesive structure.

15. An adhesive structure comprising: First substrate; Second substrate; The heat-removable two-component polyurethane composition layer according to any one of claims 1 to 12 or the cured product layer according to claim 13; as well as Adhesive layer, The heat-detachable two-component polyurethane composition is disposed on the surface of the first substrate and / or the surface of the second substrate, and the adhesive layer is disposed on top of the heat-detachable two-component polyurethane composition layer, wherein the adhesive layer is preferably formed of an adhesive selected from the following: epoxy adhesives, acrylic adhesives, polyurethane adhesives, cyanoacrylate adhesives, silicone adhesives, polyimide adhesives, silane-modified polymers, butyl rubber, hot melt adhesives, and mixtures thereof.

16. A method for debonding the adhesive structure according to claim 15, the method comprising the following steps: i) Apply heat; as well as, ii) Debonding the surface, The temperature applied in step i) is preferably 60 to 200°C, and the duration of application is preferably 15 seconds to 60 minutes.

Citation Information

Patent Citations

  • A curable composition