A porous graphite adsorbent material filter tube assembly and its preparation method
By preparing porous graphite adsorption material filter tube assemblies, the problems of insufficient temperature resistance, limited pressure bearing capacity, single function, and insufficient pore size control precision of existing graphite filter tube assemblies have been solved. Stable operation and precise filtration and adsorption effects at high temperatures have been achieved, and production costs have been reduced.
Patent Information
- Application Number
- CN202611471790.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing graphite filter tube assemblies suffer from insufficient temperature resistance, limited pressure resistance, single function, insufficient pore size control precision, and high cost due to reliance on imports.
Using calcined petroleum coke or pitch coke as aggregate, combined with pore-forming agents and coal tar pitch binders, porous graphite adsorbent material filter tube components are prepared through isostatic pressing and segmented sintering processes to achieve precise pore size control and adsorption and decolorization functions.
It can operate stably for a long time under high temperature conditions of 400~550℃, has high mechanical strength and precise pore size, and has the functions of physical filtration and adsorption decolorization, reducing production costs and delivery cycle.
Smart Images

Figure CN123102040A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new materials technology, and in particular to a porous graphite adsorption material filter tube assembly and its preparation method. Background Technology
[0002] In fluid handling processes in industries such as chemical, pharmaceutical, and food processing, it is often necessary to adsorb, decolorize, and precisely filter materials under high-temperature and high-pressure conditions. Graphite materials are widely used in the manufacture of filtration and adsorption components for high-temperature applications due to their excellent high-temperature resistance, chemical stability, and good electrical and thermal conductivity.
[0003] Currently, the main technical solutions for graphite filter tube assemblies used in fluid processing fall into the following categories: Filtering devices for graphite heat exchangers. Existing technologies include filtration devices installed in graphite heat exchangers, using filter boxes or screens at the feed end to perform preliminary filtration of materials entering the heat exchanger. These devices are mainly used to intercept large particulate impurities, but their filtration accuracy is limited and they lack the ability to adsorb and remove dissolved pigment impurities; Carbon-based filtration membranes. In recent years, carbon-based filtration membranes with micro / nano composite pore sizes have emerged, containing micron-sized carbon-based porous adsorbents and polymer binders. However, these products use polymer binder systems, resulting in poor temperature resistance and inability to operate stably for extended periods at temperatures above 400°C; Porous graphite adsorbent materials. Existing technologies include methods for preparing porous graphite materials through molding or isostatic pressing and high-temperature sintering, allowing for adjustment of pore size and distribution by controlling process parameters. However, these studies primarily focus on the preparation of the material itself and have not yet resulted in integrated filter tube assembly products that can be directly used for fluid processing.
[0004] Existing technologies suffer from the following defects and shortcomings: 1. Insufficient temperature resistance. Existing carbon-based filter components mostly use polymer binders, which soften or even melt above 300℃, making long-term stable operation impossible under high-temperature conditions of 400~550℃. 2. Limited pressure resistance. The structural design of existing filter components does not fully consider the tension conditions from the inside out, making them prone to structural failure. 3. Limited functionality. Most existing products only have physical filtration functions and lack adsorption and decolorization capabilities, failing to meet the dual requirements of removing both particles and pigments. 4. Insufficient pore size control precision. Existing products have a wide pore size distribution and poor pore size uniformity, making it difficult to achieve the precise control requirements of a maximum pore size ≤50μm and an average pore size ≈25μm. 5. Dependence on imports and high costs. High-performance porous graphite filter tube components have long relied on imports, resulting in high prices and uncertain supply cycles, severely restricting cost reduction and efficiency improvement in related industries. Summary of the Invention
[0005] The purpose of this invention is to provide a porous graphite adsorption material filter tube assembly and its preparation method, so as to solve the technical problems of insufficient temperature resistance, limited pressure bearing capacity, single function, insufficient pore size control accuracy, and high cost due to reliance on imports in the prior art of carbon-based filter assemblies.
[0006] To achieve the above objectives, the present invention provides a porous graphite adsorption material filter tube assembly, which is a cylindrical structure comprising: using calcined petroleum coke or pitch coke as aggregate, and completing the process by adding a pore-forming agent for thermal decomposition and gasification and escape, and a binder for carbonization and shrinkage, and utilizing the π-π stacking effect of graphite itself to adsorb pigment impurities in the fluid for adsorption, decolorization and precision filtration.
[0007] Optionally, the maximum pore size of the porous graphite adsorption material filter tube assembly is ≤45μm, and the average pore size is 20~30μm.
[0008] Secondly, the present invention provides a method for preparing a porous graphite adsorption material filter tube assembly as described above, comprising the following steps:
[0009] (1) Raw material preparation and pretreatment: graphite raw materials are crushed, ground and screened to obtain graphite particles; calcined petroleum coke or pitch coke is crushed and ground to obtain coke powder, which is used as the shell material of composite particles; modified coal pitch is ground to obtain coal pitch powder, which is used as a binder; starch is used as a pore-forming agent.
[0010] (2) Mixing and molding: The graphite particles, coke powder, starch and coal tar powder are mechanically fused together. Under the compression, shearing and impact forces generated by high-speed rotation, the coal tar powder is coated on the surface of the coke. The composite particles are loaded into a mold, vacuum sealed and then molded by hydraulic uniaxial pressure to obtain a green body.
[0011] (3) First roasting: The green blank is roasted and carbonized under a protective atmosphere to obtain a carbon blank;
[0012] (4) Impregnation treatment: The carbon blank is placed in a high-pressure impregnation tank, and after vacuuming, liquid coal tar pitch is introduced for impregnation treatment. Then, the impregnation-calcination cycle is repeated 1 to 3 times to obtain a porous graphite adsorption material filter tube assembly.
[0013] Optionally, in step (1), the graphite particles have a particle size of 50~200μm, the coke powder adopts a three-stage gradation, with coarse particles having a particle size of 0.1~0.2mm, medium particles having a particle size of 0.045~0.1mm, and fine powder having a particle size of <0.045mm, the starch having an average particle size of 10~15μm, and the coal tar pitch having a particle size of ≤20μm;
[0014] The softening point of the modified coal tar pitch is 100~130℃.
[0015] Optionally, in step (2), when the graphite particles, coke powder, starch, and coal tar powder are mechanically fused, the mass ratio of coke powder:graphite:starch:coal tar powder is 55~70:12~20:0~5:10~25, and the sum of the mass fractions of each component is 100%.
[0016] The mechanical fusion rotation speed is 50~150 r / min, the mechanical fusion temperature is 150~170℃, and the mechanical fusion time is 140~160 min.
[0017] Optionally, in step (2), the molding pressure is 15~30MPa and the holding time is ≤60min.
[0018] Optionally, in step (3), the roasting and carbonization treatment adopts a segmented heating process: the heating rate in the 100~300℃ stage is 3~6℃ / h, and the temperature is held at 300℃ for 2h; the heating rate in the 300~650℃ stage is 1~2℃ / h, and the temperature is held at 450~500℃ for 6~10h, and at 650℃ for 4h; the heating rate in the 650~1100℃ stage is 5~10℃ / h; the highest roasting temperature is 900~1100℃, and the temperature is held for 2~8h.
[0019] Optionally, in step (4), the softening point of the liquid coal tar pitch is 60~100℃;
[0020] The impregnation treatment is performed at a pressure of 1.5~2MPa, at a temperature of 180~250℃, and for a duration of ≥4h.
[0021] Optionally, the protective atmosphere described in step (3) is nitrogen.
[0022] In this invention, in step (3), the roasting is carried out under air-isolated conditions, and the maximum roasting temperature is 900~1100℃, so that the coal tar pitch binder undergoes pyrolysis and condensation reaction to transform into pitch carbon, thereby giving the green body mechanical strength and pore structure; and the temperature is kept at 450~500℃ for 6~10h to allow the volatiles generated by the decomposition of the pore-forming agent and binder to fully escape.
[0023] Optionally, the following steps may also be included:
[0024] (5) Precision machining: The calcined blank is turned and bored by CNC machine tools to obtain the filter tube assembly with the final size and shape;
[0025] (6) Post-processing: Cleaning and drying the precision machined products.
[0026] The key point of this invention is:
[0027] Structural Innovation: This invention uses calcined petroleum coke or pitch coke as the main matrix material and coal tar pitch as the binder phase. Both coke powder and graphite particles have been treated at high temperatures, so they do not undergo significant volume shrinkage during subsequent roasting. The pore structure of the product is directly determined by the aggregate gradation and the amount of pore-forming agent, resulting in good pore size controllability. In addition, the graphite particles have a layered crystal structure, which can undergo interlayer slippage during pressure molding, playing a role in solid lubrication and stress buffering, promoting particle rearrangement and improving the uniformity of green body density.
[0028] To ensure the filter component has a certain porosity, this invention does not rely on the random distribution of aggregate particle gaps as the primary means of porosity control. Instead, it achieves pore structure regulation through the quantitative addition of a pore-forming agent. The pore-forming agent undergoes concentrated decomposition and gasification at 250-500℃, forming pores with a particle size comparable to the pore-forming agent at their original sites. Therefore, the pore size is determined by the particle size of the pore-forming agent, and the porosity is determined by the amount of pore-forming agent added; both can be independently controlled. Simultaneously, the volume shrinkage of the coal tar binder during carbonization and the escape of light components form through-hole throats, while the three-stage gradation of the aggregate determines the scale and distribution of the skeleton gaps. These three factors work synergistically to enable the product to possess through-hole channels within a relatively narrow pore size distribution.
[0029] Compared with the prior art, the present invention has at least the following advantages:
[0030] (1) Excellent high temperature resistance. The present invention uses graphite as the main material and asphalt as the binder as an inorganic system. After high temperature graphitization treatment, it can work stably for a long time under high temperature conditions of 400~550℃, overcoming the defect of insufficient temperature resistance of existing polymer binder systems.
[0031] (2) Excellent mechanical strength. This invention prepares high-density (≥1.84 g / cm³) materials through isostatic pressing and optimized sintering processes. 3 The high-strength graphite tube assembly can withstand an internal to external tension of ≥2.5MPa, has a stable structure, is not easily broken, and significantly extends the service life of the product.
[0032] (3) Precise and controllable pore size. This invention achieves precise control of pore size (maximum pore size ≤ 45 μm, average pore size about 25 μm) through the coordinated regulation of three-stage aggregate gradation, isostatic pressing pressure and segmented slow firing process. The pore size distribution is narrow and the uniformity is good, which ensures stable filtration accuracy and fluid throughput.
[0033] (4) Adsorption-filtration integration. The product of this invention has both physical interception and adsorption decolorization functions. It can adsorb and remove pigment impurities in the fluid while filtering particulate matter, achieving the treatment goal of colorless and particle-free, eliminating the need for additional adsorption units and simplifying the process.
[0034] (5) Low production cost and short delivery cycle.
[0035] (6) Recyclable and low overall cost. The product of this invention has good temperature resistance, long service life, and can recover some performance through regeneration after failure. The overall cost of use is significantly lower than that of imported products.
[0036] (7) High adaptability. This invention can quickly adapt to the specific working conditions of different customers by adjusting the billet formula and machining dimensions, and can achieve seamless replacement without the need for customers to adjust existing process parameters. Attached Figure Description
[0037] Figure 1 This is a physical image of the porous adsorption carbon nanotubes of the present invention.
[0038] Figure 2 This is a schematic diagram of the process flow of the present invention. Detailed Implementation
[0039] The present application is further illustrated below with reference to specific embodiments. The following descriptions are merely a few embodiments of the present application and are not intended to limit the present application in any way. Although the present application discloses preferred embodiments as follows, they are not intended to limit the present application. Any modifications or variations made by those skilled in the art without departing from the scope of the technical solution of the present application using the disclosed technical content are equivalent to equivalent implementation cases and all fall within the scope of the technical solution.
[0040] Unless otherwise specified, the raw materials used in the embodiments of this application are all purchased commercially and used directly without any special treatment.
[0041] Unless otherwise specified, the analytical methods in the embodiments all adopt conventional instrument or equipment settings and conventional analytical methods.
[0042] Example 1
[0043] A method for preparing a porous graphite adsorption material filter tube assembly, comprising the following steps:
[0044] (1) Raw material preparation and pretreatment: The graphite raw material and coke powder were crushed, ground and sieved to obtain 50μm graphite particles; the coke powder contained coarse particles with a particle size of 0.1~0.2mm accounting for 50wt% of the coke powder mass, medium particles with a particle size of 0.045~0.1mm accounting for 25wt% of the coke powder mass, and fine powder with a particle size <0.045mm accounting for 25wt% of the coke powder mass;
[0045] (2) Mixing and molding: The graphite particles, coke powder, starch and coal tar powder are mechanically fused at a mass ratio of 60:13:2:25 (the mechanical fusion speed is 100 r / min, the mechanical fusion temperature is 180℃, and the mechanical fusion time is 150 min); the composite particles are loaded into a rigid mold and subjected to a uniaxial pressure of 20 MPa to obtain a green body;
[0046] (3) First roasting: The green blank is placed in a roasting furnace and roasted and carbonized under a nitrogen atmosphere according to the following curve: 100℃ to 300℃ at a rate of 3℃ / h, and held for 2h; 300℃ to 650℃ at a rate of 1℃ / h, and held at 450℃ for 8h, and held at 650℃ for 4h; 650℃ to 1000℃ at a rate of 5℃ / h; held at 1000℃ for 8h and then naturally cooled to room temperature to obtain the carbon blank;
[0047] (4) Impregnation treatment: The carbon blank is placed in a high-pressure impregnation tank, and after vacuuming, liquid coal tar pitch is introduced. The impregnation treatment is carried out at 1.8 MPa and 230℃ for 4 hours. After taking it out, it is roasted a second time according to the first roasting curve.
[0048] (5) Precision machining: The cylindrical blank after secondary firing is clamped on a CNC lathe. First, rough turn the outer diameter and rough bore the inner hole (350 rpm, feed 0.15 mm / rev, depth of cut 0.5 mm), then finish turn the outer diameter and finish bore the inner hole (700 rpm, feed 0.05 mm / rev, depth of cut 0.12 mm) to the final size of the product;
[0049] (6) Post-processing: The precision-machined product is ultrasonically cleaned, dried, and annealed at 120℃ for 8 hours. The final porous graphite adsorption material filter tube assembly is as follows: Figure 1 As shown in the diagram, the process flow chart is as follows: Figure 2 As shown.
[0050] Comparative Example 1
[0051] The difference between this comparative example and Example 1 is that the coke powder gradation is adjusted to 65wt% coarse particles, 20wt% medium particles, and 15wt% fine powder; the mass ratio of coke powder:graphite:starch:binder is the same as in Example 1, which is 60:13:2:25, and the sum of each component is 100%. As shown in Table 1, under this formula, the proportion of coarse particles is too high and the fine powder is insufficient to fill the gaps between the aggregates. The bulk density and compressive strength of the product show a decreasing trend, while the average pore size increases accordingly, and the maximum pore size tends to exceed 45μm.
[0052] Table 1. Performance of adsorbent materials prepared with different proportions of coke powder particles
[0053]
[0054] Comparative Example 2
[0055] The only difference between this comparative example and Example 1 is that no starch pore-forming agent is added, and the mass ratio of coke powder:graphite:starch:binder is 62:13:0:25, with the sum of all components being 100%. All other raw materials and process parameters are the same as in Example 1. Under this formulation, the bulk density and compressive strength of the product are higher than in Example 1, but due to the lack of interconnected pores formed by the thermal decomposition of the pore-forming agent, its average pore size is significantly reduced, and its porosity decreases.
[0056] Table 2 Performance comparison between Sample Example 1 and Sample Comparative Example 2
[0057]
[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A porous graphite adsorption material filter tube assembly, characterized in that, The porous graphite adsorption material filter tube assembly has a cylindrical structure and includes: using calcined petroleum coke or pitch coke as aggregate, the process is completed by adding a pore-forming agent for thermal decomposition and gasification, and a binder for carbonization and shrinkage. It also utilizes the π-π stacking effect of graphite itself to adsorb pigment impurities in the fluid for adsorption, decolorization, and precision filtration.
2. The porous graphite adsorption material filter tube assembly according to claim 1, characterized in that, The maximum pore size of the porous graphite adsorption material filter tube assembly is ≤45μm, and the average pore size is 20~30μm.
3. A method for preparing a porous graphite adsorption material filter tube assembly as described in claim 1 or 2, characterized in that, Includes the following steps: (1) Raw material preparation and pretreatment: graphite raw materials are crushed, ground and screened to obtain graphite particles; calcined petroleum coke or pitch coke is crushed and ground to obtain coke powder, which is used as the shell material of composite particles; modified coal pitch is ground to obtain coal pitch powder, which is used as a binder; starch is used as a pore-forming agent. (2) Mixing and molding: The graphite particles, coke powder, starch and coal tar powder are mechanically fused together. Under the compression, shearing and impact forces generated by high-speed rotation, the coal tar powder is coated on the surface of the coke. The composite particles are loaded into a mold, vacuum sealed and then molded by hydraulic uniaxial pressure to obtain a green body. (3) First roasting: The green blank is roasted and carbonized under a protective atmosphere to obtain a carbon blank; (4) Impregnation treatment: The carbon blank is placed in a high-pressure impregnation tank, and after vacuuming, liquid coal tar pitch is introduced for impregnation treatment. Then, the impregnation-calcination cycle is repeated 1 to 3 times to obtain a porous graphite adsorption material filter tube assembly.
4. The method for preparing a porous graphite adsorption material filter tube assembly according to claim 3, characterized in that, In step (1), the graphite particles have a particle size of 50~200μm, the coke powder adopts a three-stage gradation, with coarse particles having a particle size of 0.1~0.2mm, medium particles having a particle size of 0.045~0.1mm, and fine powder having a particle size of <0.045mm, the starch having an average particle size of 10~15μm, and the coal tar pitch having a particle size of ≤20μm; The softening point of the modified coal tar pitch is 100~130℃.
5. The method for preparing a porous graphite adsorption material filter tube assembly according to claim 3, characterized in that, In step (2), when the graphite particles, coke powder, starch, and coal tar powder are mechanically fused, the mass ratio of coke powder:graphite:starch:coal tar powder is 55~70:12~20:0~5:10~25, and the sum of the mass fractions of each component is 100%. The mechanical fusion rotation speed is 50~150 r / min, the mechanical fusion temperature is 150~170℃, and the mechanical fusion time is 140~160 min.
6. The method for preparing a porous graphite adsorption material filter tube assembly according to claim 3, characterized in that, In step (2), the molding pressure is 15~30MPa and the holding time is ≤60min.
7. The method for preparing a porous graphite adsorption material filter tube assembly according to claim 3, characterized in that, In step (3), the roasting and carbonization process adopts a segmented heating process: the heating rate in the 100~300℃ stage is 3~6℃ / h, and the temperature is held at 300℃ for 2h; the heating rate in the 300~650℃ stage is 1~2℃ / h, and the temperature is held at 450~500℃ for 6~10h, and at 650℃ for 4h; the heating rate in the 650~1100℃ stage is 5~10℃ / h; the highest roasting temperature is 900~1100℃, and the temperature is held for 2~8h.
8. The method for preparing a porous graphite adsorption material filter tube assembly according to claim 3, characterized in that, In step (4), the softening point of the liquid coal tar pitch is 60~100℃; The impregnation treatment is performed at a pressure of 1.5~2MPa, at a temperature of 180~250℃, and for a duration of ≥4h.
9. The method for preparing a porous graphite adsorption material filter tube assembly according to claim 3, characterized in that, The protective atmosphere mentioned in step (3) is nitrogen.
10. The method for preparing a porous graphite adsorption material filter tube assembly according to claim 3, characterized in that, It also includes the following steps: (5) Precision machining: The calcined blank is turned and bored by CNC machine tools to obtain the filter tube assembly with the final size and shape; (6) Post-processing: Cleaning and drying the precision machined products.