Conductive Janus membranes, their preparation methods and applications, and electric field-assisted emulsion separation systems and methods
By utilizing the asymmetric structure of a polypropylene porous base membrane, a polydopamine adhesion layer, and a nickel-based conductive layer, and combining it with the gas-liquid interface confinement method to prepare a conductive Janus membrane, the problems of low separation efficiency and complex preparation in existing technologies are solved, and efficient oily wastewater treatment is achieved.
Patent Information
- Application Number
- CN202611380460.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing conductive Janus membranes suffer from low separation efficiency, easy pore clogging, and cumbersome preparation processes when treating oily wastewater. In particular, they are difficult to achieve both high permeation flux and high oil droplet rejection rate at the same time, and existing preparation methods are prone to damaging the membrane substrate structure.
A conductive Janus membrane was prepared by using an asymmetric structure consisting of a polypropylene porous base membrane, a polydopamine adhesion layer, and a nickel-based conductive layer, via a gas-liquid interface confinement method. Electrostatic repulsion was used to suppress oil droplet migration, and a continuous conductive network was formed by chemical nickel plating to keep the membrane pores open.
It achieves efficient directional transport of aqueous phase and oil droplet retention, reduces membrane surface enrichment and pore blockage, has a simple preparation process, does not damage the membrane substrate structure, and is suitable for large-scale treatment of oily wastewater.
Smart Images

Figure CN123102166A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of membrane separation and oily wastewater treatment technology, and specifically relates to a conductive Janus membrane, its preparation method and application, and an electric field-assisted emulsion separation system and separation method. Background Technology
[0002] Industries such as petrochemicals, machinery manufacturing, and food processing generate large amounts of oily wastewater. Among them, oil-in-water emulsions stabilized by surfactants have characteristics such as small oil droplet size, strong interfacial stability, and resistance to aggregation. When treated by traditional processes such as sedimentation, flotation, centrifugation, or flocculation, there are generally problems such as limited separation efficiency, large amount of reagents added, and easy to cause secondary pollution.
[0003] Membrane separation technology offers advantages such as ease of operation, compact equipment, and the ability to retain fine oil droplets. However, traditional filter membranes rely primarily on pore size sieving as the separation mechanism, making it difficult to simultaneously achieve high permeate flux and high oil droplet rejection rate. Furthermore, oil droplets tend to accumulate on the membrane surface, causing pore blockage. While conventional Janus membranes can achieve directional transport of the aqueous phase and block oil droplets by relying on the difference in wettability across the membrane, they cannot actively inhibit the migration and deposition of charged oil droplets on the membrane surface.
[0004] Electric field-assisted membrane separation can mitigate membrane fouling by utilizing the electrostatic repulsion effect between the cathode and negatively charged oil droplets. However, most existing conductive Janus membranes are prepared by overall modification followed by methods such as peeling, sacrificial layer, or plasma unilateral etching, which have drawbacks such as cumbersome processes, easy damage to the membrane substrate structure, and high requirements for preparation equipment.
[0005] Therefore, existing conductive Janus films and their preparation methods still need improvement. Summary of the Invention
[0006] The purpose of this application is to provide a conductive Janus membrane, its preparation method, and its application in an electric field-assisted emulsion separation system and separation method. The conductive Janus membrane of this application can promote the directional transport of the aqueous phase through asymmetric wettability, making it suitable for the separation of oil-in-water emulsions. It can also use electrostatic repulsion to suppress the accumulation of negatively charged oil droplets on the membrane surface. Furthermore, the preparation method of this conductive Janus membrane does not require stripping, sacrificial layers, or plasma etching, making the process simple and less likely to damage the membrane substrate structure.
[0007] The first aspect of this application provides a conductive Janus film, which includes a polypropylene porous base film, a polydopamine adhesive layer and a nickel-based conductive layer sequentially stacked along the thickness direction of the conductive Janus film. The polydopamine adhesive layer has silver activation sites distributed on the side surface opposite to the polypropylene porous base film, and the nickel-based conductive layer is bonded to the surface of the polydopamine adhesive layer through the silver activation sites.
[0008] In some embodiments of this application, the silver activation sites include silver particles distributed on the polydopamine adhesion layer.
[0009] In some embodiments of this application, the nickel-based conductive layer comprises nickel particles nucleated on the silver activation sites, and the nickel particles are interconnected to form the nickel-based conductive layer.
[0010] In some embodiments of this application, the nominal pore size of the polypropylene porous base membrane is 0.22 μm.
[0011] In some embodiments of this application, the conductive Janus film has a first side and a second side disposed opposite to each other along its thickness direction. The surface of the polypropylene porous base film facing away from the polydopamine adhesion layer is formed as the first side of the conductive Janus film, and the surface of the nickel-based conductive layer facing away from the polydopamine adhesion layer is formed as the second side of the conductive Janus film. The two sides of the conductive Janus film have asymmetric wettability, and the second side is conductive.
[0012] In some embodiments of this application, the initial water contact angle of the first side of the conductive Janus membrane is not less than 125°.
[0013] In some embodiments of this application, the initial water contact angle of the second side of the conductive Janus membrane is not higher than 30°, and the underwater oil contact angle of the second side when n-hexane is used as the test oil droplet is 150°~155°.
[0014] In some embodiments of this application, the conductive Janus membrane, under filtration conditions, allows oily wastewater to be directionally transported from the first side to the second side.
[0015] The second aspect of this application also provides a method for preparing the conductive Janus film described in the first aspect of this application, comprising the following steps: obtaining a polypropylene porous base film having a first surface and a second surface along its thickness direction; floating the ultrasonically cleaned polypropylene porous base film at the gas-liquid interface of a dopamine solution, wherein the first surface of the polypropylene porous base film faces the gas phase, the second surface of the polypropylene porous base film faces the liquid phase and reacts with the dopamine solution to form a polydopamine adhesion layer on the second surface, thereby obtaining a PP-PDA Janus film; floating the PP-PDA Janus film at the gas-liquid interface of a silver salt solution, wherein the first surface of the polypropylene porous base film faces the gas phase, the surface of the polydopamine adhesion layer opposite to the polypropylene porous base film faces the liquid phase and reacts with the silver salt solution to form silver activation sites on the surface of the polydopamine adhesion layer; and placing the PP-PDA with the formed silver activation sites... The Janus membrane floats at the gas-liquid interface of the electroless nickel plating solution. The first surface of the polypropylene porous base membrane faces the gas phase, and the surface of the polydopamine adhesion layer, which has the silver activation sites, faces the liquid phase and is in contact with the electroless nickel plating solution. Using the silver activation sites as nucleation sites, a nickel-based conductive layer is formed on the polydopamine adhesion layer to obtain the conductive Janus membrane.
[0016] In some embodiments of this application, the concentration of dopamine hydrochloride in the dopamine solution is 2 mg·mL. -1 .
[0017] In some embodiments of this application, the pH of the dopamine solution is 8.5.
[0018] In some embodiments of this application, the polypropylene porous base membrane floats at the gas-liquid interface of the dopamine solution and reacts with the dopamine solution for 6 hours.
[0019] In some embodiments of this application, the concentration of the silver salt solution is 1.5 g·L. -1 .
[0020] In some embodiments of this application, the silver salt solution is a silver nitrate solution.
[0021] In some embodiments of this application, the surface of the polydopamine adhesion layer facing away from the polypropylene porous base film is oriented towards the liquid phase and reacts with the silver salt solution for 30 minutes.
[0022] In some embodiments of this application, each liter of the electroless nickel plating solution comprises 25 g of nickel sulfate hexahydrate, 50 g of sodium pyrophosphate decahydrate, 40 mL of ammonia water with a mass fraction of 28%, and 1.5 g of dimethylaminoborane.
[0023] In some embodiments of this application, the surface of the polydopamine adhesion layer with the silver activation sites is oriented towards the liquid phase and reacts with the electroless nickel plating solution at 35°C for 5 min to 20 min.
[0024] In some embodiments of this application, the surface of the polydopamine adhesion layer with the silver activation sites is oriented toward the liquid phase and reacts with the electroless nickel plating solution at 35°C for 10 min.
[0025] A third aspect of this application also provides an electric field-assisted emulsion separation system, comprising a filter assembly, a DC power supply, a cathode, and an anode spaced apart from the cathode; wherein the cathode is the conductive Janus membrane described in the first aspect of this application or the conductive Janus membrane prepared using the preparation method described in the second aspect of this application; the nickel-based conductive layer of the conductive Janus membrane is electrically connected to the negative terminal of the DC power supply, and the anode is electrically connected to the positive terminal of the DC power supply; the filter assembly includes a filter cup and a filtrate receiver arranged vertically but vertically. The filter cup has a through-chamber for holding the oil-containing emulsion to be separated, and the anode is immersed in the oil-containing emulsion. The top of the filtrate receiver is open, and the bottom opening of the filter cup is opposite to the top opening of the filtrate receiver. The conductive Janus membrane is clamped and assembled between the mating end faces of the bottom opening of the filter cup and the top opening of the filtrate receiver, and the side of the polypropylene porous base membrane of the conductive Janus membrane facing away from the polydopamine adhesion layer faces the oil-containing emulsion feed side, and the nickel-based conductive layer of the conductive Janus membrane faces the permeation side.
[0026] In some embodiments of this application, the distance between the anode and the cathode is 0.2 cm.
[0027] In some embodiments of this application, the voltage applied by the DC power supply is greater than 0 V and not higher than 12 V.
[0028] In some embodiments of this application, the voltage applied by the DC power supply is 9 V.
[0029] In some embodiments of this application, the anode is a platinum sheet electrode.
[0030] The fourth aspect of this application also provides a method for separating an oil-in-water emulsion, the separation method being based on the electric field-assisted emulsion separation system described in the third aspect of this application; the oil-in-water emulsion is an anionic surfactant-stabilized oil-in-water emulsion, and the separation method includes the following steps: clamping and assembling a conductive Janus membrane between the mating end faces of the lower opening of a filter cup and the upper opening of a filtrate receiver; placing an anode inside the filter cup, adding the oil-in-water emulsion to be separated into the filter cup and immersing the anode; using the conductive Janus membrane as a cathode and applying a DC electric field, causing the continuous aqueous phase to permeate from the side of the polypropylene porous base membrane opposite to the polydopamine adhesion layer in the conductive Janus membrane to the nickel-based conductive layer side of the conductive Janus membrane under the action of gravity and the capillary driving force formed by the difference in wettability on both sides of the conductive Janus membrane, and utilizing the electrostatic repulsion of the cathode on the negatively charged emulsified oil droplets to inhibit the enrichment, adhesion, and clogging of the membrane pores of the emulsified oil droplets on the surface of the conductive Janus membrane.
[0031] In some embodiments of this application, the anionic surfactant is sodium dodecyl sulfate, and the concentration of the anionic surfactant is 0.5 g·L. -1 .
[0032] In some embodiments of this application, the volume fraction of the oil phase in the oil-in-water emulsion is 15% to 30%.
[0033] In some embodiments of this application, the oil phase includes at least one of n-hexane, petroleum ether, n-hexadecane, and gasoline.
[0034] The fifth aspect of this application also provides the application of the conductive Janus membrane described in the first aspect of this application, or the conductive Janus membrane prepared by the preparation method described in the second aspect of this application, or the electric field-assisted emulsion separation system described in the third aspect of this application, in the treatment of oily wastewater.
[0035] This application has at least the following beneficial effects: (1) The polydopamine adhesion layer improves the interfacial bonding stability between the polypropylene porous base film and the nickel-based conductive layer. Appropriate electroless nickel plating can form a continuous conductive network and a hydrophilic and underwater oleophobic interface while keeping the film pores open.
[0036] (2) The delayed wetting characteristics of the first side of the conductive Janus membrane are coupled with the capillary traction of the second side, enabling the oily wastewater to be directionally transported from the first side to the second side. When the conductive Janus membrane is used as the cathode, the cathode generates electrostatic repulsion against the negatively charged emulsified oil droplets, which can reduce the accumulation, adhesion and pore blockage of oil droplets on the membrane surface.
[0037] (3) This application utilizes the gas-liquid interface to spatially confine the reaction area, so that polydopamine modification, silver activation and electroless nickel plating mainly occur on the same surface of the polypropylene porous base film from the beginning, directly constructing an asymmetric structure in an additive manner without the need for tape peeling, sacrificial hydrophobic layer or vacuum plasma etching.
[0038] (4) The preparation process provided in this application can be completed under normal pressure liquid phase conditions. The process steps are simple, the equipment requirements are low, and the damage to the polypropylene porous base membrane is small. It remains stable in different pH environments, different oil emulsions and multiple cycles, and has the potential for large-scale treatment of oily wastewater.
[0039] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description
[0040] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0041] Figure 1 This is a schematic diagram of the interface confinement preparation process of the conductive Janus film according to some embodiments of this application.
[0042] Figure 2 Original polypropylene base film (original PP film), single-sided polydopamine modified film (PP-PDA Janus film), PP-PDA-Ni (10) Scanning electron microscope image of a conductive Janus film; in which, Figure 2 (1) shows scanning electron microscope images of the original PP film at scale bars of 1 μm and 2 μm; Figure 2 (2) shows scanning electron microscope images of the PP-PDA Janus film at scale bars of 1 μm and 2 μm; Figure 2 (3) shows PP-PDA-Ni (10) Scanning electron microscope images of the nickel-plated side of the conductive Janus film at scale bars of 1 μm and 2 μm; Figure 2 (4) shows PP-PDA-Ni (10) Scanning electron microscope images of the unmodified side of the conductive Janus film at scale bars of 1 μm and 2 μm.
[0043] Figure 3 These are the test results of the dynamic water contact angle and the underwater oil contact angle on the nickel-plated side of the conductive Janus film prepared with different electroless nickel plating times in some embodiments of this application; wherein, Figure 3 (1) shows the change in wettability of the conductive Janus film surface with time of nickel plating: the time evolution of water contact angle on both sides of the film and underwater oil contact angle on the nickel plating side. The sample plating time was 0 minutes, 5 minutes, 15 minutes and 20 minutes, which were PP-PDA Janus (0 minute sample refers to unplated PP-PDA Janus film), PP-PDA-Ni (5), PP-PDA-Ni (15) and PP-PDA-Ni (20). Figure 3 (2) is PP-PDA-Ni (10) Representative image of the underwater oil contact angle on the nickel-plated side; Figure 3 (3) is PP-PDA-Ni (10) Representative image of the water contact angle on the nickel-plated side; Figure 3 (4) is PP-PDA-Ni (10) Water contact angle on the unmodified side of the membrane; Figure 3 (5) is PP-PDA-Ni (10) Summary of characteristic contact angles and wetting times of membranes.
[0044] Figure 4 For some embodiments of this application, PP-PDA-Ni (10) Diagrams illustrating the forward water transport through the membrane, the forward water transport against gravity, and the reverse water transport process; among which, Figure 4 (1) in the text indicates that the water droplet is placed on PP-PDA-Ni (10) The unmodified side of the membrane; Figure 4 (2) in the text indicates that PP-PDA-Ni is in contact with water droplets. (10) The unmodified side of the membrane is transported upwards against gravity; Figure 4 (3) in the text indicates that it is placed in PP-PDA-Ni (10) Water droplets on the nickel-plated side; green and grayish-white semicircles represent PP-PDA-Ni respectively. (10) Nickel-plated side and unmodified side.
[0045] Figure 5 The separation performance of conductive Janus membranes prepared with different electroless nickel plating times in some embodiments of this application for hexane / water mixtures and PP-PDA-Ni (10) Results of 20-cycle stability tests on the membrane; among which, Figure 5 (1) represents the permeation flux and oil rejection rate of conductive Janus membranes prepared with different nickel plating times; Figure 5 (2) in the text represents PP-PDA-Ni (10)Membrane separation performance during 20 filtration-cleaning cycles.
[0046] Figure 6 The effects of applied voltage, oil phase volume fraction, and oil type on PP-PDA-Ni (10) The effect of membrane electric field-assisted oil-in-water emulsion separation performance; among which... Figure 6 (1) refers to applying a DC voltage to the PP-PDA-Ni (10) The effect of membrane permeation flux and the effect of n-hexane oil-in-water emulsion on φ oil =20% oil retention rate; Figure 6 (2) represents the oil phase volume fraction for PP-PDA-Ni (10) The effect of membrane permeation flux and the oil rejection rate of n-hexane oil-in-water emulsion at -9 V DC voltage; Figure 6 In (3), under a bias of -9 V, φoil = 15% (φ oil When representing the oil phase volume fraction, different oil pairs were used to prepare PP-PDA-Ni (10) Membrane permeation flux and oil rejection rate.
[0047] Figure 7 PP-PDA-Ni (10) Test results of water contact angles on both sides of the membrane after treatment with solutions of different pH values.
[0048] Figure 8 PP-PDA-Ni (10) Test results of membrane cyclic separation performance of different oil-in-water emulsions at 9 V voltage. Detailed Implementation
[0049] Exemplary embodiments of this application will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of this application are shown in the drawings, it should be understood that this application may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided to enable a more thorough understanding of this application and to fully convey the scope of this application to those skilled in the art.
[0050] It should be understood that the terminology used herein is for the purpose of describing particular exemplary embodiments only and is not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms “a,” “an,” and “described” as used herein may also include the plural forms. The terms “comprising,” “including,” “containing,” and “having” are inclusive and therefore indicate the presence of the stated features, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, elements, components, and / or combinations thereof. The method steps, processes, and operations described herein are not construed as requiring them to be performed in a particular order described or illustrated unless the order of performance is explicitly indicated. It should also be understood that additional or alternative steps may be used.
[0051] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0052] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0053] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).
[0054] The terms "first," "second," etc., used in this application are only used to distinguish the two opposing surfaces of the polypropylene porous base membrane and the two opposing surfaces of the conductive Janus membrane, and do not indicate relative importance, quantity, order, or primary / secondary relationship. Specifically, the first surface refers to the surface of the polypropylene porous base membrane facing the gas phase during the preparation process, where a continuous nickel-based conductive layer has not yet formed; the second surface refers to the surface of the polypropylene porous base membrane facing the liquid phase during the preparation process, where a polydopamine adhesion layer, silver activation sites, and a nickel-based conductive layer are sequentially formed; the first side surface refers to the surface of the conductive Janus membrane facing the emulsion feed side during use, which corresponds to the first surface of the polypropylene porous base membrane in the conductive Janus membrane; the second side surface refers to the surface of the conductive Janus membrane facing the permeation side during use, which corresponds to the surface of the nickel-based conductive layer in the conductive Janus membrane facing away from the polydopamine adhesion layer. The term "gas-liquid interface confinement" as used in this article refers to floating a porous polypropylene membrane on the surface of the reaction liquid, with the first surface facing the gas phase and the second surface in contact with the liquid phase. This utilizes the gas-liquid interface to limit the continuous wetting of the membrane in the thickness direction by the reaction liquid and the expansion of the reaction area toward the first surface.
[0055] The first aspect of this application provides a conductive Janus film, which includes a polypropylene porous base film, a polydopamine adhesive layer and a nickel-based conductive layer stacked sequentially along the thickness direction of the conductive Janus film. The polydopamine adhesive layer has silver activation sites distributed on the side surface opposite to the polypropylene porous base film, and the nickel-based conductive layer is composited to the surface of the polydopamine adhesive layer through the silver activation sites.
[0056] In an embodiment of this application, the conductive Janus membrane comprises a polypropylene porous base membrane having a first surface and a second surface disposed opposite to each other along its thickness direction. The first surface retains the hydrophobicity of the polypropylene porous base membrane and has delayed wetting characteristics. A polydopamine adhesion layer is disposed on the second surface of the polypropylene porous base membrane, and silver activation sites are distributed on the surface of the polydopamine adhesion layer, and a nickel-based conductive layer is formed on the silver-activated polydopamine adhesion layer. It is understood that the nickel-based conductive layer is distributed on one side surface of the conductive Janus membrane, and the channels between adjacent fibers remain interconnected, thereby giving the two sides of the conductive Janus membrane asymmetric wettability and making one side surface conductive, which helps the oily wastewater to be directionally transported from the first side to the second side. When the conductive Janus membrane is used as a cathode, the cathode generates electrostatic repulsion against negatively charged emulsified oil droplets, which can reduce the enrichment, adhesion and pore blockage of oil droplets on the membrane surface.
[0057] In some embodiments of this application, the conductive Janus film has a first side and a second side disposed opposite to each other along its thickness direction. The surface of the polypropylene porous base film away from the polydopamine adhesive layer is formed as the first side (unmodified side) of the conductive Janus film, and the surface of the nickel-based conductive layer away from the polydopamine adhesive layer is formed as the second side (nickel-plated side) of the conductive Janus film. The two sides of the conductive Janus film have asymmetric wettability, and the second side is conductive.
[0058] In some embodiments of this application, the initial water contact angle of the first side of the conductive Janus membrane is not less than 125°.
[0059] In some embodiments of this application, the initial water contact angle of the second side of the conductive Janus membrane is not higher than 30°.
[0060] In some embodiments of this application, the underwater oil contact angle of the second side of the conductive Janus film when using n-hexane as a test oil droplet is 150° to 155°. As an example, the underwater oil contact angle of the second side of the conductive Janus film when using n-hexane as a test oil droplet can be one of 150°, 151°, 152°, 153°, 154°, and 155°, or any value satisfying the above range.
[0061] The difference in wettability between the two surfaces of the conductive Janus membrane allows oily wastewater to be directionally transported from the first side to the second side during filtration, while reverse transport is suppressed.
[0062] In some embodiments of this application, the nominal pore size of the polypropylene porous base membrane is 0.22 μm.
[0063] In some embodiments of this application, the silver activation sites include silver particles distributed on the polydopamine adhesion layer.
[0064] In some embodiments of this application, the nickel-based conductive layer includes nickel particles nucleated at silver activation sites, which are interconnected to form the nickel-based conductive layer. It is understood that the nickel-based conductive layer is deposited on the polydopamine adhesion layer using silver activation sites as nucleation sites.
[0065] In a preferred embodiment of this application, the conductive Janus membrane achieves an oil rejection rate of over 99% for n-hexane / water mixtures under gravity-driven conditions, with a separation flux reaching 2000 L·m⁻¹. -2 ·h -1 The above indicates that, under 9 V DC electric field assistance, the oil rejection rate of anionic surfactant-stabilized oil-in-water emulsions reaches over 98%, and the separation flux reaches 270 L·m⁻². -2 ·h -1 above.
[0066] In some embodiments of this application, the conductive Janus membrane is obtained by sequentially floating an ultrasonically cleaned polypropylene porous base membrane at the gas-liquid interface of a dopamine solution, a silver nitrate solution, and a chemical nickel plating solution, thereby continuously forming a polydopamine adhesion layer, silver activation sites, and a nickel-based conductive layer on the same surface of the polypropylene porous base membrane, while the other surface of the polypropylene porous base membrane remains hydrophobic. In use, the unplated nickel side of the conductive Janus membrane faces the emulsion feed side, while the nickel-plated side acts as the cathode and faces the permeation side. Asymmetric wettability promotes the directional transport of the aqueous phase, and electrostatic repulsion inhibits the accumulation of negatively charged oil droplets on the membrane surface.
[0067] The second aspect of this application provides an interface-confined preparation method for a conductive Janus film, which confines the reaction to one side of the film during the modification process, thereby obtaining the conductive Janus film described in the first aspect of this application.
[0068] In the embodiments of this application, a conductive Janus film is prepared by sequentially performing polydopamine modification, silver activation, and electroless nickel plating on one side of the substrate through gas-liquid interface confinement. In the three consecutive modification processes of polydopamine modification, silver activation, and electroless nickel plating, the polydopamine porous membrane floats on the gas-liquid interface of the corresponding reaction liquid in the interface confinement preparation method. The same surface of the polydopamine porous membrane to be modified faces the liquid phase and is in contact with the reaction liquid, while the surface of the polydopamine porous membrane opposite to the surface to be modified faces the gas phase, thereby using the gas-liquid interface to spatially confine the reaction area.
[0069] In some embodiments of this application, combined with Figure 1 As shown, the method for preparing conductive Janus films through interface confinement mainly follows these steps.
[0070] (1) Ultrasonic cleaning of polypropylene porous base membrane.
[0071] In some embodiments of this application, a polypropylene porous base membrane is first obtained, which has a first surface and a second surface along its thickness direction.
[0072] In some embodiments of this application, before performing interface confinement modification, the polypropylene porous base membrane is immersed in anhydrous ethanol and ultrasonically cleaned for 15 min to remove deposits and contaminants from the membrane surface.
[0073] (2) Preparation of PP-PDA Janus membrane.
[0074] In some embodiments of this application, a polypropylene porous membrane after ultrasonic cleaning is floated at the gas-liquid interface of a dopamine solution. The first surface of the polypropylene porous membrane faces the gas phase, and the second surface of the polypropylene porous membrane faces the liquid phase and reacts with the dopamine solution to form a polydopamine adhesion layer on the second surface, thereby obtaining a PP-PDA Janus membrane.
[0075] In some embodiments of this application, after the reaction is completed, the obtained PP-PDA Janus membrane is rinsed sequentially with deionized water and anhydrous ethanol.
[0076] In some embodiments of this application, the concentration of dopamine hydrochloride in the dopamine solution is 2 mg·mL. -1 .
[0077] In some embodiments of this application, the pH of the dopamine solution is 8.5. It is understood that dopamine undergoes oxidative self-polymerization under weakly alkaline conditions and deposits on the second surface of the polypropylene porous substrate membrane, forming a polydopamine adhesion layer.
[0078] In some embodiments of this application, the polypropylene porous base membrane floats at the gas-liquid interface of the dopamine solution and reacts with the dopamine solution for 6 hours.
[0079] (3) Silver activation sites are formed on the polydopamine adhesion layer.
[0080] In some embodiments of this application, a PP-PDA Janus membrane (a porous polypropylene membrane with a polydopamine adhesion layer) is floated at the gas-liquid interface of a silver salt solution. The first surface of the porous polypropylene membrane faces the gas phase, and the surface of the polydopamine adhesion layer facing away from the porous polypropylene membrane faces the liquid phase and reacts with the silver salt solution. By utilizing the adsorption, complexation, and reduction of silver ions by the catechol groups and amine groups in polydopamine, silver activation sites are formed on the surface of the polydopamine adhesion layer.
[0081] In some embodiments of this application, the concentration of the silver salt solution is 1.5 g·L⁻¹. -1 .
[0082] In some embodiments of this application, the silver salt solution can be a silver nitrate solution with a concentration of 1.5 g·L⁻¹. -1 .
[0083] In some embodiments of this application, the surface of the polydopamine adhesion layer facing away from the polypropylene porous base film is oriented towards the liquid phase and reacts with the silver salt solution for 30 minutes.
[0084] (4) Prepare PP-PDA-Ni conductive Janus film, i.e. conductive Janus film.
[0085] In some embodiments of this application, a PP-PDA Janus film with silver activation sites is floated at the gas-liquid interface of an electroless nickel plating solution. The first surface of the polypropylene porous base film faces the gas phase, and the surface of the polydopamine adhesion layer with silver activation sites faces the liquid phase and is in contact with the electroless nickel plating solution. Using the silver activation sites as nucleation sites, i.e., using the silver activation sites as nucleation and catalytic sites for the electroless nickel plating reaction, a nickel-based conductive layer is formed on the polydopamine adhesion layer to obtain a PP-PDA-Ni conductive Janus film.
[0086] In some embodiments of this application, the temperature of the electroless nickel plating reaction is 35°C.
[0087] In some embodiments of this application, the electroless nickel plating reaction time is 5 min to 20 min. As an example, the electroless nickel plating reaction time can be one of 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, or 20 min, or any value that satisfies the above range.
[0088] In some embodiments of this application, each liter of electroless nickel plating solution comprises 25 g of nickel sulfate hexahydrate, 50 g of sodium pyrophosphate decahydrate, 40 mL of ammonia solution with a mass fraction of 28%, and 1.5 g of dimethylaminoborane.
[0089] In some embodiments of this application, the surface of the polydopamine adhesion layer with silver activation sites faces the liquid phase and reacts with the electroless nickel plating solution at 35°C for 5 to 20 minutes. As an example, the reaction time can be one of 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, and 20 minutes, or any value within the range described above.
[0090] In the embodiments of this application, the electroless nickel plating time simultaneously affects the coverage of nickel particles, the continuity of the conductive network, and the openness of the membrane pores. If the electroless nickel plating time is too short, the nickel particles are not sufficiently covered, making it difficult to form a continuous and stable conductive interface; while if the electroless nickel plating time is too long, the nickel particles grow excessively and agglomerate, leading to membrane pore shrinkage and increased resistance to aqueous phase transport. In the embodiments of this application, the electroless nickel plating reaction time can be understood as the reaction time of the polydopamine adhesion layer with silver activation sites facing the liquid phase and in contact with the electroless nickel plating solution at 35°C, ranging from 5 min to 20 min.
[0091] In some embodiments of this application, a preferred electroless nickel plating time of 10 min is used to balance the continuous nickel-based conductive layer and open channels.
[0092] (5) Rinse and dry the prepared conductive Janus film.
[0093] In some embodiments of this application, after the electroless nickel plating reaction is completed, the resulting conductive Janus film is rinsed and dried with deionized water.
[0094] In some embodiments of this application, the drying temperature is 60°C.
[0095] A third aspect of this application provides an electric field-assisted emulsion separation system, which includes a filter assembly, a DC power supply, a cathode, and an anode spaced apart from the cathode. The cathode is either the conductive Janus membrane described in the first aspect of this application or the conductive Janus membrane prepared using the preparation method described in the second aspect of this application. The nickel-based conductive layer of the conductive Janus membrane is electrically connected to the negative terminal of the DC power supply, and the anode is electrically connected to the positive terminal of the DC power supply. The filter assembly includes a filter cup and a filtrate receiver arranged vertically and vertically. The filter cup has a through-chamber for containing the oil-containing emulsion to be separated, and the anode is immersed in the oil-containing emulsion. The top of the filtrate receiver is open, and the lower opening of the filter cup is opposite to the top opening of the filtrate receiver. The conductive Janus membrane is clamped and assembled between the mating surfaces of the lower opening of the filter cup and the top opening of the filtrate receiver, with the side of the polypropylene porous base membrane in the conductive Janus membrane facing away from the polydopamine adhesion layer facing the oil-containing emulsion feed side, and the nickel-based conductive layer of the conductive Janus membrane facing the permeation side.
[0096] In the embodiments of this application, a conductive Janus membrane serves as the cathode, and the nickel-based conductive layer of the conductive Janus membrane is electrically connected to the negative terminal of a DC power supply. The anode is disposed in a filter cup and immersed in the oil-containing emulsion to be separated, and the anode is electrically connected to the positive terminal of a DC power supply. During operation, the side of the polypropylene porous base membrane in the conductive Janus membrane that faces away from the polydopamine adhesion layer faces the oil-containing emulsion feed side, and the nickel-based conductive layer side of the conductive Janus membrane faces the permeation side. That is, the liquid after filtration and separation enters the filtrate receiver through the nickel-based conductive layer side of the conductive Janus membrane.
[0097] In some embodiments of this application, the filtration assembly further includes a fastening component for engaging with the mating portion of the filter cup and the filtrate receiver, thereby achieving a tight seal between the filter cup, the conductive Janus membrane, and the filtrate receiver.
[0098] In some embodiments of this application, the sidewall of the filtrate receiver may also be provided with an air extraction port, which is used to connect a negative pressure source to form a negative pressure inside the filtrate receiver, thereby driving the oil-containing emulsion to be separated from the filter cup through the conductive Janus membrane into the filtrate receiver.
[0099] In some embodiments of this application, the distance between the anode and the cathode is 0.2 cm.
[0100] In some embodiments of this application, the anode is a platinum sheet electrode.
[0101] In some embodiments of this application, the voltage applied by the DC power supply is greater than 0 V and not higher than 12 V. As an example, the voltage applied by the DC power supply can be one of 11 V, 10 V, 9 V, 8 V, 7 V, 6 V, 5 V, 4 V, 3 V, 2 V, 1 V, or any value that satisfies the above range.
[0102] In some embodiments of this application, the filtration component can be a vacuum filtration device, which is convenient to operate.
[0103] The fourth aspect of this application provides a method for separating oil-in-water emulsions, which is based on the electric field-assisted emulsion separation system described in the third aspect of this application; wherein the oil-in-water emulsion is an anionic surfactant-stabilized oil-in-water emulsion to simulate oily wastewater.
[0104] In some embodiments of this application, the oil-in-water emulsion is stabilized using an anionic surfactant at a concentration of 0.5 g·L⁻¹. -1 .
[0105] In some embodiments of this application, the anionic surfactant is sodium dodecyl sulfate, and the concentration of sodium dodecyl sulfate is 0.5 g·L⁻¹. -1 .
[0106] In some embodiments of this application, the volume fraction of the oil phase in the oil-in-water emulsion is 15% to 30%. As an example, the volume fraction of the oil phase in the oil-in-water emulsion can be one of 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, or 30%, or any value satisfying the above range.
[0107] In some embodiments of this application, the oil phase includes at least one of n-hexane, petroleum ether, n-hexadecane, and gasoline.
[0108] In some embodiments of this application, the method for separating oil-in-water emulsions is mainly carried out according to the following steps.
[0109] First, the conductive Janus membrane is clamped and assembled between the mating end faces of the lower opening of the filter cup and the upper opening of the filtrate receiver.
[0110] Next, the anode is placed inside the filter cup, and the oil-in-water emulsion to be separated is added to the filter cup and the anode is submerged.
[0111] Next, a conductive Janus membrane is used as the cathode and a DC electric field is applied. Under the action of gravity and the capillary driving force formed by the difference in wettability on both sides of the conductive Janus membrane, the continuous aqueous phase permeates from the side of the polypropylene porous base membrane away from the polydopamine adhesion layer to the nickel-based conductive layer side of the conductive Janus membrane. The electrostatic repulsion of negatively charged emulsified oil droplets by the cathode is used to suppress the enrichment, adhesion and blockage of the membrane pores of the emulsified oil droplets on the surface of the conductive Janus membrane.
[0112] The fifth aspect of this application applies the conductive Janus membrane described in the first aspect of this application, or the conductive Janus membrane prepared by the preparation method described in the second aspect of this application, or the electric field-assisted emulsion separation system described in the third aspect of this application, to the treatment of oily wastewater.
[0113] In some embodiments of this application, it is applied to the treatment of oily wastewater containing emulsified oil droplets.
[0114] Under the capillary driving force formed by gravity and the difference in wetting properties on both sides of the conductive Janus membrane, the continuous aqueous phase permeates from the feed side of the oil-containing emulsion to the permeate side; the negatively charged emulsion oil droplets are electrostatically repelled by the cathode and are not easy to accumulate, adhere to or block the membrane pores on the membrane surface.
[0115] Unless otherwise defined, the technical terms used in the following embodiments have the same meaning as commonly understood by those skilled in the art to which this application pertains. Unless otherwise specified, the experimental reagents used in the following embodiments are all conventional analytical chemical reagents; the raw materials, instruments, and equipment used in the following embodiments can all be obtained commercially or through existing methods; the amounts of experimental reagents used are, unless otherwise specified, the amounts used in conventional experimental operations; and the experimental methods used are, unless otherwise specified, conventional methods. It should be further noted that the following descriptions are merely exemplary and not intended to limit the scope of this application. Moreover, the comparative examples below are selected to compare with the technical solutions of this application to demonstrate the advancement of the technical solutions of this application, and do not necessarily represent prior art in this technical field.
[0116] In the following examples, test methods and operating conditions not explicitly described can be employed using conventional methods in the art. Unless otherwise specified, the water is deionized water, and the room temperature is 20°C to 30°C. The conductive Janus film is abbreviated as PP-PDA-Ni film. Films obtained with different electroless nickel plating times are denoted as PP-PDA-Ni(x), where x represents the electroless nickel plating time in minutes; PP-PDA-Ni (10) This is a preferred implementation method.
[0117] Example 1 PP-PDA-Ni (10) Preparation of conductive Janus films (1) Immerse a polypropylene porous base membrane with a nominal pore size of 0.22 μm in anhydrous ethanol and ultrasonically clean it for 15 min to remove the deposits and contaminants on the membrane surface. After ultrasonic cleaning, take out the polypropylene porous base membrane, drain off the residual anhydrous ethanol on the membrane surface, and immediately use it for subsequent one-sided polydopamine modification.
[0118] (2) Prepare a solution with a concentration of 2 mg·mL -1 A dopamine hydrochloride solution with a pH of 8.5 was prepared by dissolving 0.2 g of dopamine hydrochloride and 0.6 g of tris(hydroxymethyl)aminomethane (Tris) granules in 14.7 mL of 0.1 mol / L HCl solution and then adding deionized water to bring the volume to 100 mL, thus preparing a solution with a concentration of 2 mg / mL. -1 Dopamine hydrochloride solution (pH=8.5).
[0119] A porous polypropylene membrane, ultrasonically cleaned with anhydrous ethanol, was laid flat and floated at the gas-liquid interface of a dopamine solution, with the first surface of the membrane facing the gas phase and the second surface facing the liquid phase and in contact with the dopamine solution. The reaction was carried out at room temperature for 6 hours to form a polydopamine adhesion layer on the second surface. After the reaction, the membrane was rinsed sequentially with deionized water and anhydrous ethanol to obtain a PP-PDA Janus membrane.
[0120] (3) To prepare a silver nitrate solution, dissolve 0.45 g of silver nitrate in 300 mL of deionized water to prepare a solution of 1.5 g·L⁻¹. -1 silver nitrate solution.
[0121] PP-PDA Janus membrane was floated in 1.5 g·L⁻¹ water. -1 At the gas-liquid interface of the silver nitrate solution, the first surface of the polypropylene porous base membrane faces the gas phase, while the second surface, which has a polydopamine adhesion layer, faces the liquid phase and comes into contact with the silver nitrate solution. After reacting for 30 minutes, silver activation sites are formed on the polydopamine adhesion layer, followed by rinsing with deionized water.
[0122] (4) Prepare a chemical nickel plating solution containing 25 g nickel sulfate hexahydrate, 50 g sodium pyrophosphate decahydrate, 40 mL ammonia water with a mass fraction of 28% and 1.5 g dimethylaminoborane per liter of the chemical nickel plating solution.
[0123] A PP-PDA Janus film with silver activation sites was floated at the gas-liquid interface of an electroless nickel plating solution, with the first surface of the porous polypropylene base film facing the gas phase and the surface of the polydopamine adhesion layer with silver activation sites facing the liquid phase and in contact with the electroless nickel plating solution. The reaction was carried out at 35°C for 10 min. Using the silver activation sites as nucleation sites—that is, using the silver activation sites as nucleation and catalytic sites for the electroless nickel plating reaction—a nickel-based conductive layer was formed on the polydopamine adhesion layer, thus obtaining a conductive Janus film, namely PP-PDA-Ni. (10) .
[0124] (5) Rinse the obtained conductive Janus film thoroughly with deionized water and dry it in an oven at 60°C.
[0125] Example 2 PP-PDA-Ni (5) Preparation of conductive Janus films The preparation method of Example 2 is the same as that of Example 1, except that the electroless nickel plating time in Example 2 is 5 minutes, and the resulting conductive Janus film is denoted as PP-PDA-Ni. (5) .
[0126] Example 3 PP-PDA-Ni (15) Preparation of conductive Janus films The preparation method of Example 3 is the same as that of Example 1, except that the electroless nickel plating time in Example 3 is 15 min, and the resulting film is denoted as PP-PDA-Ni. (15) .
[0127] Example 4 PP-PDA-Ni (20) Preparation of conductive Janus films The preparation method of Example 4 is the same as that of Example 1, except that the electroless nickel plating time in Example 4 is 20 min, and the resulting film is denoted as PP-PDA-Ni. (20) .
[0128] Comparative Example 1 PP-PDA Janus film without chemical nickel plating The PP-PDA Janus membrane was prepared according to the steps of polypropylene porous base membrane pretreatment and unilateral polydopamine modification in Example 1, without silver activation and chemical nickel plating, and was used as Comparative Example 1.
[0129] Comparative Example 2 The original polypropylene base film, i.e. the original PP film, was used as Comparative Example 2.
[0130] Performance testing Experiment 1) Membrane Surface Morphology Scanning electron microscopy was used to examine the original PP film, PP-PDA Janus film, and PP-PDA-Ni film. (10) The conductive Janus film was observed.
[0131] See Figure 2 It can be seen that the original PP membrane is composed of randomly interwoven smooth fibers. After unilateral polydopamine modification, a uniform thin layer is formed on the fiber surface on the liquid phase contact side. PP-PDA-Ni (10) A continuous granular nickel layer is formed on the nickel-plated side of the membrane, and open channels are still retained between the fibers; PP-PDA-Ni (10) The unmodified side of the membrane still exhibits the smooth morphology of the original PP fibers, and no continuous nickel layer has been formed.
[0132] Experiment 2) Membrane surface wettability The dynamic water contact angle and underwater oil contact angle of different membranes were measured using a contact angle meter. The water droplet volume used for the water contact angle test was 3 μL; the underwater oil contact angle test used n-hexane as the oil droplet volume, with a droplet volume of 3 μL. Three different locations were selected for testing for each sample, and the average value was taken.
[0133] The dynamic contact angle results on both sides of the conductive Janus film are as follows: Figure 3 As shown. PP-PDA-Ni (10) The initial water contact angle on the nickel-plated side was 24.3°, decreasing to near 0° within 3 seconds; the underwater oil contact angle was 150°~155°. PP-PDA-Ni (10) The initial water contact angle of the first side of the membrane (unmodified side) was 134.6°, which decreased slowly in the first 7 seconds and then accelerated wetting occurred, exhibiting delayed wetting characteristics.
[0134] like Figure 4 As shown, when a water droplet contacts the conductive Janus film from its first side, the droplet is gradually absorbed and transported to the nickel-plated side. Even when the film is inverted, the droplet can still overcome gravity and migrate from the first side to the second side. When the droplet directly contacts the second side, it cannot penetrate back to the first side, indicating that the conductive Janus film has significant directional water transport properties.
[0135] Experiment 3) Oil-water mixture separation performance The aqueous phase stained with methylene blue and the n-hexane stained with Oil Red O were mixed at a volume ratio of 1:1. An effective membrane area of 1.81 cm² was used. 2A dead-end filtration device is used to separate oil-water mixtures under gravity. Before the experiment, the membrane is pre-wetted in anhydrous ethanol for 20 min, with the first surface facing the feed side. Membrane flux J (L·m⁻¹) -2 ·h -1 Calculate according to formula (1): (1) In the formula, V is the permeate volume (L); A is the effective membrane filtration area (m²). 2 Δt is the infiltration time, in hours.
[0136] The mass of the oil phase before and after filtration was measured, and the oil retention rate was calculated using equation (2). R 1.
[0137] (2) In the formula, m1 is the mass of the oil phase in the feed before filtration; m2 is the mass of the oil phase that is trapped by the membrane after filtration and does not permeate through the membrane.
[0138] The separation results of conductive Janus films prepared with different electroless nickel plating times are detailed in Table 1.
[0139] Table 1. Effect of electroless nickel plating time on the separation performance of n-hexane / water mixtures.
[0140] Combining Table 1 and Figure 5 It can be seen that the separation flux does not change monotonically with the electroless nickel plating time. At 5 min of plating, the nickel particles are scattered and have not yet formed a continuous hydrophilic conductive layer, but they have already partially occupied the channels, increasing the resistance to aqueous phase transport. At 10 min of plating, a better balance is reached between the continuous hydrophilic nickel layer and the open channels, resulting in the highest flux. Further extending the plating time leads to channel contraction and increased aqueous phase transport resistance, causing the flux to decrease. Therefore, 10 min is the optimal electroless nickel plating time.
[0141] PP-PDA-Ni (10) The membrane underwent 20 consecutive cycles of hexane / water mixture filtration and washing. The flux during these 20 cycles was 2264.9 L·m⁻¹. -2 ·h -1 ~2492.4 L·m -2 ·h -1 The flux of the 20th cycle was approximately 2279.0 L·m. -2 ·h -1 The oil rejection rate was consistently above 99%, indicating that the nickel-based conductive layer and asymmetric wetting structure have good operational stability.
[0142] Experiment 4) Water-in-oil emulsion separation performance At 0.5 g·L-1 SDS was used as a surfactant. A mixture was prepared with water and n-hexane at a volume ratio of 80:20, and stirred at high speed for 6 hours to obtain an SDS-stabilized oil-in-water emulsion. PP-PDA-Ni (10) The membrane is installed at an effective membrane area of 1.81 cm². 2 In the dead-end filtration device, the first side faces the feed, and the second side faces the permeate side and is connected to the negative terminal of the DC power supply; the platinum sheet is connected to the positive terminal of the DC power supply, and the distance between the membrane and the platinum sheet is 0.2 cm. Before filtration, the membrane is pre-wetted with deionized water for 20 min.
[0143] The oil content in the feed emulsion and filtrate was determined at 507 nm using a UV-Vis spectrophotometer, and the oil rejection rate R was calculated according to formula (3): (3) In the formula, c is the oil concentration in the filtrate, in mg. mL -1 ; c 0 represents the oil concentration in the feed emulsion, in mg. mL -1 .
[0144] Representative results under different applied voltages are detailed in Table 2.
[0145] Table 2 Effect of applied voltage on the separation performance of n-hexane oil-in-water emulsions
[0146] Combine Table 2 and Figure 6 It is evident that the flux at 9 V is approximately three times that at 0 V, and the oil rejection rate increases from 94.5% to 98.3%. The applied electric field makes the membrane act as a cathode, electrostatically repelling negatively charged oil droplets and reducing oil droplet accumulation and pore blockage on the membrane surface. When the voltage increases to 12 V, microbubbles appear near the electrodes, adhering to and occupying part of the transport channels, causing a decrease in flux. Therefore, under the electrode spacing and emulsion system of this embodiment, 9 V is the optimal voltage.
[0147] Experiment 5) Applicability of oil phase volume fraction and oil type Oil-in-water emulsions of n-hexane with oil phase volumes of 15%, 20%, 25%, and 30% were tested under conditions of a conductive Janus membrane as the cathode and an applied voltage of 9 V. The flux was 356.7 L·m⁻¹ when the oil phase volume fraction was 15%. -2 ·h -1 The oil rejection rate was 99.3%; the fluxes were approximately 275.9 L·m³ when the oil phase volume fraction was 20%, 25%, and 30%, respectively. -2 ·h -1 254.6 L·m-2 ·h -1 and 200.0 L·m -2 ·h -1 The oil retention rate was higher than 98%.
[0148] Under the conditions of 9 V voltage and 15% oil phase volume fraction, further tests were conducted on oil-in-water emulsions of n-hexadecane, gasoline, n-hexane, and petroleum ether. The results are detailed in Table 3.
[0149] Table 3. Separation performance of oil-in-water emulsions of different oil products
[0150] The flux differences of different oil emulsions are related to the oil phase viscosity, interfacial tension, and the interaction between oil droplets and the membrane surface. Hexadecane has a higher viscosity and greater transport resistance; petroleum ether has a lower viscosity and achieves higher flux. All four oils maintain high oil rejection rates, indicating that the conductive Janus membrane in this embodiment has good applicability to different oil emulsions.
[0151] Experiment 6) Acid and alkali resistance and cyclic separation stability PP-PDA-Ni (10) The membranes were treated in solutions with pH values of 3, 5, 7, 9, and 11 for 24 h, and the initial water contact angles on both sides were measured. Since the water contact angle changes significantly over time, this acid and alkali resistance stability test employed an independent experimental series, using untreated PP-PDA-Ni membranes from the same batch. (10) The membrane was used as an internal control; the apparent water contact angle of each sample was recorded 1 second after water droplet addition for comparison, and the results are detailed in Table 4.
[0152] Table 4 Initial water contact angles across the conductive Janus membrane after different pH treatments
[0153] Combine Table 4 and Figure 7 It can be seen that after treatment with a solution of pH=3~11, the nickel-plated side still retains hydrophilicity, while the first side retains hydrophobicity, indicating that the asymmetric wetting structure of the conductive Janus film has good acid and alkali resistance.
[0154] See Figure 8 It can be seen that, under a voltage of 9 V, the four types of oil-in-water emulsions were subjected to 8 cycles of filtration and ethanol washing. The flux of the n-hexane emulsion was 307.0 L·m⁻¹. -2 ·h -1 ~359.8 L·m -2 ·h -1 The oil retention rate was 98.4%–99.5%; the gasoline emulsion flux was 178.2 L·m³. -2 ·h-1 ~195.0 L·m -2 ·h -1 The oil rejection rate was 99.3%–99.9%; the petroleum ether emulsion flux was 412.7 L·m⁻¹. -2 ·h -1 ~485.1 L·m -2 ·h -1 The oil rejection rate was 99.0%–99.8%; the hexadecane emulsion flux was 80.7 L·m⁻¹. -2 ·h -1 ~88.2 L·m -2 ·h -1 The oil rejection rate was 97.5%–98.6%. These results demonstrate that the conductive Janus membrane can maintain stable flux and oil rejection performance during multiple cycles of different oil emulsions.
[0155] Experiment 6) Conductivity Test The surface resistance of the membrane was tested using a digital multimeter. Before testing, the membrane was dried at 60°C and laid flat on an insulating plate. Two probes were placed parallel to each other on the membrane surface with a probe spacing of 1 cm. Three different locations were selected for testing for each sample, and the average value was taken. The upper limit of the instrument's range was 20 MΩ; values exceeding this range were considered over-range.
[0156] Tests revealed that neither the original PP film nor the PP-PDA Janus film without chemical nickel plating were conductive on either side, and their surface resistance exceeded the test range.
[0157] After electroless nickel plating, the surface resistivity of the nickel-plated side of the conductive Janus film decreased significantly, particularly in PP-PDA-Ni films. (10) The average surface resistance of the nickel-plated side of the film is 2.6 Ω when the probe spacing is 1 cm, indicating that the nickel particles grown with silver activation sites as nucleation sites have been interconnected and formed a continuous conductive network on the surface of the polydopamine adhesion layer. This nickel-based conductive layer can meet the requirements of applying a DC electric field as a cathode.
[0158] Meanwhile, the surface resistance of the unmodified side of each conductive Janus film still exceeded the test range, comparable to that of the original PP film. This indicates that the electroless nickel plating reaction was confined to the side facing the liquid phase and did not extend along the film thickness direction to the first side facing the gas phase. This resulted in an asymmetric conductive structure with one side conductive and the other side insulating. Figure 2 The differences in appearance between the two sides corroborate each other.
[0159] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.
Claims
1. A conductive Janus film, characterized in that, It includes a polypropylene porous base film, a polydopamine adhesion layer, and a nickel-based conductive layer, which are sequentially stacked along the thickness direction of the conductive Janus film. The polydopamine adhesive layer has silver activation sites distributed on the side of its surface opposite to the polypropylene porous base film, and the nickel-based conductive layer is bonded to the surface of the polydopamine adhesive layer through the silver activation sites.
2. The conductive Janus film as described in claim 1, characterized in that, The silver activation sites include silver particles distributed on the polydopamine adhesion layer; And / or, the nickel-based conductive layer comprises nickel particles nucleated at the silver activation sites, and the nickel particles are interconnected to form the nickel-based conductive layer; Optionally, the nominal pore size of the polypropylene porous base membrane is 0.22 μm.
3. The conductive Janus film as described in claim 1, characterized in that, The conductive Janus film has a first side and a second side disposed opposite to each other along its thickness direction. The surface of the polypropylene porous base film facing away from the polydopamine adhesion layer is formed as the first side of the conductive Janus film, and the surface of the nickel-based conductive layer facing away from the polydopamine adhesion layer is formed as the second side of the conductive Janus film. The conductive Janus film has asymmetric wettability on two sides, and the second side is conductive.
4. The conductive Janus film as described in claim 3, characterized in that, The initial water contact angle of the first side of the conductive Janus membrane is not less than 125°; And / or, the initial water contact angle of the second side of the conductive Janus membrane is not higher than 30°, and the underwater oil contact angle of the second side when n-hexane is used as the test oil droplet is 150°~155°; Optionally, under filtration conditions, the conductive Janus membrane allows oily wastewater to be directionally transported from the first side to the second side.
5. A method for preparing a conductive Janus film according to any one of claims 1 to 4, characterized in that, Includes the following steps: A porous polypropylene membrane is obtained, having a first surface and a second surface along its thickness direction. The ultrasonically cleaned polypropylene porous membrane is floated at the gas-liquid interface of a dopamine solution. The first surface of the polypropylene porous membrane faces the gas phase, and the second surface of the polypropylene porous membrane faces the liquid phase and reacts with the dopamine solution to form a polydopamine adhesion layer on the second surface, thus obtaining a PP-PDA Janus membrane. The PP-PDA Janus membrane is floated at the gas-liquid interface of the silver salt solution, with the first surface of the polypropylene porous base membrane facing the gas phase and the surface of the polydopamine adhesion layer facing away from the polypropylene porous base membrane facing the liquid phase and reacting with the silver salt solution to form silver activation sites on the surface of the polydopamine adhesion layer. The PP-PDA Janus film with the silver activation sites is floated at the gas-liquid interface of the electroless nickel plating solution. The first surface of the polypropylene porous base film faces the gas phase, and the surface of the polydopamine adhesion layer with the silver activation sites faces the liquid phase and is in contact with the electroless nickel plating solution. Using the silver activation sites as nucleation sites, a nickel-based conductive layer is formed on the polydopamine adhesion layer to obtain the conductive Janus film.
6. The method for preparing the conductive Janus film as described in claim 5, characterized in that, The concentration of dopamine hydrochloride in the dopamine solution is 2 mg mL -1 The pH of the dopamine solution is 8.
5. Optionally, the polypropylene porous base membrane floats at the gas-liquid interface of the dopamine solution and reacts with the dopamine solution for 6 hours; Optionally, the concentration of the silver salt solution is 1.5 g L -1 ; The silver salt solution may be selected as a silver nitrate solution; Optionally, the surface of the polydopamine adhesion layer facing away from the polypropylene porous base membrane is oriented towards the liquid phase and reacts with the silver salt solution for 30 minutes; Optionally, each liter of the electroless nickel plating solution comprises 25 g of nickel sulfate hexahydrate, 50 g of sodium pyrophosphate decahydrate, 40 mL of ammonia solution with a mass fraction of 28%, and 1.5 g of dimethylaminoborane. Optionally, the surface of the polydopamine adhesion layer with the silver activation sites is oriented towards the liquid phase and reacts with the electroless nickel plating solution at 35°C for 5 min to 20 min, preferably 10 min.
7. An electric field-assisted emulsion separation system, characterized in that, It includes a filter assembly, a DC power supply, a cathode, and an anode spaced apart from the cathode; wherein the cathode is a conductive Janus membrane according to any one of claims 1 to 4 or a conductive Janus membrane prepared by the preparation method according to any one of claims 5 to 6; The nickel-based conductive layer of the conductive Janus film is electrically connected to the negative terminal of the DC power supply, and the anode is electrically connected to the positive terminal of the DC power supply. The filtration assembly includes a filter cup and a filtrate receiver vertically joined together. The filter cup has a through-chamber for holding the oil-containing emulsion to be separated. The anode is immersed in the oil-containing emulsion. The top of the filtrate receiver is open, and the lower opening of the filter cup is opposite to the top opening of the filtrate receiver. A conductive Janus membrane is clamped and assembled between the mating end faces of the lower opening of the filter cup and the top opening of the filtrate receiver. The side of the polypropylene porous base membrane of the conductive Janus membrane facing away from the polydopamine adhesion layer faces the oil-containing emulsion feed side, and the nickel-based conductive layer of the conductive Janus membrane faces the permeation side.
8. The electric field-assisted emulsion separation system as described in claim 7, characterized in that, The distance between the anode and the cathode is 0.2 cm; Optionally, the voltage applied by the DC power supply is greater than 0 V and not higher than 12 V, preferably 9 V; Optionally, the anode is a platinum sheet electrode.
9. A method for separating oil-in-water emulsions, characterized in that, The separation method is based on the electric field-assisted emulsion separation system according to claim 7 or 8; the oil-in-water emulsion is an anionic surfactant-stabilized oil-in-water emulsion, and the separation method includes the following steps: The conductive Janus membrane is clamped and assembled between the mating end face of the lower opening of the filter cup and the upper opening of the filtrate receiver; The anode is placed inside the filter cup, and the oil-in-water emulsion to be separated is added to the filter cup and the anode is submerged. The conductive Janus membrane is used as the cathode and a DC electric field is applied. Under the action of gravity and the capillary driving force formed by the difference in wettability on both sides of the conductive Janus membrane, the continuous aqueous phase permeates from the side of the polypropylene porous base membrane away from the polydopamine adhesion layer to the nickel-based conductive layer side of the conductive Janus membrane. The electrostatic repulsion of negatively charged emulsified oil droplets by the cathode is used to suppress the enrichment, adhesion and blockage of the membrane pores of the emulsified oil droplets on the surface of the conductive Janus membrane. Optionally, the anionic surfactant is sodium dodecyl sulfate, and the concentration of the anionic surfactant is 0.5 g L -1 ; Optionally, the volume fraction of the oil phase in the oil-in-water emulsion is 15% to 30%. Optionally, the oil phase includes at least one of n-hexane, petroleum ether, n-hexadecane, and gasoline.
10. The application of the conductive Janus membrane according to any one of claims 1 to 4, or the conductive Janus membrane prepared by the preparation method according to any one of claims 5 to 6, or the electric field-assisted emulsion separation system according to claim 7 or 8, in the treatment of oily wastewater.