polymer composition

By mixing and annealing the polymer composition PC0, the problem of reduced flame retardancy and mechanical properties of flame retardant polymer compounds during recycling was solved, thus upgrading the recycled products and achieving improved mechanical properties and flame retardancy.

CN123076633APending Publication Date: 2026-11-10BASF SE
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580028182.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-12-02
Filing Date
2025-04-11
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In typical mechanical recycling processes, the flame retardancy and mechanical properties of flame-retardant polymer compounds decrease, leading to a decline in the quality of recycled products.

Method used

By providing a polymer composition PC0 comprising polymer PC0-P1 and additive PC0-A1, and mixing and annealing it in a mixture M1, optimizing the mixing time and temperature, and processing it using a twin-screw extruder, flame retardancy and mechanical properties are improved.

Benefits of technology

It improves the mechanical properties and flame retardancy of recycled products, increases the recycling content, and improves combustion behavior.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The polymer compositions described herein are specific polymer compositions PC1 and polymer products PP1, as well as their specific manufacturing methods.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This document discloses (specific) methods for producing polymer compositions or polymer products, (specific) mixtures for producing polymer compositions, and (specific) polymer compositions and products.

[0002] Flame-retardant polymer compounds with improved mechanical properties, such as flame-retardant polyamides, are widely used in a variety of applications. Furthermore, and importantly, these polymer compounds have high recycling content. However, during typical mechanical recycling processes, the flame retardancy and mechanical properties of these polymer compounds decrease, resulting in downgraded recycled products.

[0003] Therefore, the object of the present invention is to provide a recycling method that exhibits at least one of the following: -Products that are upgraded and recycled -Increase the amount of recycled material - Improve mechanical properties - Improve flame retardancy, and / or - Improve combustion behavior.

[0004] This objective is at least partially achieved by a method comprising the following steps: i) Provide a polymer composition PC0, The polymer composition PC0 comprises, and preferably consists of, the following substances: a) One or more polymers PC0-P1, and b) One or more additives PC0-A1; ii) Mix and anneal the mixture M1 to obtain the polymer composition PC1. The mixture M1 contains, and preferably consists of, the following substances: a) Polymer composition PC0, b) Preferably one or more polymers M1-P1.

[0005] In a preferred embodiment, the method includes (additional) steps: iii) Convert the polymer composition PC1 to obtain the polymer product PP1.

[0006] The objective is also at least partially achieved by a method comprising the following steps: iii) Convert the polymer composition PC1 that can be obtained by the methods described herein or the chemical material that can be obtained by the methods described herein or the chemical material that can be obtained by the methods described herein to obtain product PRF1.

[0007] In a preferred embodiment, step ii) is performed in an extruder, preferably a twin-screw extruder. Therefore, the mechanical properties are improved.

[0008] In a preferred embodiment, the mixture M1 is mixed in step ii) for 5 seconds or longer, preferably 10 seconds or longer, more preferably 20 seconds or longer, more preferably 30 seconds or longer, more preferably 45 seconds or longer, more preferably 60 seconds or longer, more preferably 120 seconds or longer, more preferably 180 seconds or longer, more preferably 240 seconds or longer, and / or the mixture M1 is mixed in step ii) for 15 minutes or less, preferably 10 minutes or less, more preferably 5 minutes or less, more preferably 240 seconds or less, more preferably 180 seconds or less, more preferably 120 seconds or less, more preferably 100 seconds or less, more preferably 80 seconds or less, more preferably 60 seconds or less, more preferably 45 seconds or less. Therefore, flame retardancy and mechanical properties are improved.

[0009] In a preferred embodiment, the mixture M1 is annealed in step ii) to 140°C or higher, preferably 160°C or higher, more preferably 170°C or higher, more preferably 180°C or higher, more preferably 190°C or higher, more preferably 200°C or higher, more preferably 210°C or higher, more preferably 220°C or higher, more preferably 230°C or higher, more preferably 240°C or higher, more preferably 250°C or higher, more preferably 260°C or higher, more preferably 270°C or higher, more preferably 280°C or higher, more preferably 290°C or higher, more preferably 300°C or higher, and / or the mixture M1 is annealed in step ii) to 500°C or lower, preferably 400°C or lower, more preferably 300°C or lower, more preferably 280°C or lower, more preferably 260°C or lower, more preferably 240°C or lower, more preferably 220°C or lower, more preferably 200°C or lower. Therefore, flame retardancy and mechanical properties are improved.

[0010] In a preferred embodiment, the mixture M1 is annealed in step ii) to (Tm of a polymer composition PC0 or PC1, in °C) or higher, preferably (Tm of a polymer composition PC0 or PC1, in °C) +10 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +20 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +30 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +40 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +60 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +80 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +80 °C or higher. The mixture M1 is annealed in step ii) to (Tm of a polymer composition PC0 or PC1, in °C) + 100 °C or higher, preferably (Tm of a polymer composition PC0 or PC1, in °C) + 200 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) + 150 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) + 100 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) + 80 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) + 60 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) + 40 °C or lower, and more preferably (Tm of a polymer composition PC0 or PC1, in °C) + 20 °C or lower. Therefore, flame retardancy and mechanical properties are improved.

[0011] In a preferred embodiment, the throughput in step ii) is 0.5 kg / h or greater and 25,000 kg / h or less, preferably 1 kg / h or greater and 10,000 kg / h or less, more preferably 5 kg / h or greater and 5,000 kg / h or less, more preferably 10 kg / h or greater and 2,500 kg / h or less, more preferably 13 kg / h or greater and 1,000 kg / h or less, more preferably 16 kg / h or greater and 500 kg / h or less, and more preferably 19 kg / h or greater and 300 kg / h or less. Therefore, flame retardancy and mechanical properties are improved.

[0012] In a preferred embodiment, the method is a method for producing a polymer composition, preferably polymer composition PC1 and / or a polymer product, preferably polymer product PP1.

[0013] Furthermore, the above-mentioned objective is at least partially achieved by using mixture M1 in the production of polymer composition PC1. The mixture M1 contains, and preferably consists of, the following substances: a) Polymer composition PC0, and b) Preferably one or more polymers M1-P1; and The polymer composition PC0 comprises, and preferably consists of, the following substances: a) One or more polymers PC0-P1, and b) One or more additives PC0-A1; and Preferably, the polymer composition PC1 comprises, and more preferably consists of, the following substances: a) One or more polymers PC1-P1, and b) One or more additives PC1-A1.

[0014] In a preferred embodiment, one or more additives PC0-A1 comprise one or more reinforcing agents PC0-R1, preferably consisting of one or more reinforcing agents PC0-R1. Therefore, mechanical properties are improved.

[0015] In a preferred embodiment, mixture M1 comprises one or more additives M1-A1, preferably wherein one or more additives M1-A1 and one or more additives PC0-A1 are not the same. This means that some types of one or more additives in PC0 and M1 may be the same; however, at least one type of one or more additives is different. In PC0 and M1, the amounts of one or more additives may be the same or different, and preferably, they are different.

[0016] In a preferred embodiment, mixture M1 comprises one or more additives M1-A1, preferably wherein the one or more additives M1-A1 comprise one or more reinforcing agents M1-R1, preferably consisting of one or more reinforcing agents M1-R1, and / or one or more additives PC1-A1 comprise one or more reinforcing agents PC1-R1, preferably consisting of one or more reinforcing agents PC1-R1. Therefore, mechanical properties are improved.

[0017] In a preferred embodiment, one or more additives PC0-A1 comprise one or more reinforcing compounds PC0-R1, preferably consisting of one or more reinforcing compounds PC0-R1, and / or mixture M1 comprises one or more additives M1-A1, wherein the one or more additives M1-A1 comprise one or more reinforcing compounds M1-R1, preferably consisting of one or more reinforcing compounds M1-R1. Therefore, mechanical properties are improved.

[0018] In a preferred embodiment, one or more reinforcements PC0-R1, M1-R1, and / or PC1-R1 are made of glass. More preferably, one or more reinforcements M1-R1, PC0-R1, and / or PC1-R1 comprise glass fibers M1-GF1, PC0-GF1, and / or PC1-GF1, preferably composed of glass fibers M1-GF1, PC0-GF1, and / or PC1-GF1. Alternatively, one or more reinforcements PC0-R1, M1-R1, and / or PC1-R1 comprise, preferably composed of, fibers or beads, more preferably fibers, and even more preferably glass fibers M1-GF1, PC0-GF1, and / or PC1-GF1. Therefore, the mechanical properties are improved. The inventors recognized that, surprisingly, if the polymer composition PC0 contains one or more reinforcing members PC0-R1, preferably one or more of the reinforcing members PC0-R1 being made of glass, more preferably one or more of the reinforcing members PC0-R1 containing glass fiber PC0-GF1, preferably composed of glass fiber PC0-GF1, the mechanical properties of the polymer composition PC1, especially the elongation at break, are improved.

[0019] In a preferred embodiment, the length L of one or more reinforcements PC0-R1 is... arit The length L is 20µm or greater, preferably 30µm or greater, more preferably 40µm or greater, more preferably 50µm or greater, more preferably 60µm or greater, more preferably 70µm or greater, more preferably 80µm or greater, more preferably 90µm or greater, more preferably 100µm or greater, more preferably 110µm or greater, more preferably 120µm or greater, more preferably 130µm or greater, more preferably 140µm or greater, and / or the length L of one or more reinforcements PC0-R1 arit The micrometer diameter is 1000µm or less, preferably 750µm or less, more preferably 500µm or less, more preferably 250µm or less, more preferably 225µm or less, more preferably 200µm or less, more preferably 180µm or less, more preferably 170µm or less, more preferably 160µm or less, more preferably 150µm or less, and more preferably 140µm or less. Therefore, the mechanical properties and flame-retardant properties are improved.

[0020] In a preferred embodiment, the thickness T of one or more reinforcements PC0-R1 aritThe thickness is 1µm or greater and 40µm or less, preferably 3µm or greater and 35µm or less, more preferably 5µm or greater and 30µm or less, more preferably 6µm or greater and 25µm or less, more preferably 7µm or greater and 20µm or less, more preferably 8µm or greater and 15µm or less, more preferably 9µm or greater and 12µm or less, and more preferably about 10µm. Therefore, the mechanical properties and flame-retardant properties are improved.

[0021] In a preferred embodiment, the length L of one or more reinforcements PC0-R1 arit With one or more reinforcements PC0-R1, the thickness T arit The ratio [µm / µm] is 1 or greater and 1000 or less, preferably 2 or greater and 500 or less, more preferably 4 or greater and 250 or less, more preferably 6 or greater and 100 or less, more preferably 8 or greater and 50 or less, more preferably 10 or greater and 25 or less, more preferably 12 or greater and 20 or less, more preferably 13 or greater and 15 or less, and more preferably about 14. Therefore, the mechanical properties and flame-retardant properties are improved.

[0022] In a preferred embodiment, the length L of one or more reinforcements M1-R1 arit The length L is 20µm or greater, preferably 100µm or greater, more preferably 250µm or greater, more preferably 500µm or greater, more preferably 1000µm or greater, more preferably 2000µm or greater, more preferably 3000µm or greater, more preferably 4000µm or greater, and / or the length L of one or more reinforcements M1-R1 arit The micrometer diameter is 1 cm or less, preferably 9000 µm or less, more preferably 7500 µm or less, more preferably 6000 µm or less, more preferably 5000 µm or less, more preferably 4000 µm or less, more preferably 3000 µm or less, more preferably 2000 µm or less, more preferably 1000 µm or less, more preferably 500 µm or less, and more preferably 250 µm or less. Therefore, the mechanical properties and flame-retardant properties are improved.

[0023] In a preferred embodiment, the thickness T of one or more reinforcements M1-R1 arit The thickness is 1µm or greater and 40µm or less, preferably 3µm or greater and 35µm or less, more preferably 5µm or greater and 30µm or less, more preferably 6µm or greater and 25µm or less, more preferably 7µm or greater and 20µm or less, more preferably 8µm or greater and 15µm or less, more preferably 9µm or greater and 12µm or less, and more preferably about 10µm. Therefore, the mechanical properties and flame-retardant properties are improved.

[0024] In a preferred embodiment, the length L of one or more reinforcements M1-R1 arit With the thickness T of one or more reinforcements M1-R1 arit The ratio [µm / µm] is 1 or greater and 10000 or less, preferably 50 or greater and 5000 or less, more preferably 75 or greater and 2500 or less, more preferably 100 or greater and 1000 or less, more preferably 200 or greater and 700 or less, more preferably 250 or greater and 600 or less, more preferably 300 or greater and 500 or less, more preferably 350 or greater and 450 or less, more preferably about 400. Therefore, mechanical properties and flame-retardant properties are improved.

[0025] In a preferred embodiment, the length L of one or more reinforcements PC1-R1 is... arit The length L is 20µm or greater, preferably 30µm or greater, more preferably 40µm or greater, more preferably 50µm or greater, more preferably 60µm or greater, more preferably 70µm or greater, more preferably 80µm or greater, more preferably 90µm or greater, more preferably 100µm or greater, more preferably 110µm or greater, more preferably 115µm or greater, and / or the length L of one or more reinforcements PC1-R1 arit The thickness is 1000µm or less, preferably 750µm or less, more preferably 500µm or less, more preferably 250µm or less, more preferably 225µm or less, more preferably 200µm or less, more preferably 180µm or less, more preferably 170µm or less, more preferably 160µm or less, more preferably 150µm or less, more preferably 140µm or less, more preferably 130µm or less, more preferably 120µm or less, and more preferably about 118µm. Therefore, mechanical properties and flame-retardant properties are improved.

[0026] In a preferred embodiment, the thickness T of one or more reinforcements PC1-R1 arit The thickness is 1µm or greater and 40µm or less, preferably 3µm or greater and 35µm or less, more preferably 5µm or greater and 30µm or less, more preferably 6µm or greater and 25µm or less, more preferably 7µm or greater and 20µm or less, more preferably 8µm or greater and 15µm or less, more preferably 9µm or greater and 12µm or less, and more preferably about 10µm. Therefore, the mechanical properties and flame-retardant properties are improved.

[0027] In a preferred embodiment, the length L of one or more reinforcements PC1-R1 is... arit With one or more reinforcements PC1-R1, the thickness T aritThe ratio [µm / µm] is 1 or greater and 1000 or less, preferably 2 or greater and 500 or less, more preferably 4 or greater and 250 or less, more preferably 6 or greater and 100 or less, more preferably 8 or greater and 50 or less, more preferably 9 or greater and 20 or less, more preferably 10 or greater and 15 or less, more preferably 11 or greater and 13 or less, and more preferably about 12. Therefore, the mechanical properties and flame-retardant properties are improved.

[0028] In a preferred embodiment, one or more additives PC0-A1 comprise one or more reinforcing members PC0-R1, preferably consisting of one or more reinforcing members PC0-R1, and one or more additives PC1-A1 comprise one or more reinforcing members PC1-R1, preferably consisting of one or more reinforcing members PC1-R1, and the length L of the one or more reinforcing members PC1-R1 is... arit With the length L of one or more reinforcements PC0-R1 arit The ratio [µm / µm] is 0.50 to 1.00, preferably 0.60 to 0.95, more preferably 0.70 to 0.92, more preferably 0.80 to 0.90, and even more preferably 0.82 to 0.88. Therefore, mechanical properties and flame-retardant properties are improved.

[0029] In a preferred embodiment, one or more additives PC0-A1 comprise one or more reinforcing members PC0-R1, preferably consisting of one or more reinforcing members PC0-R1, and the length L of the one or more reinforcing members PC0-R1 is... arit With one or more reinforcements PC1-R1, the length L arit The ratio [µm / µm] is 1.00 or greater and 100.00 or less, preferably 1.05 or greater and 25.0 or less, more preferably 1.08 or greater and 20.0 or less, more preferably 1.10 or greater and 10.0 or less, more preferably 1.15 or greater and 5.0 or less, and more preferably 1.18 or greater and 2.0 or less.

[0030] In a preferred embodiment, one or more additives PC0-A1 comprise one or more flame retardants PC0-FR1, preferably composed of one or more flame retardants PC0-FR1, and preferably wherein one or more additives PC0-A1 comprise one or more flame retardants PC0-FR1 and one or more reinforcing agents PC0-R1, preferably composed of one or more flame retardants PC0-FR1 and one or more reinforcing agents PC0-R1. Therefore, the flame retardant properties are improved.

[0031] In a preferred embodiment, one or more additives PC0-A1 do not contain one or more flame retardants PC0-FR1 and / or one or more reinforcing agents PC0-R1.

[0032] In a preferred embodiment, the mixture M1 comprises one or more additives M1-A1, preferably comprising one or more flame retardants M1-FR1, more preferably composed of one or more flame retardants M1-FR1, and more preferably comprising one or more flame retardants M1-FR1 and one or more reinforcing agents M1-R1, preferably composed of one or more flame retardants M1-FR1 and one or more reinforcing agents M1-R1. Therefore, mechanical and flame-retardant properties are improved.

[0033] In a preferred embodiment, one or more additives M1-A1 do not contain one or more flame retardants M1-FR1 and / or one or more reinforcing agents M1-R1.

[0034] In a preferred embodiment, one or more additives PC1-A1 comprise one or more flame retardants PC1-FR1, preferably consisting of one or more flame retardants PC1-FR1. Therefore, flame retardant properties are improved.

[0035] In a preferred embodiment, one or more flame retardants M1-FR1, PC0-FR1, and / or PC1-FR1 comprise, preferably, a flame retardant containing H, O, N, and C, more preferably a complex containing cyanuric acid, and even more preferably melamine cyanurate. Therefore, flame retardant properties are improved. The inventors have recognized that, surprisingly, flame retardant properties are improved if the polymer composition PC0 comprises one or more reinforcing agents PC0-R1, preferably glass fiber, and the polymer composition PC1 comprises one or more flame retardants PC1-FR1, preferably a flame retardant containing H, O, N, and C, more preferably a complex containing cyanuric acid, and even more preferably melamine cyanurate. Therefore, upgraded recycled products with enhanced recycling content can be obtained.

[0036] In a preferred embodiment, one or more additives PC0-A1 comprise one or more flame retardants PC0-FR1, preferably consisting of one or more flame retardants PC0-FR1, and / or mixture M1 comprises one or more additives M1-A1, wherein one or more additives M1-A1 comprise one or more flame retardants M1-FR1, preferably consisting of one or more flame retardants M1-FR1. Therefore, flame retardant properties are improved.

[0037] In a preferred embodiment, one or more polymers PC0-P1, M1-P1, and / or PC1-P1 comprise, and preferably consist of, a thermoplastic polymer, preferably thermoplastic polyurethane and / or polyamide, more preferably PA6 and / or PA66, even more preferably PA6. Therefore, mechanical properties and flame-retardant properties are improved.

[0038] In a preferred embodiment, one or more polymers PC0-P1, M1-P1, and / or PC1-P1 are substantially the same, preferably identical. Therefore, mechanical properties are improved. In this document, the term "substantial" preferably means 50% by weight or more.

[0039] In a preferred embodiment, the mixture M1 comprises one or more polymers M1-P1. Therefore, mechanical and flame-retardant properties are improved.

[0040] In a preferred embodiment, mixture M1 comprises, and preferably consists of, the following substances by weight percent: a) 5 to 95, preferably 20 to 70, polymer composition PC0, b) 0 to 95, preferably 5 to 40, one or more polymers M1-P1 c) 0 to 50, preferably 0.1 to 30, one or more reinforcing agents M1-R1, d) 0 to 35, preferably 3 to 25, one or more flame retardants M1-FR1, and e) 0 to 20, preferably 0.1 to 15, one or more additives A2.

[0041] Therefore, mechanical properties and combustion behavior are improved.

[0042] In a preferred embodiment, the ratio [weight % / weight %] of the polymer composition PC0 to one or more polymers M1-P1 is 0.5 or greater and 40.0 or less, preferably 1.0 or greater and 20.0 or less, more preferably 1.5 or greater and 10.0 or less, more preferably 2.0 or greater and 5.0 or less, and more preferably 2.5 or greater and 3.5. Therefore, mechanical properties and flame-retardant properties are improved.

[0043] In a preferred embodiment, the polymer composition PC0 is at least partially waste or obtained from waste, preferably wherein the waste is post-consumer waste and / or post-industrial waste.

[0044] In a preferred embodiment, the lifespan of the polymer composition PC0 is one day or longer, preferably one week or longer, more preferably one year or longer; and / or the lifespan of the polymer composition PC0 is 100 years or less, preferably 50 years or less, more preferably 25 years or less. Therefore, the recycling content is enhanced.

[0045] In a preferred embodiment, the polymer composition PC0 comprises, and preferably consists of, the following substances: a) 20 to 90, preferably 30 to 80, one or more polymers PC0-P1, and b) 5 to 50, preferably 10 to 35, one or more reinforcing agents PC0-R1, c) 0 to 20, preferably 1 to 10, one or more flame retardants PC0-FR1, and d) 0 to 20, preferably 0.1 to 10, one or more additives A2.

[0046] Therefore, mechanical properties and combustion behavior are improved, and the recycling content is enhanced.

[0047] In a preferred embodiment, the polymer composition PC1 comprises, and preferably consists of, the following substances: a) 20 to 90, preferably 30 to 80, one or more polymers PC1-P1, and b) 5 to 50, preferably 10 to 35, one or more reinforcing agents PC1-R1, c) 0 to 20, preferably 3 to 15, one or more flame retardants PC1-FR1, and d) 0 to 20, preferably 0.1 to 10, one or more additives A2.

[0048] Therefore, mechanical properties and combustion behavior are improved, and the recycling content is enhanced.

[0049] Unless otherwise specified, polymer compositions PC0, PC1, and / or mixture M1 may contain additional additives. Preferably, polymer compositions PC0, PC1, and / or mixture M1 contain one or more additives A2, wherein the one or more additives A2 are selected from antioxidants, stabilizers, lubricants, minerals, chain extenders, impact modifiers, colorants, pigments, soot, talc, and mixtures thereof.

[0050] In a preferred embodiment, the tensile modulus of the polymer composition PC1 is 1000 MPa or higher and 10000 MPa or lower, preferably 4000 MPa or higher and 8000 MPa or lower, more preferably 4000 MPa or higher and 7500 MPa or lower, more preferably 5000 MPa or higher and 7000 MPa or lower, more preferably 5500 MPa or higher and 6750 MPa or lower, more preferably 6000 MPa or higher and 6500 MPa or lower, more preferably 6100 MPa or higher and 6250 MPa or lower, and more preferably 6120 MPa or higher and 6150 MPa or lower. Meeting these parameters improves mechanical and flame-retardant properties and enhances the recycling content.

[0051] In a preferred embodiment, the tensile stress at break of the polymer composition PC1 is 10 MPa or higher and 1000 MPa or lower, preferably 25 MPa or higher and 500 MPa or lower, more preferably 50 MPa or higher and 250 MPa or lower, more preferably 60 MPa or higher and 200 MPa or lower, more preferably 70 MPa or higher and 150 MPa or lower, more preferably 80 MPa or higher and 125 MPa or lower, more preferably 90 MPa or higher and 110 MPa or lower, and more preferably 95 MPa or higher and 100 MPa or lower. If these parameters are met, the mechanical and flame-retardant properties are improved, and the recycling content is enhanced.

[0052] In a preferred embodiment, the elongation at break of the polymer composition PC1 is 1.1% or higher and 10.0% or lower, preferably 2.0% or higher and 9.0% or lower, more preferably 3.0% or higher and 7.0% or lower, more preferably 3.5% or higher and 6.0% or lower, more preferably 3.8% or higher and 5.2% or lower, more preferably 4.1% or higher and 4.9% or lower, more preferably 4.2% or higher and 4.7% or lower, and more preferably 4.3% or higher and 4.5% or lower. Meeting these parameters improves mechanical and flame-retardant properties and enhances the recycling content.

[0053] In a preferred embodiment, the polymer composition PC1 has an impact resistance of 10 kJ / m. 2 Or even greater and 100kJ / m 2 Or even lower, preferably 20 kJ / m 2 Or larger and 75kJ / m 2 Or less, more preferably 30 kJ / m 2 Or even greater and 50kJ / m 2 Or less, more preferably 35 kJ / m 2 Or even greater and 48kJ / m 2Or less, more preferably 40 kJ / m 2 Or even greater and 44kJ / m 2 Or even less. If this parameter is met, mechanical and flame-retardant properties are improved, and the recycling content is enhanced.

[0054] In a preferred embodiment, the notched impact resistance of the polymer composition PC1 is 1.0 kJ / m. 2 Or larger and 20kJ / m 2 Or even smaller, preferably 2.0 kJ / m 2 Or larger and 10 kJ / m 2 Or less, more preferably 2.5 kJ / m 2 Or even greater and 8kJ / m 2 Or smaller, more preferably 3.0 kJ / m 2 Or larger and 6kJ / m 2 Or less, more preferably 3.5 kJ / m 2 Or larger and 4kJ / m 2 Or even less. If this parameter is met, mechanical and flame-retardant properties are improved, and the recycling content is enhanced.

[0055] In a preferred embodiment, the polymer composition PC1 exhibits a value of V-2, preferably V-1, and more preferably V-0 in the UL94 V test. Meeting this parameter improves flame retardant properties and combustion behavior.

[0056] In a preferred embodiment, the polymer composition PC1 exhibits a total afterflame time of 2 seconds or longer and 100 seconds or shorter, preferably 5 seconds or longer and 80 seconds or shorter, more preferably 10 seconds or longer and 60 seconds or shorter, more preferably 15 seconds or longer and 40 seconds or shorter, more preferably 18 seconds or longer and 30 seconds or shorter, and more preferably 20 seconds or longer and 25 seconds or shorter. If these parameters are met, the flame retardant properties and combustion behavior are improved.

[0057] In a preferred embodiment, the polymer composition PC1 passed the GWFI test. Meeting this parameter improves flame retardant properties and combustion behavior.

[0058] Furthermore, the above-mentioned objectives are at least partially achieved by a polymer composition PC1 that can be obtained by the methods described herein or obtained by the methods described herein.

[0059] Furthermore, the above objectives are at least partially achieved by polymer product PP1 that can be obtained by the methods described herein.

[0060] In a preferred embodiment, polymer composition PC0, polymer composition PC1, and / or polymer product PP1 are either or a component of the following: - Automotive parts; preferably cylinder head covers, engine hoods, turbocharger housings, coatings, covers, elevator load-bearing components, foils, fibers, films, foams, damping elements, machine drive belts, turbocharger baffles, intake pipes, intake manifolds, connectors, gaskets, drive pulleys, fan pulleys, coolant tanks, hoses, housings, heat exchanger housing components, coolant coolers, turbocharger coolers, laminates, shoe midsoles, vehicle linings, thermoplastic modifiers, molding bodies, roofs or floors of buildings or vehicles, nonwoven fabrics, packaging materials, passenger conveyors, passenger transport... Handrails, profiles, rollers, rope arrangements, saddles, shoe soles, belts, thermostats, water pumps, radiators, fasteners, battery system components for electric vehicles, dashboards, cushions, steering column switches, seats, headrests, center consoles, transmission components, door modules, A, B, C, or D pillar trim panels, spoilers, door handles, exterior mirrors, windshield wipers, windshield wiper housings, wiper blades, decorative grilles, trim strips, roof rails, window frames, sunroof frames, antenna panels, headlights and taillights, hoods, cylinder head covers, intake manifolds, airbags, steering wheels, cushioning pads, or coatings; - Fabric; preferably shirts, trousers, sweaters, boots, shoes, shoe soles, tights or jackets; - Electrical components; preferably electrical or electronic passive or active components, cables, cable connectors, cable sheaths for mobile phones, circuit breakers, circuit boards, printed circuit boards, terminals, housing components, foil, wires, switches, switching devices, plugs, sockets, distributors, relays, resistors, capacitors, inductors, spools, lamps, diodes, LEDs, transistors, connectors, voltage regulators, integrated circuits (ICs), processors, controllers, memory, sensors, microswitches, microbuttons, semiconductors, reflector housings for light-emitting diodes (LEDs), fasteners for electrical or electronic components, solar modules, gaskets, bolts, strips, slide-in guides, screws, nuts, televisions, drag cables, membrane hinges, spring hooks (snap-on) or spring tongues; - Consumer goods, agricultural products, or pharmaceutical products; preferably tennis ropes, climbing ropes, bristles, brushes, artificial turf, 3D printing filaments, lawnmowers, zippers, Velcro, fabrics for papermaking machines, extrusion coatings, fishing lines, fishing nets, marine ropes, vials, syringes, ampoules, bottles, and bags; preferably organic waste bags, vegetable or fruit bags; sliding elements, spindle nuts, chain conveyors, sliding bearings, rollers, wheels, gears, ring gears, screws and spring dampers, hoses, pipes, cable sheaths, sockets, switches, cable ties, fan wheels, carpets, nonwovens, cosmetic boxes or bottles, mattresses, cushions, insulation, refrigerators, freezers, hot and cold food warmers, water heaters, hot water storage tanks, pipes, insulation boards, insulation panels, detergents, dishwasher tablets or powders, shampoos, shower gels, soaps, fertilizers, covers, fungicides, or insecticides; - Packaging; preferably packaging for the food industry; preferably blown or cast film, more preferably single or multi-layer blown film or single or multi-layer cast film; axially stretched film, preferably biaxial or multiaxial film, or laminated film; a molded article; preferably injection molded article, more preferably coffee capsule; thermoformed article; preferably coffee capsule; or - Building components; preferably rotor blades, insulation materials; preferably sound insulation or heat insulation materials; frames, shells, walls, coatings, facades, windows, doors or partitions.

[0061] In a preferred embodiment, the content of polymer composition PC0 in polymer composition PC1 and / or mixture M1 and / or polymer product PP1 is 1% by weight or more, preferably 2% by weight or more, more preferably 5% by weight or more, more preferably 15% by weight or more, more preferably 30% by weight or more, more preferably 40% by weight or more, more preferably 60% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more, more preferably 95% by weight or more; and / or the content of polymer composition PC0 in polymer composition PC1 and / or mixture M1 and / or polymer product PP1 is 100% by weight or less, preferably 95% by weight or less, more preferably 90% by weight or less, more preferably 50% by weight or less, more preferably 25% by weight or less, more preferably 10% by weight or less; and preferably the content is determined based on identity preservation and / or segregation and / or quality balance and / or book and claims custody model, preferably based on quality balance, preferably based on the International Sustainability and Carbon Certification (ISCC) standard.

[0062] In a preferred embodiment, the polymer composition PC1 and / or polymer product PP1 exhibit enhanced recycling content, improved mechanical properties, and / or improved flame retardancy; and / or the method and / or application produce upgraded recycled products.

[0063] In a preferred embodiment, the polymer composition PC1 comprises, and preferably consists of, the following substances: a) One or more polymers PC1-P1, and b) One or more additives PC1-A1.

[0064] In a preferred embodiment, the content of one or more additives PC0-A1 (preferably one or more flame retardants PC0-FR1 and / or one or more reinforcing agents PC0-R1, more preferably one or more flame retardants PC0-FR1, more preferably melamine cyanurate) in the polymer composition PC0 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 2% by weight or more, more preferably 3% by weight or more, more preferably 4% by weight or more, more preferably 5% by weight or more, more preferably 6% by weight or more, more preferably 7% by weight or more, more preferably 8% by weight or more, more preferably 9% by weight or more, more preferably 10% by weight or more, more preferably 11% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 30% by weight or more. Therefore, the mechanical properties and combustion behavior are improved.

[0065] In a preferred embodiment, the content of one or more additives PC0-A1 (preferably one or more flame retardants PC0-FR1 and / or one or more reinforcing agents PC0-R1, more preferably one or more flame retardants PC0-FR1, more preferably melamine cyanurate) in the polymer composition PC0 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, more preferably 5% by weight or less. Therefore, the mechanical properties and combustion behavior are improved.

[0066] In a preferred embodiment, the content of one or more additives M1-A1 (preferably one or more flame retardants M1-FR1 and / or one or more reinforcing agents M1-R1, more preferably one or more flame retardants M1-FR1, more preferably melamine cyanurate) in mixture M1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 2% by weight or more, more preferably 3% by weight or more, more preferably 4% by weight or more, more preferably 5% by weight or more, more preferably 6% by weight or more, more preferably 7% by weight or more, more preferably 8% by weight or more, more preferably 9% by weight or more, more preferably 10% by weight or more, more preferably 11% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 30% by weight or more. Therefore, the mechanical properties and combustion behavior are improved.

[0067] In a preferred embodiment, the content of one or more additives M1-A1 (preferably one or more flame retardants M1-FR1 and / or one or more reinforcing agents M1-R1, more preferably one or more flame retardants M1-FR1, more preferably melamine cyanurate) in mixture M1 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, more preferably 5% by weight or less. Therefore, mechanical properties and combustion behavior are improved.

[0068] In a preferred embodiment, the content of one or more additives PC1-A1 (preferably one or more flame retardants PC1-FR1 and / or one or more reinforcing agents PC1-R1, more preferably one or more flame retardants PC1-FR1, more preferably melamine cyanurate) in the polymer composition PC1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 2% by weight or more, more preferably 3% by weight or more, more preferably 4% by weight or more, more preferably 5% by weight or more, more preferably 6% by weight or more, more preferably 7% by weight or more, more preferably 8% by weight or more, more preferably 9% by weight or more, more preferably 10% by weight or more, more preferably 11% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 30% by weight or more. Therefore, the mechanical properties and combustion behavior are improved.

[0069] In a preferred embodiment, the content of one or more additives PC1-A1 (preferably one or more flame retardants PC1-FR1 and / or one or more reinforcing agents PC1-R1, more preferably one or more flame retardants PC1-FR1, more preferably melamine cyanurate) in the polymer composition PC1 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, more preferably 5% by weight or less. Therefore, mechanical properties and combustion behavior are improved.

[0070] In a preferred embodiment, the content of one or more additives PC0-A1 (preferably one or more reinforcing agents PC0-R1, more preferably glass fiber PC0-GF1) in the polymer composition PC0 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 8% by weight or more, more preferably 10% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 25% by weight or more, more preferably 30% by weight or more, more preferably 35% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more. Therefore, mechanical properties and combustion behavior are improved.

[0071] In a preferred embodiment, the content of one or more additives PC0-A1 (preferably one or more reinforcing agents PC0-R1, more preferably glass fiber PC0-GF1) in the polymer composition PC0 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, more preferably 5% by weight or less. Therefore, mechanical properties and combustion behavior are improved.

[0072] In a preferred embodiment, the content of one or more additives M1-A1 (preferably one or more reinforcing materials M1-R1, more preferably glass fiber M1-GF1) in mixture M1 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, more preferably 5% by weight or less. Therefore, mechanical properties and combustion behavior are improved.

[0073] In a preferred embodiment, the content of one or more additives M1-A1 (preferably one or more reinforcing materials M1-R1, more preferably glass fiber M1-GF1) in mixture M1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 8% by weight or more, more preferably 10% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 25% by weight or more, more preferably 30% by weight or more, more preferably 35% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more. Therefore, mechanical properties and combustion behavior are improved.

[0074] In a preferred embodiment, the content of one or more additives PC1-A1 (preferably one or more reinforcing agents PC1-R1, more preferably glass fiber PC1-GF1) in the polymer composition PC1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 8% by weight or more, more preferably 10% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 25% by weight or more, more preferably 30% by weight or more, more preferably 35% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more. Therefore, mechanical properties and combustion behavior are improved.

[0075] In a preferred embodiment, the content of one or more additives PC1-A1 (preferably one or more reinforcing agents PC1-R1, more preferably glass fiber PC1-GF1) in the polymer composition PC1 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, more preferably 5% by weight or less. Therefore, mechanical properties and combustion behavior are improved.

[0076] In a preferred embodiment, the content of one or more polymers PC0-P1 in the polymer composition PC0 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 10% by weight or more, more preferably 20% by weight or more, more preferably 30% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, and more preferably 90% by weight or more. Therefore, mechanical properties and combustion behavior are improved, and the recycling content is enhanced.

[0077] In a preferred embodiment, the content of one or more polymers PC0-P1 in the polymer composition PC0 is 99% by weight or less, preferably 95% by weight or less, more preferably 90% by weight or less, more preferably 80% by weight or less, more preferably 70% by weight or less, more preferably 60% by weight or less, more preferably 50% by weight or less, more preferably 40% by weight or less, more preferably 30% by weight or less, and more preferably 20% by weight or less. Therefore, mechanical properties and combustion behavior are improved, and the recycling content is enhanced.

[0078] In a preferred embodiment, the content of one or more polymers PC1-P1 in the polymer composition PC1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 10% by weight or more, more preferably 20% by weight or more, more preferably 30% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, and more preferably 90% by weight or more. Therefore, mechanical properties and combustion behavior are improved, and the recycling content is enhanced.

[0079] In a preferred embodiment, the content of one or more polymers PC1-P1 in the polymer composition PC1 is 99% by weight or less, preferably 95% by weight or less, more preferably 90% by weight or less, more preferably 80% by weight or less, more preferably 70% by weight or less, more preferably 60% by weight or less, more preferably 50% by weight or less, more preferably 40% by weight or less, more preferably 30% by weight or less, and more preferably 20% by weight or less. Therefore, mechanical properties and combustion behavior are improved, and the recycling content is enhanced.

[0080] In a preferred embodiment, the polymer composition PC0 can be obtained by mixing and annealing a mixture M0 comprising one or more polymers PC0-P1 and one or more additives PC0-A1, preferably one or more polymers PC0-P1 and one or more additives PC0-A1.

[0081] In a preferred embodiment, the polymer composition PC0 comprises particles, preferably consists of particles, and wherein the particles are at least partially homogeneous, preferably homogeneous.

[0082] In a preferred embodiment, one or more polymers PC1-P1 comprise one or more polymers PC0-P1 and preferably one or more polymers M1-P1, and is preferably composed of one or more polymers PC0-P1 and preferably one or more polymers M1-P1.

[0083] In a preferred embodiment, one or more polymers PC1-P1 are of the same type as one or more polymers PC0-P1, and preferably of the same type as one or more polymers M1-P1.

[0084] In the preferred embodiment, the length L arit It is the average length L arit And / or, preferably, the thickness T arit The average thickness T arit .

[0085] In the preferred embodiment, the length L arit And / or preferably, and thickness T arit As described in this article. Methods and Definitions

[0086] Unless otherwise specified, the following method is preferred, and definitions apply.

[0087] Tm and Tg were measured using DSC. DSC measurements were performed on a Perkin Elmer DSC 8000 with a heating / cooling rate of 20 K / min, within a temperature range of 0°C to 350°C, according to DIN EN ISO 11357. Tensile modulus [MPa] was measured according to ISO 527. Tensile stress at break [MPa] was measured according to ISO 527. Elongation at break [%] was measured according to ISO 527. Impact resistance [kJ / m] was measured according to ISO 179-2 / 1eU. 2 Notched impact resistance [kJ / m] is measured according to ISO 179-2 / 1eA. 2 ].

[0088] The UL 94 V test was performed according to the UL 94 V method described in Underwriters Laboratories Inc., “Standard of Safety, Test for Flammability of Plastic Materials for Parts in Devices and Appliances,” pages 14-18, Northbrook, 1998. The specimen thickness was 0.8 mm.

[0089] Glow wire resistance is determined by the GWFI (Glow Wire Flammability Index) test according to DIN 60695-2-12. The GWFI test is performed on three test samples (60mm × 60mm × h plates, where h is a thickness of 0.8mm, 1.0mm, or 1.5mm) using a glow wire at 960°C. The test sample is pressed against the heated glow wire with a force of 1 Newton for 30 seconds. The penetration depth of the glow wire is limited to 7mm. The test is considered passed if the afterflame time of the test sample after the glow wire is removed is less than 30 seconds, and if the tissue paper placed under the test sample does not ignite in three consecutive tests.

[0090] The length and thickness of the glass fibers were measured as follows. First, the polymer compound containing the glass fibers was pyrolyzed at 650°C for 1.5 hours to obtain the glass fibers. Then, a spatula (approximately 5 mg) of the glass fiber tip was dispersed in a mixture of 100 mL of water and 2 drops of glycerol and transferred to a petri dish. The petri dish was placed on the surface of an Epson Perfection V850 Pro flatbed scanner. This type of scanner is capable of analyzing the length of approximately 80,000 fibers simultaneously. Due to the limited resolution of the scanner, fibers shorter than 21.2 μm could not be detected. Therefore, fibers shorter than 21.2 μm were not considered.

[0091] Value calculation : Arithmetic length L of glass fiber arit = (L total ) / (L sum ); Where L total It is the sum of the lengths of all fibers, and Where L sum It is the sum of all fibers.

[0092] The thickness of the glass fiber is preferably determined as follows: First, a polymer compound containing glass fibers is pyrolyzed at 650°C for 1.5 h to obtain glass fibers. Then, a spatula (approximately 5 mg) of the glass fiber tip is dispersed in a mixture of 100 mL of water and 2 drops of glycerol and transferred to a petri dish, which is then placed under a microscope. The diameters of ten different glass fibers are electronically measured using an image capture system (Zeiss). The average value of the ten glass fibers is taken as the thickness T of the glass fiber. arit .

[0093] Unless otherwise specified, normal conditions are used and / or applied, such as room temperature, preferably 25°C, and 1 bar, preferably 1013.25 mbar.

[0094] Those skilled in the art will understand that the properties of additives, especially (glass) fibers, can change with each processing step (e.g., mixing and annealing). Therefore, the type of additive is the same before and after processing steps; however, it can have other properties, for example, the length of the (glass) fibers can be changed during the mixing process.

[0095] Those skilled in the art will understand that the properties of a polymer can change with each processing step (e.g., mixing and annealing). Therefore, the type of polymer is the same before and after a processing step; however, it can have different properties, for example, the molecular weight can change during the mixing process. Thus, those skilled in the art will understand that one or more polymers PC1-P1 are of the same type as one or more polymers PC0-P1, and preferably the same type as one or more polymers M1-P1. However, the properties of one or more polymers PC0-P1, preferably and one or more polymers M1-P1, can change during processing steps (e.g., mixing and annealing). For example, if one or more polymers PC0-P1 are polyamide 6 and one or more polymers M1-P1 are polyamide 6, then one or more polymers PC1-P1 are also polyamide 6; however, the properties of the polyamides (e.g., molecular weight and viscosity) may differ.

[0096] In summary, the embodiments and preferred embodiments are as follows. The scope of protection is defined by the claims. Further preferred are combinations of two or more embodiments, such as three, four, or eight embodiments. The definitions and general descriptions herein preferably also apply to the following embodiments and preferred embodiments. Furthermore, unless otherwise stated, the definitions and general statements of the methods mentioned herein also apply to the polymer composition PC1, the polymer product PP1, or the use, and vice versa. Preferably, where present in the claims, the embodiments are arranged in the following order and / or as follows: Figure 1 The steps described in the following implementation scheme are carried out as depicted.

[0097] 1. A method comprising the following steps, preferably in this order: i) Provide a polymer composition PC0, The polymer composition PC0 comprises, and preferably consists of, the following substances: a) One or more polymers PC0-P1, and b) One or more additives PC0-A1; ii) Mix and anneal the mixture M1 to obtain the polymer composition PC1. The mixture M1 contains, and preferably consists of, the following substances: a) The polymer composition PC0, b) Preferably one or more polymers M1-P1; and Preferably, the polymer composition PC1 comprises, and more preferably consists of, the following substances: a) One or more polymers PC1-P1, and b) One or more additives PC1-A1.

[0098] 2. Preferably, the method according to embodiment 1, wherein the method includes the following steps: iii) The polymer composition PC1, which can be obtained by the method according to embodiment 1 or by the method according to embodiment 1, or the chemical material that can be obtained by the method according to embodiment 1 or by the method according to embodiment 1, is converted to obtain product PRF1.

[0099] 3. The method described according to implementation scheme 1 or 2, Step ii) is performed in an extruder, preferably a twin-screw extruder.

[0100] 4. The method according to any one of the foregoing embodiments, wherein the mixture M1 is mixed in step ii) for 5 seconds or longer, preferably 10 seconds or longer, more preferably 20 seconds or longer, more preferably 30 seconds or longer, more preferably 45 seconds or longer, more preferably 60 seconds or longer, more preferably 120 seconds or longer, more preferably 180 seconds or longer, more preferably 240 seconds or longer.

[0101] 5. The method according to any one of the foregoing embodiments, wherein the mixture M1 is mixed in step ii) for 15 min or less, preferably 10 min or less, more preferably 5 min or less, more preferably 240 s or less, more preferably 180 s or less, more preferably 120 s or less, more preferably 100 s or less, more preferably 80 s or less, more preferably 60 s or less, more preferably 45 s or less.

[0102] 6. The method according to any one of the foregoing embodiments, wherein the mixture M1 is annealed in step ii) to 140°C or higher, preferably 160°C or higher, more preferably 170°C or higher, more preferably 180°C or higher, more preferably 190°C or higher, more preferably 200°C or higher, more preferably 210°C or higher, more preferably 220°C or higher, more preferably 230°C or higher, more preferably 240°C or higher, more preferably 250°C or higher, more preferably 260°C or higher, more preferably 270°C or higher, more preferably 280°C or higher, more preferably 290°C or higher, more preferably 300°C or higher.

[0103] 7. The method according to any one of the foregoing embodiments, wherein the mixture M1 is annealed in step ii) to 500°C or lower, preferably 400°C or lower, more preferably 300°C or lower, more preferably 280°C or lower, more preferably 260°C or lower, more preferably 240°C or lower, more preferably 220°C or lower, more preferably 200°C or lower.

[0104] 8. The method according to any one of the foregoing embodiments, wherein the mixture M1 is annealed in step ii) to (Tm of a polymer composition PC0 or PC1, in °C) or higher, preferably (Tm of a polymer composition PC0 or PC1, in °C) +10 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +20 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +30 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +40 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +60 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +80 °C or higher, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +100 °C or higher.

[0105] 9. The method according to any one of the foregoing embodiments, wherein the mixture M1 is annealed in step ii) to (Tm of a polymer composition PC0 or PC1, in °C) +200 °C or lower, preferably (Tm of a polymer composition PC0 or PC1, in °C) +150 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +100 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +80 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +60 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +40 °C or lower, more preferably (Tm of a polymer composition PC0 or PC1, in °C) +20 °C or lower.

[0106] 10. The method according to any one of the foregoing embodiments, wherein the throughput in step ii) is 0.5 kg / h or greater and 25,000 kg / h or less, preferably 1 kg / h or greater and 10,000 kg / h or less, more preferably 5 kg / h or greater and 5,000 kg / h or less, more preferably 10 kg / h or greater and 2,500 kg / h or less, more preferably 13 kg / h or greater and 1,000 kg / h or less, more preferably 16 kg / h or greater and 500 kg / h or less, more preferably 19 kg / h or greater and 300 kg / h or less.

[0107] 11. The method according to any one of the foregoing embodiments, wherein the method is used for producing a polymer composition, preferably polymer composition PC1 and / or a polymer product, preferably polymer product PP1.

[0108] 12. Use of mixture M1 in the production of polymer composition PC1, The mixture M1 contains, and preferably consists of, the following substances: a) Polymer composition PC0, and b) Preferably one or more polymers M1-P1; and The polymer composition PC0 comprises, and preferably consists of, the following substances: a) One or more polymers PC0-P1, and b) One or more additives PC0-A1; and Preferably, the polymer composition PC1 comprises, and more preferably consists of, the following substances: a) One or more polymers PC1-P1, and b) One or more additives PC1-A1.

[0109] 13. The method or use according to any one of the foregoing embodiments, The one or more additives PC0-A1 contain one or more reinforcing agents PC0-R1, preferably consisting of one or more reinforcing agents PC0-R1.

[0110] 14. The method or use according to any one of the foregoing embodiments, The mixture M1 contains one or more additives M1-A1, preferably wherein the one or more additives M1-A1 and the one or more additives PC0-A1 are not the same.

[0111] 15. The method or use according to any one of the foregoing embodiments, The mixture M1 contains one or more additives M1-A1, preferably the one or more additives M1-A1 contains one or more reinforcing agents M1-R1, preferably composed of one or more reinforcing agents M1-R1.

[0112] 16. The method or use according to any one of the foregoing embodiments, The one or more additives PC1-A1 contain one or more reinforcing agents PC1-R1, preferably consisting of one or more reinforcing agents PC1-R1.

[0113] 17. The method or use according to any one of the foregoing embodiments, The condition is that the one or more additives PC0-A1 contain one or more reinforcing agents PC0-R1, preferably composed of one or more reinforcing agents PC0-R1, and / or the mixture M1 contains one or more additives M1-A1, wherein the one or more additives M1-A1 contain one or more reinforcing agents M1-R1, preferably composed of one or more reinforcing agents M1-R1.

[0114] 18. The method or use according to any one of the foregoing embodiments, The one or more reinforcements PC0-R1, M1-R1 and / or PC1-R1 are made of glass, and more preferably the one or more reinforcements M1-R1, PC0-R1 and / or PC1-R1 comprise glass fibers M1-GF1, PC0-GF1 and / or PC1-GF1, preferably composed of glass fibers M1-GF1, PC0-GF1 and / or PC1-GF1.

[0115] 19. The method or use according to any one of the foregoing embodiments, The one or more reinforcements PC0-R1, M1-R1 and / or PC1-R1 contain, preferably consist of, the following substances: fibers or beads, more preferably fibers, more preferably glass fibers M1-GF1, PC0-GF1 and / or PC1-GF1.

[0116] 20. The method or use according to any one of the foregoing embodiments, The length L of said one or more reinforcements PC0-R1 arit The value is 20µm or greater, preferably 30µm or greater, more preferably 40µm or greater, more preferably 50µm or greater, more preferably 60µm or greater, more preferably 70µm or greater, more preferably 80µm or greater, more preferably 90µm or greater, more preferably 100µm or greater, more preferably 110µm or greater, more preferably 120µm or greater, more preferably 130µm or greater, more preferably 140µm or greater.

[0117] 21. The method or use according to any one of the foregoing embodiments, The length L of said one or more reinforcements PC0-R1 arit The value is 1000µm or less, preferably 750µm or less, more preferably 500µm or less, more preferably 250µm or less, more preferably 225µm or less, more preferably 200µm or less, more preferably 180µm or less, more preferably 170µm or less, more preferably 160µm or less, more preferably 150µm or less, more preferably 140µm or less.

[0118] 22. The method or use according to any one of the foregoing embodiments, The thickness T of the one or more reinforcements PC0-R1 arit The value is 1µm or larger and 40µm or smaller, preferably 3µm or larger and 35µm or smaller, more preferably 5µm or larger and 30µm or smaller, more preferably 6µm or larger and 25µm or smaller, more preferably 7µm or larger and 20µm or smaller, more preferably 8µm or larger and 15µm or smaller, more preferably 9µm or larger and 12µm or smaller, and more preferably about 10µm.

[0119] 23. The method or use according to any one of the foregoing embodiments, The length L of said one or more reinforcements PC0-R1 arit The thickness T of the one or more reinforcements PC0-R1 arit The ratio [µm / µm] is 1 or greater and 1000 or less, preferably 2 or greater and 500 or less, more preferably 4 or greater and 250 or less, more preferably 6 or greater and 100 or less, more preferably 8 or greater and 50 or less, more preferably 10 or greater and 25 or less, more preferably 12 or greater and 20 or less, more preferably 13 or greater and 15 or less, more preferably about 14.

[0120] 24. The method or use according to any one of the foregoing embodiments, The length L of the one or more reinforcements M1-R1 arit The value is 20µm or larger, preferably 100µm or larger, more preferably 250µm or larger, more preferably 500µm or larger, more preferably 1000µm or larger, more preferably 2000µm or larger, more preferably 3000µm or larger, and more preferably 4000µm or larger.

[0121] 25. The method or use according to any one of the foregoing embodiments, The length L of the one or more reinforcements M1-R1 arit The value is 1 cm or less, preferably 9000 µm or less, more preferably 7500 µm or less, more preferably 6000 µm or less, more preferably 5000 µm or less, more preferably 4000 µm or less, more preferably 3000 µm or less, more preferably 2000 µm or less, more preferably 1000 µm or less, more preferably 500 µm or less, more preferably 250 µm or less.

[0122] 26. The method or use according to any one of the foregoing embodiments, The thickness T of the one or more reinforcements M1-R1 aritThe value is 1µm or larger and 40µm or smaller, preferably 3µm or larger and 35µm or smaller, more preferably 5µm or larger and 30µm or smaller, more preferably 6µm or larger and 25µm or smaller, more preferably 7µm or larger and 20µm or smaller, more preferably 8µm or larger and 15µm or smaller, more preferably 9µm or larger and 12µm or smaller, and more preferably about 10µm.

[0123] 27. The method or use according to any one of the foregoing embodiments, The length L of the one or more reinforcements M1-R1 arit The thickness T of the one or more reinforcements M1-R1 arit The ratio [µm / µm] is 1 or greater and 10000 or less, preferably 50 or greater and 5000 or less, more preferably 75 or greater and 2500 or less, more preferably 100 or greater and 1000 or less, more preferably 200 or greater and 700 or less, more preferably 250 or greater and 600 or less, more preferably 300 or greater and 500 or less, more preferably 350 or greater and 450 or less, more preferably about 400.

[0124] 28. The method or use according to any one of the foregoing embodiments, The length L of said one or more reinforcements PC1-R1 arit The value is 20µm or greater, preferably 30µm or greater, more preferably 40µm or greater, more preferably 50µm or greater, more preferably 60µm or greater, more preferably 70µm or greater, more preferably 80µm or greater, more preferably 90µm or greater, more preferably 100µm or greater, more preferably 110µm or greater, more preferably 115µm or greater.

[0125] 29. The method or use according to any one of the foregoing embodiments, The length L of said one or more reinforcements PC1-R1 arit The value is 1000µm or less, preferably 750µm or less, more preferably 500µm or less, more preferably 250µm or less, more preferably 225µm or less, more preferably 200µm or less, more preferably 180µm or less, more preferably 170µm or less, more preferably 160µm or less, more preferably 150µm or less, more preferably 140µm or less, more preferably 130µm or less, more preferably 120µm or less, more preferably about 118µm.

[0126] 30. The method or use according to any one of the foregoing embodiments, The thickness T of the one or more reinforcements PC1-R1 aritThe value is 1µm or larger and 40µm or smaller, preferably 3µm or larger and 35µm or smaller, more preferably 5µm or larger and 30µm or smaller, more preferably 6µm or larger and 25µm or smaller, more preferably 7µm or larger and 20µm or smaller, more preferably 8µm or larger and 15µm or smaller, more preferably 9µm or larger and 12µm or smaller, and more preferably about 10µm.

[0127] 31. The method or use according to any one of the foregoing embodiments, The length L of said one or more reinforcements PC1-R1 arit The thickness T of the one or more reinforcements PC1-R1 arit The ratio [µm / µm] is 1 or greater and 1000 or less, preferably 2 or greater and 500 or less, more preferably 4 or greater and 250 or less, more preferably 6 or greater and 100 or less, more preferably 8 or greater and 50 or less, more preferably 9 or greater and 20 or less, more preferably 10 or greater and 15 or less, more preferably 11 or greater and 13 or less, more preferably about 12.

[0128] 32. The method or use according to any one of the foregoing embodiments, The one or more additives PC0-A1 comprise one or more reinforcing agents PC0-R1, preferably consisting of one or more reinforcing agents PC0-R1, and The one or more additives PC1-A1 comprise one or more reinforcing agents PC1-R1, preferably consisting of one or more reinforcing agents PC1-R1, and The length L of said one or more reinforcements PC1-R1 arit The length L of the one or more reinforcements PC0-R1 arit The ratio [μm / μm] is 0.50 to 1.00, preferably 0.60 to 0.95, more preferably 0.70 to 0.92, more preferably 0.80 to 0.90, and even more preferably 0.82 to 0.88.

[0129] 33. The method or use according to any one of the foregoing embodiments, The one or more additives PC0-A1 comprise one or more reinforcing agents PC0-R1, preferably consisting of one or more reinforcing agents PC0-R1, and The one or more additives PC1-A1 comprise one or more reinforcing agents PC1-R1, preferably consisting of one or more reinforcing agents PC1-R1, and The length L of said one or more reinforcements PC0-R1 aritThe length L of the one or more reinforcements PC1-R1 arit The ratio [µm / µm] is 1.00 or greater and 100.00 or less, preferably 1.05 or greater and 25.0 or less, more preferably 1.08 or greater and 20.0 or less, more preferably 1.10 or greater and 10.0 or less, more preferably 1.15 or greater and 5.0 or less, and more preferably 1.18 or greater and 2.0 or less.

[0130] 34. The method or use according to any one of the foregoing embodiments, The one or more additives PC0-A1 contain one or more flame retardants PC0-FR1, preferably composed of one or more flame retardants PC0-FR1. Preferably, the one or more additives PC0-A1 comprises one or more flame retardants PC0-FR1 and one or more reinforcing agents PC0-R1, and is preferably composed of one or more flame retardants PC0-FR1 and one or more reinforcing agents PC0-R1.

[0131] 35. The method or use according to any one of the foregoing embodiments, The one or more additives PC0-A1 mentioned therein do not contain one or more flame retardants PC0-FR1 and / or one or more reinforcing agents PC0-R1.

[0132] 36. The method or use according to any one of the foregoing embodiments, The mixture M1 contains one or more additives M1-A1, preferably wherein the one or more additives M1-A1 contain one or more flame retardants M1-FR1, and preferably is composed of one or more flame retardants M1-FR1. More preferably, the one or more additives M1-A1 comprise one or more flame retardants M1-FR1 and one or more reinforcing agents M1-R1, preferably consisting of one or more flame retardants M1-FR1 and one or more reinforcing agents M1-R1.

[0133] 37. The method or use according to any one of the foregoing embodiments, The one or more additives M1-A1 mentioned therein do not contain one or more flame retardants M1-FR1 and / or one or more reinforcing agents M1-R1.

[0134] 38. The method or use according to any one of the foregoing embodiments, The one or more additives PC1-A1 contain one or more flame retardants PC1-FR1, preferably composed of one or more flame retardants PC1-FR1.

[0135] 39. The method or use according to any one of the foregoing embodiments, The one or more flame retardants M1-FR1, PC0-FR1 and / or PC1-FR1 contain, preferably consist of, the following substances: flame retardants containing H, O, N and C, more preferably complexes containing cyanuric acid, and more preferably melamine cyanurate.

[0136] 40. The method or use according to any one of the foregoing embodiments, The condition is that the one or more additives PC0-A1 contain one or more flame retardants PC0-FR1, preferably composed of one or more flame retardants PC0-FR1, and / or the mixture M1 contains one or more additives M1-A1, wherein the one or more additives M1-A1 contain one or more flame retardants M1-FR1, preferably composed of one or more flame retardants M1-FR1.

[0137] 41. The method or use according to any one of the foregoing embodiments, The one or more polymers PC0-P1, M1-P1 and / or PC1-P1 contain, preferably consist of: thermoplastic polymers, preferably thermoplastic polyurethane and / or polyamide, more preferably PA6 and / or PA66, even more preferably PA6.

[0138] 42. The method or use according to any one of the foregoing embodiments, The one or more polymers PC0-P1, M1-P1 and / or PC1-P1 are primarily the same, preferably the same.

[0139] 43. The method or use according to any one of the foregoing embodiments, The mixture M1 contains one or more polymers M1-P1.

[0140] 44. The method or use according to any one of the foregoing embodiments, The mixture M1, by weight percent, comprises, preferably, the following substances: a) 5 to 95, preferably 20 to 70, polymer composition PC0, b) 0 to 95, preferably 5 to 40, one or more polymers M1-P1 c) 0 to 50, preferably 0.1 to 30, one or more reinforcing agents M1-R1, d) 0 to 35, preferably 3 to 25, one or more flame retardants M1-FR1, and e) 0 to 20, preferably 0.1 to 15, one or more additives A2.

[0141] 45. The method or use according to any one of the foregoing embodiments, The ratio [weight % / weight %] of the polymer composition PC0 to the one or more polymers M1-P1 is 0.5 or greater and 40.0 or less, preferably 1.0 or greater and 20.0 or less, more preferably 1.5 or greater and 10.0 or less, more preferably 2.0 or greater and 5.0 or less, and more preferably 2.5 or greater and 3.5.

[0142] 46. ​​The method or use according to any one of the foregoing embodiments, The polymer composition PC0 is at least partially waste or obtained from waste, preferably said waste is post-consumer waste and / or post-industrial waste.

[0143] 47. The method or use according to any one of the foregoing embodiments, The lifespan of the polymer composition PC0 is one day or longer, preferably one week or longer, more preferably one year or longer; and / or The polymer composition PC0 has a lifespan of 100 years or less, preferably 50 years or less, and more preferably 25 years or less.

[0144] 48. The method or use according to any one of the foregoing embodiments, The polymer composition PC0 comprises, and preferably consists of, the following substances: a) 20 to 90, preferably 30 to 80, one or more polymers PC0-P1, and b) 5 to 50, preferably 10 to 35, one or more reinforcing agents PC0-R1, c) 0 to 20, preferably 1 to 10, one or more flame retardants PC0-FR1, and d) 0 to 20, preferably 0.1 to 10, one or more additives A2.

[0145] 49. The method or use according to any one of the foregoing embodiments, The polymer composition PC1 comprises, and preferably consists of, the following substances: a) 20 to 90, preferably 30 to 80, one or more polymers PC1-P1, and b) 5 to 50, preferably 10 to 35, one or more reinforcing agents PC1-R1, c) 0 to 20, preferably 3 to 15, one or more flame retardants PC1-FR1, and d) 0 to 20, preferably 0.1 to 10, one or more additives A2.

[0146] 50. The method or use according to any one of the foregoing embodiments, The polymer composition PC0, the polymer composition PC1, and / or the mixture M1 contain one or more additives A2.

[0147] 51. The method or use according to any one of the foregoing embodiments, The one or more additives A2 mentioned above are selected from antioxidants, stabilizers, lubricants, minerals, chain extenders, impact modifiers, colorants, pigments, soot, talc, and mixtures thereof.

[0148] 52. The method or use according to any one of the foregoing embodiments, The tensile modulus of the polymer composition PC1 is 1000 MPa or higher and 10000 MPa or lower, preferably 4000 MPa or higher and 8000 MPa or lower, more preferably 4000 MPa or higher and 7500 MPa or lower, more preferably 5000 MPa or higher and 7000 MPa or lower, more preferably 5500 MPa or higher and 6750 MPa or lower, more preferably 6000 MPa or higher and 6500 MPa or lower, more preferably 6100 MPa or higher and 6250 MPa or lower, and more preferably 6120 MPa or higher and 6150 MPa or lower.

[0149] 53. The method or use according to any one of the foregoing embodiments, The tensile stress at break of the polymer composition PC1 is 10 MPa or higher and 1000 MPa or lower, preferably 25 MPa or higher and 500 MPa or lower, more preferably 50 MPa or higher and 250 MPa or lower, more preferably 60 MPa or higher and 200 MPa or lower, more preferably 70 MPa or higher and 150 MPa or lower, more preferably 80 MPa or higher and 125 MPa or lower, more preferably 90 MPa or higher and 110 MPa or lower, more preferably 95 MPa or higher and 100 MPa or lower.

[0150] 54. The method or use according to any one of the foregoing embodiments, The elongation at break of the polymer composition PC1 is 1.1% or higher and 10.0% or lower, preferably 2.0% or higher and 9.0% or lower, more preferably 3.0% or higher and 7.0% or lower, more preferably 3.5% or higher and 6.0% or lower, more preferably 3.8% or higher and 5.2% or lower, more preferably 4.1% or higher and 4.9% or lower, more preferably 4.2% or higher and 4.7% or lower, and more preferably 4.3% or higher and 4.5% or lower.

[0151] 55. The method or use according to any one of the foregoing embodiments, The impact resistance of the polymer composition PC1 is 10 kJ / m. 2 Or even greater and 100kJ / m 2 Or even lower, preferably 20 kJ / m 2 Or larger and 75kJ / m 2 Or less, more preferably 30 kJ / m 2 Or even greater and 50kJ / m 2 Or less, more preferably 35 kJ / m 2 Or even greater and 48kJ / m 2 Or less, more preferably 40 kJ / m 2 Or even greater and 44kJ / m 2 Or smaller.

[0152] 56. The method or use according to any one of the foregoing embodiments, The notched impact resistance of the polymer composition PC1 is 1.0 kJ / m. 2 Or larger and 20kJ / m 2 Or even smaller, preferably 2.0 kJ / m 2 Or larger and 10 kJ / m 2 Or less, more preferably 2.5 kJ / m 2 Or even greater and 8kJ / m 2 Or smaller, more preferably 3.0 kJ / m 2 Or larger and 6kJ / m 2 Or less, more preferably 3.5 kJ / m 2 Or larger and 4kJ / m 2 Or smaller.

[0153] 57. The method or use according to any one of the foregoing embodiments, The polymer composition PC1 exhibits V-2, preferably V-1, and more preferably V-0 in the UL94 V test.

[0154] 58. The method or use according to any one of the foregoing embodiments, The polymer composition PC1 described therein exhibits a total afterflame time of 2s or longer and 100s or shorter, preferably 5s or longer and 80s or shorter, more preferably 10s or longer and 60s or shorter, more preferably 15s or longer and 40s or shorter, more preferably 18s or longer and 30s or shorter, and more preferably 20s or longer and 25s or shorter.

[0155] 59. The method or use according to any one of the foregoing embodiments, The polymer composition PC1 described therein passed the GWFI test.

[0156] 60. A polymer composition, preferably polymer composition PC1, said polymer composition being obtainable by the method according to any one of the foregoing embodiments.

[0157] 61. A polymer product, preferably polymer product PP1, said polymer product being obtainable by the method according to any one of the foregoing embodiments.

[0158] 62. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, The polymer composition PC0, the polymer composition PC1, and / or the polymer product PP1 are either or are components of the following: - Automotive parts; preferably cylinder head covers, engine hoods, turbocharger housings, coatings, covers, elevator load-bearing components, foils, fibers, films, foams, damping elements, machine drive belts, turbocharger baffles, intake pipes, intake manifolds, connectors, gaskets, drive pulleys, fan pulleys, coolant tanks, hoses, housings, heat exchanger housing components, coolant coolers, turbocharger coolers, laminates, shoe midsoles, vehicle linings, thermoplastic modifiers, molding bodies, roofs or floors of buildings or vehicles, nonwoven fabrics, packaging materials, passenger conveyors, passenger transport... Handrails, profiles, rollers, rope arrangements, saddles, shoe soles, belts, thermostats, water pumps, radiators, fasteners, battery system components for electric vehicles, dashboards, cushions, steering column switches, seats, headrests, center consoles, transmission components, door modules, A, B, C, or D pillar trim panels, spoilers, door handles, exterior mirrors, windshield wipers, windshield wiper housings, wiper blades, decorative grilles, trim strips, roof rails, window frames, sunroof frames, antenna panels, headlights and taillights, hoods, cylinder head covers, intake manifolds, airbags, steering wheels, cushioning pads, or coatings; - Fabric; preferably shirts, trousers, sweaters, boots, shoes, shoe soles, tights or jackets; - Electrical components; preferably electrical or electronic passive or active components, cables, cable connectors, cable sheaths for mobile phones, circuit breakers, circuit boards, printed circuit boards, terminals, housing components, foil, wires, switches, switching devices, plugs, sockets, distributors, relays, resistors, capacitors, inductors, spools, lamps, diodes, LEDs, transistors, connectors, voltage regulators, integrated circuits (ICs), processors, controllers, memory, sensors, microswitches, microbuttons, semiconductors, reflector housings for light-emitting diodes (LEDs), fasteners for electrical or electronic components, solar modules, gaskets, bolts, strips, slide-in guides, screws, nuts, televisions, drag cables, membrane hinges, spring hooks (snap-on) or spring tongues; - Consumer goods, agricultural products, or pharmaceutical products; preferably tennis ropes, climbing ropes, bristles, brushes, artificial turf, 3D printing filaments, lawnmowers, zippers, Velcro, fabrics for papermaking machines, extrusion coatings, fishing lines, fishing nets, marine ropes, vials, syringes, ampoules, bottles, and bags; preferably organic waste bags, vegetable or fruit bags; sliding elements, spindle nuts, chain conveyors, sliding bearings, rollers, wheels, gears, ring gears, screws and spring dampers, hoses, pipes, cable sheaths, sockets, switches, cable ties, fan wheels, carpets, nonwovens, cosmetic boxes or bottles, mattresses, cushions, insulation, refrigerators, freezers, hot and cold food warmers, water heaters, hot water storage tanks, pipes, insulation boards, insulation panels, detergents, dishwasher tablets or powders, shampoos, shower gels, soaps, fertilizers, covers, fungicides, or insecticides; - Packaging; preferably packaging for the food industry; preferably blown or cast film, more preferably single or multi-layer blown film or single or multi-layer cast film; axially stretched film, preferably biaxial or multiaxial film, or laminated film; a molded article; preferably injection molded article, more preferably coffee capsule; thermoformed article; preferably coffee capsule; or - Building components; preferably rotor blades, insulation materials; preferably sound insulation or heat insulation materials; frames, shells, walls, coatings, facades, windows, doors or partitions.

[0159] 63. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, The content of polymer composition PC0 in the polymer composition PC1 and / or mixture M1 and / or polymer product PP1 is 1% by weight or more, preferably 2% by weight or more, more preferably 5% by weight or more, more preferably 15% by weight or more, more preferably 30% by weight or more, more preferably 40% by weight or more, more preferably 60% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more, more preferably 95% by weight or more; and / or The content of polymer composition PC0 in the polymer composition PC1 and / or mixture M1 and / or polymer product PP1 is 100% by weight or less, preferably 95% by weight or less, more preferably 90% by weight or less, more preferably 50% by weight or less, more preferably 25% by weight or less, and more preferably 10% by weight or less; and Preferably, the content is determined based on an identity preservation and / or segregation and / or quality balance and / or book and claims custody model, preferably based on quality balance, and preferably based on the International Sustainability and Carbon Certification (ISCC) standard.

[0160] 64. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The polymer composition PC1 and / or polymer product PP1 exhibit enhanced recycling content, improved mechanical properties, and / or improved flame retardancy; and / or the method and / or application produce upgraded recycled products.

[0161] 65. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The polymer composition PC1 comprises, and preferably consists of, the following substances: a) One or more polymers PC1-P1, and b) One or more additives PC1-A1.

[0162] 66. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The polymer composition PC0 contains one or more additives PC0-A1, preferably one or more flame retardants PC0-FR1 and / or one or more reinforcing agents PC0-R1, more preferably one or more flame retardants PC0-FR1, and more preferably melamine cyanurate, at a content of 0.1% by weight or more, preferably 1% by weight or more, more preferably 2% by weight or more, more preferably 3% by weight or more, more preferably 4% by weight or more, more preferably 5% by weight or more, more preferably 6% by weight or more, more preferably 7% by weight or more, more preferably 8% by weight or more, more preferably 9% by weight or more, more preferably 10% by weight or more, more preferably 11% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, and more preferably 30% by weight or more.

[0163] 67. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, The polymer composition PC0 contains one or more additives PC0-A1, preferably one or more flame retardants PC0-FR1 and / or one or more reinforcing agents PC0-R1, more preferably one or more flame retardants PC0-FR1, and more preferably melamine cyanurate, at a content of 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, and more preferably 5% by weight or less.

[0164] 68. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The content of the one or more additives M1-A1, preferably the one or more flame retardants M1-FR1 and / or the one or more reinforcing agents M1-R1, more preferably the one or more flame retardants M1-FR1, and more preferably melamine cyanurate in the mixture M1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 2% by weight or more, more preferably 3% by weight or more, more preferably 4% by weight or more, more preferably 5% by weight or more, more preferably 6% by weight or more, more preferably 7% by weight or more, more preferably 8% by weight or more, more preferably 9% by weight or more, more preferably 10% by weight or more, more preferably 11% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, and more preferably 30% by weight or more in the mixture M1.

[0165] 69. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The content of the one or more additives M1-A1, preferably the one or more flame retardants M1-FR1 and / or the one or more reinforcing agents M1-R1, more preferably the one or more flame retardants M1-FR1, and more preferably melamine cyanurate in the mixture M1 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, and more preferably 5% by weight or less in the mixture M1.

[0166] 70. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The polymer composition PC1 contains one or more additives PC1-A1, preferably one or more flame retardants PC1-FR1 and / or one or more reinforcing agents PC1-R1, more preferably one or more flame retardants PC1-FR1, and more preferably melamine cyanurate, at a content of 0.1% by weight or more, preferably 1% by weight or more, more preferably 2% by weight or more, more preferably 3% by weight or more, more preferably 4% by weight or more, more preferably 5% by weight or more, more preferably 6% by weight or more, more preferably 7% by weight or more, more preferably 8% by weight or more, more preferably 9% by weight or more, more preferably 10% by weight or more, more preferably 11% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, and more preferably 30% by weight or more.

[0167] 71. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The polymer composition PC1 contains one or more additives PC1-A1, preferably one or more flame retardants PC1-FR1 and / or one or more reinforcing agents PC1-R1, more preferably one or more flame retardants PC1-FR1, and more preferably melamine cyanurate, at a content of 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, and more preferably 5% by weight or less.

[0168] 72. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, The content of one or more additives PC0-A1, preferably one or more reinforcing agents PC0-R1, and more preferably glass fiber PC0-GF1 in the polymer composition PC0 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 8% by weight or more, more preferably 10% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 25% by weight or more, more preferably 30% by weight or more, more preferably 35% by weight or more, more preferably 40% by weight or more, and more preferably 50% by weight or more in the polymer composition PC0.

[0169] 73. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The content of one or more additives PC0-A1, preferably one or more reinforcing agents PC0-R1, and more preferably glass fiber PC0-GF1 in the polymer composition PC0 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, more preferably 5% by weight or less.

[0170] 74. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The content of the one or more additives M1-A1, preferably the one or more reinforcing agents M1-R1, and more preferably glass fiber M1-GF1 in the mixture M1 is 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, more preferably 5% by weight or less.

[0171] 75. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The content of one or more additives M1-A1, preferably one or more reinforcing materials M1-R1, and more preferably glass fiber M1-GF1 in the mixture M1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 8% by weight or more, more preferably 10% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 25% by weight or more, more preferably 30% by weight or more, more preferably 35% by weight or more, more preferably 40% by weight or more, and more preferably 50% by weight or more.

[0172] 76. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The content of one or more additives PC1-A1, preferably one or more reinforcing agents PC1-R1, and more preferably glass fiber PC1-GF1 in the polymer composition PC1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 8% by weight or more, more preferably 10% by weight or more, more preferably 12% by weight or more, more preferably 15% by weight or more, more preferably 20% by weight or more, more preferably 25% by weight or more, more preferably 30% by weight or more, more preferably 35% by weight or more, more preferably 40% by weight or more, and more preferably 50% by weight or more.

[0173] 77. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The polymer composition PC1 contains one or more additives PC1-A1, preferably one or more reinforcing agents PC1-R1, and more preferably glass fiber PC1-GF1 in an amount of 50% by weight or less, preferably 40% by weight or less, more preferably 35% by weight or less, more preferably 30% by weight or less, more preferably 25% by weight or less, more preferably 20% by weight or less, more preferably 15% by weight or less, more preferably 14% by weight or less, more preferably 13% by weight or less, more preferably 12% by weight or less, more preferably 11% by weight or less, more preferably 10% by weight or less, more preferably 9% by weight or less, more preferably 8% by weight or less, more preferably 7% by weight or less, more preferably 6% by weight or less, and more preferably 5% by weight or less.

[0174] 78. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, The content of one or more polymers PC0-P1 in the polymer composition PC0 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 10% by weight or more, more preferably 20% by weight or more, more preferably 30% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more.

[0175] 79. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The content of one or more polymers PC0-P1 in the polymer composition PC0 is 99% by weight or less, preferably 95% by weight or less, more preferably 90% by weight or less, more preferably 80% by weight or less, more preferably 70% by weight or less, more preferably 60% by weight or less, more preferably 50% by weight or less, more preferably 40% by weight or less, more preferably 30% by weight or less, more preferably 20% by weight or less.

[0176] 80. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The content of one or more polymers PC1-P1 in the polymer composition PC1 is 0.1% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, more preferably 5% by weight or more, more preferably 10% by weight or more, more preferably 20% by weight or more, more preferably 30% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more.

[0177] 81. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, The content of one or more polymers PC1-P1 in the polymer composition PC1 is 99% by weight or less, preferably 95% by weight or less, more preferably 90% by weight or less, more preferably 80% by weight or less, more preferably 70% by weight or less, more preferably 60% by weight or less, more preferably 50% by weight or less, more preferably 40% by weight or less, more preferably 30% by weight or less, more preferably 20% by weight or less.

[0178] 82. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, The polymer composition PC0 can be obtained by mixing and annealing a mixture M0 comprising one or more polymers PC0-P1 and one or more additives PC0-A1, preferably one or more polymers PC0-P1 and one or more additives PC0-A1.

[0179] 83. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The polymer composition PC0 comprises particles, preferably consists of particles, and the particles are at least partially homogeneous, preferably homogeneous.

[0180] 84. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The one or more polymers PC1-P1 comprises the one or more polymers PC0-P1 and preferably the one or more polymers M1-P1, and is preferably composed of the one or more polymers PC0-P1 and preferably the one or more polymers M1-P1.

[0181] 85. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments. The type of one or more polymers PC1-P1 is the same as that of one or more polymers PC0-P1, and preferably the same as that of one or more polymers M1-P1.

[0182] 86. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, Where the length L arit It is the average length L arit And / or, preferably, the thickness T arit The average thickness T arit Preferably, and wherein the length L arit And / or preferably, the thickness T arit Measure as described in the instruction manual.

[0183] 87. The polymer composition PC1, polymer product PP1, method, or use according to any one of the foregoing embodiments, Where the length L arit And / or preferably, the thickness T arit Measure as described in the instruction manual. Experimental Section

[0184] Component A: Polyamide-6 (from BASF SE's Ultramid) ® B27).

[0185] Component B: Recycled material containing polyamide-6 and 30% glass fiber (L arit = 142µm; T arit = 10µm).

[0186] Component C: Melamine cyanurate (from BASF SE's Melapur) ® MC 25)

[0187] Component D: Standard chopped glass fibers (L) used for polyamidearit = 4.0mm, T arit = 10.0µm).

[0188] Component E: A mixture of 3,3'-bis(3,5-di-tert-butyl-4-hydroxyphenyl)-N,N'-hexamethylene-dipropionamide (CAS No. 23128-74-7), ethylene bis-stearamide (CAS No. 100-30-5) and calcium stearate (CAS No. 1592-23-0).

[0189] The sum of the proportions of components A) to E) in Table 1 is 100% by weight. Table 1 shows the composition and test results of the molding composition.

[0190] As shown in Table 1, the components A to E were mixed in a ZSK 26 (Berstorff) twin-screw extruder with a flat temperature characteristic curve and a throughput of 20 kg / h at approximately 250°C to 270°C, discharged as a filament, cooled until granulation was possible, and then granulated.

[0191] The test samples listed in Table 1 were used for testing and were injection molded in an Arburg 420C injection molding machine at a melt temperature of approximately 250°C to 290°C and a mold temperature of approximately 80°C.

[0192] Table 1: Composition and experimental results of Comparative Example 1 and Invention Example 1.

[0193] Attached Figure

[0194] exist Figure 1 The method according to the invention is described in the figure. In step i), a polymer composition PC0 is provided, wherein the polymer composition PC0 comprises one or more polymers PC0-P1 and one or more additives PC0-A1, and in step ii), a mixture M1 is mixed and annealed to obtain a polymer composition PC1, wherein the mixture M1 comprises the polymer composition PC0 and preferably one or more polymers M1-P1.

Claims

1. A method, the method comprising the following steps: i) Provide a polymer composition PC0, The polymer composition PC0 comprises, and preferably consists of, the following substances: a) One or more polymers PC0-P1, and b) One or more additives PC0-A1; ii) Mix and anneal the mixture M1 to obtain the polymer composition PC1. The mixture M1 contains, and preferably consists of, the following substances: a) The polymer composition PC0, b) Preferably one or more polymers M1-P1.

2. Preferably, the method according to claim 1, the method includes the following steps: i) Provide a polymer composition PC0, The polymer composition PC0 comprises, and preferably consists of, the following substances: a) One or more polymers PC0-P1, and b) One or more additives PC0-A1; ii) Mix and anneal the mixture M1 to obtain the polymer composition PC1. The mixture M1 contains, and preferably consists of, the following substances: a) The polymer composition PC0, b) Preferably, one or more polymers M1-P1; and The condition is that the one or more additives PC0-A1 contain one or more reinforcing agents PC0-R1, preferably composed of one or more reinforcing agents PC0-R1, and / or the mixture M1 contains one or more additives M1-A1, wherein the one or more additives M1-A1 contain one or more reinforcing agents M1-R1, preferably composed of one or more reinforcing agents M1-R1; and / or The condition is that the one or more additives PC0-A1 contain one or more flame retardants PC0-FR1, preferably composed of one or more flame retardants PC0-FR1, and / or the mixture M1 contains one or more additives M1-A1, wherein the one or more additives M1-A1 contain one or more flame retardants M1-FR1, preferably composed of one or more flame retardants M1-FR1.

3. The method according to any one of the preceding claims, The one or more additives PC0-A1 contain one or more reinforcing agents PC0-R1, preferably consisting of one or more reinforcing agents PC0-R1.

4. The method according to any one of the preceding claims, The condition is that the polymer composition PC0 contains one or more additives PC0-A1, wherein the one or more additives PC0-A1 contains one or more flame retardants PC0-FR1, preferably consisting of one or more flame retardants PC0-FR1, and / or the mixture M1 contains one or more additives M1-A1, wherein the one or more additives M1-A1 contains one or more flame retardants M1-FR1, preferably consisting of one or more flame retardants M1-FR1.

5. The method according to any one of the preceding claims, The mixture M1 is mixed in step ii) for 5 seconds or longer, preferably 10 seconds or longer, more preferably 20 seconds or longer, more preferably 30 seconds or longer, more preferably 45 seconds or longer, more preferably 60 seconds or longer, more preferably 120 seconds or longer, more preferably 180 seconds or longer, more preferably 240 seconds or longer; and / or The mixture M1 is mixed in step ii) for 15 minutes or less, preferably 10 minutes or less, more preferably 5 minutes or less, more preferably 240 seconds or less, more preferably 180 seconds or less, more preferably 120 seconds or less, more preferably 100 seconds or less, more preferably 80 seconds or less, more preferably 60 seconds or less, more preferably 45 seconds or less; and / or In step ii), the mixture M1 is annealed to 140°C or higher, preferably 160°C or higher, more preferably 170°C or higher, more preferably 180°C or higher, more preferably 190°C or higher, more preferably 200°C or higher, more preferably 210°C or higher, more preferably 220°C or higher, more preferably 230°C or higher, more preferably 240°C or higher, more preferably 250°C or higher, more preferably 260°C or higher, more preferably 270°C or higher, more preferably 280°C or higher, more preferably 290°C or higher, more preferably 300°C or higher; and / or In step ii), the mixture M1 is annealed to 500°C or lower, preferably 400°C or lower, more preferably 300°C or lower, more preferably 280°C or lower, more preferably 260°C or lower, more preferably 240°C or lower, more preferably 220°C or lower, and more preferably 200°C or lower.

6. Preferably, the method according to any one of the preceding claims comprises the following steps: iii) Convert the polymer composition PC1, which can be obtained by the method according to any one of the preceding claims, or the chemical material, which can be obtained by the method according to any one of the preceding claims, to obtain product PRF1.

7. The method according to any one of the preceding claims, One or more of the reinforcements PC0-R1 and / or M1-R1 are made of glass, more preferably the one or more reinforcements M1-R1 and / or PC0-R1 comprise glass fibers M1-GF1 and / or PC0-GF1, preferably composed of glass fibers M1-GF1 and / or PC0-GF1.

8. The method according to any one of the preceding claims, The length L of said one or more reinforcements PC0-R1 arit The thickness T of the one or more reinforcements PC0-R1 arit The ratio [µm / µm] is 1 or greater and 1000 or less, preferably 2 or greater and 500 or less, more preferably 4 or greater and 250 or less, more preferably 6 or greater and 100 or less, more preferably 8 or greater and 50 or less, more preferably 10 or greater and 25 or less, more preferably 12 or greater and 20 or less, more preferably 13 or greater and 15 or less, more preferably about 14.

9. The method according to any one of the preceding claims, The polymer composition PC1 contains one or more additives PC1-A1, and The one or more additives PC0-A1 comprise one or more reinforcing agents PC0-R1, preferably consisting of one or more reinforcing agents PC0-R1, and The one or more additives PC1-A1 comprise one or more reinforcing agents PC1-R1, preferably consisting of one or more reinforcing agents PC1-R1, and The length L of said one or more reinforcements PC1-R1 arit The length L of the one or more reinforcements PC0-R1 arit The ratio [μm / μm] is 0.50 to 1.00, preferably 0.60 to 0.95, more preferably 0.70 to 0.92, more preferably 0.80 to 0.90, and even more preferably 0.82 to 0.88; and / or.

10. The method according to any one of the preceding claims, The mixture M1 contains one or more additives M1-A1, preferably wherein the one or more additives M1-A1 contain one or more flame retardants M1-FR1, and preferably is composed of one or more flame retardants M1-FR1. Preferably, the one or more additives M1-A1 comprise one or more flame retardants M1-FR1 and one or more reinforcing agents M1-R1, and preferably consist of one or more flame retardants M1-FR1 and one or more reinforcing agents M1-R1.

11. The method according to any one of the preceding claims, The one or more flame retardants M1-FR1 and / or PCO-FR1 comprise, and preferably consist of, the following substances: Flame retardants containing H, O, N and C, more preferably complexes containing cyanuric acid, and even more preferably melamine cyanurate.

12. A polymer composition obtained by or capable of being obtained by the method according to any one of the preceding claims.

13. A polymer product obtained by the method according to any one of claims 1 to 12, or obtainable by the method according to any one of claims 1 to 12.

14. Use of mixture M1 in the production of polymer composition PC1, The mixture M1 contains, and preferably consists of, the following substances: a) Polymer composition PC0, and b) Preferably, one or more polymers M1-P1; and The polymer composition PC0 comprises, and preferably consists of, the following substances: a) One or more polymers PC0-P1, and b) One or more additives PC0-A1.

15. The method, polymer composition PC1, polymer product PP1, and / or use according to any one of the preceding claims, The polymer composition PC1 and / or polymer product PP1 exhibit enhanced recycling content, improved mechanical properties, and / or improved flame retardancy; and / or the method and / or application produce upgraded recycled products.

Citation Information