Electrolytic cell components and their manufacturing methods
By setting a water vapor oxidation resistant layer and improving the emissivity on the surface of the power supply board substrate, the problems of temperature rise and thinning caused by water vapor oxidation of the power supply components were solved, and the stable operation and efficient electrolysis of the battery stack were achieved.
Patent Information
- Application Number
- CN202580026126.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-02
- Filing Date
- 2025-01-20
- Publication Date
- 2026-11-10
AI Technical Summary
During high-temperature steam electrolysis, steam oxidation of the power supply components leads to temperature rise and thinning, affecting the performance and stability of the battery stack.
A water vapor oxidation resistant layer and an emissivity-enhancing structure are applied to the surface of the power supply board substrate. Water vapor oxidation resistant materials and increased emissivity of the power supply board are used to suppress temperature rise and improve heat dissipation.
It effectively inhibits water vapor oxidation of power supply components, keeps the temperature within the allowable range, reduces resistivity and improves heat dissipation efficiency, and prevents corrosion and thinning of power supply components.
Smart Images

Figure CN123076697A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to electrolytic cell components and manufacturing methods thereof, and particularly to an electrolytic cell component and manufacturing method thereof suitable for electrolyzing high-temperature water vapor in a Solid Oxide Electrolysis Cell (SOEC). Background Technology
[0002] In recent years, in order to achieve carbon neutrality, there has been a need to develop inexpensive and high-capacity hydrogen production systems that do not emit CO2.
[0003] Water electrolysis, which electrochemically decomposes water to produce hydrogen and oxygen, is a hydrogen production method that does not involve the emission of carbon dioxide. It has excellent environmental characteristics and includes alkaline electrolysis, solid polymer electrolysis, and steam electrolysis, which electrolyzes water vapor.
[0004] Among them, the solid oxide electrolysis cell (SOEC: hereinafter referred to as "electrolyte") for electrolyzing high-temperature water vapor uses ceramics such as yttrium-stabilized zirconium oxide, which have oxygen ion conductivity, as the electrolyte. It can utilize the thermal energy of the high-temperature water vapor as part of the energy required for the electrolysis reaction, thus producing hydrogen with high efficiency compared to other electrolysis methods. Alternatively, a mixture of high-temperature water vapor and carbon dioxide (CO2) can be supplied, allowing the hydrogen and carbon dioxide generated through electrolysis to react in the electrolyte, directly producing carbon monoxide (CO) and hydrocarbon compounds through co-electrolysis.
[0005] Furthermore, in solid oxide electrolyzers, a reversible solid oxide electrochemical cell (RSOC: hereinafter referred to as "reversible cell") is being developed, which has the dual function of supplying electricity and high-temperature water vapor from the outside and producing hydrogen and oxygen through reverse reaction, as well as generating electricity as a fuel cell.
[0006] Patent document 1 discloses a hydrogen generation system with a cylindrical battery stack, wherein the battery stack has multiple electrolytic cells with hydrogen electrodes, solid electrolyte membranes, and oxygen electrodes arranged on a substrate tube. In such a hydrogen generation system, multiple battery stacks are aggregated (modularized) for utilization.
[0007] The electrolysis reaction in SOEC is an endothermic reaction. Therefore, compared to the solid oxide fuel cell (SOFC) unit for power generation described in Patent Document 2, a higher current can be applied in SOEC. With cells of the same specifications, SOEC can apply approximately several times the current of SOFC.
[0008] Existing technical documents
[0009] Patent documents
[0010] Patent Document 1: Japanese Patent No. 7282968
[0011] Patent Document 2: Japanese Patent No. 5106884 Summary of the Invention
[0012] The problem that the invention aims to solve
[0013] In the SOFC of Patent Document 2, multiple battery packs are electrically connected using a thin plate current collector. The use of such a thin plate as a power supply component for the battery stack of an SOEC was investigated.
[0014] However, in SOEC, which carries a higher current compared to SOFC, the self-heating caused by the resistance of the power supply components increases proportionally to the square of the current as the current flows laterally through the power supply components, resulting in a greater temperature rise. Therefore, if the current collector components used in SOFC are directly applied to SOEC, the temperature of the power supply components may rise to levels unacceptable from the perspective of corrosion and thermal stress (exceeding 650°C). This becomes a constraint on fully utilizing the performance of the battery stack, thus requiring countermeasures.
[0015] Furthermore, the power supply components of SOEC are exposed to an atmosphere containing a high concentration of water vapor, which becomes the raw material for electrolysis. Therefore, when the temperature reaches a certain level (e.g., above approximately 500°C for SUS304 power supply plates), water vapor oxidation accelerates. If water vapor oxidation progresses, oxide scale will form and thin the power supply components. Oxide scale formation is a major cause of increased resistance at the junction with the battery stack. If wall thinning occurs, the cross-sectional area of the power supply component (thin plate) decreases, thereby increasing resistance and leading to a further rise in temperature.
[0016] This disclosure was made in view of the following circumstances, and its purpose is to provide an electrolytic cell assembly that can suppress water vapor oxidation of the power supply components, thereby solving the problem of thinning of the power supply components due to water vapor oxidation.
[0017] The purpose of this disclosure is to provide an electrolytic cell assembly that can suppress the temperature rise of the power supply component caused by water vapor oxidation to within an acceptable level, thereby solving the problem of thinning of the power supply component caused by water vapor oxidation.
[0018] Methods for solving problems
[0019] To address the aforementioned issues, the electrolytic cell assembly and its manufacturing method disclosed herein employ the following approach.
[0020] One aspect of this disclosure provides an electrolytic cell assembly comprising: a plurality of electrolytic cell stacks having electrolytic cells for electrolyzing water vapor; and a power supply board having holes for inserting the electrolytic cell stacks, wherein the plurality of electrolytic cell stacks are electrically connected by inserting the electrolytic cell stacks into the holes in the power supply board, wherein the power supply board comprises: a plate-shaped stainless steel substrate having holes for inserting the electrolytic cell stacks; and a water vapor oxidation resistance layer covering the surface of the substrate, the water vapor oxidation resistance layer being formed of a material having higher water vapor oxidation resistance than the substrate.
[0021] By applying a water vapor oxidation resistance layer to the surface of the substrate, a power supply board is created that can suppress water vapor oxidation corrosion caused by temperature rise due to self-heating of the power supply board during high current operation. Since the structure incorporates the water vapor oxidation resistance layer as part of the power supply board, cost increases are minimized even when expensive materials are used for the water vapor oxidation resistance layer. Furthermore, when a material with higher conductivity than stainless steel is used for the water vapor oxidation resistance layer, it is foreseeable that temperature rise suppression and resistance loss will be achieved by reducing the resistivity of the power supply board.
[0022] One aspect of this disclosure provides an electrolytic cell assembly comprising: a plurality of electrolytic cell stacks having an electrolytic cell for electrolyzing water vapor; and a power supply board electrically connecting the plurality of electrolytic cell stacks, the power supply board having: a plate-shaped stainless steel substrate having holes for inserting the electrolytic cell stacks; and an emissivity enhancement structure for increasing the emissivity of the power supply board on its surface.
[0023] By incorporating an emissivity-enhancing structure, the emissivity of the power supply board can be increased. This, in turn, increases the heat transfer (dissipation) generated by radiation from the surface of the power supply board, suppressing its temperature to a level acceptable even when high current is applied.
[0024] One aspect of this disclosure provides a method for manufacturing an electrolytic cell assembly comprising: a plurality of electrolytic cell stacks having an electrolytic cell for electrolyzing water vapor; and a power supply board electrically connecting the plurality of electrolytic cell stacks in parallel, the power supply board having a stainless steel plate-shaped substrate having holes for inserting the electrolytic cell stacks, wherein the surface roughness of the power supply board is increased by shot peening or grinding.
[0025] Invention Effects
[0026] This disclosure provides an electrolytic cell assembly that can suppress water vapor oxidation of power supply components by providing a water vapor oxidation resistant layer on the surface of a substrate.
[0027] This disclosure provides an electrolytic cell assembly that suppresses the temperature rise of the power supply components within an acceptable level by providing an emissivity-enhancing structure on the surface of the power supply board. Attached Figure Description
[0028] Figure 1 This is a diagram illustrating one embodiment of a cylindrical electrolytic cell stack according to the present disclosure.
[0029] Figure 2 This is a diagram illustrating one embodiment of a cylindrical electrolytic cell assembly according to the present disclosure.
[0030] Figure 3 yes Figure 2 A top-down view of the area surrounding the battery stack.
[0031] Figure 4 This is a schematic diagram illustrating the relationship between the upper power supply board and the battery stack.
[0032] Figure 5 This is a partial cross-sectional view of the power supply board according to the first embodiment.
[0033] Figure 6 This is a partial cross-sectional view of another power supply board according to the first embodiment.
[0034] Figure 7 This is a diagram illustrating one embodiment of a cylindrical electrolytic cell module according to the present disclosure.
[0035] Figure 8 This is a partial cross-sectional view of the power supply board according to the second embodiment.
[0036] Figure 9 It is a graph showing the relationship between the power supply board temperature and the heat transferred from the power supply board.
[0037] Figure 10 This is a graph representing an estimated example of the temperature reduction effect of increased emissivity on the power supply board.
[0038] Figure 11 This is a schematic diagram illustrating radiative heat transfer in the lower power supply board.
[0039] Figure 12 This is a graph showing the relationship between the surface roughness Rz of each test object and the rate of increase in emissivity. Detailed Implementation
[0040] Hereinafter, an embodiment of the electrolytic cell assembly and its manufacturing method of the present disclosure will be described with reference to the accompanying drawings.
[0041] The electrolytic cell assembly disclosed herein includes multiple electrolytic cell stacks and a power supply board that connects the multiple electrolytic cell stacks in parallel.
[0042] For ease of explanation, the positional relationships of the constituent elements described below, using "up" and "down" as a reference on the paper, are respectively represented as the vertical upper side and the vertical lower side. In this embodiment, when the same effect is obtained in the vertical and horizontal directions, the vertical direction on the paper is not necessarily limited to the vertical vertical direction; for example, it may correspond to the horizontal direction orthogonal to the vertical direction.
[0043] [First Implementation]
[0044] (Electrolytic cell stack)
[0045] First, refer to Figure 1 As an example of this embodiment, a cylindrical electrolytic cell stack (hereinafter referred to as a battery stack) using a substrate tube will be described. In the absence of a substrate tube, for example, the fuel electrode can be formed thicker and also serve as a substrate tube; the use of a substrate tube is not limited. In this embodiment, a cylindrical substrate tube will be used, but any cylindrical substrate tube is acceptable, and the cross-section is not necessarily limited to a circle; for example, it can also be elliptical. A flat tubular battery stack, formed by vertically flattening the circumferential side of a cylinder, is also possible. Here, Figure 1 This is a diagram illustrating one embodiment of a battery stack. As an example, the battery stack 101 includes a cylindrical substrate tube 103, a plurality of electrolytic cells 105 formed on the outer peripheral surface of the substrate tube 103, and interconnects 107 formed between adjacent electrolytic cells 105. Each electrolytic cell 105 is formed by stacking a hydrogen electrode 109, a solid electrolyte membrane 111, and an oxygen electrode 113. The battery stack 101 includes a lead film 115 electrically connected via the interconnects 107 to the oxygen electrode 113 of the electrolytic cell 105 formed on the outer peripheral surface of the substrate tube 103, which is formed axially at one end of the substrate tube 103, and also includes a lead film 115 electrically connected to the hydrogen electrode 109 formed at the other end of the electrolytic cell 105.
[0046] The substrate tube 103 is made of a porous material, such as CaO-stabilized ZrO2 (CSZ), a mixture of CSZ and nickel oxide (NiO) (CSZ+NiO), Y2O3-stabilized ZrO2 (YSZ), or MgAl2O4 as the main components. The substrate tube 103 supports the electrolytic cell 105, the interconnect 107, and the lead film 115, and allows the water vapor supplied to the inner peripheral surface of the substrate tube 103 to diffuse through the fine pores of the substrate tube 103 to the hydrogen electrode 109 formed on the outer peripheral surface of the substrate tube 103.
[0047] The hydrogen electrode 109 is composed of an oxide of a composite material of Ni and a zirconium oxide-based electrolyte material, such as Ni / YSZ. The thickness of the hydrogen electrode 109 is 50 μm to 250 μm, and the hydrogen electrode 109 can be formed by screen printing a paste.
[0048] The solid electrolyte membrane 111 primarily uses YSZ, which possesses excellent gas tightness and high oxygen ion conductivity at high temperatures. This solid electrolyte membrane 111 allows oxygen ions (O2) generated at the hydrogen electrode 109 to... 2- The hydrogen electrode 109 moves to the oxygen electrode 113. The solid electrolyte membrane 111 on the surface of the hydrogen electrode 109 has a thickness of 5 μm to 100 μm and can be formed by screen printing the paste.
[0049] The oxygen electrode 113 is composed, for example, of LaSrMnO3-based oxides or LaCoO3-based oxides. For the oxygen electrode 113, a slurry-like material is coated using screen printing or a distributor. The oxygen electrode 113 can also be a two-layer structure. In this case, the oxygen electrode layer (oxygen electrode intermediate layer) on the solid electrolyte membrane 111 side is composed of a material exhibiting high ionic conductivity and excellent catalytic activity. The oxygen electrode intermediate layer can be composed of Sm-doped cerium dioxide exhibiting high ionic conductivity, and the oxygen electrode layer (oxygen electrode conductive layer) above the oxygen electrode intermediate layer can be composed of perovskite-type oxides such as Sr and Ca-doped LaMnO3.
[0050] In addition to the water vapor used in electrolysis, most of the gases supplied to / discharged from the hydrogen electrode 109 contain hydrogen. However, in the following description, to avoid confusion, the supply gas containing hydrogen will be referred to as "supply water vapor", and the hydrogen gas containing water vapor discharged from the hydrogen electrode 109 will be referred to as "generated hydrogen".
[0051] By applying a negative voltage to the hydrogen electrode 109 and a positive voltage to the oxygen electrode 113, the water vapor contained in the supplied water vapor is electrolyzed by accepting electrons in the hydrogen electrode 109, generating hydrogen molecules and oxygen ions (O2). 2- (Refer to the following reaction formula (1)). The generated hydrogen is extracted to the outside along with the supplied water vapor.
[0052] On the other hand, due to the potential difference, oxygen ions move through the solid electrolyte membrane 111 to the oxygen electrode 113, releasing electrons to become oxygen molecules (refer to reaction formula (2) below). The generated oxygen, together with the oxidizing gas supplied to the oxygen electrode 113, is discharged to the outside.
[0053] H2O + 2e - →H2+O 2- ...(1)
[0054] 2O 2- →O2+4e - ...(2)
[0055] Oxidizing gases do not directly participate in the electrolysis reaction, but they supply the heat required for the electrolysis reaction (endothermic) and remove the residual heat generated during the electrolysis reaction. They are typically gases containing approximately 15% to 30% oxygen, with air being the most preferred. However, in addition to air, mixtures of combustion exhaust gas and air, mixtures of oxygen and air, and inert gases such as nitrogen can also be used.
[0056] Interconnector 107 is made of SrTiO3 or similar M 1-x L x The conductive perovskite-type oxide, represented by TiO3 (M being an alkaline earth metal element and L being a lanthanide element) and lanthanum chromate (LaCrO3), is used to screen print the slurry-like material. The interconnect 107 is a dense film to prevent the supply of water vapor from mixing with the oxidizing gas. The interconnect 107 exhibits stable durability and electronic conductivity in both oxidizing and reducing atmospheres. In adjacent electrolytic cells 105, the interconnect 107 electrically connects the oxygen electrode 113 of one electrolytic cell 105 to the hydrogen electrode 109 of another electrolytic cell 105, thus connecting the adjacent electrolytic cells 105 in series.
[0057] The lead film 115 needs to possess electronic conductivity and a coefficient of thermal expansion close to that of other materials constituting the battery stack 101. Therefore, it is made of composite materials of Ni and zirconium oxide electrolytes such as Ni / YSZ, or SrTiO3-based electrolytes. 1-x L x It is composed of TiO3 (M is an alkaline earth metal element, L is a lanthanide element). The lead film 115 connects multiple electrolytic cells 105 in series via interconnect 107, applying the DC power required for the electrolysis reaction to the end of the battery stack 101. In order to prevent the metal materials such as Ni from being oxidized, the surface on the oxidizing gas side can be protected with an hermetically sealed oxidation-resistant material.
[0058] (Electrolyte cell assembly)
[0059] like Figure 2 As shown, the electrolytic cell assembly (hereinafter referred to as the assembly) 203 includes multiple battery stacks 101, a steam electrolysis chamber 215, a steam supply manifold 217, a hydrogen generation discharge manifold 219, an oxidizing gas (air) supply manifold 221, an oxidizing gas discharge manifold 223, and a power supply unit. The assembly 203 includes an upper tube sheet 225a, a lower tube sheet 225b, an upper heat insulation body 227a, and a lower heat insulation body 227b. It should be noted that, in this embodiment, the assembly 203 utilizes... Figure 2The configuration of the water vapor supply manifold 217, the hydrogen generation discharge manifold 219, the oxidizing gas supply manifold 221, and the oxidizing gas discharge manifold 223 creates a structure in which water vapor and oxidizing gas flow opposite to each other on the inner and outer sides of the battery stack 101. However, this is not necessarily required. For example, the water vapor and oxidizing gas can also flow parallel to each other on the inner and outer sides of the battery stack 101, or the oxidizing gas can flow in a direction orthogonal to the long dimension of the battery stack 101.
[0060] The steam electrolysis chamber 215 is the region formed between the upper insulation body 227a and the lower insulation body 227b. This steam electrolysis chamber 215 is the area of the electrolytic cell 105 where the battery stack 101 is located, and it is the area where water vapor is electrolyzed to generate hydrogen. The temperature near the center of the battery stack 101 in the longitudinal direction of the steam electrolysis chamber 215 can be monitored using a temperature measuring unit 620 (temperature sensor, thermocouple, etc.), and during stable operation of the module 201 (described later), it becomes a high-temperature atmosphere of approximately 700°C to 1000°C.
[0061] The steam supply manifold 217 is the area surrounded by the upper housing 229a and the upper tube sheet 225a of the assembly 203. It is connected to the steam supply branch pipe 207a (described later) via a steam supply pipe 231a located on the upper part of the upper housing 229a. The multiple battery stacks 101 are connected to the upper tube sheet 225a via an upper sealing member 237a. The steam supply manifold 217 guides the steam supplied from the steam supply branch pipe 207a via the steam supply pipe 231a into the interior of the base tube 103 of the multiple battery stacks 101 at a substantially uniform flow rate, thereby making the hydrogen production performance of the multiple battery stacks 101 substantially uniform.
[0062] The hydrogen generation discharge manifold 219 is the area surrounded by the lower housing 229b and lower tube sheet 225b of the assembly 203. It is connected to the hydrogen generation discharge branch pipe 209a (described later) via the hydrogen generation discharge pipe 231b provided in the lower housing 229b. Multiple battery stacks 101 are connected to the lower tube sheet 225b via a lower sealing member 237b. The hydrogen generation manifold 219 receives the hydrogen generation collected from the interior of the base tubes 103 of the multiple battery stacks 101 and supplies it to the hydrogen generation discharge manifold 219, which is then guided to the hydrogen generation discharge branch pipe 209a via the hydrogen generation discharge pipe 231b.
[0063] The oxidizing gas supply main pipe (not shown) branches off to the oxidizing gas supply branch pipe (not shown) at a specified flow rate corresponding to the operating temperature of module 201, and supplies gas to multiple components 203. The oxidizing gas supply manifold 221 is the area surrounded by the lower housing 229b, lower tube sheet 225b, and lower insulation 227b of component 203, and is connected to the oxidizing gas supply branch pipe (not shown) via an oxidizing gas supply pipe 233a located on the side of the lower housing 229b. This oxidizing gas supply manifold 221 guides the oxidizing gas supplied at a specified flow rate via the oxidizing gas supply branch pipe (not shown) through the oxidizing gas supply pipe 233a to the steam electrolysis chamber 215 via the lower oxidizing gas through-hole 235a (described later).
[0064] The oxidizing gas exhaust manifold 223 is the area surrounded by the upper shell 229a, upper tube sheet 225a, and upper insulation 227a of the assembly 203. It is connected to an oxidizing gas exhaust branch pipe (not shown) via an oxidizing gas exhaust pipe 233b located on the side of the upper shell 229a. Oxidizing gas exhaust supplied from the steam electrolysis chamber 215 via the oxidizing gas upper through-hole 235b (described later) is guided through the oxidizing gas exhaust pipe 233b to the oxidizing gas exhaust branch pipe (not shown).
[0065] Power supply boards (power supply units) are respectively disposed on the upper and lower ends of the battery stack 101, and the multiple battery stacks 101 are connected in parallel to ground.
[0066] The upper power supply plate (upper power supply plate) 11a is disposed within the steam supply manifold 217. The upper power supply plate 11a has a plurality of holes for inserting the battery stack 101. The number of holes corresponds to the number of battery stacks 101.
[0067] Figure 3 express Figure 2 A top-down view of the area surrounding the battery stack. Figure 4 This is a schematic diagram illustrating the relationship between the upper power supply board and the battery stack. The upper power supply board supplies power by contacting the lead film 115 of the battery stack 101 with an elastic force (elastic force generating part 13) generated by bending a part of the power supply board.
[0068] One end of the conductive member 12a is joined to the upper power supply board 11a. The other end of the conductive member 12a passes through the upper housing 229a and is connected to an electrode terminal (not shown) located on the outside of the assembly 203.
[0069] The lower power supply plate (lower power supply plate) 11b is disposed within the hydrogen generation discharge manifold 219. The lower power supply plate 11b has a plurality of holes for insertion of the battery stack 101. The number of holes corresponds to the number of battery stacks 101.
[0070] The lower power supply board 11b, like the upper power supply board 11a, supplies power by contacting the lead film 115 of the battery stack 101 with the elastic force generated by bending a part of the power supply board.
[0071] One end of a conductive member 12b is joined to the lower power supply board 11b. The other end of the conductive member 12b passes through the lower housing 229b and is connected to an electrode terminal (not shown) located on the outside of the assembly 203.
[0072] In each component 203, power is supplied to the electrolytic cells 105 of each battery stack 101 via the upper power supply board 11a and the lower power supply board 11b.
[0073] Figure 5 This is a partial cross-sectional view of the power supply board. The power supply board (upper power supply board 11a and lower power supply board 11b) has a substrate 20 and a water vapor oxidation resistance layer 21. The substrate 20 is a thin sheet of stainless steel. Although in Figure 5 Not shown in the figure, but formed on the substrate 20 with Figure 3 The holes correspond to multiple holes into which the battery stack 101 is inserted.
[0074] The water vapor oxidation resistance layer 21 is provided to cover the surface of the substrate 20. It is preferable that the water vapor oxidation resistance layer 21 covers both sides of the substrate 20. The water vapor oxidation resistance layer 21 is made of a material with higher water vapor corrosion resistance than stainless steel, which is the material of the substrate 20. By covering the surface of the substrate 20 with the water vapor oxidation resistance layer 21, the water vapor oxidation resistance of the power supply board at high temperatures can be ensured.
[0075] The material of the water vapor oxidation resistance layer 21 can be nickel, titanium or copper.
[0076] Compared to stainless steel, nickel has higher resistance to water vapor oxidation and higher conductivity. Therefore, it can reduce the resistivity of the power supply board. However, the strength of nickel decreases significantly at high temperatures, so it cannot be used as a power supply board on its own. But by providing a water vapor oxidation resistance layer 21 on the surface of the substrate 20, the strength of the power supply board at high temperatures can be ensured, and the water vapor oxidation resistance of the power supply board can be improved.
[0077] Titanium, with a thickness of only tens of μm, can prevent oxidation by water vapor. While titanium is an expensive material, in this embodiment, it is only applied to the surface of the power supply board, thus reducing costs compared to using titanium alone to fabricate the power supply board.
[0078] The power supply board can be a structure (composite steel) formed by bonding the substrate 20 to the water vapor oxidation resistance layer 21 through cold pressing or the like. The power supply board can also be a structure in which the water vapor oxidation resistance layer 21 is plated on the surface of the substrate 20.
[0079] It should be noted that, as Figure 6 As shown, the power supply boards (upper power supply board 11a and lower power supply board 11b) may have a conductive layer 22 between the substrate 20 and the water vapor oxidation resistance layer 21. The conductive layer 22 is made of a material with a higher conductivity than stainless steel, which is the material of the substrate 20. The material of the conductive layer 22 may be copper. By providing the conductive layer 22, the resistance of the power supply board is reduced.
[0080] The upper tube sheet 225a is located between the top plate of the upper housing 229a and the upper insulation 227a, and is fixed to the side plate of the upper housing 229a in a manner that is substantially parallel to the upper tube sheet 225a, the top plate of the upper housing 229a, and the upper insulation 227a. The upper tube sheet 225a has a plurality of holes corresponding to the number of battery stacks 101 included in the assembly 203, and each battery stack 101 is inserted into a hole. The upper tube sheet 225a hermetically supports one end of the plurality of battery stacks 101 via either or both of the upper sealing member 237a and the adhesive member, and isolates the water vapor supply manifold 217 from the oxidizing gas exhaust manifold 223.
[0081] The upper heat insulation body 227a is arranged substantially parallel to the top plate of the upper heat insulation body 227a, the upper shell 229a, and the upper tube sheet 225a at the lower end of the upper shell 229a, and is fixed to the side plate of the upper shell 229a. The upper heat insulation body 227a has multiple holes corresponding to the number of battery stacks 101 included in the assembly 203. The diameter of these holes is set to be larger than the outer diameter of the battery stacks 101. The upper heat insulation body 227a has an oxidizing gas upper passage 235b formed between the inner surface of the holes and the outer surface of the battery stacks 101 inserted into the upper heat insulation body 227a.
[0082] The upper insulation 227a separates the steam electrolysis chamber 215 from the oxidizing gas discharge manifold 223, suppressing the high temperature of the atmosphere surrounding the upper tube sheet 225a, which would reduce its strength and increase corrosion caused by the oxidizing agent contained in the oxidizing gas. To suppress thermal deformation of the upper tube sheet 225a and other components exposed to the high temperature within the steam electrolysis chamber 215 due to temperature differences, a high-temperature durable metal material such as a Ni-based alloy can be used. The upper insulation 227a guides the exhaust gas from the steam electrolysis chamber 215, exposed to high temperatures, through the upper oxidizing gas passage 235b to the oxidizing gas discharge manifold 223.
[0083] According to this embodiment, through the structure of the aforementioned component 203, water vapor and oxidizing gas are supplied to flow oppositely inside and outside the battery stack 101. As a result, heat exchange occurs between the exhaust oxidizing gas and the water vapor supplied to the water vapor electrolysis chamber 215 through the interior of the base tube 103, cooling the upper tube sheet 225a, etc., made of metallic material, to a temperature that prevents damage caused by stress, and supplying it to the oxidizing gas exhaust manifold 223. The supplied water vapor is heated by heat exchange with the exhaust oxidizing gas discharged from the water vapor electrolysis chamber 215 and then supplied to the water vapor electrolysis chamber 215. Consequently, water vapor that is preheated to the temperature required for the electrolysis reaction without the use of a heater or the like can be supplied to the water vapor electrolysis chamber 215.
[0084] The lower tube sheet 225b is fixed to the side plate of the lower housing 229b between the bottom plate of the lower housing 229b and the lower insulation 227b, in a manner that is substantially parallel to the lower tube sheet 225b, the bottom plate of the lower housing 229b, and the lower insulation 227b. The lower tube sheet 225b has a plurality of holes corresponding to the number of battery stacks 101 included in the assembly 203, and each battery stack 101 is inserted into a hole. The lower tube sheet 225b hermetically supports the other end of the plurality of battery stacks 101 via either or both of the lower sealing member 237b and the adhesive member, and isolates the hydrogen generation exhaust manifold 219 from the oxidizing gas supply manifold 221.
[0085] The lower heat insulation body 227b is arranged substantially parallel to the bottom plate of the lower heat insulation body 227b, the lower housing 229b, and the lower tube sheet 225b at the upper end of the lower housing 229b, and is fixed to the side plate of the lower housing 229b. The lower heat insulation body 227b has multiple holes corresponding to the number of battery stacks 101 included in the assembly 203. The diameter of these holes is set to be larger than the outer diameter of the battery stacks 101. The lower heat insulation body 227b has an oxidizing gas lower penetration portion 235a formed between the inner surface of the holes and the outer surface of the battery stacks 101 inserted into the lower heat insulation body 227b.
[0086] The lower insulation 227b separates the steam electrolysis chamber 215 from the oxidizing gas supply manifold 221, preventing the surrounding atmosphere of the lower tube sheet 225b from becoming too hot, thus reducing its strength and increasing corrosion caused by the oxidizing agent contained in the oxidizing gas. To suppress thermal deformation of the lower tube sheet 225b and other components exposed to the high temperatures within the steam electrolysis chamber 215 due to temperature differences, a high-temperature durable metal material such as a Ni-based alloy can be used. The lower insulation 227b allows the oxidizing gas supplied to the oxidizing gas supply manifold 221 to be introduced into the steam electrolysis chamber 215 through the lower oxidizing gas passage 235a.
[0087] According to this embodiment, through the structure of the aforementioned component 203, generated hydrogen and oxidizing gas flow opposite each other inside and outside the battery stack 101. As a result, heat exchange occurs between the generated hydrogen passing through the interior of the base tube 103 and the steam electrolysis chamber 215, and the oxidizing gas supplied to the steam electrolysis chamber 215. This cools the lower tube sheet 225b, etc., made of metallic material, to a temperature that prevents damage caused by stress, and supplies it to the generated hydrogen discharge manifold 219. The oxidizing gas is heated through heat exchange with the generated hydrogen and supplied to the steam electrolysis chamber 215. Consequently, oxidizing gas heated to the temperature required for the electrolysis reaction can be supplied to the steam electrolysis chamber 215 without using a heater or the like.
[0088] (Electrolyte cell module)
[0089] like Figure 7 As shown, the electrolytic cell module (hereinafter referred to as module) 201 includes, for example, multiple components 203 and a module container 205 for housing these multiple components 203. Module 201 includes a steam supply main pipe 207 and multiple steam supply branch pipes 207a, as well as a hydrogen generation discharge main pipe 209 and multiple hydrogen generation discharge branch pipes 209a. Module 201 includes an oxidizing gas supply main pipe (not shown) and multiple oxidizing gas supply branch pipes (not shown).
[0090] A steam supply main pipe 207 is located inside the module container 205, connected to a steam supply section that supplies steam with a specified gas composition and flow rate corresponding to the hydrogen production of module 201, and connected to multiple steam supply branch pipes 207a. The steam supply main pipe 207 branches off and guides the specified flow rate of steam supplied from the steam supply section to the multiple steam supply branch pipes 207a. The steam supply branch pipes 207a are connected to the steam supply main pipe 207 and to the steam supply pipes 231a of multiple components 203. The steam supply branch pipes 207a guide the steam supplied from the steam supply main pipe 207 to the multiple components 203 at approximately equal flow rates, thereby substantially homogenizing the electrolysis voltage of the multiple components 203.
[0091] A hydrogen generation outlet branch pipe 209a is connected to hydrogen generation outlet pipes 231b of multiple components 203 and to a hydrogen generation outlet main pipe 209. This hydrogen generation outlet branch pipe 209a guides the hydrogen generation discharged from components 203 to the hydrogen generation outlet main pipe 209. The hydrogen generation outlet main pipe 209 is connected to multiple hydrogen generation outlet branch pipes 209a and is partially disposed outside the module container 205. This hydrogen generation outlet main pipe 209 guides the hydrogen generation discharged from the hydrogen generation outlet branch pipes 209a at approximately equal flow rates to the outside of the module container 205.
[0092] The modular container 205 is used when the internal pressure is atmospheric pressure to several MPa and the surface temperature is atmospheric temperature to about 300°C. For example, from the point of view of cost reduction, carbon steel is preferred.
[0093] In this embodiment, a scheme in which multiple components 203 are aggregated and housed in module container 205 is described, but it is not limited to this. For example, a scheme in which components 203 are not aggregated and housed in module container 205 is also possible.
[0094] The DC power required for the electrolysis reaction is converted into a specified voltage by a power conversion device such as a power regulator and supplied to module 201. The power supplied to module 201 is determined according to the number of series and parallel connections of each component. In each component 203, power is supplied via power supply boards (upper power supply board 11a and lower power supply board 11b), and then supplied to the electrolytic cells 105 after being energized through lead films 115 made of Ni / YSZ or the like, which are located in multiple electrolytic cells 105.
[0095] [Second Implementation]
[0096] The power supply board (upper power supply board and lower power supply board) of the components in this embodiment has a different structure than that in the first embodiment. The configuration of the power supply board is the same as that in the first embodiment.
[0097] Figure 8 A partial cross-sectional view of the power supply board of this embodiment is shown as an example.
[0098] In this embodiment, the power supply board 30 is a thin plate-shaped substrate 32 with an emissivity-enhancing structure 31 on its surface. Like the substrate 20 in the first embodiment, the substrate 32 has a plurality of holes corresponding to the number of battery stacks 101. The substrate 32 is made of stainless steel.
[0099] Emissivity Enhancement Structure 31 is a structure that enhances the emissivity of the power supply board surface.
[0100] For example, the emissivity-enhancing structure 31 can be an uneven structure formed on the surface of the substrate. By increasing the surface roughness of the substrate 32, the emissivity can be increased. This uneven structure can be formed by shot peening or grinding. For example, the emissivity-enhancing structure 31 can be a heat-dissipating coating applied to the surface of the substrate. It should be noted that... Figure 8 The emissivity enhancement structure 31 of the power supply board 30 described herein is an uneven structure formed on the surface of the substrate.
[0101] It should be noted that the emissivity-enhancing structure 31 can also be applied to the power supply board of the first embodiment. In this case, for example, after covering the surface of the substrate with the water vapor oxidation resistance layer 21, an uneven surface is formed on the surface of the water vapor oxidation resistance layer 21, which becomes the surface of the power supply board. Thus, a power supply board with an emissivity-enhancing structure can be obtained.
[0102] The effects of the power supply board in this embodiment will be explained below.
[0103] (Radiative heat transfer)
[0104] The temperature of the power supply board is determined by the convective heat transfer with the surrounding gas and the heat transfer generated by the radiative heat transfer to the surrounding components.
[0105] The heat transfer Q from the power supply board to the heated object can be calculated using the Stefan-Boltzmann equation (3).
[0106] Q=ε・E G ・σA(T1 4 -T2 4 )……(3)
[0107] Q: Radiative heat transfer (W / m²) 2 )
[0108] ε: emissivity
[0109] E G Morphological coefficients
[0110] σ: Stefan-Boltzmann coefficient (=5.67032×10) -8 W / m 2 ・K 4 )
[0111] A: Surface area of the sample (m²) 2 )
[0112] T1: Absolute temperature of the power supply board (K)
[0113] T2: Absolute temperature (K) of the object on the heated side.
[0114] The following comparison of convective heat transfer and radiative heat transfer is performed using equation (3). It is assumed that the highest temperature T1 of the power supply board is above 500℃, the ambient temperature around the power supply board and the temperature T2 of the object on the heated side are both 500℃ (constant), and the convective heat transfer rate is 5 W / m. 2 K, morphological coefficient E G The value is 1, and the sample surface area A is 1. The atmosphere temperature inside the modular container of the housing component is approximately 400℃.
[0115] Figure 9 The results are shown. Figure 9 This is a graph showing the relationship between the power supply board temperature and the heat transferred from the power supply board. Figure 9 In the diagram, the horizontal axis represents the power supply board temperature (°C), and the vertical axis represents the heat transfer from the power supply board (kW / m²). 2 The solid line represents convective heat transfer, the dashed line represents radiative heat transfer (emissivity 0.1), and the dotted line represents radiative heat transfer (emissivity 0.3).
[0116] The higher the temperature of the power supply board, the more heat is transferred from it. According to... Figure 9 When comparing at the same temperature, the higher the temperature, the greater the difference between the heat transfer generated by convection and the heat transfer generated by radiation. If the temperature of the power supply board is 600℃, then the heat transfer by radiation is about three times that by convection. Therefore, it can be seen that by increasing the emissivity ε of the power supply board surface, the heat transfer generated by radiation can be increased, effectively suppressing the temperature rise of the power supply board.
[0117] Figure 10 This figure shows an estimation example of the temperature reduction effect of the power supply board caused by the increase in emissivity. In this figure, the horizontal axis represents the emissivity of the power supply board and the object on the heated side, and the vertical axis represents the temperature of the power supply board (°C).
[0118] according to Figure 10 By increasing the emissivity from 0.1 to 0.3, a temperature reduction effect of approximately 100°C is expected.
[0119] Figure 11 This is a schematic diagram illustrating radiative heat transfer in the lower power supply board 11b. The heat (RH) radiated from the lower power supply board 11b moves to the lower tube sheet 225b and the hydrogen generation discharge manifold 219, and is then dissipated from the module to the outside through heat conduction and heat transfer.
[0120] However, the heat from the power supply board is relatively small compared to the heat that would normally dissipate to the outside of the module from the lower tube sheet 225b and the hydrogen generation exhaust manifold 219 through heat transfer and conduction. Therefore, by increasing the emissivity of the power supply board, the effects of temperature rise in the lower tube sheet 225b and the hydrogen generation exhaust manifold 219 can be ignored.
[0121] Emissivity can be increased by surface treatment of the power supply board to increase surface roughness.
[0122] (Surface treatment and emissivity)
[0123] To evaluate the effect of surface treatment on emissivity, elemental tests were conducted. A substrate (Ni-SUS304-Ni, 50 μm thick Ni layer) with Ni layers on both sides was surface-treated to create test specimens with an uneven texture, and emissivity was measured using a radiometer. Surface treatment was performed by grinding or shot peening. For comparison, the emissivity of untreated test specimens was also measured.
[0124] The results are shown in Figure 12 In this figure, the horizontal axis represents the surface roughness Rz (μm), and the vertical axis represents the emissivity ratio. The emissivity ratio is the ratio with the untreated material set to 1.
[0125] according to Figure 12 Compared with the untreated test specimens, the test specimens with an uneven surface texture formed by surface treatment have higher emissivity, and the emissivity ratio also shows an increasing trend as the surface roughness increases.
[0126] <Postscript>
[0127] The electrolytic cell assembly and its manufacturing method described in the above-described embodiments are as follows.
[0128] The first embodiment of this disclosure includes an electrolytic cell assembly comprising: a plurality of electrolytic cell stacks (101) having an electrolytic cell (105); and a power supply plate (11a, 11b) having holes for insertion of the electrolytic cell stacks, wherein the plurality of electrolytic cell stacks are electrically connected by inserting the electrolytic cell stacks into the holes in the power supply plate (11a, 11b), wherein the power supply plate comprises: a stainless steel plate-shaped substrate (20) having holes for insertion of the electrolytic cell stacks; and a water vapor oxidation resistance layer (21) covering the surface of the substrate, the water vapor oxidation resistance layer being formed of a material having higher water vapor oxidation resistance than the substrate.
[0129] By applying a water vapor oxidation resistance layer to the surface of the substrate, a power supply board is created that can suppress water vapor oxidation corrosion caused by temperature rise during high current operation. Since the structure incorporates the water vapor oxidation resistance layer as part of the power supply board, cost increases are minimized even when expensive materials are used for the water vapor oxidation resistance layer. Furthermore, when a material with higher conductivity than stainless steel is used for the water vapor oxidation resistance layer, it is foreseeable that temperature rise suppression and resistance loss will be achieved by reducing the resistivity of the power supply board.
[0130] For the electrolytic cell assembly of the second aspect of this disclosure, in the first aspect described above, the material of the water vapor oxidation resistance layer is selected from nickel, titanium, and copper.
[0131] Nickel, titanium, and copper all have higher resistance to water vapor oxidation than stainless steel. Nickel and copper have higher electrical conductivity than stainless steel. Nickel cannot be used alone as a power supply board because its strength decreases significantly at high temperatures. However, by applying it as a water vapor oxidation resistant layer on the surface of the substrate, its strength at high temperatures can be ensured, and the water vapor oxidation resistance of the power supply board can be improved.
[0132] For the electrolytic cell assembly of the third aspect of this disclosure, in the first or second aspect described above, the power supply board has a conductive layer (22) formed of a material with a higher conductivity than the substrate between the substrate and the water vapor oxidation resistance layer.
[0133] By adding a conductive layer, the conductivity of the power supply board can be reliably improved.
[0134] The fourth embodiment of the present disclosure includes an electrolytic cell assembly comprising: a plurality of electrolytic cell stacks having electrolytic cells; and a power supply board for electrically connecting the plurality of electrolytic cell stacks in parallel, the power supply board having: a plate-shaped stainless steel substrate having holes for inserting the electrolytic cell stacks; and an emissivity enhancement structure (31) for enhancing the emissivity of the power supply board on its surface.
[0135] By incorporating an emissivity-enhancing structure, the emissivity of the power supply board can be increased. This, in turn, increases the heat transfer generated by radiative heat transfer from the surface of the power supply board, reducing its temperature to a level acceptable even when high current is applied.
[0136] For the electrolytic cell assembly of the fifth embodiment of this disclosure, in the fourth embodiment described above, the emissivity enhancement structure is an irregularity provided on the surface of the power supply board.
[0137] By adding bumps and grooves to increase the surface roughness of the power supply board, the emissivity of the power supply board is increased.
[0138] The method for manufacturing an electrolytic cell assembly according to the sixth aspect of this disclosure includes: a plurality of electrolytic cell stacks having electrolytic cells; and a power supply board electrically connecting the plurality of electrolytic cell stacks, the power supply board having a stainless steel plate-shaped substrate having holes for insertion of the electrolytic cell stacks, wherein the surface roughness of the power supply board is increased by shot peening or grinding in the method for manufacturing the electrolytic cell assembly.
[0139] Explanation of reference numerals in the attached figures
[0140] 11a, 11b, 30: Power supply board;
[0141] 12a, 12b: Conductive components;
[0142] 13: Elastic force generating part;
[0143] 20, 32: Substrate;
[0144] 21: Water vapor oxidation resistant layer;
[0145] 22: Conductive layer;
[0146] 31: Emissivity-enhancing structures;
[0147] 101: Battery stack (electrolytic battery stack);
[0148] 103: Matrix tube;
[0149] 105: Electrolytic cell;
[0150] 107: Interconnector;
[0151] 109: Hydrogen electrode (fuel electrode);
[0152] 111: Solid electrolyte membrane;
[0153] 113: Oxygen pole;
[0154] 115: Lead film;
[0155] 201: Module (Electrolytic Cell Module);
[0156] 203: Components (electrolyte cell components);
[0157] 205: Module container;
[0158] 207: Steam supply main pipe;
[0159] 207a: Steam supply branch pipe;
[0160] 209: Hydrogen is generated and discharged from the main pipe;
[0161] 209a: Hydrogen generation outlet branch pipe;
[0162] 215: Steam electrolysis chamber;
[0163] 217: Steam supply manifold;
[0164] 219: Hydrogen is generated and discharged from the manifold;
[0165] 221: Oxidizing gas supply manifold;
[0166] 223: Oxidizing gas exhaust manifold;
[0167] 225a: Upper tube sheet;
[0168] 225b: Lower tube sheet;
[0169] 227a: Upper insulation;
[0170] 227b: Lower insulation;
[0171] 229a: Upper shell;
[0172] 229b: Lower shell;
[0173] 231a: Steam supply pipe;
[0174] 231b: Hydrogen emission tube;
[0175] 233a: Oxidizing gas supply pipe;
[0176] 233b: Oxidizing gas exhaust pipe;
[0177] 235a: Lower penetration section for oxidizing gases;
[0178] 235b: Upper penetration section for oxidizing gas;
[0179] 237a: Upper sealing component;
[0180] 237b: Lower sealing component;
[0181] 620: Thermometer measuring part.
Claims
1. An electrolytic cell assembly, comprising: Multiple electrolytic cell stacks, including electrolytic cells for electrolyzing water vapor; and A power supply board has holes for inserting the electrolytic cell stacks, wherein multiple electrolytic cell stacks are electrically connected by inserting the electrolytic cell stacks into the holes. The power supply board comprises: a stainless steel plate-shaped substrate having holes for insertion of the electrolytic cell stack; and a water vapor oxidation-resistant layer covering the surface of the substrate. The water vapor oxidation resistance layer is formed of a material with higher water vapor oxidation resistance than the substrate.
2. The electrolytic cell assembly according to claim 1, wherein, The material of the water vapor oxidation resistance layer is selected from nickel, titanium, and copper.
3. The electrolytic cell assembly according to claim 1, wherein, The power supply board has a conductive layer formed of a material with a higher conductivity than the substrate between the substrate and the water vapor oxidation resistance layer.
4. An electrolytic cell assembly, comprising: Multiple electrolytic cell stacks, each containing an electrolytic cell for electrolyzing water vapor; and a power supply board electrically connecting the multiple electrolytic cell stacks. The power supply board has: a plate-shaped stainless steel substrate with holes for insertion of the electrolytic cell stack; and an emissivity-enhancing structure for increasing the emissivity of the power supply board on its surface.
5. The electrolytic cell assembly according to claim 4, wherein, The emissivity enhancement structure is an irregularity or undulation on the surface of the power supply board.
6. A method for manufacturing an electrolytic cell assembly, the assembly comprising: a plurality of electrolytic cell stacks, each having an electrolytic cell for electrolyzing water vapor; and a power supply board for electrically connecting the plurality of electrolytic cell stacks in parallel, the power supply board having a stainless steel plate-shaped substrate, the substrate having holes for inserting the electrolytic cell stacks, wherein in the method for manufacturing the electrolytic cell assembly, The surface roughness of the power supply board is increased by sandblasting or grinding.